A preparation method of sodium bis(oxalato)borate

Sodium bioxalic acid borate was prepared by solid phase synthesis and over-column adsorption purification methods, which solved the problem of poor stability of sodium ion battery electrolyte materials, and achieved high purity, high yield and excellent battery circulation performance.

CN116425787BActive Publication Date: 2025-07-25QUZHOU JIUZHOU CHEM IND CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310410521.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-18
Publication Date
2025-07-25
Estimated Expiration
2043-04-18

AI Technical Summary

Technical Problem

The existing sodium ion battery electrolyte materials are sensitive to trace amounts of moisture, resulting in poor stability and poor battery circulation performance, making it difficult to meet the usage requirements.

Method used

Sodium bisoxalic acid borate was prepared by solid-phase synthesis method combined with systolic crystallization and thermal crystallization, and metal ion impurities were removed by column adsorption purification, and purified by fluoropropylene/carboxypolystyrene microsphere resin adsorbent.

Benefits of technology

The synthesis and purification time is significantly shortened, and the purity and yield of sodium bioxalate borate is improved. The prepared electrolyte shows better cycling performance than commercial electrolytes at low magnifications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004183006200000011
    Figure HDA0004183006200000011
Patent Text Reader

Abstract

The present invention relates to the field of fine chemicals, and specifically relates to a preparation method of sodium bis(oxalato)borate; the present invention uses a sodium source, boric acid, and oxalic acid as raw materials, and synthesizes sodium bis(oxalato)borate by a solid-phase method, and uses a method combining antisolvent crystallization and thermal crystallization to purify sodium bis(oxalato)borate. The present invention has the advantages of high yield and rapid purification process; the present invention uses a solid-phase synthesis method combined with a purification method, which can greatly shorten the synthesis and purification time; the sodium bis(oxalato)borate prepared by the present invention has high purity, high yield, and high conductivity, and can be used as an electrolyte for batteries; the electrolyte prepared from the sodium bis(oxalato)borate prepared by the present invention has better cycling performance at low rates than commercial electrolytes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of fine chemicals, and particularly to a method for preparing sodium bis(oxalato)borate. Background Art

[0002] For a long time, mankind has been troubled by resource shortages and energy depletion. Researchers have been committed to developing new types of green energy. Among various energy sources, solar energy, bioenergy, and wind energy have received extensive attention. However, these new energy sources are restricted by time and seasons and are not easy to store, thus limiting the development of these new energy sources. In addition, with the emergence of various portable electronic devices, there are higher requirements for miniaturized, high-energy-density, and lightweight energy sources. The emergence of lithium-ion batteries meets this demand.

[0003] Compared with lithium resources, sodium reserves are very abundant, with a crustal abundance of about 2.64%, and there is also a large amount of sodium in seawater. At the same time, sodium and lithium are elements in the same main group, with similar chemical properties, and the recycling of sodium is more mature and inexpensive. Replacing lithium with sodium to develop sodium-ion secondary batteries has broad application prospects.

[0004] CN201910686922.5: discloses a method for synthesizing sodium bis(oxalato)borate. According to the stoichiometric ratio of each element in sodium bis(oxalato)borate, a certain amount of boric acid, oxalic acid, and sodium compounds are dried at high temperature, then mixed, pressed into tablets, and subjected to a solid-solid reaction at high temperature to obtain a white solid. Then, the white solid is thoroughly dried and extracted in a non-aqueous solvent. Finally, the extraction solution is evaporated and crystallized to obtain the final product sodium bis(oxalato)borate. The reaction conversion rate of the process route provided by the present invention is high, the yield is up to more than 70%, the reaction time is short, the reaction conditions are simple and easy to operate, and it is easy to realize industrial production.

[0005] CN201210440894.7: relates to a method for preparing a negative electrode material and a negative electrode of a sodium-ion battery and a sodium-ion battery. The negative electrode material of the sodium-ion battery is prepared by a high-temperature solid-phase method by reacting Na2S, elemental niobium, and elemental sulfur in one step to obtain a sulfide negative electrode material without impurity phases. Since NaxNbS2 (0≤x≤1) compounds will be formed during the electrochemical charge and discharge process of NbS2, and the reversible reduction and oxidation of the Nb4+ / Nb3+ electrode pair, the prepared sodium-ion negative electrode material has a high charge and discharge capacity and good cycle performance. Furthermore, the prepared sodium-ion battery negative electrode and sodium-ion battery have a high charge and discharge capacity and good cycle performance. In addition, the process of the present invention is simple and easy to operate, has high production efficiency, high product yield and high purity; there is no need to use an organic solvent as an extraction agent, and the production line required for preparation is compatible with the existing liquid lithium-ion battery production line, and the existing production line can be directly used.

[0006] CN201510076973.8: It relates to battery technology, specifically a solid-state sodium battery electrolyte and its preparation and application. The electrolyte is a carbonate polymer, a sodium salt, and a porous support material; its thickness is 20 - 600 μm; the ionic conductivity is 1×10 -5 S / cm - 1×10 -3 S / cm; the electrochemical window is greater than 3.6V. The preparation is to dissolve the carbonate polymer and the sodium salt in a solvent in a certain proportion, form a film on the porous support material, and then dry it under vacuum to obtain the solid polymer electrolyte material. The solid-state sodium battery assembled by the present invention has good rate performance and excellent long-cycle stability; no electrolyte is added, and the safety is high; the main material is a carbonate polymer, which is cheap and has low cost; and the preparation of the solid polymer electrolyte material is simple.

[0007] Currently, the sodium salts applied to sodium ion electrolyte materials are mainly sodium hexafluorophosphate and sodium perchlorate. Both of them have poor resistance to trace moisture. Therefore, although the electrolyte material has high ionic conductivity, its stability is poor, resulting in poor final cycle performance of the battery and not meeting the usage requirements. Summary of the Invention

[0008] The technical solutions adopted by the present invention to solve the above technical problems are as follows:

[0009] On the one hand, the present invention provides a preparation method of sodium bis(oxalato)borate, and its operation steps are as follows:

[0010] S1: Weigh 12 - 18 parts of boric acid and 25 - 40 parts of oxalic acid by weight, mix them at 50 - 70°C for 30 - 50 minutes, and refine them by passing through a column.

[0011] S2: Weigh 12 - 18 parts of sodium source and the mixed acid obtained in S1, and ball mill them in a ball mill.

[0012] S3: After ball milling, put it into a vacuum drying oven for drying.

[0013] S4: Put the dried mixture into a reactor, raise the temperature, and react.

[0014] S5: After the reaction ends, dry it under vacuum, add 100 - 150 parts of polar solvent, and raise the temperature to 50 - 70°C to dissolve it.

[0015] S6: Filter, add 100 - 150 parts of non-polar solvent to the filtrate, and stop adding the non-polar solvent when crystals start to precipitate.

[0016] S7: Add the obtained solution to a rotary evaporator, rotate and evaporate, remove the polar solvent, separate the obtained crystals from the solution, and after vacuum drying, obtain sodium bis(oxalato)borate.

[0017] In some embodiments, the sodium source is sodium oxalate, sodium acetate, sodium hydroxide or sodium carbonate.

[0018] In some embodiments, the ball milling time is 3 - 5 h.

[0019] In some embodiments, the vacuum degree of the vacuum drying is -0.06 to -0.1 Mpa, the temperature is 80 - 130 °C, and the time is 3 - 10 h.

[0020] In some embodiments, the reaction temperature is 70 - 100 °C, and the time is 4 - 7 h.

[0021] In some embodiments, the polar solvent is acetone, acetonitrile or toluene.

[0022] In some embodiments, the non-polar solvent is ethylene carbonate, propylene carbonate or dimethyl carbonate.

[0023] In some embodiments, the rotary evaporation temperature is 60 - 120 °C.

[0024] On the other hand, the present invention provides a method for purification by column adsorption, and the specific steps are as follows:

[0025] 50 - 100 parts of boric acid oxalic acid mixture are flowed into an adsorption column filled with a resin adsorbent accounting for 30 - 40% of the volume of the exchange column from bottom to top. The adsorption conditions are: the flow rate is 0.5 - 2 BV / h, the temperature is 40 - 50 °C. After passing through the column, the filtrate is further distilled under reduced pressure to remove xylene, and a high-purity boric acid oxalic acid mixture is obtained.

[0026] On the other hand, the present invention provides a preparation method of a resin adsorbent. Through an acylation reaction of carboxyl polystyrene microspheres with 2-fluoropropionyl chloride, fluoropropene / carboxyl polystyrene microspheres are obtained; then a thiol addition reaction is respectively carried out with 5,5'-divinyl-2,2'-bipyridine and sodium dimercaptosuccinate, and the product is treated with high-purity boric acid to obtain a resin adsorbent; metal ion impurities in the boric acid oxalic acid mixture can be removed.

[0027] The specific steps are as follows:

[0028] S1: By weight, 100 - 120 parts of carboxyl polystyrene microspheres are swollen in 1000 - 1500 parts of dichloroethane solution, then 20 - 40 parts of 2-fluoropropionyl chloride and 2 - 5 parts of aluminum trichloride are added, and the mixture is stirred and reacted at 30 - 50 °C for 100 - 200 min;

[0029] S2: Then add 30 - 40 parts of sodium dimercaptosuccinate, 5 - 8 parts of sodium methoxide, 0.05 - 0.4 part of 5,5 - divinyl - 2,2 - bipyridine, and stir and react at 50 - 60 °C for 50 - 100 min. Filter, wash with high - purity boric acid with a mass percentage concentration of 10 - 20%, wash with water, and dry to obtain the resin adsorbent.

[0030] Technical effects:

[0031] A preparation method of sodium bis(oxalato)borate of the present invention has the following remarkable effects compared with the prior art:

[0032] 1. The present invention adopts a solid - phase synthesis method combined with a purification method, which can greatly shorten the synthesis and purification time;

[0033] 2. The sodium bis(oxalato)borate prepared by the present invention has high purity, high yield, and high conductivity, and can be used as an electrolyte for batteries;

[0034] 3. The electrolyte prepared from the sodium bis(oxalato)borate of the present invention has better cycling performance at low rates than commercial electrolytes. Description of the drawings

[0035] Figure 1 It is the infrared spectrum diagram of the sodium bis(oxalato)borate prepared in Example 1. Detailed implementation manners

[0036] The following will clearly and completely describe the technical solutions in the embodiments of the present invention with reference to the accompanying drawings in the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all of the embodiments. All other embodiments obtained by those of ordinary skill in the art based on the embodiments of the present invention without creative efforts shall fall within the protection scope of the present invention.

[0037] The product purity and reaction yield in the specific implementation manners of the present invention are calculated by the following formulas:

[0038] 1. Purity: The purity of sodium bis(oxalato)borate = the mass of sodium bis(oxalato)borate in the mixture ÷ the mass of the mixture × 100%;

[0039] 2. Yield: The yield of sodium bis(oxalato)borate = the actual amount of sodium bis(oxalato)borate produced / the theoretical amount of sodium bis(oxalato)borate produced × 100%.

[0040] Example 1

[0041] A preparation method of sodium bis(oxalato)borate, and its operation steps are as follows:

[0042] S1: Weigh 12 g of boric acid and 25 g of oxalic acid, mix at 50 °C for 30 minutes, and carry out column purification;

[0043] S2: Weigh 12 g of the sodium source and the mixed acid obtained in S1, and put them into a ball mill for ball milling.

[0044] S3: After ball milling, put it into a vacuum drying oven for drying.

[0045] S4: Put the dried mixture into a reactor, raise the temperature and react.

[0046] S5: After the reaction ends, after vacuum drying, add 100 g of polar solvent, raise the temperature to 50 °C and dissolve.

[0047] S6: Filter, add 100 g of non-polar solvent to the filtrate, and stop adding the non-polar solvent when crystals start to precipitate.

[0048] S7: Add the obtained solution to a rotary evaporator, perform rotary evaporation, remove the polar solvent, separate the obtained crystals from the solution, and after vacuum drying, obtain sodium bis(oxalato)borate(III).

[0049] The sodium source described above is sodium oxalate.

[0050] The ball milling time described above is 3 h.

[0051] The vacuum degree of the vacuum drying described above is -0.06 Mpa, the temperature is 80 °C, and the time is 3 h.

[0052] The reaction temperature described above is 70 °C, and the time is 4 h.

[0053] The polar solvent described above is acetone.

[0054] The non-polar solvent described above is ethylene carbonate.

[0055] The rotary evaporation temperature described above is 60 °C.

[0056] For the purification by column adsorption described above, the method is as follows:

[0057] Flow 50 g of the boric acid oxalic acid mixture from bottom to top into an adsorption column filled with a resin adsorbent accounting for 30% of the volume of the exchange column. The adsorption conditions are: the flow rate is 0.5 BV / h, the temperature is 40 °C. After passing through the column, the filtrate is then subjected to vacuum distillation to remove xylene, and a high-purity boric acid oxalic acid mixture is obtained.

[0058] The preparation method of the resin adsorbent described above is as follows:

[0059] S1: Swell 100 g of carboxyl polystyrene microspheres in 1000 g of dichloroethane solution, then add 20 g of 2-fluoropropionyl chloride and 2 g of aluminum trichloride, and stir and react at 30 °C for 100 min.

[0060] S2: Then add 30 g of sodium dimercaptosuccinate, 5 g of sodium methoxide, 0.05 g of 5,5'-divinyl-2,2'-bipyridine, stir and react at 50 °C for 50 min, filter, wash with high-purity boric acid with a mass percentage concentration of 10%, wash with water, and dry to obtain the resin adsorbent.

[0061] After analysis and calculation: The product purity in this implementation scheme is 99.2%, and the reaction yield is 92.7%.

[0062] Example 2

[0063] A preparation method of sodium bis(oxalato)borate, and its operation steps are as follows:

[0064] S1: Weigh 14 g of boric acid and 30 g of oxalic acid, mix them at 55 °C for 35 minutes, and carry out column purification;

[0065] S2: Weigh 14 g of sodium source and the mixed acid obtained in S1, and put them into a ball mill for ball milling;

[0066] S3: After ball milling, put it into a vacuum drying oven for drying;

[0067] S4: Put the dried mixture into a reactor, raise the temperature, and react;

[0068] S5: After the reaction is completed, carry out vacuum drying, add 110 g of polar solvent, raise the temperature to 55 °C, and dissolve;

[0069] S6: Filter, add 110 g of non-polar solvent to the filtrate, and stop adding the non-polar solvent when crystals start to precipitate;

[0070] S7: Add the obtained solution to a rotary evaporator, carry out rotary evaporation, remove the polar solvent, separate the obtained crystals from the solution, and after vacuum drying, obtain sodium bis(oxalato)borate.

[0071] The sodium source described above is sodium acetate.

[0072] The ball milling time described above is 4 h.

[0073] The vacuum degree of the vacuum drying described above is -0.07 Mpa, the temperature is 100 °C, and the time is 5 h.

[0074] The reaction temperature described above is 80 °C, and the time is 5 h.

[0075] The polar solvent described above is acetone or acetonitrile or toluene.

[0076] The non-polar solvent described above is propylene carbonate.

[0077] The rotary evaporation temperature described above is 80 °C.

[0078] The method of column adsorption and purification described above is as follows:

[0079] 60 g of the boric acid - oxalic acid mixture is flowed from bottom to top into an adsorption column filled with a resin adsorbent accounting for 35% of the volume of the exchange column. The adsorption conditions are as follows: the flow rate is 1 BV / h, the temperature is 45 °C. After passing through the column, the filtrate is further subjected to vacuum distillation to remove xylene, and a high - purity boric acid - oxalic acid mixture is obtained.

[0080] The preparation method of the resin adsorbent is as follows:

[0081] S1: 105 g of carboxyl polystyrene microspheres are swollen in 1100 g of dichloroethane solution, then 25 g of 2 - fluoropropionyl chloride and 3 g of aluminum trichloride are added, and the mixture is stirred and reacted at 35 °C for 140 min;

[0082] S2: Then 34 g of sodium dimercaptosuccinate, 6 g of sodium methoxide, and 0.2 g of 5,5 - divinyl - 2,2 - bipyridine are added, and the mixture is stirred and reacted at 55 °C for 60 min, filtered, washed with high - purity boric acid with a mass percentage concentration of 15%, washed with water, and dried to obtain the resin adsorbent.

[0083] Through analysis and calculation: the product purity in this embodiment is 99.5%, and the reaction yield is 92.9%.

[0084] Example 3

[0085] A preparation method of sodium bis(oxalato)borate, and its operation steps are as follows:

[0086] S1: Weigh 16 g of boric acid and 35 g of oxalic acid, mix them at 65 °C for 45 minutes, and carry out column purification;

[0087] S2: Weigh 16 g of sodium source and the mixed acid obtained in S1, and put them into a ball mill for ball milling;

[0088] S3: After ball milling, put it into a vacuum drying oven for drying;

[0089] S4: Put the dried mixture into a reactor, raise the temperature, and react;

[0090] S5: After the reaction is completed, carry out vacuum drying, add 140 g of polar solvent, raise the temperature to 65 °C, and dissolve;

[0091] S6: Filter, add 140 g of non - polar solvent to the filtrate, and stop adding the non - polar solvent when crystals start to precipitate;

[0092] S7: Add the obtained solution to a rotary evaporator, carry out rotary evaporation, remove the polar solvent, then separate the obtained crystals from the solution, and after vacuum drying, sodium bis(oxalato)borate is obtained.

[0093] The sodium source is sodium hydroxide.

[0094] The ball milling time is 4 h.

[0095] The degree of vacuum for the vacuum drying is -0.09 Mpa, the temperature is 120 °C, and the time is 8 h.

[0096] The reaction temperature is 90 °C and the time is 6 h.

[0097] The polar solvent is acetonitrile.

[0098] The non-polar solvent is propylene carbonate.

[0099] The rotary evaporation temperature is 110 °C.

[0100] For the column adsorption and purification, the method is as follows:

[0101] 90 g of the boric acid oxalic acid mixture is flowed into an adsorption column filled with a resin adsorbent accounting for 35% of the volume of the exchange column from bottom to top. The adsorption conditions are: the flow rate is 1.5 BV / h, the temperature is 45 °C. After passing through the column, the filtrate is further subjected to vacuum distillation to remove xylene, and then a high-purity boric acid oxalic acid mixture is obtained.

[0102] The preparation method of the resin adsorbent is as follows:

[0103] S1: 115 g of carboxyl polystyrene microspheres are swollen in 1400 g of dichloroethane solution, then 35 g of 2-fluoropropionyl chloride and 4 g of aluminum trichloride are added, and the mixture is stirred and reacted at 45 °C for 180 min;

[0104] S2: Then 38 g of sodium dimercaptosuccinate, 7 g of sodium methoxide, and 0.3 g of 5,5'-divinyl-2,2'-bipyridine are added, and the mixture is stirred and reacted at 55 °C for 90 min, filtered, washed with high-purity boric acid with a mass percentage concentration of 15%, washed with water, and dried to obtain the resin adsorbent.

[0105] Through analysis and calculation: In this implementation, the product purity is 99.7% and the reaction yield is 93.6%.

[0106] Example 4

[0107] A preparation method of sodium bis(oxalato)borate, and its operation steps are as follows:

[0108] S1: Weigh 18 g of boric acid and 40 g of oxalic acid, mix them at 70 °C for 50 minutes, and carry out column purification;

[0109] S2: Weigh 18 g of sodium source and the mixed acid obtained in S1, and put them into a ball mill for ball milling;

[0110] S3: After ball milling, put it into a vacuum drying oven for drying;

[0111] S4: Put the dried mixture into a reactor, raise the temperature, and react;

[0112] S5: After the reaction is completed, it is dried under vacuum, 150 g of polar solvent is added, and the temperature is raised to 70 °C for dissolution;

[0113] S6: Filter, add 150 g of non-polar solvent to the filtrate, and stop adding the non-polar solvent when crystals start to precipitate;

[0114] S7: Add the obtained solution to a rotary evaporator, perform rotary evaporation, remove the polar solvent, separate the obtained crystals from the solution, and after vacuum drying, sodium bis(oxalato)borate is obtained.

[0115] The sodium source described above is sodium carbonate.

[0116] The ball milling time described above is 5 h.

[0117] The vacuum degree of the vacuum drying described above is -0.1 Mpa, the temperature is 130 °C, and the time is 10 h.

[0118] The reaction temperature described above is 100 °C, and the time is 7 h.

[0119] The polar solvent described above is toluene.

[0120] The non-polar solvent described above is dimethyl carbonate.

[0121] The rotary evaporation temperature described above is 120 °C.

[0122] For the column adsorption purification described above, the method is as follows:

[0123] Flow 100 g of boric acid oxalic acid mixture from bottom to top into an adsorption column filled with a resin adsorbent accounting for 40% of the volume of the exchange column. The adsorption conditions are: the flow rate is 2 BV / h, the temperature is 50 °C. After passing through the column, the filtrate is further distilled under reduced pressure to remove xylene, and a high-purity boric acid oxalic acid mixture is obtained.

[0124] The preparation method of the resin adsorbent described above is as follows:

[0125] S1: Swell 120 g of carboxyl polystyrene microspheres in 1500 g of dichloroethane solution, then add 40 g of 2-fluoropropionyl chloride and 5 g of aluminum trichloride, and stir and react at 50 °C for 200 min;

[0126] S2: Then add 40 g of sodium dimercaptosuccinate, 8 g of sodium methoxide, 0.4 g of 5,5'-divinyl-2,2'-bipyridine, stir and react at 60 °C for 100 min, filter, wash with high-purity boric acid with a mass percentage concentration of 20%, wash with water, and dry to obtain the resin adsorbent.

[0127] Through analysis and calculation: In this implementation plan, the product purity is 99.9%, and the reaction yield is 94.1%.

[0128] Comparative Example 1

[0129] A preparation method of sodium bis(oxalato)borate, and its operation steps are as follows:

[0130] S1: Weigh 12 g of boric acid and 25 g of oxalic acid, mix them at 50 °C for 30 minutes;

[0131] S2: Weigh 12 g of sodium source and the mixed acid obtained in S1, and put them into a ball mill for ball milling;

[0132] S3: After ball milling, put it into a vacuum drying oven for drying;

[0133] S4: Put the dried mixture into a reactor, raise the temperature and react;

[0134] S5: After the reaction is completed, carry out vacuum drying, add 100 g of polar solvent, raise the temperature to 50 °C and dissolve;

[0135] S6: Filter, add 100 g of non-polar solvent to the filtrate, and stop adding non-polar solvent when crystals start to precipitate;

[0136] S7: Add the obtained solution to a rotary evaporator, carry out rotary evaporation, after removing the polar solvent, separate the obtained crystals from the solution, and after vacuum drying, obtain sodium bis(oxalato)borate.

[0137] The sodium source described above is sodium oxalate.

[0138] The ball milling time described above is 3 h.

[0139] The vacuum degree of the vacuum drying described above is -0.06 Mpa, the temperature is 80 °C, and the time is 3 h.

[0140] The reaction temperature described above is 70 °C, and the time is 4 h.

[0141] The polar solvent described above is acetone.

[0142] The non-polar solvent described above is ethylene carbonate.

[0143] The rotary evaporation temperature described above is 60 °C.

[0144] Through analysis and calculation: In this implementation scheme, the product purity is 87.9%, and the reaction yield is 80.5%.

[0145] Comparative Example 2

[0146] A preparation method of sodium bis(oxalato)borate, and its operation steps are as follows:

[0147] S1: Weigh 12 g of boric acid and 25 g of oxalic acid, mix them at 50 °C for 30 minutes, and carry out column purification;

[0148] S2: Weigh 12 g of sodium source and the mixed acid obtained in S1, and put them into a ball mill for ball milling;

[0149] S3: After ball milling, it is placed in a vacuum drying oven for drying;

[0150] S4: The dried mixture is placed in a reactor, heated up, and reacted;

[0151] S5: After the reaction ends, after vacuum drying, 100 g of polar solvent is added, and the temperature is raised to 50 °C for dissolution;

[0152] S6: Filter, add 100 g of non-polar solvent to the filtrate, and stop adding the non-polar solvent when crystals start to precipitate;

[0153] S7: The obtained solution is added to a rotary evaporator, rotary evaporated, after removing the polar solvent, the obtained crystals are separated from the solution, and after vacuum drying, sodium bis(oxalato)borate is obtained.

[0154] The sodium source described above is sodium oxalate.

[0155] The ball milling time described above is 3 h.

[0156] The vacuum degree of the vacuum drying described above is -0.06 Mpa, the temperature is 80 °C, and the time is 3 h.

[0157] The reaction temperature described above is 70 °C, and the time is 4 h.

[0158] The polar solvent described above is acetone.

[0159] The non-polar solvent described above is ethylene carbonate.

[0160] The rotary evaporation temperature described above is 60 °C.

[0161] For the purification by column adsorption described above, the method is as follows:

[0162] 50 g of boric acid oxalic acid mixture is flowed from bottom to top into an adsorption column filled with a resin adsorbent accounting for 30% of the volume of the exchange column. The adsorption conditions are: the flow rate is 0.5 BV / h, the temperature is 40 °C. After passing through the column, the filtrate is further distilled under reduced pressure to remove xylene, and then a high-purity boric acid oxalic acid mixture is obtained.

[0163] The preparation method of the resin adsorbent described above is as follows:

[0164] S1: 100 g of carboxyl polystyrene microspheres are swollen in 1000 g of dichloroethane solution, then 2 g of aluminum trichloride is added, and the reaction is stirred at 30 °C for 100 min;

[0165] S2: Then 30 g of sodium dimercaptosuccinate, 5 g of sodium methoxide, 0.05 g of 5,5'-divinyl-2,2'-bipyridine are added, and the reaction is stirred at 50 °C for 50 min, filtered, washed with high-purity boric acid with a mass percentage concentration of 10%, washed with water, and dried to obtain the resin adsorbent.

[0166] After analysis and calculation: In this implementation scheme, the product purity is 90.3%, and the reaction yield is 84.7%.

[0167] Comparative Example 3

[0168] A preparation method of sodium bis(oxalato)borate, and its operation steps are as follows:

[0169] S1: Weigh 12 g of boric acid and 25 g of oxalic acid, mix them at 50 °C for 30 minutes, and then refine them by column chromatography;

[0170] S2: Weigh 12 g of sodium source and the mixed acid obtained in S1, and put them into a ball mill for ball milling;

[0171] S3: After ball milling, put it into a vacuum drying oven for drying;

[0172] S4: Put the dried mixture into a reactor, raise the temperature, and react;

[0173] S5: After the reaction is completed, carry out vacuum drying, add 100 g of polar solvent, raise the temperature to 50 °C, and dissolve;

[0174] S6: Filter, add 100 g of non-polar solvent to the filtrate, and stop adding non-polar solvent when crystals start to precipitate;

[0175] S7: Add the obtained solution to a rotary evaporator, carry out rotary evaporation, remove the polar solvent, separate the obtained crystals from the solution, and after vacuum drying, obtain sodium bis(oxalato)borate.

[0176] The sodium source described above is sodium oxalate.

[0177] The ball milling time described above is 3 h.

[0178] The vacuum degree of the vacuum drying described above is -0.06 Mpa, the temperature is 80 °C, and the time is 3 h.

[0179] The reaction temperature described above is 70 °C, and the time is 4 h.

[0180] The polar solvent described above is acetone.

[0181] The non-polar solvent described above is ethylene carbonate.

[0182] The rotary evaporation temperature described above is 60 °C.

[0183] The method of column adsorption and purification described above is as follows:

[0184] Let 50 g of boric acid and oxalic acid mixture flow from bottom to top into an adsorption column filled with a resin adsorbent accounting for 30% of the volume of the exchange column. The adsorption conditions are: the flow rate is 0.5 BV / h, the temperature is 40 °C. After passing through the column, the filtrate is further distilled under reduced pressure to remove xylene, and then a high-purity boric acid and oxalic acid mixture is obtained.

[0185] The preparation method of the resin adsorbent described above is as follows:

[0186] S1: Swell 100 g of carboxyl polystyrene microspheres in 1000 g of dichloroethane solution, then add 20 g of 2-fluoropropionyl chloride and 2 g of aluminum trichloride, and stir and react at 30 °C for 100 min;

[0187] S2: Then add 30 g of sodium dimercaptosuccinate and 5 g of sodium methoxide, stir and react at 50 °C for 50 min, filter, wash with high-purity boric acid with a mass percentage concentration of 10%, wash with water, and dry to obtain the resin adsorbent.

[0188] Through analysis and calculation: the product purity in this embodiment is 91.5%, and the reaction yield is 86.1%.

[0189] The above are only the preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent replacements, and improvements made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A preparation method of sodium bis(oxalato)borate, and its operation steps are as follows: S1: Weigh 12 - 18 parts by weight of boric acid, 25 - 40 parts of oxalic acid, mix them at 50 - 70 °C for 30 - 50 minutes, and carry out column purification. S2: Weigh 12 - 18 parts of sodium source and the mixed acid obtained in S1, and put them into a ball mill for ball milling. S3: After ball milling, put it into a vacuum drying oven for drying. S4: Put the dried mixture into a reactor, raise the temperature and react. S5: After the reaction ends, carry out vacuum drying, add 100 - 150 parts of polar solvent, raise the temperature to 50 - 70 °C and dissolve. S6: Filter, add 100 - 150 parts of non - polar solvent to the filtrate, and stop adding non - polar solvent when crystals start to precipitate. S7: Add the obtained solution into a rotary evaporator, carry out rotary evaporation, remove the polar solvent, separate the obtained crystals from the solution, and after vacuum drying, obtain sodium bis(oxalato)borate. The method of column purification is as follows: Let 50 - 100 parts of the boric acid - oxalic acid mixture flow from bottom to top into an adsorption column filled with a resin adsorbent accounting for 30 - 40% of the volume of the exchange column. The adsorption conditions are: the flow rate is 0.5 - 2 BV / h, the temperature is 40 - 50 °C. After passing through the column, the filtrate is further distilled under reduced pressure to remove xylene, and then the boric acid - oxalic acid mixture is obtained. The preparation method of the resin adsorbent is as follows: S1: Weigh 100 - 120 parts by weight of carboxyl polystyrene microspheres and swell them in 1000 - 1500 parts of dichloroethane solution. Then add 20 - 40 parts of 2 - fluoropropionyl chloride and 2 - 5 parts of aluminum trichloride, and stir and react at 30 - 50 °C for 100 - 200 min. S2: Then add 30 - 40 parts of sodium dimercaptosuccinate, 5 - 8 parts of sodium methoxide, 0.05 - 0.4 parts of 5,5 - divinyl - 2,2 - bipyridine, stir and react at 50 - 60 °C for 50 - 100 min, filter, wash with boric acid with a mass percentage concentration of 10 - 20%, wash with water, and dry to obtain the resin adsorbent.

2. The preparation method of sodium bis(oxalato)borate according to claim 1, wherein: The sodium source is sodium oxalate or sodium acetate or sodium carbonate.

3. A preparation method of sodium bis(oxalato)borate according to claim 1, characterized in that: The ball milling time is 3 - 5 h.

4. The preparation method of sodium bis(oxalato)borate according to claim 1, characterized in that: The vacuum degree of the vacuum drying is - 0.06~ - 0.1 Mpa, the temperature is 80 - 130 °C, and the time is 3 - 10 h.

5. The preparation method of sodium bis(oxalato)borate according to claim 1, characterized in that: The reaction temperature is 70 - 100 °C, and the time is 4 - 7 h.

6. The preparation method of sodium bis(oxalato)borate according to claim 1, wherein: The polar solvent is acetone or acetonitrile or toluene.

7. A preparation method of sodium bis(oxalato)borate according to claim 1, characterized in that: The non - polar solvent is ethylene carbonate or propylene carbonate or dimethyl carbonate.

8. A method for preparing sodium bis(oxalato)borate according to claim 1, characterized in that: The rotary evaporation temperature is 60 - 120 °C.

Citation Information

Patent Citations

  • Method for manufacturing sodion battery negative pole material and negative pole and sodion battery

    CN102916186B

  • A solid sodium battery electrolyte and its preparation and application

    CN105633468B

  • Synthesis method and application of sodium bis(oxalato)borate

    CN110305153A

  • Synthesis and purification process of sodium bis (oxalato) borate

    CN115557980A

  • Preparation method of sodium bis (oxalato) borate and obtained product

    CN115850312A