Resin composition, battery binder, battery electrode composite layer, electrolyte layer, battery sheet, battery, and method for manufacturing the resin composition.
By using a disulfide bond resin composition containing phosphorus and sulfur as a binder for batteries, the problem of reduced ionic conductivity caused by increasing the amount of binder added in the prior art is solved, and the battery achieves high-efficiency cycle characteristics and wide temperature range battery performance.
Patent Information
- Application Number
- CN202180072679.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-11-09
- Filing Date
- 2021-11-05
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2041-11-05
AI Technical Summary
Existing battery binders suffer from reduced ionic conductivity when the amount added is increased to improve material adhesion.
A resin composition containing phosphorus and sulfur as constituent elements and having disulfide bonds is used. The raw material compound is oxidized by an oxidant to form compound α, which is then mixed with a thermoplastic resin to serve as a binder for batteries.
It effectively suppresses the decrease in ion conductivity, improves the cycle characteristics and operating temperature range of the battery, enhances coating properties and uniformity, and has excellent heat resistance.
Smart Images

Figure QLYQS_1 
Figure BDA0004195874710000031 
Figure BDA0004195874710000131
Abstract
Description
Technical Field
[0001] This invention relates to a method for manufacturing a battery binder, a resin composition capable of suppressing the reduction of ion conductivity, a battery binder, a battery electrode composite layer, an electrolyte layer, a battery sheet, a battery, and a resin composition. Background Technology
[0002] All-solid-state batteries, such as all-solid-state lithium-ion batteries, typically consist of a positive electrode layer, a solid electrolyte layer (sometimes simply called the "electrolyte layer"), and a negative electrode layer. By including binders in these layers, the individual layers or their laminates can be sheeted.
[0003] Polymerization of PS4 on the surface of electrode active materials is disclosed in Non-Patent Documents 1 and 2. Furthermore, Non-Patent Document 3 discloses a chemical structural change in 70Li2S-30P2S5 caused by heat treatment.
[0004] Existing technical documents
[0005] Non-patent literature
[0006] Non-patent literature 1: Masato Sumita et al., “Possible Polymerization of PS4 at a Li3PS4 / FePO4 Interface with Reduction of the FePO4 Phase,” The Journal of Physical Chemistry C, April 24, 2017, Vol. 121, pp. 9698-9704.
[0007] Non-Patent Literature 2: Takashi Hakari et al., 10, “Structural and Electronic-State Changes of a Sulfide Solid Electrolyte during the Li Deinsertion-Insertion Processes”, Chemistry of Materials, May 3, 2017, Vol. 29, pp. 4768-4774.
[0008] Non-Patent Document 3: Yuichi Hasegawa, "Chemical Structure Analysis of Sulfide Solid Electrolyte 70Li2S-30P2S5", [Online], February 1, 2018, TORAY RESEA RCH CENTER Co., Ltd., [Searched July 9, 2019], URL link<URL:https: / / www.toray-research.co.jp / technical-info / trcnews / pdf / 201802-01.pdf> Summary of the Invention
[0009] As a binder, polyvinylidene fluoride (PVDF) or carboxymethyl cellulose (CMC) can be considered. However, such binders have a technical problem: if the amount added is increased to obtain adhesion between the materials constituting the layer (e.g., electrode composites), the ionic conductivity decreases.
[0010] One of the objectives of this invention is to provide a resin composition that can be used as a battery binder and can suppress the reduction of ionic conductivity.
[0011] The inventors conducted in-depth research and discovered that a resin composition containing a compound and a thermoplastic resin, wherein the compound contains phosphorus and sulfur as constituent elements and has disulfide bonds, can be used as an ion-conductive binder, thus completing the present invention.
[0012] According to the present invention, the following resin compositions, etc., can be provided.
[0013] 1. A resin composition comprising a compound and a thermoplastic resin, said compound comprising phosphorus and sulfur as constituent elements and having disulfide bonds.
[0014] 2. The resin composition as described in 1, wherein the compound is a compound obtained by oxidizing a raw material compound containing phosphorus and sulfur as constituent elements using an oxidizing agent.
[0015] 3. The resin composition as described in 1 or 2, wherein the compound comprises a disulfide bond formed by any one of the following reaction formulas (1) to (3).
[0016]
Chemistry 1
[0017]
[0018] (In the formula, X is a halogen. n is an integer.)
[0019] 4. The resin composition as described in 3, wherein X in the reaction formulas (1) to (3) is iodine (I), fluorine (F), chlorine (Cl) or bromine (Br).
[0020] 5. The resin composition according to any one of 1 to 4, wherein the compound has a peak in Raman spectrophotometry originating from a disulfide bond to which two phosphorus elements are bonded.
[0021] 6. The resin composition according to any one of 1 to 5, wherein the thermoplastic resin is selected from one or more of the group consisting of styrene-butadiene thermoplastic elastomers, cellulose ethers, carboxymethyl cellulose, fluorinated resins, polyethers, polyacrylonitrile, polyvinyl acetate, polymethyl methacrylate, polyphosphazene, polyvinylpyrrolidone, polyethylene oxide, polyacrylic acid and polyamide-imide resins.
[0022] 7. The resin composition according to any one of 1 to 6, wherein the compound comprises one or more constituent elements selected from the group consisting of lithium, sodium, magnesium and aluminum.
[0023] 8. The resin composition as described in any one of 1 to 7, further comprising a halogen.
[0024] 9. The resin composition as described in 8, wherein the halogen is iodine or bromine.
[0025] 10. A battery adhesive comprising the resin composition described in any one of 1 to 9.
[0026] 11. A battery electrode composite material layer or electrolyte layer comprising the battery binder described in 10.
[0027] 12. The battery electrode composite material layer or electrolyte layer as described in 11, further comprising a solid electrolyte other than the battery binder.
[0028] 13. A battery sheet comprising one or more layers selected from the group consisting of a battery electrode composite material layer and an electrolyte layer as described in 11 or 12.
[0029] 14. A battery comprising the resin composition described in any one of 1 to 9.
[0030] 15. A method for manufacturing a resin composition, comprising: adding an oxidizing agent to a raw material compound containing phosphorus and sulfur as constituent elements to oxidize the raw material compound; and mixing the compound obtained by the oxidation with a thermoplastic resin.
[0031] According to the present invention, a resin composition that can be used as a battery binder with ion conductivity can be provided. Attached Figure Description
[0032] Figure 1 The image shows the Raman spectrum of compound α obtained in Example 1. Detailed Implementation
[0033] The following describes in detail the resin composition, battery binder, battery electrode composite material layer, electrolyte layer, battery sheet, battery, and method for manufacturing the resin composition of the present invention.
[0034] In addition, in this specification, "x~y" refers to a numerical range of "above x and below y". The upper and lower limits of the numerical range can be combined arbitrarily.
[0035] Solutions obtained by combining two or more of the various solutions of the present invention described below are also solutions of the present invention.
[0036] 1. Resin composition
[0037] One embodiment of the present invention comprises a compound (hereinafter also referred to as "compound α") and a thermoplastic resin, said compound comprising phosphorus and sulfur as constituent elements and having disulfide bonds.
[0038] The above-mentioned resin composition can be widely used as an ion-conducting binder in various applications, primarily batteries.
[0039] <Compound α>
[0040] Compound α contains phosphorus and sulfur as constituent elements and has disulfide bonds.
[0041] In one embodiment, compound α exhibits a peak in Raman spectrophotometry originating from a disulfide bond with two phosphorus elements.
[0042] In one embodiment, it is possible to achieve a Raman shift of 425 cm⁻¹ in Raman spectrophotometry. -1 Above 500cm -1 The following, preferably 440cm -1 Above 490cm -1 The following, or more preferably, is 460cm -1 Above 480cm -1 The following range has a peak (hereinafter also referred to as "peak A"), and the Raman shift is 370 cm⁻¹. -1 Above and below 425cm -1 The preferred size is 380cm. -1 Above 423cm -1 The following, or more preferably, is 390cm -1 Above 420cm -1 The following range of peaks (hereinafter also referred to as "peak B") is used to identify compound α.
[0043] Alternatively, the presence of peak A can also be used to identify the presence of disulfide bonds (SS) in compound α of one embodiment of the present invention.
[0044] Peak A originates from a disulfide bond (SS) in compound α containing two phosphorus atoms. Peak B originates from PS4. 3- Symmetrical stretching of the PS bond in the unit (also known as the PS4 structure).
[0045] Raman spectrophotometric analysis of compound α was performed using the method described in the examples. At this point, it is crucial to treat compound α with toluene before measurement. This is to remove monomeric sulfur that may be mixed in with compound α. Monomeric sulfur has peaks at positions that may overlap with peak A. Therefore, by removing monomeric sulfur, peak A originating from compound α can be measured well. The toluene treatment was performed according to the procedure described in the examples.
[0046] In one embodiment of the present invention, compound α preferably comprises one or more elements selected from the group consisting of lithium, sodium, and magnesium as constitutive elements. In one embodiment, these constitutive elements are bonded to S in compound α via ionic bonds.
[0047] <Thermoplastic Resins>
[0048] The thermoplastic resin contained in the resin composition is not particularly limited.
[0049] In one embodiment, the thermoplastic resin is selected from one or more of the following groups: cellulose derivatives represented by styrene-butadiene thermoplastic elastomers (SBS), ethyl cellulose, carboxymethyl cellulose (CMC), fluorinated resins represented by polyvinylidene fluoride or polyvinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP), polyethers represented by polyethylene oxide (PEO), polypropylene oxide, polyacrylonitrile, polyvinyl acetate, polymethyl methacrylate, polyphosphazene, polyvinylpyrrolidone, polyacrylic acid, and polyamide-imide resins.
[0050] Examples of styrene-butadiene thermoplastic elastomers (SBS) include block copolymers of polystyrene forming hard segments and polybutadiene forming soft segments.
[0051] There is no particular limitation on the mass ratio of compound α in the resin composition to the thermoplastic resin.
[0052] In one embodiment, the mass ratio of compound α to thermoplastic resin in the resin composition (compound α: thermoplastic resin) is 99:1 to 1:99, 95:5 to 5:95, 90:10 to 10:90, 85:15 to 15:85, 80:20 to 20:80, 75:25 to 25:75, or 70:30 to 30:70.
[0053] <halogen>
[0054] In one embodiment, the resin composition further comprises a halogen (halogen-containing substance). The halogen may also be a halogen derived from an oxidant or the like used in the manufacture of compound α.
[0055] In one embodiment, the halogen is selected from one or more of the group consisting of iodine, fluorine, chlorine and bromine.
[0056] In one embodiment, the halogen is selected from one or more of the group consisting of iodine and bromine.
[0057] The form of the halogen is not particularly limited. For example, it can be a salt of one or more elements selected from the group consisting of lithium, sodium, magnesium, and aluminum, and a halogen; or one or more elements selected from the group consisting of halogen monomers. Examples of salts include LiI, NaI, MgI2, AlI3, LiBr, NaBr, MgBr2, and AlBr3. Among these, LiI and LiBr are preferred from the viewpoint of ionic conductivity. Examples of halogen monomers include iodine (I2), fluorine (F2), chlorine (Cl2), and bromine (Br2). Among these, iodine (I2) and bromine (Br2) are preferred from the viewpoint of reducing corrosion when remaining in the binder (A).
[0058] In one embodiment, by including halogens as the aforementioned salts in a battery binder (A), higher ionic conductivity can be achieved.
[0059] The content of halogenated substances (halogen monomers and halogen compounds) in the resin composition is not particularly limited. For example, from the viewpoint of the conductivity of ions that serve as carriers and the binding force of active substances or solid electrolytes, when the total mass of the resin composition is set as 100% by mass, it can be 50% by mass or less, 40% by mass or less, 30% by mass or less, 20% by mass or less, 15% by mass or less, 10% by mass or less, 8% by mass or less, 5% by mass or less, 3% by mass or less, 2% by mass or less, 1% by mass or less, 0.5% by mass or less, 0.1% by mass or less, 0.05% by mass or less, or 0.01% by mass or less.
[0060] There are no particular limitations on the content of compound α in the resin composition, the resin composition itself, and halogen-containing substances.
[0061] In one embodiment, 50% or more, 60% or more, 70% or more, 80% or more, 85% or more, 90% or more, 95% or more, 98% or more, 99% or more, 99.5% or more, 99.8% or more, 99.9% or more, or substantially 100% by mass of the resin composition is compound α and the resin composition, or is compound α, a thermoplastic resin, and a halogen-containing substance.
[0062] In addition, in the case of "substantially 100% by mass", unavoidable impurities may also be included.
[0063] 2. Battery adhesive
[0064] A battery adhesive (hereinafter referred to as battery adhesive (A)) according to one aspect of the present invention comprises the above-described resin composition.
[0065] In one embodiment, the battery adhesive (A) is composed of the above-described resin composition.
[0066] The battery binder (A) can be used in various types of batteries. Examples of batteries include rechargeable batteries such as lithium-ion batteries. Furthermore, the battery can be an all-solid-state battery. The "binder" can be incorporated into any element in such a battery, for example, one or more layers selected from the group consisting of battery electrode composite material layers and electrolyte layers, and exerts adhesive properties (also known as "adhesive force" or "adhesive strength") to maintain the integrity of the other components contained in that element (e.g., the layer) by bonding them together.
[0067] Existing battery electrode composite material layers (such as the positive or negative electrodes described later) are difficult to keep up with the expansion and contraction (volume change) of the electrode active materials during charging and discharging, which easily leads to capacity degradation and other problems. The electrolyte layer, which is close to the battery electrode composite material layer, may also be affected by the volume change of the battery electrode composite material layer, resulting in degradation and other problems. In contrast, by using a battery binder (A), the battery electrode composite material layer or electrolyte layer can absorb volume changes through the flexibility of the battery binder (A), thus preventing capacity degradation and other problems. As a result, the battery can exhibit excellent cycle characteristics. Furthermore, since the battery binder (A) itself has ionic conductivity, even if the amount of battery binder (A) added is increased to improve the adhesion between the constituent materials (e.g., electrode composite materials), the decrease in ionic conductivity can be suppressed, and the battery characteristics can be well utilized. Moreover, in one embodiment, since the battery binder (A) has superior heat resistance compared to conventional organic binders or polymeric solid electrolytes (e.g., polyethylene oxide), the operating temperature range of the battery can be expanded.
[0068] Furthermore, in the battery binder (A), the thermoplastic resin functions as a tackifier, thus improving coatability. For example, a coating liquid (slurry) obtained by adding the solvent described later to the battery binder (A) exhibits excellent coatability. Consequently, the uniformity of the coating film can also be improved.
[0069] Furthermore, in the battery binder (A), the ionic conductivity can be adjusted by selecting a thermoplastic resin. For example, by selecting a polymer electrolyte such as a polyethylene oxide composite containing an electrolyte salt as the thermoplastic resin, the ionic conductivity can be improved.
[0070] 3. Electrode composite material layer or electrolyte layer for batteries
[0071] One aspect of the present invention comprises a battery electrode composite material layer or electrolyte layer comprising the aforementioned battery binder (A).
[0072] In one embodiment, the battery binder (A) is unevenly or uniformly distributed (dispersed) within the battery electrode composite material layer or electrolyte layer. In another embodiment, the battery binder (A) is uniformly distributed (dispersed) within the layer, thereby better maintaining the integrity of the layer.
[0073] The electrode composite material layer or electrolyte layer for the battery preferably includes a solid electrolyte (hereinafter referred to as solid electrolyte (B)) other than the battery binder (A). Solid electrolyte (B) is not particularly limited; for example, oxide solid electrolytes and sulfide solid electrolytes can be used. Among these, sulfide solid electrolytes are preferred, and examples include those with a sulfide-germanium sulfide crystal structure, Li3PS4 crystal structure, Li4P2S6 crystal structure, and Li7P3S6 crystal structure. 11 Crystal structure, Li 4-x Ge 1-x P x S4 type sulfide crystalline lithium superionic conductor thio-LISICON Region II crystal structure, and Li 4-x Ge 1-x P x S4 type sulfide crystalline lithium superion conductors, similar to the thio-LISICON Region II type crystal structure (hereinafter sometimes referred to as RII type crystal structure), are sulfide solid electrolytes.
[0074] Examples of electrode composite material layers used in batteries include positive electrodes and negative electrodes.
[0075] When the electrode composite material layer for a battery is the positive electrode, the positive electrode can further include a positive electrode active material. The positive electrode active material is a material capable of lithium-ion insertion and extraction, and can be a material known in the battery field as a positive electrode active material.
[0076] Examples of positive electrode active materials include metal oxides and sulfides. Sulfides include metal sulfides and non-metal sulfides.
[0077] The metal oxide is, for example, a transition metal oxide. Specifically, V2O5, V6O 13 , LiCoO2, LiNiO2, LiMnO2, LiMn2O4, Li(Ni a Co b Mn c )O2 (where 0<a<1, 0<b<1, 0<c<1, a+b+c=1), LiNi 1-Y Co Y O2, LiCo 1-Y Mn Y O2, LiNi 1-Y Mn Y O2 (where 0≦Y<1), Li(Ni a Co b Mn c )O4 (0<a<2, 0<b<2, 0<c<2, a+b+c=2), LiMn 2-Z Ni Z O4, LiMn 2-Z Co Z O4 (where 0<Z<2), LiCoPO4, LiFePO4, CuO, Li(Ni a Co b Al c )O2 (where 0<a<1, 0<b<1, 0<c<1, a+b+c=1) and the like can be exemplified.
[0078] As the metal sulfide, lithium sulfide (Li2S), lithium polysulfide (Li2Sx, 1<x≦8), titanium sulfide (TiS2), molybdenum sulfide (MoS2), iron sulfide (FeS, FeS2), copper sulfide (CuS), nickel sulfide (Ni3S2) and the like can be exemplified.
[0079] In addition, as the metal oxide, bismuth oxide (Bi2O3), bismuth lead acid (Bi2Pb2O5) and the like can be exemplified.
[0080] As the non-metal sulfide, elemental sulfur, organic disulfide compound, carbon sulfide compound and the like can be exemplified.
[0081] Besides, niobium selenide (NbSe3), metallic indium, and sulfur can also be used as the positive electrode active material.
[0082] When the electrode composite material layer for a battery is a negative electrode, the negative electrode can further contain a negative electrode active material.
[0083] The negative electrode active material can be any of the materials commonly used in lithium-ion secondary batteries, such as: carbon materials like graphite, natural graphite, artificial graphite, hard carbon, and soft carbon; composite metal oxides like polyphenylene conductive polymers and lithium titanate; and compounds that form alloys with lithium, such as silicon, silicon alloys, silicon composite oxides, tin, and tin alloys. Preferably, the negative electrode active material includes one or more materials selected from the group consisting of Si (silicon, silicon alloys, silicon-graphite composites, silicon composite oxides, etc.) and Sn (tin, tin alloys).
[0084] One or both of the positive and negative electrodes may contain conductive additives. When the electronic conductivity of the active material is low, it is preferable to add conductive additives. This improves the rate performance of the battery.
[0085] Specific examples of conductive additives include carbon materials, substances containing at least one element selected from the group consisting of nickel, copper, aluminum, indium, silver, cobalt, magnesium, lithium, chromium, gold, ruthenium, platinum, beryllium, iridium, molybdenum, niobium, osmium, rhodium, tungsten, and zinc, more preferably carbon monomers with high conductivity, carbon materials other than carbon monomers; and metal monomers, mixtures, or compounds containing nickel, copper, silver, cobalt, magnesium, lithium, ruthenium, gold, platinum, niobium, osmium, or rhodium.
[0086] In addition, specific examples of carbon materials include Ketjen black, acetylene black, Denka black, thermal cracking carbon black, channel black, etc.; graphite, carbon fiber, activated carbon, etc. These can be used alone or in combination of two or more. Among them, acetylene black and Ketjen black, with their high electronic conductivity, are preferred.
[0087] The electrolyte layer can contain either a battery binder (A) or a solid electrolyte (B) other than the battery binder (A) as an arbitrary component.
[0088] The composition of the positive electrode is not particularly limited. For example, by mass ratio, it can be: positive electrode active material: solid electrolyte (B): battery binder (A): conductive additive = 50-99: 0-30: 1-30: 0-30.
[0089] The positive electrode may contain 30% or more by mass, 50% or more by mass, 80% or more by mass, 90% or more by mass, 95% or more by mass, 98% or more by mass, or 99% or more by mass of positive electrode active material, solid electrolyte (B), battery binder (A), and conductive additive.
[0090] The composition of the negative electrode is not particularly limited. For example, by mass ratio, it can be: negative electrode active material: solid electrolyte (B): battery binder (A): conductive additive = 40~99: 0~30: 1~30: 0~30.
[0091] The negative electrode may contain 30% or more by mass, 50% or more by mass, 80% or more by mass, 90% or more by mass, 95% or more by mass, 98% or more by mass, or 99% or more by mass of negative electrode active material, solid electrolyte (B), battery binder (A), and conductive additive.
[0092] The composition of the electrolyte layer is not particularly limited. For example, by mass ratio, it can be solid electrolyte (B): battery binder (A) = 99.9:0.1 to 0:100.
[0093] When the mass ratio of the solid electrolyte (B) is 0, the battery binder (A) can also function as a solid electrolyte.
[0094] The electrolyte layer may contain 30% or more by mass, 50% or more by mass, 80% or more by mass, 90% or more by mass, 95% or more by mass, 98% or more by mass, 99% or more by mass, or 99.9% or more by mass of solid electrolyte (B) and battery binder (A).
[0095] The method for forming a layer containing compound α and a thermoplastic resin, such as the method for forming the layers constituting the battery described above, is not particularly limited; for example, a coating method can be used. In the coating method, a coating liquid obtained by dissolving or dispersing the components contained in each layer in a solvent can be used. As the solvent contained in the coating liquid, chain-like, cyclic, or aromatic ethers (e.g., dimethyl ether, dibutyl ether, tetrahydrofuran, anisole, etc.), esters (e.g., ethyl acetate, ethyl propionate, etc.), alcohols (e.g., methanol, ethanol, etc.), amines (e.g., tributylamine, etc.), amides (e.g., N-methylformamide, etc.), lactams (e.g., N-methyl-2-pyrrolidone, etc.), hydrazine, acetonitrile, etc. can be used. After coating, the solvent is dried, thereby forming a layer (the dried coating film). From the viewpoint of easy drying of the solvent, anisole is preferred. The drying method is not particularly limited; for example, one or more methods selected from the group consisting of heating drying, air drying, and reduced pressure drying (including vacuum drying) can be used.
[0096] The component to which the coating solution is applied is not particularly limited. The formed layer can be used in the battery along with the component, or the formed layer can be peeled off from the component and used in the battery. In one embodiment, the coating solution for forming the positive electrode is applied to the positive electrode current collector. In one embodiment, the coating solution for forming the negative electrode is applied to the negative electrode current collector. In one embodiment, the coating solution for forming the electrolyte layer is applied to either the positive or negative electrode. In one embodiment, after the coating solution for forming the electrolyte layer is applied to an easily peelable component, the formed layer is peeled off from the easily peelable component and disposed between the positive and negative electrodes.
[0097] It is preferable to stamp the dried coating (layer). Stamping simply involves pressing and compressing the layer. For example, stamping can be performed to reduce the porosity of the layer. The stamping apparatus is not particularly limited; for example, a roller press or a uniaxial press can be used. The stamping temperature is not particularly limited; it can be around room temperature (23°C), or a lower or higher temperature relative to room temperature. By performing stamping, the battery binder (A) contained in the layer deforms appropriately according to its flexibility, promoting the formation of interfaces between the electrode composite materials contained in the layer. As a result, the battery characteristics are further improved.
[0098] Each layer can be stamped, or multiple layers (such as "battery sheet" as described later) can be pressed in the stacking direction to perform stamping.
[0099] 4. Battery sheet
[0100] One aspect of the present invention provides a battery sheet comprising one or more layers selected from the group consisting of an electrode composite material layer and an electrolyte layer. By including compound α and a thermoplastic resin or a battery adhesive (A) in the battery sheet, excellent flexibility is achieved, preventing breakage or peeling from the current collector.
[0101] 5. Battery
[0102] One aspect of the present invention comprises a battery containing the above-described resin composition.
[0103] In one embodiment, the battery is an all-solid-state battery.
[0104] In one embodiment, the all-solid-state battery comprises a stack comprising, in sequence, a positive current collector, a positive electrode, an electrolyte layer, a negative electrode, and a negative current collector. The current collector can be a plate-like or foil-like material made of copper, magnesium, stainless steel, titanium, iron, cobalt, nickel, zinc, aluminum, germanium, indium, lithium, or alloys thereof.
[0105] In the battery, it is preferable to select one or more layers from the group consisting of a positive electrode, an electrolyte layer and a negative electrode that contain the above-described resin composition.
[0106] The above description (and the embodiments described below) mainly focuses on the use of the resin composition of the present invention in batteries, but is not limited thereto. The resin composition of the present invention has excellent flexibility, ionic conductivity, and other properties, making it widely applicable to various applications.
[0107] 6. Methods for preparing compound α
[0108] The method for manufacturing compound α described above is not particularly limited.
[0109] In one embodiment, the method for producing compound α includes adding an oxidant to a raw material compound containing phosphorus and sulfur as constituent elements; and reacting the raw material compound with the oxidant.
[0110] By reacting the above-mentioned raw material compound with an oxidizing agent, compound α, as a product, can be obtained.
[0111] In one embodiment, compound α is a compound obtained by oxidizing a raw material compound containing phosphorus and sulfur as constituent elements using an oxidizing agent.
[0112] In one embodiment, the feedstock compound (hereinafter referred to as feedstock compound (C)) contains phosphorus and sulfur as constituent elements.
[0113] The raw material compound (C) preferably contains one or more elements selected from the group consisting of lithium, sodium, magnesium and aluminum as constituent elements.
[0114] As one embodiment, the starting compound (C) preferably contains a PS4 structure. Examples of starting compounds containing a PS4 structure include Li3PS4, Li4P2S7, Na3PS4, and Na4P2S7. Furthermore, the starting compound (C) may contain two or more PS4 structures, such as Li4P2S7 and Na4P2S7. In the case where the starting compound (C) contains two adjacent PS4 structures, these two PS4 structures may share one S atom.
[0115] Li3PS4 can be produced, for example, by reacting Li2S with P2S5 in the presence of a dispersion medium using a mechanochemical method (mechanical milling). Examples of dispersion media include n-heptane. The mechanochemical method can utilize, for example, a planetary ball mill.
[0116] In one embodiment, compound α can be produced by reacting Li₂S, P₂S₅ with an oxidant in the presence of a dispersion medium (e.g., n-heptane) using a mechanochemical method (mechanical grinding). Planetary ball mills, for example, can also be used in this mechanochemical method.
[0117] In the above explanation, Na2S can also be used instead of Li2S.
[0118] Examples of oxidizing agents include halogen monomers, oxygen or ozone, oxides (Fe₂O₃, MnO₂, Cu₂O, Ag₂O, etc.), oxyacid salts (chlorates, hypochlorites, iodates, bromates, chromates, permanganates, vanadates, bismuthates, etc.), peroxides (lithium peroxide, sodium peroxide, etc.), halide salts (AgI, CuI, PbI₂, AgBr, CuCl, etc.), cyanide salts (AgCN, etc.), thiocyanates (AgSCN, etc.), and sulfoxides (dimethyl sulfoxide, etc.). In one embodiment, from the viewpoint of improving ionic conductivity by utilizing the halide metal produced as a byproduct, the oxidizing agent is preferably a halogen monomer. The "halide metal" can be a salt of one or more elements selected from the group consisting of lithium, sodium, magnesium, and aluminum derived from the raw material compound (C) and a halogen (e.g., lithium halide if the raw material compound (C) contains lithium).
[0119] Examples of halogen monomers include iodine (I₂), fluorine (F₂), chlorine (Cl₂), and bromine (Br₂). From the viewpoint of obtaining higher ionic conductivity, iodine (I₂) and bromine (Br₂) are preferred halogen monomers.
[0120] As an oxidizing agent, it can be used alone or in combination with multiple agents.
[0121] In one embodiment, when the starting compound (C) is Li3PS4 and the oxidant is a halogen monomer (X2), the reactions shown in the following reaction formulas (1) to (3) are carried out. In one embodiment, compound α has a PSS chain (a chain formed by repeating units composed of PSS) (reaction formulas (1) and (2)). In one embodiment, the PSS chain of compound α forms a branch (reaction formula (3)). In one embodiment, two phosphorus elements and the disulfide bond that bonds these two phosphorus elements form a PSS chain.
[0122]
Chemistry 2
[0123]
[0124] (In the formula, X is a halogen. n is an integer.)
[0125] In one embodiment, compound α contains disulfide bonds formed by any one of reaction formulas (1) to (3).
[0126] In one embodiment, X in reaction formulas (1) to (3) is iodine (I), fluorine (F), chlorine (Cl) or bromine (Br).
[0127] In one embodiment, X in reaction formulas (1) to (3) is iodine (I).
[0128] The molar ratio of Li3PS4 to I2 used in the reaction (Li3PS4:I2) is not particularly limited, and can be, for example, 10:1 to 1:10, 5:1 to 1:5, 3:1 to 1:3, 2:1 to 1:2, 4:3 to 3:4, 5:4 to 4:5 or 8:7 to 7:8. Furthermore, relative to 100 moles of Li3PS4, the amount of I2 can be 0.1 moles or more, 0.2 moles or more, 0.5 moles or more, 0.7 moles or more, or 1 mole or more, or it can be less than 300 moles, less than 250 moles, less than 200 moles, less than 180 moles, less than 150 moles, less than 130 moles, less than 100 moles, less than 80 moles, less than 50 moles, less than 30 moles, less than 20 moles, less than 15 moles, less than 10 moles, less than 8 moles, less than 5 moles, less than 3 moles, or less than 2 moles. The higher the proportion of I2, the longer the PSS chain can be extended.
[0129] Furthermore, the above molar ratio is not limited to the reaction of Li3PS4 with I2; for example, it can also be applied to the reaction of PS containing a PS4 structure. m The reaction of a starting material compound (or the starting material of the starting material compound; for example, a combination of Li2S and P2S5, a combination of Na2S and P2S5, etc.) with a halogen monomer in a unit structure of (m = 3, 3.5, 4).
[0130] In the process of reacting the raw material compound (C) and the oxidant (reaction process), it is preferable to use one or more types of energy selected from the group consisting of physical energy, thermal energy and chemical energy to react the raw material compound (C) and the oxidant.
[0131] In the reaction process, it is preferable to use energy containing physical energy to react the raw material compound (C) and the oxidant. Physical energy can be supplied, for example, by using mechanochemical methods (mechanical grinding). Mechanochemical methods can use, for example, planetary ball mills.
[0132] In mechanochemical methods using planetary ball mills, there are no particular limitations on the processing conditions. For example, the rotation speed can be 100 rpm to 700 rpm, the processing time can be 1 hour to 100 hours, and the ball diameter can be 1 mm to 10 mm.
[0133] In the reaction process, it is preferable to react the raw material compound (C) and the oxidant in a liquid. In this case, the raw material compound (C) and the oxidant can react in the presence of a dispersion medium. From the viewpoint of improving the reactivity of mechanical energy, it is preferable to react the raw material compound (C) and the oxidant in the presence of a dispersion medium using a mechanochemical method (mechanical grinding).
[0134] Examples of dispersion media include, for example, aprotic liquids. Aprotic liquids are not particularly limited, and examples include: preferred chain or cyclic alkanes with 5 or more carbon atoms, such as n-heptane; aromatic hydrocarbons such as benzene, toluene, xylene, and anisole; chain or cyclic ethers such as dimethyl ether, dibutyl ether, and tetrahydrofuran; haloalkyl groups such as chloroform and dichloromethane; and esters such as ethyl propionate.
[0135] In one embodiment, when the raw material compound (C) and the oxidant are reacted in a liquid, one or both of the raw material compound (C) and the oxidant can be reacted in a state of being mixed with a solvent.
[0136] As a solvent, a solvent in the dispersion medium described above that can dissolve one or both of the raw material compound (C) and the oxidant can be used, such as anisole, dibutyl ether, etc.
[0137] In such a solution, one or more types of energy selected from the group consisting of physical energy, thermal energy, and chemical energy, such as stirring, grinding, and ultrasonic vibration, can be used to react the raw material compound (C) and the oxidant. For example, when using thermal energy, the solution can be heated. There is no particular limitation on the heating temperature; for example, it can be 40–200°C, 50–120°C, or 60–100°C.
[0138] In the reaction process, compound α can be generated by oxidizing the raw material compound (C) with an oxidant.
[0139] When compound α is generated by a reaction in a liquid, the liquid (dispersion medium or solvent) can be removed as needed. By removing the liquid, a solid (powder) of compound α can be obtained. There are no particular limitations on the method of liquid removal; for example, drying, solid-liquid separation, etc., or a combination of two or more of them, can be used.
[0140] In the case of solid-liquid separation, compound α can also be redeprecipitated. In this case, the liquid containing compound α can be added to a poor solvent (a solvent unsuitable for compound α) or a non-solvent (a solvent that does not dissolve compound α), and compound α can be recovered as a solid (solid phase). For example, a method of solid-liquid separation can be performed by adding an anisole solution containing compound α to n-heptane, which is a poor solvent. There are no particular limitations on the solid-liquid separation method; examples include evaporation, filtration, and centrifugation. Using solid-liquid separation can result in improved purity.
[0141] In one embodiment, LiI is generated as a byproduct along with the formation of compound α. This LiI may or may not be separated from compound α. As described above, by leaving LiI as a residue in the mixture, compound α can possess higher ionic conductivity.
[0142] Here, the crystal phase of LiI can be, for example, c-LiI (cubic) (ICSD 414244), h-LiI (hexagonal) (ICSD414242), etc. Generally, when a mechanochemical method (mechanical grinding) is used as a method to generate compound α, it is c-LiI (cubic), and when a method is used to carry out the reaction in a liquid (preferably in a solution), it is h-LiI (hexagonal).
[0143] Capable of being detected by powder X-ray diffraction or solid-state X-ray diffraction 7 Li-NMR measurements are used to determine which crystalline phase LiI belongs to. In solid-state... 7 In Li-NMR measurements, a peak originating from LiI (chemical shift -4.57 ppm) is identified as c-LiI, and a peak originating from LiI is identified as h-LiI when no peak originating from LiI is observed.
[0144] 7. Method for manufacturing resin composition
[0145] The method for manufacturing the resin composition of one aspect of the present invention is not particularly limited.
[0146] A method for manufacturing a resin composition according to one aspect of the present invention includes: adding an oxidizing agent to a raw material compound containing phosphorus and sulfur as constituent elements to oxidize the raw material compound; and mixing the compound obtained by said oxidation with a thermoplastic resin.
[0147] Thus, a resin composition according to one aspect of the present invention can be manufactured.
[0148] In one embodiment, a compound obtained by oxidation, a thermoplastic resin, and one or more components other than the compound α described in "3. Battery Electrode Composite Material Layer or Electrolyte Layer" (e.g., a solid electrolyte) are mixed. This allows the manufacture of a resin composition suitable for use as a battery electrode composite material layer or electrolyte layer.
[0149] Example
[0150] The following describes embodiments of the present invention, but the present invention is not limited to the following embodiments.
[0151] (Example 1)
[0152] (1) Manufacturing of Li3PS4 glass
[0153] Mechanochemical reaction (mechanical milling) using a planetary ball mill (Premium line PL-7) was carried out in the presence of a dispersion medium (n-heptane) under the following conditions: 1.379 g of Li₂S (manufactured by Furuchi Chemical Co., Ltd., 3N powder, 200 mesh) was reacted with 2.222 g of P₂S₅ (manufactured by Merck). The dispersion medium was then removed by drying to obtain Li₃PS₄ glass (powder).
[0154] [Conditions for mechanical grinding]
[0155] Sample mass: 3.6g
[0156] Form: Wet grinding (n-heptane: 11.7 mL)
[0157] Ball: Material: ZrO2, Diameter: 5mm, Total Weight: 106g
[0158] Bottle: Made of ZrO2, capacity 80mL
[0159] Rotation: 500 rpm
[0160] Processing time: 20 hours
[0161] (2) Preparation of compound α
[0162] I2 (5N irregular grains (high purity chemical)) was pulverized in a mortar and then added to the Li3PS4 glass obtained in the above "(1) Manufacturing of Li3PS4 glass" in a molar ratio of Li3PS4:I2 = 1:1.
[0163] Next, Li3PS4 glass was reacted with I2 under the following conditions using a mechanochemical method (mechanical milling) with a planetary ball mill (Premium line PL-7). The dispersion medium (n-heptane) was then removed by drying to obtain compound α (powder).
[0164] [Conditions for mechanical grinding]
[0165] Sample mass: 1g
[0166] Form: Wet grinding (n-heptane: 3 mL)
[0167] Ball: Material: ZrO2, Diameter: 5mm, Total Weight: 53g
[0168] Bottle: Made of ZrO2, capacity 45mL
[0169] Rotation: 500 rpm
[0170] Processing time: 20 hours
[0171] (3) Raman spectrophotometry
[0172] After the compound α (powder) obtained in “(2) Manufacturing of compound α” was subjected to the following toluene treatment, micro Raman spectrophotometry was performed using a laser Raman spectrophotometer (NRS-3100 manufactured by Nippon Spectroscopy Co., Ltd.).
[0173] [Toluene processing flow]
[0174] a. Collect 1g of compound α into a vial, add 10mL of toluene (manufactured by Fujifilm and Koichi Chemical Co., Ltd., ultra-dehydrated), stir and let stand.
[0175] b. After removing the supernatant, add 10 mL of toluene to the solid component (precipitate), stir and let stand.
[0176] c. Repeat step b above once.
[0177] d. After removing the supernatant, the solid component (precipitate) was dried under vacuum at 60°C for 10 hours to obtain compound α treated with toluene.
[0178] exist Figure 1 The image shows the Raman spectra obtained by micro-Raman spectrophotometry. A Raman shift of 475 cm⁻¹ was confirmed for the disulfide (SS) bond originating from the PSS chain. -1 Nearby peaks.
[0179] (4) Preparation of coating solution
[0180] Prepare a coating solution with the following composition.
[0181] [Composition of the coating solution]
[0182] Li3PS4 solid electrolyte (Li3PS4 glass obtained in “(1) Manufacturing of Li3PS4 glass” above): 95 parts by weight
[0183] Compound α (powder): 3.5 parts by weight
[0184] Styrene-butadiene thermoplastic elastomer (SBS) (JSR Corporation "TR2000"): 1.5 parts by weight
[0185] Anisole: 81 parts by mass relative to the total amount of the above 3 components (solid components) per 100 parts by mass.
[0186] Specifically, first, SBS is dissolved in anisole to prepare a 20% by mass SBS solution. Then, 0.06g of the SBS solution and 0.400mL of anisole are added to 0.028g of compound α (powder) and allowed to dissolve.
[0187] Then, 0.76 g of Li3PS4 solid electrolyte was added to the solution, and kneaded under the following kneading conditions using a planetary stirring degassing device (MAZERUSTAR KK-250S manufactured by Kurashiki Textile Co., Ltd.).
[0188] [Kneading Conditions]
[0189] Rotation speed: 1600 rpm
[0190] Revolution: 1600rpm
[0191] Processing time: 180 seconds × 3
[0192] Next, the sample was treated with an ultrasonic cleaner for 5 minutes, and then kneaded again under the same kneading conditions as above.
[0193] Next, 0.2 mL of anisole was added to the sample, and kneading was performed under the same kneading conditions as described above to obtain a slurry-like resin composition (slurry solids concentration 55% by mass).
[0194] (5) Manufacturing of battery sheet
[0195] The coating solution obtained in “(4) Preparation of Coating Solution” above is applied to a 5cm×10cm aluminum foil to form a coating film. Then, the coating film is dried at 60°C for 10 hours to remove the solvent (anisole) and produce a solid electrolyte sheet (battery sheet).
[0196] (6) Measurement of ionic conductivity
[0197] The solid electrolyte sheet obtained in “(5) Manufacturing of Battery Sheet” above, together with aluminum foil, is punched into a circular plate shape, placed in a cylindrical container, and clamped by cylindrical SUS shafts inserted from both ends of the container, thereby being punched at room temperature (23°C) under a pressure of 333 MPa. The thickness of the solid electrolyte sheet obtained by punching is shown in Table 1.
[0198] While maintaining the stamping state, the ionic conductivity was measured by connecting a wire to the solid electrolyte sheet. The measurement was performed using a Solartron Analytical Cell test system 1470E. The ionic conductivity calculated based on the thickness of the stamped solid electrolyte sheet is shown in Table 1.
[0199] (7) Evaluation of Adhesion 1
[0200] The solid electrolyte sheet obtained in “(5) Manufacturing of battery sheet” above is punched together with aluminum foil into a circular plate shape, and wound on a cylinder with a diameter of 16 mm. The solid electrolyte sheet is visually observed for breakage or peeling from the aluminum foil, and the adhesion is evaluated according to the following evaluation criteria 1.
[0201] [Evaluation Criteria]
[0202] A: No breakage or peeling of the solid electrolyte sheet from the aluminum foil was observed during either the punching or winding process into the cylinder.
[0203] B: During punching or winding into a cylinder, breakage or peeling of the solid electrolyte sheet from the aluminum foil was observed.
[0204] (8) Evaluation of Adhesion Strength 2
[0205] After applying adhesive tape to the surface of the solid electrolyte sheet obtained by the above-mentioned "(5) Manufacturing of battery sheet", peel off the tape and visually observe whether the solid electrolyte sheet is peeled off from the aluminum foil. The adhesion strength 2 is evaluated according to the following evaluation criteria.
[0206] [Evaluation Criteria]
[0207] AA: Neither peeling of the solid electrolyte sheet from the aluminum foil nor intralayer peeling of the solid electrolyte sheet was observed.
[0208] A: Although no solid electrolyte sheet was observed to peel off from the aluminum foil glass, intralayer peeling of the solid electrolyte sheet was observed.
[0209] B: Solid electrolyte sheet was observed peeling off from aluminum foil.
[0210] (Example 2)
[0211] Except for changing the composition of the coating liquid to the following composition in Example 1, the operation is the same as in Example 1.
[0212] [Composition of the coating solution]
[0213] Li3PS4 solid electrolyte: 95 parts by weight
[0214] Compound α (powder): 2.5 parts by weight
[0215] Styrene-butadiene thermoplastic elastomer (SBS): 2.5 parts by weight
[0216] Anisole: 85 parts by mass relative to the total amount of the above 3 components (solid components) per 100 parts by mass.
[0217] (Example 3)
[0218] Except for changing the composition of the coating liquid to the following composition in Example 1, the operation is the same as in Example 1.
[0219] [Composition of the coating solution]
[0220] Li3PS4 solid electrolyte: 95 parts by weight
[0221] Compound α (powder): 1.5 parts by weight
[0222] Styrene-butadiene thermoplastic elastomer (SBS): 3.5 parts by weight
[0223] Anisole: 89 parts by mass relative to the total amount of the above 3 components (solid components) per 100 parts by mass.
[0224] (Comparative Example 1)
[0225] Except for changing the composition of the coating liquid to the following composition in Example 1, the operation is the same as in Example 1.
[0226] [Composition of the coating solution]
[0227] Li3PS4 solid electrolyte: 95 parts by weight
[0228] Styrene-butadiene thermoplastic elastomer (SBS): 5.0 parts by weight
[0229] Anisole: 82 parts by mass relative to the total amount of the above two components (solid components) per 100 parts by mass.
[0230] (Comparative Example 2)
[0231] Except for changing the composition of the coating liquid to the following composition in Example 1, the same operation as (5) in Example 1 was attempted to produce a battery sheet, but the solid electrolyte sheet peeled off from the aluminum foil and the physical properties could not be evaluated.
[0232] [Composition of the coating solution]
[0233] Li3PS4 solid electrolyte: 100 parts by weight
[0234] Anisole: 99 parts by mass relative to 100 parts by mass of the above-mentioned Li3PS4 solid electrolyte (solid component).
[0235] (Comparative Example 3)
[0236] Except for changing the composition of the coating liquid to the following composition in Example 1, the operation is the same as in Example 1.
[0237] [Composition of the coating solution]
[0238] Li3PS4 solid electrolyte: 95 parts by weight
[0239] Compound α (powder): 5.0 parts by weight
[0240] Anisole: 87 parts by mass relative to the total amount of the above two components (solid components) per 100 parts by mass.
[0241] The results are shown in Table 1.
[0242] [Table 1]
[0243]
[0244] <Evaluation>
[0245] As shown in Table 1, by using a resin composition containing compound α and thermoplastic resin as a binder, it is possible to appropriately balance ionic conductivity and adhesive strength.
[0246] (Example 4)
[0247] (A) Manufacturing of sulfide-germanium ore type solid electrolytes
[0248] A precursor for a sulfide-germanium ore-type solid electrolyte was obtained by reacting 0.492 g of Li₂S (manufactured by Furuch Chemicals, 200 mesh 3N powder), 0.626 g of P₂S₅ (manufactured by Merck), and 0.382 g of LiCl (manufactured by Nacalai Tesque) under the following conditions using a mechanochemical method (mechanical grinding) with a planetary ball mill (P-7, manufactured by Furuch Chemicals).
[0249] [Conditions for mechanical grinding]
[0250] Sample mass: 1.5g
[0251] Form: Dry grinding
[0252] Sphere: Material: ZrO2, Diameter: 10mm, Total Weight: 32g
[0253] Bottle: Made of ZrO2, capacity 45mL
[0254] Rotation: 370 rpm
[0255] Processing time: 15 hours
[0256] The above mechanical grinding was performed twice to obtain approximately 2.6 g of precursor for the silver-germanium sulfide-type solid electrolyte. The precursor was placed in a quartz tube and heat-treated at 430°C for 8 hours under an argon atmosphere to produce the silver-germanium sulfide-type solid electrolyte.
[0257] After pulverizing the sulfogermanium ore-type solid electrolyte in a mortar, it was then micronized using a planetary ball mill (using the same apparatus as described above) under the following conditions to obtain the sulfogermanium ore-type solid electrolyte (powder). The micronization process was carried out in two stages.
[0258] [Conditions for micro-refinement processing]
[0259] Sample mass: 1.5g
[0260] Form: Wet grinding (toluene: 15.5 mL, isobutyronitrile: 3.9 mL)
[0261] Sphere: Material: ZrO2, Diameter: 0.5mm, Total Weight: 34g
[0262] Bottle: Made of ZrO2, capacity 45mL
[0263] Grinding conditions: 370 rpm for 30 minutes in stage 1.
[0264] In the second stage, the speed is 150 rpm for 1 hour.
[0265] (B) Fabrication of positive electrode composite material (positive electrode sheet)
[0266] (1) Coating the positive electrode active material with LiNbO3
[0267] Weigh 2g of LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (NMC, manufactured by MTI) was added, followed by 3 mL of LiNb(OEt)6 (Alfa Aesar, lithium ethoxyniobium, 99+% (metal substrate), 5% w / v ethanol solution). Then, 7 mL of ultra-dehydrated ethanol (Fujifilm and Koichi Chemical Co., Ltd.) was added. The resulting sample was ultrasonically cleaned for 30 minutes and dried at 40°C for 10 hours in an Ar atmosphere. Next, the sample was vacuum dried at 100°C for 1 hour. The dried sample was then placed in a desiccator with a relative humidity of approximately 40%–50% for a 10-hour hydrolysis reaction. Finally, the reacted sample was heat-treated at 350°C for 1 hour to obtain LiNi coated with LiNbO3. 1 / 3 Co 1 / 3 Mn 1 / 3 O2(LiNbO3-coated NMC). The LiNbO3 content in the obtained LiNbO3-coated NMC is 3% by mass.
[0268] (2) Preparation of adhesive solution
[0269] First, SBS was dissolved in anisole to prepare a 20% by mass SBS solution. 0.495 g of the SBS solution and 0.45 mL of anisole were added to 0.0396 g of compound α (powder) from Example 1 and allowed to dissolve.
[0270] (3) Fabrication of positive electrode sheet
[0271] LiNbO3-coated NMC, the sulfogermanium sulfide solid electrolyte (SE) obtained in (A) above, and acetylene black (AB) (manufactured by DENKA) were mixed at a mass ratio of LiNbO3-coated NMC:SE:AB = 85:15:1 (total mass 1g).
[0272] The binder solution was added to the obtained mixture. The composition after addition was LiNbO3-coated NMC:SE:compound α:SBS:AB = 85:15:4:1:1. The composition was kneaded to obtain a slurry (solids concentration 68% by mass). The obtained slurry was coated onto a 5×10cm Al foil to form a coating film. The coating film was dried at 60°C for 10 hours, and then vacuum dried at 160°C for 3 hours. The resulting sheet was punched to obtain a positive electrode sheet with a diameter of 9.9 mm.
[0273] Even when wound onto a cylinder with a diameter of 16 mm, the positive electrode sheet did not break or peel off from the Al foil. Furthermore, the positive electrode sheet can be readily cut using a punch.
[0274] (Example 5)
[0275] <The Fabrication of All-Solid-State Batteries>
[0276] A 100 mg sulfide-germanium ore-type solid electrolyte, prepared in the same manner as in Example 4(A), was placed in a cylindrical container with SUS shafts on both sides for pressing to form a solid electrolyte layer. Next, the positive electrode sheet obtained in Example 4 was placed in the cylindrical container, overlapping the solid electrolyte layer. Then, In foil and Li foil were sequentially placed on the side of the solid electrolyte layer opposite to the electrode sheet within the cylindrical container, and the layers were stacked by stamping to fabricate an all-solid-state battery (a single cell for testing). The single cell was secured using a special fixture, and AC impedance measurements were performed.
[0277] <AC Impedance Measurement>
[0278] The object obtained by securing the individual cells with a special clamp was charged to 3.6V at 0.1C. Then, AC impedance was measured using a Solartron 1470ECell Testsystem manufactured by Solartron Analytical, and a Cole-Cole diagram was obtained. The interfacial impedance was estimated to be 16Ω.
[0279] (Example 6)
[0280] The positive electrode sheet was prepared in the same manner as in Example 4, except that the amount of compound α was 0.0445 g, the amount of SBS solution was 0.0247 g, and the amount of anisole was 0.5 mL. Even when wound onto a cylinder with a diameter of 16 mm, the positive electrode sheet did not break or peel off from the Al foil. Furthermore, the positive electrode sheet could be readily cut using a punch.
[0281] In addition, the interfacial resistance was measured using the same positive electrode sheet as in Example 5, and the result was 15Ω.
[0282] (Comparative Example 4)
[0283] The positive electrode sheet was prepared in the same manner as in Example 4, except that SBS was not used and the amount of compound α was set to 0.0495 g and the amount of anisole to 0.5 mL. The positive electrode sheet did not break or peel off from the Al foil even when wound on a cylinder with a diameter of 16 mm. The positive electrode sheet could be punched using a punch, but peeling was observed at the punched end, indicating insufficient adhesion.
[0284] In addition, the interfacial resistance was measured using the same positive electrode sheet as in Example 5, and the result was 15Ω.
[0285] (Comparative Example 5)
[0286] The positive electrode sheet was prepared using the method described in Example 4, except that the SBS solution was 0.0495 g and the anisole was 0.4 mL, without the use of compound α. The positive electrode sheet did not break or peel off from the Al foil even when wound on a cylinder with a diameter of 16 mm. The positive electrode sheet could also be punched using a punch, but peeling was observed at the punched end, indicating insufficient adhesion.
[0287] In addition, the interfacial resistance was measured using the same positive electrode sheet as in Example 5, and the result was 34Ω.
[0288] As can be seen from Examples 4, 5, Comparative Examples 4 and 5, by using compound α and SBS together, it is possible to simultaneously improve the adhesion of the electrode composite material layer and reduce the interfacial resistance of the single cell.
[0289] (Example 7)
[0290] Fabrication of Solid Electrolyte Sheets Using a Composite Binder of Compound α and Cellulose Ethers
[0291] (1) Preparation of coating solution
[0292] Cellulose ether (ETHOCEL, manufactured by Nisshin Chemical Co., Ltd.) was dissolved in anisole to prepare a 20% by mass cellulose ether solution. 0.76g of Li3PS4 solid electrolyte and 0.7mL of anisole were added to 0.1g of this solution, and after stirring, 0.1g of anisole solution of compound α (20% by mass) was added and dissolved. Then, the mixture was kneaded under the following kneading conditions using a planetary stirring degassing apparatus (MAZERUSTARKK-250S, manufactured by Kurashiki Textile Co., Ltd.).
[0293] [Kneading Conditions]
[0294] Rotation speed: 1600 rpm
[0295] Revolution: 1600rpm
[0296] Processing time: 180 seconds × 3
[0297] After treating the kneaded sample with an ultrasonic cleaner for 5 minutes, knead it again under the same kneading conditions as described above.
[0298] Next, 0.2 mL of anisole was added to the sample, and kneading was performed under the same kneading conditions as described above to obtain a slurry-like resin composition (slurry solids concentration 48% by mass).
[0299] (2) Fabrication of solid electrolyte sheets
[0300] The coating solution obtained in (1) above was applied to a 5cm × 10cm aluminum foil to form a coating film. Then, the coating film was dried at 60°C for 10 hours to remove the solvent (anisole) and produce a solid electrolyte sheet.
[0301] The obtained solid electrolyte sheet did not break or peel off from the Al foil even when wound onto a cylinder with a diameter of 16 mm. This demonstrates that it functions well as a binder even when cellulose ether is used instead of SBS.
[0302] (Example 8)
[0303] Fabrication of solid electrolyte sheets using a composite binder of compound α and polyethylene oxide>
[0304] Polyethylene oxide (PEO) (manufactured by Sigma-Aldrich, "Poly(ethylene oxide) average Mv600,000") was dissolved in anisole to prepare a 5% by mass polyethylene oxide solution. 0.76 g of Li3PS4 solid electrolyte and 0.8 mL of anisole were added to 0.24 g of this solution, and after stirring, 0.14 g of anisole solution of compound α (concentration 20% by mass) was added and dissolved. A slurry-like resin composition (compound α:PEO = 70:30 "mass ratio") was prepared in the same manner as in Example 7, except that no additional anisole was added.
[0305] The resulting resin composition can also be used to produce solid electrolyte sheets in the same manner as in Example 7.
[0306] (Example 9)
[0307] Fabrication of solid electrolyte sheets using a composite binder of compound α and polyethylene oxide>
[0308] PEO was dissolved in anisole to prepare a 5% by mass polyethylene oxide solution. 0.76 g of Li3PS4 solid electrolyte and 0.6 mL of anisole were added to 0.04 g of this solution, and after stirring, 0.19 g of anisole solution of compound α (20% by mass) was added and dissolved. A slurry-like resin composition (compound α:PEO = 95:5 "mass ratio") was prepared in the same manner as in Example 7, except that no additional anisole was added.
[0309] The resulting resin composition can also be used to produce solid electrolyte sheets in the same manner as in Example 7.
[0310] As can be seen from Examples 8 and 9, the composite using PEO instead of SBS also functions as an adhesive.
[0311] In the foregoing, several embodiments and / or examples of the present invention have been described in detail. However, those skilled in the art can readily make various modifications to these embodiments and / or examples without substantially departing from the new insights and effects of the present invention. Therefore, these various modifications are included within the scope of the present invention.
[0312] All references to the literature recorded in this specification and the contents of the application which form the basis of the priority claim under the Paris Convention are incorporated herein by reference.
Claims
1. A battery electrode composite material layer or electrolyte layer, characterized in that, The battery comprises a battery binder and a sulfide solid electrolyte other than the battery binder. The battery binder comprises a resin composition, the resin composition comprising a compound, a thermoplastic resin, and a halogen. The compound comprises phosphorus and sulfur as constituent elements and has disulfide bonds, and contains a PS4 structure. The halogen is a salt of one or more elements selected from the group consisting of lithium, sodium, magnesium and aluminum, and halogen monomers; and one or more forms selected from the group consisting of halogen monomers.
2. The electrode composite material layer or electrolyte layer for batteries as described in claim 1, characterized in that, The compound is a compound obtained by oxidizing a raw material compound containing phosphorus and sulfur as constituent elements using an oxidizing agent.
3. The electrode composite material layer or electrolyte layer for batteries as described in claim 2, characterized in that, The raw material compound is a compound containing a PS4 structure.
4. The electrode composite material layer or electrolyte layer for batteries as described in claim 3, characterized in that, The raw material compound containing the PS4 structure is selected from one or more compounds selected from the group consisting of Li3PS4, Li4P2S7, Na3PS4 and Na4P2S7.
5. The electrode composite material layer or electrolyte layer for batteries as described in claim 3 or 4, characterized in that, The raw material compound containing the PS4 structure is Li3PS4.
6. The electrode composite material layer or electrolyte layer for batteries as described in claim 2 or 3, characterized in that, The oxidant is selected from one or more of the group consisting of halogen monomers, oxygen, ozone, oxides, oxyacid salts, peroxides and sulfoxides.
7. The electrode composite material layer or electrolyte layer for batteries as described in claim 1 or 2, characterized in that, The compound contains a disulfide bond formed by any one of the following reaction formulas (1) to (3), In the formula, X is a halogen and n is an integer.
8. The electrode composite material layer or electrolyte layer for batteries as described in claim 7, characterized in that, In the reaction formulas (1) to (3), X is iodine (I), fluorine (F), chlorine (Cl) or bromine (Br).
9. The electrode composite material layer or electrolyte layer for batteries as described in claim 7, characterized in that, X is iodine (I).
10. The electrode composite material layer or electrolyte layer for batteries as described in claim 1 or 2, characterized in that, The compound exhibits a peak in Raman spectrophotometry originating from a disulfide bond with two phosphorus elements.
11. The electrode composite material layer or electrolyte layer for batteries as described in claim 1 or 2, characterized in that, The compound has a peak in Raman spectroscopic analysis originating from the symmetric stretching of the P-S bond of the PS4 3- unit, i.e. the PS4 structure.
12. The electrode composite material layer or electrolyte layer for batteries as described in claim 1 or 2, characterized in that, The compound has a peak derived from a disulfide bond having 2 phosphorus elements bonded in Raman spectroscopic analysis, and has a peak derived from symmetric stretching of a P-S bond of a PS4 3- unit, i.e., a PS4 structure in Raman spectroscopic analysis.
13. The electrode composite material layer or electrolyte layer for batteries as described in claim 10, characterized in that, The compound has a Raman shift of 425 cm -1 The above 500 cm -1 The following ranges have peaks.
14. The electrode composite material layer or electrolyte layer for batteries as described in claim 11, characterized in that, The compound has a peak in the Raman shift 370 cm -1 above and less than 425 cm -1 in the Raman spectroscopic analysis.
15. The electrode composite material layer or electrolyte layer for batteries as described in claim 1 or 2, characterized in that, The thermoplastic resin is selected from one or more of the group consisting of styrene-butadiene thermoplastic elastomers, cellulose ethers, fluorinated resins, polyethers, polyvinyl acetate, polymethyl methacrylate, polyphosphazene, polyvinylpyrrolidone, polyethylene oxide, polyacrylic acid and polyamide-imide resins.
16. The electrode composite material layer or electrolyte layer for batteries as described in claim 1 or 2, characterized in that, The thermoplastic resin is a styrene-butadiene thermoplastic elastomer, cellulose ether, or polyethylene oxide.
17. The electrode composite material layer or electrolyte layer for batteries as described in claim 1 or 2, characterized in that, The compound contains one or more constituent elements selected from the group consisting of lithium, sodium and magnesium.
18. The electrode composite material layer or electrolyte layer for batteries as described in claim 1 or 2, characterized in that, The halogen monomer is iodine.
19. The electrode composite material layer or electrolyte layer for batteries as described in claim 1 or 2, characterized in that, The mass ratio of the compound to the thermoplastic resin in the resin composition, i.e., compound α: thermoplastic resin, is 99:1 to 1:
99.
20. The electrode composite material layer or electrolyte layer for batteries as described in claim 1 or 2, characterized in that, The mass ratio of the compound in the resin composition to the thermoplastic resin is 70:30 to 30:
70.
21. The electrode composite material layer or electrolyte layer for batteries as described in claim 1 or 2, characterized in that, The resin composition comprises more than 50% by mass of the compound, the thermoplastic resin, and the halogen.
22. A sheet for batteries, characterized in that, It comprises one or more layers selected from the group consisting of a battery electrode composite material layer or an electrolyte layer as described in any one of claims 1 to 21.
Citation Information
Patent Citations
Method for producing solid electrolyte
EP3598462A1
Solid electrolyte material including sulfide layer and oxide layer, and battery including the solid electrolyte material
US20180316057A1
Rubber composition with bismaleimides
US4803250A