Hemostatic powder, preparation method and preparation process of hemostatic material

By swelling the inner core and dissolving the outer shell structure of the hemostatic powder, combined with materials such as water-soluble polysaccharides and inorganic salt pore-causing dry powder, the safety and degradation problems of existing hemostatic material adhesives are solved, achieving rapid hemostasis and safe and residue-free effects. , promote wound healing.

CN116440314BActive Publication Date: 2024-10-18QINGDAO BIOTEMED BIOMATERIAL
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310421731.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-19
Publication Date
2024-10-18
Estimated Expiration
2043-04-19

AI Technical Summary

Technical Problem

The adhesives of existing hemostatic materials have poor biological safety, are easy to fall off and remain, and are not easily degraded and absorbed by the human body, posing risks of inflammation and toxicity.

Method used

It is a hemostatic powder with a structure of swelling inner core and dissolving outer shell. The swelling inner core is made of swollen chitosan, and the dissolving outer shell is made of water-soluble polysaccharide or water-soluble polysaccharide compounded with hydrosoluble additives. It utilizes the viscosity and swelling of water-soluble polysaccharide. The absorption effect of chitosan, combined with inorganic salt pore-forming dry powder and collagen fiber, can achieve rapid hemostasis and safe and residue-free effect.

Benefits of technology

The hemostatic powder achieves stable attachment to the wound surface, quickly stops bleeding, and can be safely degraded and absorbed by the body, reducing the risk of inflammation and toxicity, promoting wound healing, and avoiding scars and infection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004187086130000131
    Figure BDA0004187086130000131
  • Figure BDA0004187086130000141
    Figure BDA0004187086130000141
  • Figure BDA0004187086130000142
    Figure BDA0004187086130000142
Patent Text Reader

Abstract

The present application relates to the field of preparation of hemostatic materials, and specifically discloses a hemostatic powder, a preparation method and a preparation process of a hemostatic material; a hemostatic powder comprises the following raw materials in parts by weight: a swelling inner core and a dissolving outer shell; the swelling inner core is made of swelling chitosan; the dissolving outer shell is made of water-soluble polysaccharide or a water-soluble polysaccharide compounded with a water-soluble auxiliary agent; the preparation method is: chitosan particles are placed in a dilute acid solution for reaction, and then squeezed to obtain swelling chitosan; the swelling chitosan is frozen, and then placed in a dilute acid solution, and reacted to obtain a mixture; the mixture is post-treated, and a dissolving outer shell is formed on the outer surface of the swelling chitosan, and the inside of the swelling chitosan is a swelling inner core, so as to obtain the hemostatic powder; the surface of a non-woven fabric is atomized with water, and the hemostatic powder is evenly sprinkled on it, and the dissolving outer shell of the hemostatic powder is slightly dissolved and adhered to the surface of the medical non-woven fabric, and after post-treatment, a hemostatic material is obtained; it has the advantages of good hemostatic effect, safety, no residue, and easy degradation and absorption by the body.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of hemostatic material preparation, and more specifically, to a hemostatic powder, a preparation method and a preparation process of a hemostatic material. Background Art

[0002] Hemostatic materials are materials used to reduce or stop bleeding in humans or animals. Gauze hemostatic materials are the most commonly used in emergency hemostasis processes, especially in combat injuries, traffic accidents, engineering accidents, etc. Gauze hemostatic materials are often used to fill deep wounds to achieve a hemostatic effect.

[0003] The Chinese patent application document with publication number CN107007867A in the prior art discloses a hemostatic material, which includes a carrier layer and an adhesive layer. The adhesive layer is made of an adhesive substance, and the adhesive substance is a fusible material. The adhesive substance is adhered to the surface of the carrier layer by hot melting. However, the hot melt adhesive substance has poor biological safety. When the hemostatic material is used, the adhesive is easy to fall off and remain in the body after contacting blood. The hot melt adhesive substance is not only unable to be degraded and absorbed by the human body, but also easily produces risks such as foreign body residue, inflammation and toxicity.

[0004] Therefore, there is an urgent need to prepare a new hemostatic product that has the advantages of good hemostatic effect, safety, no residue, and easy degradation and absorption by the body. Summary of the invention

[0005] In order to prepare a hemostatic material that is safe, residue-free and easily degraded and absorbed by the body, the present application provides a hemostatic material and a processing method thereof.

[0006] In the first aspect, the present application provides a hemostatic powder, which adopts the following technical solution:

[0007] A hemostatic powder is made of the following raw materials in parts by weight: 65-95 parts of a swelling inner core and 5-35 parts of a dissolving outer shell;

[0008] The swelling core is made of swelling chitosan;

[0009] The dissolving shell is made of water-soluble polysaccharide or water-soluble polysaccharide combined with water-soluble auxiliary agent.

[0010] By adopting the above technical scheme, the hemostatic powder is prepared with two layers of a swelling inner core and a dissolving outer shell. When the hemostatic powder is sprinkled on the wound, the dissolving outer shell on the surface of the hemostatic powder gradually dissolves under the action of water in the plasma, so that the viscosity of the water-soluble polysaccharide increases, which makes it easier for the hemostatic powder to stably adhere to the wound surface and not fall off from the wound surface. The viscosity of the dissolved water-soluble polysaccharide makes it easier for the swelling chitosan to adhere to the wound surface more stably. The absorption effect of the swelling chitosan on the overflowed plasma is utilized, and the sealing effect of the viscosity of the water-soluble polysaccharide on the wound surface is combined, so that the hemostatic powder has the effect of quickly stopping bleeding.

[0011] Both water-soluble polysaccharides and swellable chitosan are safe and harmless to the human body, and the water-soluble polysaccharides can be absorbed by the human body, so that the finished hemostatic powder has the advantages of good hemostatic effect, safety and no residue, and easy degradation and absorption by the body.

[0012] Preferably, the water-soluble polysaccharide is one or more of chitosan salt, carboxyalkyl chitosan, hydroxypropyl chitosan, hydroxyethyl chitosan, carboxyalkyl chitosan succinamide, carboxyalkyl chitin, chitosan quaternary ammonium salt, sodium alginate, carboxyalkyl cellulose, and sodium hyaluronate.

[0013] By adopting the above technical scheme, the hydrophilic groups such as carboxyl, hydroxyl, and amino groups on the surface of water-soluble polysaccharides are utilized to further improve the hydrophilicity of the hemostatic powder, thereby promoting the hemostatic powder to quickly absorb water in the blood, and then promoting the dissolution of the water-soluble polysaccharide. The dissolved water-soluble polysaccharide utilizes the high content of hydrophilic groups such as carboxyl, hydroxyl, and amino groups on its surface to further improve the viscosity of the water-soluble polysaccharide and improve the stability of the hemostatic powder attached to the wound; the hemostatic powder is relatively stably bonded to the wound, which can prevent the intact skin around the wound from being aggravated by the pulling force and thus affecting the wound healing; at the same time, the hemostatic powder prepared from the water-soluble polysaccharide can also promote tissue healing, prevent the excessive proliferation of fibroblasts, and has a good antibacterial and bactericidal effect, thereby accelerating wound repair and avoiding the formation of scars or infections at the wound as much as possible.

[0014] Preferably, the water-soluble additive is one or more of inorganic salt pore-forming dry powder, water-soluble fiber, oil agent, and foaming agent.

[0015] By adopting the above technical scheme, the inorganic salt porogenic dry powder can form microporous channels on the surface of the dissolving shell, and the foaming agent can make the dissolving shell have a more porous structure. When contacting with liquids such as plasma, the swelling chitosan can quickly absorb water through the microporous channels, preventing the dissolving shell from completely wrapping the swelling core and affecting the absorption of liquids such as plasma by the swelling core.

[0016] Inorganic salt porogenic dry powder and water-soluble fiber can increase the specific surface area of ​​the dissolving shell and improve the contact area between plasma and hemostatic powder, thereby promoting the rapid dissolution of the dissolving shell on the surface of the hemostatic powder. The viscosity of the dissolving shell can be used to make the hemostatic powder adhere to the wound quickly and stably. On the one hand, its antibacterial and bactericidal effects can be used to prevent wound infection and promote wound healing. On the other hand, its large specific surface area can be used to achieve the advantages of rapid hemostasis and good hemostatic effect with a small amount of hemostatic powder, thereby achieving better hemostatic effect and meeting the requirement of as small a loading volume as possible for military equipment.

[0017] Preferably, the hydrotrope consists of collagen fibers, carboxyalkyl chitosan succinamide fibers and sodium alginate fibers in a weight ratio of 1:0.1-0.5:0.2-0.6.

[0018] By adopting the above technical scheme, the hydrophilic effect of hydroxyl and carboxyl groups in collagen fibers, carboxyl and amide groups in carboxyalkyl chitosan succinamide fibers, and carboxyl groups in sodium alginate fibers is utilized to improve the hydrophilicity and water absorption of the dissolving shell on the surface of the hemostatic powder; when the hemostatic powder comes into contact with water in plasma or water in tissue fluid, the collagen fibers, carboxyl alkyl chitosan succinamide, and sodium alginate fibers are dissolved, and after dissolution, the hydroxyl, carboxyl, amide, etc. are easily cross-linked by forming hydrogen bonds, and the cross-linked structure can not only further improve the absorption of the hemostatic powder to plasma and tissue fluid, but also The cross-linked structure can directly contact the wound and use the water-soluble collagen to prevent scarring as much as possible. The dissolved carboxyalkyl chitosan succinamide and sodium alginate have antibacterial effects and can cross-link with proteins to form a cross-linked network, which prevents large molecular proteins and other substances in the plasma from continuously seeping out with the plasma, and promotes wound healing by retaining the protein content in the wound. However, the cross-linked network has no barrier to the seepage of water in the plasma, tissue fluid, etc., ensuring that the swelling core absorbs water in the tissue fluid and plasma, thereby playing a role in quickly stopping bleeding and promoting wound healing.

[0019] In a second aspect, the present application provides a method for preparing hemostatic powder, which adopts the following technical solution:

[0020] A method for preparing hemostatic powder comprises the following steps:

[0021] S1. Weigh chitosan particles and place them in a 0.5-5% dilute acid solution, with the volume ratio of the particle mass to the dilute acid solution being 1:8-12. React at 20-40°C for 2-12h, and then squeeze dry to obtain swollen chitosan.

[0022] S2, freezing the swollen chitosan at -40 to -20°C for 5 to 24 hours, placing it in a 5 to 15% dilute acid solution, with the volume ratio of the particle mass to the dilute acid solution being 1:6 to 10, and reacting it at 0 to 4°C for 0.5 to 5 hours to obtain a mixture;

[0023] S3. The mixture is squeezed, washed with ethanol, and dried, and the outer surface of the swellable chitosan forms a dissolved shell, and the inside of the swellable chitosan forms a swellable core, thereby obtaining a finished product.

[0024] By adopting the above technical solution, the outer layer of the swelling chitosan is transformed into the soluble chitosan by means of low-temperature reaction after freezing, so that the soluble outer shell can be quickly dissolved and the swollen inner core liquid is not affected.

[0025] A method for preparing hemostatic powder comprises the following steps:

[0026] S1, weigh chitosan particles and place them in a 0.5-5% dilute acid solution, with the particle mass and dilute acid solution volume ratio of 1:8-12, react at 20-40°C for 2-12h, and then squeeze dry to obtain swollen chitosan, i.e., swollen core;

[0027] S2, adding a hydrotrope to the water-soluble polysaccharide, the weight ratio of the water-soluble polysaccharide to the hydrotrope being 10-20:0.2-2, and mixing them evenly to obtain a mixed powder;

[0028] S3. The swellable chitosan is placed in an ethanol solution with a concentration of 20-30% and stirred evenly. Then, the mixed powder and the swellable chitosan are mixed evenly at a mass ratio of 1:0.5-2. After rolling, bonding and drying, the mixed powder forms a dissolved shell on the surface of the swellable inner core to obtain a finished product.

[0029] By adopting the above technical scheme, a large number of reserved pores are generated on the surface of the dissolving shell under the action of the inorganic salt pore-forming dry powder. When the hemostatic powder comes into contact with the liquid at the wound, the connection effect of the reserved pores is utilized to facilitate the liquid to be absorbed by the swelling chitosan, thereby preventing the dissolving shell from completely wrapping the swelling inner core after dissolution, causing the swelling inner core to be unable to absorb water.

[0030] An ethanol solution with a concentration of 20-30% is combined with water-soluble chitosan, and the water in the ethanol solution is used to dissolve the water-soluble chitosan, so that the water-soluble chitosan has appropriate viscosity, thereby facilitating the adhesion of the mixed powder and the swollen inner core, making the structure of the hemostatic powder relatively stable; and the ethanol solution is used to disperse the swollen inner core and the mixed powder, so that the mixed powder is more evenly and stably adhered to the surface of the swollen inner core, so that the dissolved outer shell on the surface of the prepared hemostatic powder evenly covers the swollen inner core.

[0031] Preferably, the powder mixture can also be prepared by the following method:

[0032] The water-soluble polysaccharide is weighed at a mass ratio of 1:10-15 and dispersed in a sodium bicarbonate solution for 5-10 minutes, and then microcrystalline cellulose and coagulated polysaccharide are added, the mass ratio of the water-soluble polysaccharide, microcrystalline cellulose and coagulated polysaccharide is 1:0.05-0.2:0.1-0.3, and then freeze-dried to obtain a mixed powder.

[0033] By adopting the above technical scheme, coagulated polysaccharide, sodium bicarbonate solution, microcrystalline cellulose and freeze drying are coordinated, and the adsorption effect of coagulated polysaccharide on sodium bicarbonate solution and the bonding effect on microcrystalline cellulose are utilized, so that the microcrystalline cellulose is bonded to the surface of coagulated polysaccharide, and freeze drying is coordinated to make the mixed powder contain more pores while retaining sodium bicarbonate without being decomposed; in the preparation process of hemostatic powder, as the hot pressing composite operation is carried out, the sodium bicarbonate in the inorganic salt porogenic dry powder coated on the surface of the swelling inner core is gradually decomposed by heat to produce gas, further improving the porosity of the dissolving outer shell, ensuring that the dissolving outer shell can be quickly dissolved in water after contacting blood and tissue fluid, and in the process of gradual swelling of the swelling outer shell, a circulation channel is provided for plasma, tissue fluid, etc., so that they are in contact with the swelling inner core, thereby ensuring the absorption and storage effect of the swelling inner core on liquids such as plasma and tissue fluid.

[0034] When plasma, tissue fluid, etc. seep out and come into contact with the dissolving outer shell, the hydrophilic but water-insoluble effect of the coagulated polysaccharide and microcrystalline cellulose makes it difficult for the dissolving outer layer to block the pores after dissolution and affect the adsorption of liquid by the swollen inner core. At the same time, the coagulated polysaccharide and microcrystalline cellulose expand after absorbing water, which makes it easier to adsorb more plasma, tissue fluid, etc. that overflow from the wound, thereby enhancing the hemostatic effect of the hemostatic powder.

[0035] A method for preparing hemostatic powder comprises the following steps:

[0036] S1, weigh chitosan particles and place them in a 0.5-5% dilute acid solution, react at 20-40°C for 2-12h, the volume ratio of the particle mass to the dilute acid solution is 1:8-12, then squeeze dry, wash and obtain swollen chitosan, i.e., swollen core;

[0037] S2, dissolving the water-soluble polysaccharide in purified water to prepare a solution with a concentration of 1-10%, adding an oil agent and a foaming agent to the solution, wherein the concentration of the oil agent is 0.1%-1%, and the concentration of the PVC foaming agent is 0.1-1%, to obtain a mixed solution; the oil agent is selected from one or more of glycerin, medical silicone oil, Tween, and vaseline;

[0038] S3. The mixed liquid is evenly sprayed onto the surface of the swollen chitosan. The volume of the sprayed mixed liquid is 5-20 times the mass of the swollen chitosan. After drying, the mixed liquid forms a dissolved shell to obtain a finished product.

[0039] By adopting the above technical scheme, water-soluble chitosan is prepared into a solution with a high concentration, and then an oil agent is added, such as glycerol, medical silicone oil, vaseline, Tween, etc., to promote water to penetrate the dissolved outer shell to conduct heat to the swollen inner core, thereby promoting the swollen inner core to absorb water; and a foaming agent is used to produce pore channels in the dissolved outer shell, thereby further promoting the swollen inner core to absorb liquid, and avoiding the dissolved outer shell covering the swollen inner core and affecting the swollen inner core's absorption of liquid.

[0040] A method for preparing hemostatic powder comprises the following steps:

[0041] S1, weigh chitosan particles and place them in a 0.5-5% dilute acid solution, react at 20-40°C for 2-12h, the volume ratio of the particle mass to the dilute acid solution is 1:8-12, then squeeze dry, wash and obtain swollen chitosan, i.e., swollen core;

[0042] S2. Spread the water-soluble polysaccharide fibers flat, and then squeeze the wet swollen chitosan onto the 0.5-1.5 cm long water-soluble polysaccharide fibers. The fibers are then rolled into a ball and dried to form a dissolved shell on the surface of the swollen inner core to obtain a finished product.

[0043] By adopting the above technical scheme, the water-soluble polysaccharide fibers are wrapped around the surface of the swollen inner core, so that the water-soluble polysaccharide fibers form a network coating structure, but the interwoven and stacked polysaccharide fibers still have a high porosity, thereby facilitating the liquid to pass through the dissolved outer shell and contact the swollen inner core, thereby ensuring the hemostatic powder's absorption effect on body fluids.

[0044] In a third aspect, the present application provides a preparation process of a hemostatic material, which adopts the following technical solution:

[0045] A preparation process of a hemostatic material comprises the following steps:

[0046] Use purified water or ethanol solution to atomize and wet the surface of the medical non-woven fabric, and then evenly sprinkle hemostatic powder on it. The dissolved shell of the hemostatic powder slightly dissolves and adheres to the surface of the medical non-woven fabric. After hot pressing, compounding, drying, folding and packaging, the finished product is obtained.

[0047] By adopting the above technical solution, after the surface of the non-woven fabric is atomized and moistened, the water-soluble chitosan on the outer layer of the hemostatic powder dissolves in water to produce adhesion, so that the hemostatic powder is more stably bonded to the surface of the non-woven fabric. Chitosan and other polysaccharides have good biosafety and can be degraded and absorbed by the body, and are not prone to foreign matter residue, inflammation, toxicity and other risks.

[0048] After the hemostatic material comes into contact with the water in the plasma and tissue fluid, it has high viscosity, which not only facilitates the stable attachment of the hemostatic material to the affected area, but also has the effect of promoting wound healing. Even if the water-soluble polysaccharide enters the body, it will not cause harm to the human body.

[0049] In summary, this application has the following beneficial effects:

[0050] 1. The hemostatic powder is made of two layers, namely, a swelling inner core and a dissolving outer shell. When the hemostatic powder is sprinkled on the wound, the dissolving outer shell on the surface of the hemostatic powder gradually dissolves under the action of water in the plasma, thereby increasing the viscosity of the water-soluble polysaccharide, making it easier for the hemostatic powder to stably adhere to the wound surface and not easily fall off the wound surface. The viscosity of the dissolved water-soluble polysaccharide makes it easier for the swelling chitosan to adhere to the wound surface more stably. The absorption effect of the swelling chitosan on the overflowed plasma is combined with the blocking effect of the viscosity of the water-soluble polysaccharide on the wound surface, so that the hemostatic powder has a rapid hemostatic effect.

[0051] 2. Inorganic salt porogenic dry powder and water-soluble fiber can increase the specific surface area of ​​the dissolving shell and improve the contact area between plasma and hemostatic powder, thereby promoting the rapid dissolution of the dissolving shell on the surface of the hemostatic powder. The viscosity of the dissolving shell can be used to make the hemostatic powder adhere to the wound quickly and stably. On the one hand, its antibacterial and bactericidal effects can be used to prevent wound infection and promote wound healing. On the other hand, its large specific surface area can be used to achieve the advantages of rapid hemostasis and good hemostatic effect with a small amount of hemostatic powder, thereby achieving better hemostatic effect and meeting the requirement of minimizing the loading volume of military equipment.

[0052] 3. Collagen fiber, carboxyalkyl chitosan succinamide fiber and sodium alginate fiber are matched. After dissolution, hydroxyl, carboxyl, amide and the like are easy to form hydrogen bonds and cross-link. The cross-linked structure can not only further improve the absorption of hemostatic powder to plasma and tissue fluid, but also the cross-linked structure can directly contact the wound, and the water-soluble collagen is used to prevent the wound from leaving scars as much as possible. The dissolved carboxyalkyl chitosan succinamide and sodium alginate have antibacterial effects, and can cross-link with proteins to form a cross-linked network, which prevents macromolecular proteins and other substances in plasma from constantly seeping out with the plasma, and promotes wound healing by retaining the protein content in the wound; however, the cross-linked network has no barrier to the seepage of water in plasma, tissue fluid, etc., ensuring the absorption of water in tissue fluid and plasma by the swollen inner core, thereby playing a role in rapid hemostasis and promoting wound healing. DETAILED DESCRIPTION

[0053] The present application is further described in detail below in conjunction with embodiments.

[0054] Example

[0055] Embodiment 1: A kind of hemostatic powder:

[0056] Contains 80kg of swelling inner core and 20kg of dissolving outer shell;

[0057] The preparation method is as follows:

[0058] S1. Weigh 1 kg of chitosan particles and place them in 10 kg of a 3% dilute acid solution, wherein the particle size of the chitosan particles is 20 meshes and the dilute acid solution is a dilute acetic acid aqueous solution. React at 30° C. for 8 hours and then squeeze dry to obtain a swollen chitosan.

[0059] S2, after freezing 1 kg of swollen chitosan at -30°C for 18 hours, placing it in 8 kg of a 10% dilute acid solution, wherein the dilute acid solution is a dilute acetic acid aqueous solution, reacting at 2°C for 3 hours to obtain a mixture;

[0060] S3. The mixture is squeezed dry, then washed three times with 90% ethanol, and finally dried to form a dissolving shell on the outer surface of the swellable chitosan, and a swellable core inside the swellable chitosan. The thickness of the dissolving shell is 0.3 mm, and the particle size of the swellable core is 0.5 mm, thereby obtaining a finished product.

[0061] Embodiment 2: This embodiment differs from Embodiment 1 in that:

[0062] 65kg of the inner core was swollen and 5kg of the outer shell was dissolved;

[0063] During the preparation process:

[0064] S1. Weigh 1 kg of chitosan particles and place them in 8 kg of 0.5% dilute acid solution, react at 20° C. for 12 hours, and then squeeze dry to obtain swollen chitosan;

[0065] S2, after freezing 1 kg of swollen chitosan at -40°C for 5 hours, placing it in 6 kg of a 5% dilute acid solution, wherein the dilute acid solution is a dilute acetic acid aqueous solution, reacting it at 0°C for 5 hours to obtain a mixture;

[0066] S3. The mixture is squeezed dry, then washed three times with 90% ethanol, and finally dried to form a dissolving shell on the outer surface of the swellable chitosan, and a swellable core inside the swellable chitosan. The thickness of the dissolving shell is 0.1 mm, and the particle size of the swellable core is 0.15 mm, thereby obtaining a finished product.

[0067] Embodiment 3: This embodiment differs from Embodiment 1 in that:

[0068] 95kg of the inner core was swollen and 35kg of the outer shell was dissolved;

[0069] During the preparation process:

[0070] S1. Weigh 1 kg of chitosan particles and place them in 12 kg of 5% dilute acid solution, react at 40°C for 2 hours, and then squeeze dry to obtain swollen chitosan;

[0071] S2, after freezing 1 kg of swollen chitosan at -20°C for 24 hours, placing it in 10 kg of a 15% dilute acid solution, wherein the dilute acid solution is a dilute acetic acid aqueous solution, reacting at 4°C for 0.5 hours to obtain a mixture;

[0072] S3. The mixture is squeezed dry, then washed three times with 90% ethanol, and finally dried to form a dissolving shell on the outer surface of the swellable chitosan, and a swellable core inside the swellable chitosan. The thickness of the dissolving shell is 0.5 mm, and the particle size of the swellable core is 1 mm, thereby obtaining a finished product.

[0073] Embodiment 4: This embodiment differs from Embodiment 1 in that:

[0074] The preparation method is as follows:

[0075] S1. Weigh 1 kg of chitosan particles and place them in 10 kg of a 3% dilute acid solution, where the particle size of the chitosan particles is 20 meshes, and the dilute acid solution is a dilute acetic acid aqueous solution. React at 30° C. for 8 hours, then squeeze dry to obtain a swollen chitosan, i.e., a swollen core;

[0076] S2, adding 1 kg of hydrotrope to 15 kg of water-soluble polysaccharide, the hydrotrope is an inorganic salt pore-forming dry powder, the particle size of the inorganic salt pore-forming dry powder is 80 mesh, and mixing them evenly to obtain a mixed powder; the water-soluble polysaccharide is hydroxyethyl chitosan;

[0077] S3. Place 1 kg of swellable chitosan in 0.1 kg of 25% ethanol solution and stir evenly, the ethanol solution is ethanol-water solution; then mix the mixed powder and swellable chitosan evenly at a mass ratio of 1:1, roll and bond, and then dry; repeat the above operation 3 times, the mixed powder forms a dissolved shell on the surface of the swellable inner core, and the finished product is obtained.

[0078] Embodiment 5: This embodiment differs from Embodiment 4 in that:

[0079] The preparation method is as follows:

[0080] S1. Weigh 1 kg of chitosan particles and place them in 8 kg of a 0.5% dilute acid solution, wherein the particle size of the chitosan particles is 20 meshes and the dilute acid solution is a dilute acetic acid aqueous solution. React at 20° C. for 12 hours and then squeeze dry to obtain a swollen chitosan, i.e., a swollen core.

[0081] S2, adding 0.2 kg of hydrotrope to 10 kg of water-soluble polysaccharide, the hydrotrope is an inorganic salt pore-forming dry powder with a particle size of 80 mesh, and mixing them evenly to obtain a mixed powder; the water-soluble polysaccharide is carboxyalkyl chitosan;

[0082] S3. Place 1 kg of swellable chitosan in 0.1 kg of 20% ethanol solution and stir evenly, wherein the ethanol solution is ethanol-water solution; then mix the mixed powder and swellable chitosan evenly at a mass ratio of 1:0.5, roll and bond them 3 times, and then dry them, so that the mixed powder forms a dissolved shell on the surface of the swellable inner core to obtain a finished product.

[0083] Embodiment 6: This embodiment differs from Embodiment 4 in that:

[0084] The preparation method is as follows:

[0085] S1. Weigh 1 kg of chitosan particles and place them in 12 kg of a 5% dilute acid solution, where the particle size of the chitosan particles is 20 meshes, and the dilute acid solution is a dilute acetic acid aqueous solution. React at 40° C. for 2 hours, then squeeze dry to obtain a swollen chitosan, which is the swollen inner core;

[0086] S2, adding 2 kg of hydrotrope to 20 kg of water-soluble polysaccharide, the hydrotrope is an inorganic salt pore-forming dry powder with a particle size of 80 mesh, and mixing them evenly to obtain a mixed powder; the water-soluble polysaccharide is sodium alginate;

[0087] S3. Place 1 kg of swellable chitosan in 0.1 kg of 30% ethanol solution and stir evenly, wherein the ethanol solution is ethanol-water solution; then mix the mixed powder and swellable chitosan evenly at a mass ratio of 1:2, roll and bond them 3 times, and then dry them, so that the mixed powder forms a dissolved shell on the surface of the swellable inner core to obtain a finished product.

[0088] Embodiment 7: This embodiment differs from Embodiment 4 in that:

[0089] The hydrotrope consists of collagen fiber, carboxyalkyl chitosan succinamide fiber and sodium alginate fiber in a weight ratio of 1:0.3:0.4; the length of the collagen fiber is 0.5 mm, the length of the carboxyalkyl chitosan succinamide fiber is 0.5 mm, and the length of the sodium alginate fiber is 1 mm.

[0090] Embodiment 8: This embodiment differs from Embodiment 4 in that:

[0091] The hydrotrope consists of collagen fiber, carboxyalkyl chitosan succinamide fiber and sodium alginate fiber in a weight ratio of 1:0.1:0.2; the length of the collagen fiber is 0.5 mm, the length of the carboxyalkyl chitosan succinamide fiber is 0.5 mm, and the length of the sodium alginate fiber is 1 mm.

[0092] Embodiment 9: This embodiment differs from Embodiment 4 in that:

[0093] The hydrotrope consists of collagen fiber, carboxyalkyl chitosan succinamide fiber and sodium alginate fiber in a weight ratio of 1:0.5:0.6; the length of the collagen fiber is 0.5 mm, the length of the carboxyalkyl chitosan succinamide fiber is 0.5 mm, and the length of the sodium alginate fiber is 1 mm.

[0094] Embodiment 10: This embodiment differs from Embodiment 4 in that:

[0095] S2. Weigh 1 kg of water-soluble polysaccharide and place it in 12 kg of sodium bicarbonate solution to disperse for 8 minutes. The water-soluble polysaccharide is hydroxypropyl chitosan, and the sodium bicarbonate solution is a 10% sodium bicarbonate aqueous solution. Then, add 0.1 kg of microcrystalline cellulose and 0.2 kg of coagulated polysaccharide. The particle size of the microcrystalline cellulose is 100 mesh, and the particle size of the coagulated polysaccharide is 80 mesh. Then, freeze-drying is performed to obtain a mixed powder.

[0096] Embodiment 11: This embodiment differs from Embodiment 10 in that:

[0097] S2. Weigh 1 kg of water-soluble polysaccharide, place it in 10 kg of sodium bicarbonate solution and disperse it for 10 minutes. The water-soluble polysaccharide is carboxyalkyl chitosan, and the sodium bicarbonate solution is a 10% sodium bicarbonate aqueous solution. Then add 0.05 kg of microcrystalline cellulose and 0.1 kg of coagulated polysaccharide, the particle size of the microcrystalline cellulose is 100 mesh, and the particle size of the coagulated polysaccharide is 80 mesh. Then, freeze-drying is performed to obtain a mixed powder.

[0098] Embodiment 12: This embodiment differs from Embodiment 10 in that:

[0099] S2. Weigh 1 kg of water-soluble polysaccharide and place it in 15 kg of sodium bicarbonate solution to disperse for 5 minutes. The water-soluble polysaccharide is sodium hyaluronate, and the sodium bicarbonate solution is a 10% sodium bicarbonate aqueous solution. Then, add 0.2 kg of microcrystalline cellulose and 0.3 kg of coagulated polysaccharide. The particle size of the microcrystalline cellulose is 100 mesh, and the particle size of the coagulated polysaccharide is 80 mesh. Then, freeze-drying is performed to obtain a mixed powder.

[0100] Embodiment 13: This embodiment differs from Embodiment 4 in that:

[0101] The preparation method is as follows:

[0102] S1. Weigh 1 kg of chitosan particles and place them in 10 kg of a 3% dilute acid solution, react at 30°C for 10 hours, the dilute acid solution is a dilute acetic acid aqueous solution, then squeeze dry, wash, and obtain a swollen chitosan, i.e., a swollen core;

[0103] S2. Dissolve the water-soluble polysaccharide in purified water to obtain a 5% solution, add an oil agent and a foaming agent to the solution, the oil agent concentration is 0.5%, and the foaming agent concentration is 0.8%, to obtain a mixed solution; the oil agent is glycerin, and the foaming agent is PVC white foaming agent; S3. Spray the mixed solution evenly onto the surface of the swollen chitosan, the volume of the sprayed mixed solution is 12 times the mass of the swollen chitosan, and after drying, the mixed solution forms a dissolved shell to obtain a finished product.

[0104] Embodiment 14: This embodiment differs from Embodiment 4 in that:

[0105] The preparation method is as follows:

[0106] S1. Weigh 1 kg of chitosan particles and place them in 8 kg of a 0.5% dilute acid solution, react at 20°C for 12 hours, wherein the dilute acid solution is a dilute acetic acid aqueous solution, then squeeze dry, wash, and obtain a swollen chitosan, i.e., a swollen core;

[0107] S2, dissolving a water-soluble polysaccharide in purified water to obtain a 1% solution, adding an oil and a foaming agent to the solution, wherein the oil concentration is 0.1% and the foaming agent concentration is 0.1%, to obtain a mixed solution; the oil is vaseline and the foaming agent is PVC white foaming agent;

[0108] S3. The mixed liquid is evenly sprayed onto the surface of the swollen chitosan. The volume of the sprayed mixed liquid is 5 times the mass of the swollen chitosan. After drying, the mixed liquid forms a dissolved shell to obtain a finished product.

[0109] Embodiment 15: This embodiment differs from Embodiment 4 in that:

[0110] The preparation method is as follows:

[0111] S1. Weigh 1 kg of chitosan particles and place them in 12 kg of a 5% dilute acid solution, react at 40°C for 2 hours, wherein the dilute acid solution is a dilute acetic acid aqueous solution, then squeeze dry, wash, and obtain a swollen chitosan, i.e., a swollen core;

[0112] S2, dissolving the water-soluble polysaccharide in purified water to obtain a 10% solution, adding an oil and a foaming agent to the solution, wherein the oil concentration is 1% and the foaming agent concentration is 1%, to obtain a mixed solution; the oil is medical silicone oil and the foaming agent is PVC white foaming agent;

[0113] S3, the mixed liquid is evenly sprayed onto the surface of the swollen chitosan, the volume of the sprayed mixed liquid is 20 times the mass of the swollen chitosan, and after drying, the mixed liquid forms a dissolved shell to obtain a finished product

[0114] Embodiment 16: This embodiment differs from Embodiment 4 in that:

[0115] The preparation method is as follows:

[0116] S1. Weigh 1 kg of chitosan particles and place them in 10 kg of 3% dilute acid solution, react at 30°C for 10 hours, then squeeze and wash to obtain swollen chitosan, i.e., swollen core;

[0117] S2. Spread the water-soluble polysaccharide fiber, which is carboxyalkyl cellulose fiber, flatly, and then squeeze the wet swollen chitosan onto the 1 cm long water-soluble polysaccharide fiber. The fiber is then rolled into a ball and dried. The fiber forms a dissolved outer shell on the surface of the swollen inner core, and there are gaps between the fibers, the gaps are 1 mm, and the finished product is obtained.

[0118] Embodiment 17: This embodiment differs from Embodiment 4 in that:

[0119] The preparation method is as follows:

[0120] S1. Weigh 1 kg of chitosan particles and place them in 8 kg of 0.5% dilute acid solution, react at 20°C for 12 hours, then squeeze and wash to obtain swollen chitosan, i.e., swollen core;

[0121] S2. Spread the water-soluble polysaccharide fiber flat, the water-soluble polysaccharide fiber is carboxyalkyl chitosan fiber, and then squeeze the wet swollen chitosan onto the 0.5 cm long water-soluble polysaccharide fiber, and then roll the fiber into a ball and dry it, the fiber forms a dissolved shell on the surface of the swollen inner core, and there are gaps between the fibers, the gaps are 1 mm, and the finished product is obtained.

[0122] Embodiment 18: This embodiment differs from Embodiment 4 in that:

[0123] The preparation method is as follows:

[0124] S1. Weigh 1 kg of chitosan particles and place them in 12 kg of 5% dilute acid solution, react at 40° C. for 2 hours, then squeeze and wash to obtain swollen chitosan, i.e., swollen core;

[0125] S2. Spread the water-soluble polysaccharide fiber flat, the water-soluble polysaccharide fiber is sodium alginate fiber, and then squeeze the wet swollen chitosan onto the 1.5m long water-soluble polysaccharide fiber, and then roll the fiber into a ball and dry it, the fiber forms a dissolved shell on the surface of the swollen inner core, and there are gaps between the fibers, the gaps are 1mm, and the finished product is obtained.

[0126] Embodiment 19: This embodiment differs from Embodiment 7 in that:

[0127] The hydrotrope is sodium alginate fiber.

[0128] Embodiment 20: This embodiment differs from Embodiment 10 in that:

[0129] No sodium bicarbonate solution was added to the mixed powder raw materials.

[0130] Embodiment 21: This embodiment differs from Embodiment 10 in that:

[0131] In the mixed powder raw materials, the microcrystalline cellulose and the coagulated polysaccharide are replaced by an equal mass of sodium alginate.

[0132] Embodiment 22: This embodiment differs from Embodiment 10 in that:

[0133] The powder mix was not freeze-dried during preparation.

[0134] Comparative Example

[0135] Comparative Example 1: The difference between this comparative example and Example 1 is that:

[0136] The hemostatic powder is water-soluble chitosan, and the water-soluble chitosan is carboxymethyl chitosan.

[0137] Comparative Example 2: The difference between this comparative example and Example 1 is that:

[0138] The hemostatic powder is swelling chitosan, and the deacetylation degree of chitosan is 98%.

[0139] Application Examples

[0140] Application Example 1: Preparation process of a hemostatic material:

[0141] Purified water is used to atomize and wet the surface of the medical non-woven fabric, and then the hemostatic powder prepared in Example 1 is evenly sprinkled on it. The dissolved shell of the hemostatic powder slightly dissolves and adheres to the surface of the medical non-woven fabric. After hot pressing, compounding, drying, folding and packaging, a finished product is obtained.

[0142] Application Example 2: Preparation process of a hemostatic material:

[0143] A 20% ethanol solution was used to atomize and wet the surface of the medical non-woven fabric, and then the hemostatic powder prepared in Example 2 was evenly sprinkled on it. The dissolved shell of the hemostatic powder was slightly dissolved and adhered to the surface of the medical non-woven fabric. After hot pressing, compounding, drying, folding and packaging, a finished product was obtained.

[0144] Application Example 3: Preparation process of a hemostatic material:

[0145] The surface of the medical non-woven fabric was moistened with a 40% ethanol solution, and then the hemostatic powder prepared in Example 3 was evenly sprinkled on it. The dissolved shell of the hemostatic powder was slightly dissolved and adhered to the surface of the medical non-woven fabric. After hot pressing, compounding, drying, folding and packaging, a finished product was obtained.

[0146] Application Example 4: The difference between this application example and application example 1 is:

[0147] The hemostatic powder used was the one prepared in Example 4.

[0148] Application Example 5: The difference between this application example and application example 1 is:

[0149] The hemostatic powder used was the one prepared in Example 5.

[0150] Application Example 6: The difference between this application example and application example 1 is:

[0151] The hemostatic powder used was the one prepared in Example 6.

[0152] Application Example 7: The difference between this application example and application example 1 is:

[0153] The hemostatic powder used was the one prepared in Example 7.

[0154] Application Example 8: The difference between this application example and application example 1 is:

[0155] The hemostatic powder used was the one prepared in Example 8.

[0156] Application Example 9: The difference between this application example and application example 1 is:

[0157] The hemostatic powder used was the one prepared in Example 9.

[0158] Application Example 10: The difference between this application example and application example 1 is:

[0159] The hemostatic powder used is the hemostatic powder prepared in Example 10.

[0160] Application Example 11: The difference between this application example and application example 1 is:

[0161] The hemostatic powder used is the hemostatic powder prepared in Example 11.

[0162] Application Example 12: The difference between this application example and application example 1 is:

[0163] The hemostatic powder used is the hemostatic powder prepared in Example 12.

[0164] Application Example 13: The difference between this application example and application example 1 is:

[0165] The hemostatic powder used is the hemostatic powder prepared in Example 13.

[0166] Application Example 14: The difference between this application example and application example 1 is:

[0167] The hemostatic powder used is the hemostatic powder prepared in Example 14.

[0168] Application Example 15: The difference between this application example and application example 1 is:

[0169] The hemostatic powder used is the hemostatic powder prepared in Example 15.

[0170] Application Example 16: The difference between this application example and application example 1 is:

[0171] The hemostatic powder used is the hemostatic powder prepared in Example 16.

[0172] Application Example 17: The difference between this application example and application example 1 is:

[0173] The hemostatic powder used is the hemostatic powder prepared in Example 17.

[0174] Application Example 18: The difference between this application example and application example 1 is:

[0175] The hemostatic powder used is the hemostatic powder prepared in Example 18.

[0176] Application Example 19: The difference between this application example and application example 1 is:

[0177] The hemostatic powder used is the hemostatic powder prepared in Example 19.

[0178] Application Example 20: The difference between this application example and application example 1 is:

[0179] The hemostatic powder used is the hemostatic powder prepared in Example 20.

[0180] Application Example 21: The difference between this application example and application example 1 is:

[0181] The hemostatic powder used is the hemostatic powder prepared in Example 21.

[0182] Application Example 22: The difference between this application example and application example 1 is:

[0183] The hemostatic powder used is the hemostatic powder prepared in Example 22.

[0184] Comparative Application Examples

[0185] Comparative Application Example 1: The difference between this comparative application example and application example 1 is that:

[0186] The hemostatic powder adopts the hemostatic powder prepared in Comparative Example 1.

[0187] Comparative Application Example 2: The difference between this comparative application example and application example 1 is that:

[0188] The hemostatic powder adopts the hemostatic powder prepared in Comparative Example 2.

[0189] Performance testing

[0190] 1. Liquid absorbency test

[0191] Finished product samples were prepared using the preparation methods of Application Examples 1-22 and Comparative Application Examples 1-2 respectively;

[0192] The sample size is 5cm×5cm. Add test liquid (the test liquid is physiological saline) that is 50 times the weight of the sample into a beaker, soak the sample in the beaker, and use a glass rod to move the sample. Pour out the excess test liquid after 30 seconds, and move the sample 5 times in 30 seconds. Weigh the weight of the beaker and the sample after absorbing the liquid, record the average mass of each gram of sample after absorbing the liquid, and record the data.

[0193] The sample size is 5cm×5cm. Add test liquid (the test liquid is physiological saline) 20 times the weight of the sample into a beaker, immerse the sample in the beaker, and use a glass rod to move the sample, and record the time taken for the test liquid to be completely absorbed.

[0194] 2. Wound adhesion test

[0195] Finished product samples were prepared using the preparation methods of Application Examples 1-22 and Comparative Application Examples 1-2 respectively;

[0196] The sample size is 3cm×5cm. Place the sample in a beaker and add the test liquid (normal saline) preheated to (37±1)℃. The test liquid is 50 times the weight of the sample. After the sample is soaked for 1 minute, apply the 3cm×3cm part of the sample to the 3cm×5cm qualitative filter paper. Use a tensile testing machine to perform a peel strength test. Fix the 3cm×2cm non-woven fabric sample with the lower clamp of the tensile testing machine, and clamp the 3cm×2cm qualitative filter paper with the upper clamp. Record the force (N) when the sample is peeled off from the qualitative filter paper. Take the average value of 5 samples and record the data.

[0197] Table 1 Performance test table

[0198]

[0199]

[0200] 3. Hemostatic effect detection

[0201] The finished hemostatic material samples were prepared by using the preparation methods of Application Examples 1-22 and Comparative Application Examples 1-2 respectively;

[0202] Anesthetize a 100kg Landrace pig. After anesthesia, cut the skin of the leg, locate the femoral artery, and quickly cut the muscle with a scalpel perpendicular to the femoral artery to cut off the blood vessel and allow free bleeding for 20 seconds. Quickly apply hemostatic material to the bleeding point, fully cover the bleeding point, and press with a weighed gauze to stop bleeding, and start timing.

[0203] After pressing for 150 seconds, carefully lift the gauze to observe the hemostasis of the femoral artery; if the wound is still bleeding, continue to press the bleeding point with gauze and observe the hemostasis every 15 seconds. If the wound is no longer bleeding, continue to observe for 120 seconds to see if there will be further bleeding. When no more bleeding is observed, record the hemostasis time;

[0204] Weigh the gauze and hemostatic material after pressing to stop bleeding, and calculate the amount of bleeding; that is, the amount of bleeding (g) = weight after hemostasis (hemostatic material + gauze) - weight before hemostasis (hemostatic material + gauze);

[0205] Type I rebleeding: 10 minutes after the compression to stop bleeding, flex and extend the hip and knee joints on the injured side to the maximum extent, 20 times / min, and observe the type I rebleeding (flexion and extension rebleeding). If bleeding recurs, apply pressure to stop bleeding again.

[0206] Complete the flexion and extension test and observe the rebleeding of type II trauma (rebleeding after lifting): lift the injured limb to form a 60° angle with the trunk, 20 times / min, continue for 1min to observe the rebleeding. If bleeding recurs, apply gauze to press and stop bleeding;

[0207] Type III re-bleeding: Place the experimental animal on a stretcher to simulate the process of transporting a wounded person. Bounce it up and down for 1 minute, and walk on the spot for 1 minute. Observe the re-bleeding of the wound. If bleeding recurs, apply pressure to stop the bleeding.

[0208] Generally, in symptom observation: description of the health status of the experimental animals, whether there were any animal deaths during the experiment, and the survival rate 24 hours after the experiment;

[0209] Table 2 Hemostatic effect test table

[0210]

[0211]

[0212] 3. Hemostatic effect detection

[0213] The finished hemostatic material samples were prepared by using the preparation methods of Application Examples 1-22 and Comparative Application Examples 1-2 respectively;

[0214] After completing the above-mentioned hemostasis and rebleeding observation operations, clean the wound, clean the blood clots and hemostatic materials, and then suture the wound; after suturing, observe that there is no obvious swelling at the wound site of the pig, and continue to observe the healing and redness and swelling of the wound site for 1-3 weeks.

[0215] Table 3 Evaluation table

[0216] No redness 0 No swelling 0 Slight redness of the wound 1 Slight swelling (barely visible) 1 The wound is obviously red 2 Mild swelling (clearly visible bulge) 2 Reddish purple wound 3 Moderate swelling (uplift of about 1 cm) 3 Purple-black wound 4 Severe swelling (more than 1 cm) 4

[0217] Table 4 Analysis table based on Table 3

[0218]

[0219] It can be seen from Application Examples 1-3 and Tables 1, 2 and 4 that the hemostatic material prepared in the present application has a good hemostatic effect and can promote wound healing without causing redness, swelling and infection of the wound. At the same time, the hemostatic material has good adhesion and is not prone to layer peeling.

[0220] From Application Examples 4-6 and Tables 1, 2 and 4, it can be seen that under the action of inorganic salt pore-forming dry powder, the hemostatic material can further promote the absorption of liquid and can quickly stop bleeding. At the same time, the hemostatic powder in the hemostatic material can be more stably bonded to the surface of the non-woven fabric, and it is not easy for the hemostatic powder to separate from the gauze due to liquid immersion.

[0221] From Application Example 4 and Application Examples 7-9 and Tables 1, 2 and 4, it can be seen that the combination of collagen fiber, carboxyalkyl chitosan succinamide fiber and sodium alginate fiber in the water-soluble adjuvant can not only improve the hydrophilicity and water absorption of the dissolved shell on the surface of the hemostatic powder; but also ensure the amount of adsorbed liquid, and at the same time promote wound healing by retaining the protein content in the wound.

[0222] From Application Examples 4 and 10-12 and Tables 1, 2 and 4, it can be seen that the coagulated polysaccharide, sodium bicarbonate solution, microcrystalline cellulose and freeze-drying are coordinated, and the adsorption effect of the coagulated polysaccharide on the sodium bicarbonate solution and the bonding effect on the microcrystalline cellulose are utilized to make the microcrystalline cellulose bonded to the surface of the coagulated polysaccharide, and freeze-drying is used to ensure that the dissolving shell can be quickly dissolved in water after contacting the blood and tissue fluid, and in the process of the swelling shell gradually swelling, a flow channel is provided for plasma, tissue fluid, etc., so that they are in contact with the swelling inner core, thereby ensuring the absorption and storage effect of the swelling inner core on liquids such as plasma and tissue fluid.

[0223] It can be seen from Application Examples 13-15 and Tables 1, 2 and 4 that water-soluble chitosan is prepared into a solution with a relatively high concentration, and then an oil agent is added, such as glycerol, medical silicone oil, vaseline, Tween and the like, to promote water to penetrate the dissolved outer shell to conduct heat to the swollen inner core, thereby promoting the swollen inner core to absorb water; and a foaming agent is used to produce pore channels in the dissolved outer shell, thereby further promoting the swollen inner core to absorb liquid, and to try to avoid the dissolved outer shell covering the swollen inner core and affecting the swollen inner core's absorption of liquid.

[0224] From Application Examples 16-18 and Tables 1, 2 and 4, it can be seen that the water-soluble polysaccharide fibers are wrapped around the surface of the swollen inner core, so that the water-soluble polysaccharide fibers form a network coating structure, but the interwoven and stacked polysaccharide fibers still have a relatively high porosity, which facilitates the liquid to pass through the dissolved outer shell and contact the swollen inner core, thereby ensuring the hemostatic powder's absorption effect on body fluids.

[0225] Combining Application Example 7 and Application Example 19 and Tables 1, 2 and 4, it can be seen that the water-soluble auxiliary agent is seaweed fiber. Compared with Application Example 7, the hemostatic effect of the hemostatic material prepared in Application Example 19 is worse than that in Application Example 7, and the amount of bleeding is higher than that in Application Example 7, which shows that collagen and carboxyalkyl chitosan succinamide can cross-link with proteins to form a cross-linked network, which prevents macromolecular proteins and other substances in plasma from continuously seeping out with the plasma, and promotes wound healing by retaining the protein content in the wound; however, the cross-linked network has no barrier to the seepage of water, tissue fluid, etc. in plasma, ensuring the absorption of water in tissue fluid and plasma by the swelling inner core, thereby playing a role in rapid hemostasis and promoting wound healing.

[0226] Combining Application Example 10 and Application Examples 20-22 and Tables 1, 2 and 4, it can be seen that no sodium bicarbonate solution was added to the mixed powder raw materials of Application Example 20, microcrystalline cellulose and coagulated polysaccharides were replaced with an equal mass of sodium alginate in the mixed powder raw materials of Application Example 21, and the mixed powder of Application Example 22 was not freeze-dried during preparation. Compared with Application Example 10, the hemostatic effects of the finished hemostatic materials prepared in Application Examples 20, 21 and 22 were worse than those in Application Example 7, the average mass was less than that in Application Example 10, the average time was greater than that in Application Example 10, and the peeling force was less than that in Application Example 10; this indicates that the sodium bicarbonate solution, microcrystalline cellulose, coagulated polysaccharides and freeze-drying in the mixed powder are coordinated to increase the porosity of the dissolving shell, thereby ensuring that the dissolving shell can be quickly dissolved in water after contacting blood and tissue fluid, and in the process of gradual swelling of the swelling shell, a circulation channel is provided for plasma, tissue fluid, etc., so that they are in contact with the swelling inner core, thereby ensuring the absorption and storage effect of the swelling inner core on liquids such as plasma and tissue fluid.

[0227] Combining Application Example 1 and Comparative Application Examples 1-2 and Tables 1, 2 and 4, it can be seen that the hemostatic powder of Comparative Application Example 1 is water-soluble chitosan, and the hemostatic powder of Comparative Application Example 2 is swelling chitosan. Compared with Application Example 1, the hemostatic effects of the hemostatic materials prepared in Comparative Application Examples 1 and 2 are worse than those in Application Example 1, the average mass is less than that in Application Example 1, the average time is greater than that in Application Example 1, and the peeling force is less than that in Application Example 1; this indicates that the combination of water-soluble chitosan and swelling chitosan can ensure that the hemostatic material has good adhesion stability while absorbing blood, and will not cause irritation to the wound surface.

[0228] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A hemostatic powder, characterized in that: The invention is prepared by the following raw materials in parts by weight: 65-95 parts of a swelling inner core and 5-35 parts of a dissolving outer shell; The swelling core is made of swelling chitosan; The dissolving shell is made of water-soluble polysaccharide compounded with a hydrotrope; the hydrotrope consists of collagen fiber, carboxyalkyl chitosan succinamide fiber and sodium alginate fiber in a weight ratio of 1:0.1-0.5:0.2-0.

6.

2. A hemostatic powder according to claim 1, characterized in that: The water-soluble polysaccharide is one or more of chitosan salt, carboxyalkyl chitosan, hydroxypropyl chitosan, hydroxyethyl chitosan, carboxyalkyl chitosan succinamide, carboxyalkyl chitin, sodium alginate, carboxyalkyl cellulose and sodium hyaluronate.

3. A method for preparing hemostatic powder, characterized in that: The following steps are involved: S1. Weigh chitosan particles and place them in a 0.5-5% dilute acid solution, with a mass ratio of chitosan particles to dilute acid solution of 1:8-12, react at 20-40°C for 2-12h, and then squeeze dry to obtain swollen chitosan; S2, freezing the swollen chitosan at -40 to -20°C for 5 to 24 hours, placing it in a 5 to 15% dilute acid solution, the mass ratio of the swollen chitosan to the dilute acid solution being 1:6 to 10, reacting at 0 to 4°C for 0.5 to 5 hours, to obtain a mixture; S3. The mixture is squeezed, washed with ethanol and dried, and a dissolving shell is formed on the outer surface of the swellable chitosan, and a swellable core is formed inside the swellable chitosan, thereby obtaining a hemostatic powder; the hemostatic powder contains 65-95 parts of the swellable core and 5-35 parts of the dissolving shell.

4. A method for preparing hemostatic powder, characterized in that: The following steps are involved: S1, weigh chitosan particles and place them in a 0.5-5% dilute acid solution, with the mass ratio of chitosan particles to the dilute acid solution being 1:8-12, reacting at 20-40°C for 2-12h, and then squeezing dry to obtain a swollen chitosan, i.e., a swollen core; S2, weighing water-soluble polysaccharides at a mass ratio of 1:10-15, placing them in a sodium bicarbonate solution and dispersing them for 5-10 minutes, then adding microcrystalline cellulose and coagulated polysaccharides, the mass ratio of water-soluble polysaccharides, microcrystalline cellulose and coagulated polysaccharides being 1:0.05-0.2:0.1-0.3, and then freeze-drying to obtain a mixed powder; S3. The swellable chitosan is placed in an ethanol solution with a concentration of 20-30% and stirred evenly, and then the mixed powder and the swellable chitosan are mixed evenly at a mass ratio of 1:0.5-2. After rolling, bonding and drying, the mixed powder forms a dissolving shell on the surface of the swellable inner core to obtain a hemostatic powder; the hemostatic powder contains 65-95 parts of the swellable inner core and 5-35 parts of the dissolving shell.

5. A method for preparing hemostatic powder, characterized in that: The following steps are involved: S1, weigh chitosan particles and place them in a 0.5-5% dilute acid solution, react at 20-40°C for 2-12h, the mass ratio of chitosan particles to dilute acid solution is 1:8-12, then squeeze dry, wash and obtain swollen chitosan, i.e. swollen inner core; S2. Spread the water-soluble polysaccharide fibers flatly, and then squeeze the wet swollen chitosan onto the 0.5-1.5 cm long water-soluble polysaccharide fibers, and then roll the fibers into a ball and dry them to form a dissolving shell on the surface of the swollen core to obtain a hemostatic powder; the hemostatic powder contains 65-95 parts of the swollen core and 5-35 parts of the dissolving shell.

6. A process for preparing a hemostatic material, characterized in that: The steps include: Purified water or ethanol solution is used to atomize and wet the surface of the medical non-woven fabric, and then hemostatic powder is evenly sprinkled on it. The dissolved shell of the hemostatic powder is slightly dissolved and adheres to the surface of the medical non-woven fabric. After hot pressing, compounding, drying, folding and packaging, a finished product is obtained; the hemostatic powder is selected from any one of claims 1-2.

Citation Information

Patent Citations

  • Haemostatic material

    CN107007867A

  • Wound treatment dressing and preparation method thereof

    CN109453424A

  • Nasal hemostatic patch

    CN213607440U