A cobalt tetrasulfide@nickel disulfide / carbon composite material, its preparation method, and its application in sodium-ion batteries.
By preparing a cobalt tetrasulfide@nickel disulfide/carbon composite material as the anode of a sodium-ion battery, the problems of limited capacity and poor cycle performance of the negative electrode material were solved, and a sodium-ion battery with high capacity, long life and high rate performance was realized.
Patent Information
- Application Number
- CN202310550316.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-16
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-05-16
AI Technical Summary
Existing sodium-ion battery anode materials suffer from limited capacity, poor cycle and rate performance, which restricts the widespread application and large-scale production of sodium-ion batteries.
Cobalt tetrasulfide@nickel disulfide/carbon composite material was used as the active material to prepare irregular spherical or blocky Co3S4@NiS2/C materials through hydrothermal reaction and calcination process. Combined with carbon-encapsulated NiS2 quantum dots, the conductivity and structural stability of the material were improved.
It significantly improves the cycle stability, lifespan, and capacity of sodium-ion batteries, enhances the rate performance and electrochemical performance of materials, and is suitable for high-current long-cycle and temperature-varying environments.
Smart Images

Figure CN116470029B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of sodium-ion battery composite material technology, specifically relating to a cobalt tetrasulfide@nickel disulfide / carbon composite material, its preparation method, and its application in sodium-ion batteries. The prepared binary metal sulfide Co3S4@NiS2 / C is used as an anode material for sodium-ion batteries. Background Technology
[0002] With the expanding applications of lithium-ion batteries, the demand for lithium has increased significantly. However, lithium reserves are finite; lithium in the Earth's crust is scarce, expensive, and unevenly distributed, posing a significant challenge to the development of long-life, large-scale energy storage batteries. Against this backdrop, there is an urgent need to develop novel long-life energy storage devices. This brings to mind sodium, another alkali metal in the same group. It possesses electrochemical properties similar to metallic lithium, and sodium is widely distributed in the Earth's crust, ranking sixth in abundance at approximately 2.74%.
[0003] Rechargeable sodium-ion batteries (SIBs) are becoming an important complement to lithium-ion batteries (LIBs), thanks to their extensive energy storage capabilities based on the natural abundance and environmental friendliness of sodium resources. Sodium-ion batteries use activated carbon as the negative electrode and sodium-manganese-based as the positive electrode, with an aqueous electrolyte transferring sodium ions between the two electrodes for charging and discharging. These materials are non-toxic, and the batteries are 100% recyclable. Sodium-ion batteries can be fully charged and discharged 5000 times, and with daily charging, they can last for more than ten years. Sodium-ion batteries can also operate at temperatures ranging from -10°C to +60°C, and their price is about half that of lithium-ion batteries, making them more suitable for large-scale energy storage and enabling them to shoulder the responsibility of developing sustainable green energy for the Earth.
[0004] However, with Li + In comparison, Na is larger and heavier + This can lead to negative effects such as capacity limitation, poor cycle and rate performance. The widespread application and large-scale production of SiBs are greatly limited by suitable anode materials.
[0005] Therefore, it is crucial to study suitable SIB anode materials with excellent electrochemical performance, including high rate capacity and excellent cycle durability. Summary of the Invention
[0006] The purpose of this invention is to provide a cobalt tetrasulfide@nickel disulfide / carbon composite material and its preparation method. The prepared Co3S4@NiS2 / C composite material has an irregular spherical or blocky structure with a size of 1-2 μm, which greatly improves cycle stability, service life and battery capacity.
[0007] Another objective of this invention is to provide an application of a cobalt tetrasulfide@nickel disulfide / carbon composite material in sodium-ion batteries, which serves as an active material in the preparation of sodium-ion battery anodes, thereby preparing sodium-ion batteries.
[0008] The specific technical solution of this invention is as follows:
[0009] A method for preparing a cobalt tetrasulfide@nickel disulfide / carbon composite material includes the following steps:
[0010] 1) Prepare CoS nanosphere precursors via hydrothermal reaction;
[0011] 2) The CoS nanosphere precursor, organic ligand, surfactant and nickel source were mixed in a solvent and subjected to hydrothermal reaction to obtain the precursor CoS@Ni-MOFs nanospheres;
[0012] 3) The precursor CoS@Ni-MOFs nanospheres and sulfur powder were mixed and calcined under a protective atmosphere to obtain the Co3S4@NiS2 / C composite material.
[0013] The preparation method of the CoS nanospheres mentioned in step 1) is as follows:
[0014] CoS nanospheres are obtained by dispersing cobalt source, NH4F and urea in a solvent, adding sulfur source, and then performing a hydrothermal reaction.
[0015] In the preparation method of CoS nanospheres, the molar ratio of cobalt source, sulfur source, NH4F and urea is 1:4-5.5:1-2:2.5-3; preferably 1:5:1.5:3; the cobalt source is a soluble cobalt source, preferably Co(NO3)2·6H2O or CoSO4·7H2O; the solvent is anhydrous ethanol; the sulfur source is a soluble sulfur source, preferably thioacetamide; the concentration of the cobalt source is 0.01-0.05 mol / L; the hydrothermal reaction is carried out at 130-150℃ for 10-14 h, preferably at 140℃ for 12 h; after the hydrothermal reaction, the nanospheres are washed 4-6 times with water and 1-2 times with ethanol, centrifuged, and dried at 40-80℃ for 12-15 h.
[0016] The prepared CoS nanospheres are relatively smooth spheres with a size of 450-550 nm.
[0017] Preferably, the preparation method of CoS nanospheres is as follows: 0.5 mmol of Co(NO3)2·6H2O, 1.5 mmol of urea and 0.75 mmol of ammonium fluoride are added to 40 mL of anhydrous ethanol and stirred for 10 min. Then, 2.5 mmol of thioacetamide is added and stirred for 10 min. Then, the hydrothermal reaction is carried out at 140 °C for 12 h. After the reaction is completed, the product CoS nanospheres are obtained by washing.
[0018] In step 2), the mass ratio of the CoS nanosphere precursor, organic ligand, surfactant and nickel source is 0.08-0.12:0.15:1.0-1.5:0.40-0.50.
[0019] In step 2), the concentration of the CoS nanosphere precursor in the solvent is 0.002-0.004 g / ml;
[0020] In step 2), the solvent is a mixed solution of water and N,N-dimethylformamide or pure N,N-dimethylformamide, preferably a mixed solution of ultrapure water and N,N-dimethylformamide in a volume ratio of 1:1.
[0021] In step 2), the organic ligand is 1,3,5-pyromellitic acid;
[0022] In step 2), the surfactant is polyvinylpyrrolidone (PVP M = 58000, K29-32);
[0023] In step 2), the nickel source is a soluble nickel salt, preferably Ni(NO3)2·6H2O or NiSO4·5H2O;
[0024] In step 2), the hydrothermal reaction conditions are 150-170℃ for 10-14 hours, preferably 160℃ for 12 hours;
[0025] In step 2), after the hydrothermal reaction, the product is washed 4 to 6 times with water and 1 to 2 times with ethanol, centrifuged, and dried at 40 to 80°C for 12 to 15 hours.
[0026] The CoS@Ni-MOFs prepared in step 2) have a size of 500-700 nm.
[0027] The calcination conditions described in step 3) are: calcination at 350°C for 2 hours, preferably with a heating rate of 2°C / min, and calcination in a tube furnace.
[0028] In step 3), the mass ratio of the precursor CoS@Ni-MOF nanospheres to sulfur powder is 1:5-1:9;
[0029] The protective atmosphere mentioned in step 3) is nitrogen or argon;
[0030] The present invention provides a cobalt tetrasulfide@nickel disulfide / carbon composite material, which is prepared by the above method. The cobalt tetrasulfide@nickel disulfide / carbon composite material has an irregular spherical or blocky structure with a size of 1-2 μm.
[0031] This invention provides the application of a cobalt tetrasulfide@nickel disulfide / carbon composite material in sodium-ion batteries, which is used as an active material to prepare sodium-ion battery anodes, thereby preparing sodium-ion batteries.
[0032] Specifically, the cobalt tetrasulfide@nickel disulfide / carbon composite material is the active material. After being mixed evenly with conductive carbon black and PVDF in a ratio of 8:1:1 or 7:2:1, it is magnetically stirred for 6-8 hours to uniformly disperse it in N-methylpyrrolidone (NMP). The uniformly mixed slurry is coated onto copper foil using a coater and placed in a vacuum drying oven at 60-80°C for 12-24 hours. After drying, it is pressed into sheets using a tablet press and then cut into small circular electrode sheets using a cutting machine. The electrode sheets are assembled into button batteries in a glove box filled with high-purity argon gas and with water and oxygen values ≤0.01ppm. The electrolyte is NaCF3SO3+DEGDME. The sodium sheet has a purity of Na≥99.99% and a thickness of 0.5mm. After rolling, it is cut to the size of the electrode sheet.
[0033] The specific method for assembling the battery is as follows: After adding 1 drop of electrolyte to the positive electrode shell, place the electrode plate, then add 1 drop of electrolyte and place the glass fiber, add 3 drops of electrolyte to the glass fiber and place the sodium plate as the counter electrode, then place two pieces of nickel foam, add 4 drops of electrolyte, cover with the negative electrode shell, press and seal the battery with a hydraulic press, and let it stand for 6 to 12 hours.
[0034] Transition metal chalcogenides (TMCs) are considered excellent anode materials for silicon carbide (SIB) due to their high theoretical specific capacity and low manufacturing cost. However, the poor rate performance and durability of TMCs often lead to low conductivity during the conversion reaction. This invention improves the conductivity of TMCs by encapsulating them with carbon. The carbon-encapsulated NiS2 quantum dot composite Co3S4 material provided by this invention exhibits good cycle stability and high rate performance after carbon encapsulation.
[0035] The carbon-coated NiS2 quantum dot composite Co3S4 material provided by this invention offers numerous active sites during charge and discharge. The NiS2 quantum dot composite Co3S4 material, its polycrystalline structure, and the increased conductivity after carbon coating significantly improve cycle stability, lifespan, and battery capacity. Its unique structure allows it to withstand high current and long-term cycling, reducing the loss of active material during charge and discharge and buffering volume changes, thereby improving the electrochemical performance of the anode material. Co3S4 exhibits better conductivity, which is beneficial for sodium formation / desodium formation during the reaction process. Therefore, constructing a Co3S4@NiS2 polycrystalline structure is expected to accelerate reaction kinetics. The multi-component synergistic effect of this invention promotes rapid charge transfer, resulting in excellent rate performance and cycle performance. The interface effect of the bimetallic sulfide can introduce an internal electric field to improve reaction kinetics, while providing abundant electrochemical reaction sites, thereby improving its reversible capacity and cycle stability.
[0036] This invention develops anode materials with unique structures using a practical and direct SIB (Self-Induced Blow-Up) method. Electrode materials with micro / nanostructures are promising candidates, constructed from nanoscale subunits in a specific manner. These micro / nanostructured materials possess the structural advantages of both nanoscale subunits and micrometer-scale components (the size range is shown in the SEM images of the products according to this invention; 500 nm represents a nanostructure, and 1.5 μm represents a microstructure). Nanoscale subunits can shorten ion diffusion pathways and increase electrochemical reaction sites, while micrometer-scale components can improve the structural stability of the material. Furthermore, compositing with conductive carbon species can effectively reduce the negative impact of poor conductivity. A well-structured carbon-based composite material can improve electronic conductivity and buffer internal stress, which is beneficial to the electrochemical performance of SIBs. Therefore, combining nanostructured NiS2 quantum dots with Co3S4 nanospheres and integrating them with a carbon layer is an effective strategy for achieving high-performance SIBs.
[0037] Compared with existing technologies, the advantages of this invention are that it prepares a Co3S4@NiS2 / C nanosphere composite material of carbon-coated NiS2 quantum dot composite Co3S4 through a simple hydrothermal reaction and annealing process, wherein bimetallic sulfide Co3S4@NiS2 nanoparticles are encapsulated in a carbon layer. The heterogeneous interface between Co3S4 and NiS2 crystals can induce an internal electric field to accelerate ion diffusion kinetics, improve conductivity, and provide abundant reaction sites for sodium energy storage. Furthermore, the carbon matrix shortens the electron / ion path and mitigates strain from volume changes. Benefiting from these advantages, the prepared Co3S4@NiS2 / C composite material exhibits high conductivity at 1 A g / L. -1 After 1000 cycles at current density, the display showed 417 mAh g. -1The high reversible capacity, high specific capacity, stable cycle performance, and robust rate performance demonstrate that Co3S4@NiS2 / C is an excellent and promising SIB anode material. Furthermore, the nickel, cobalt, and sulfur sources used in this invention are inexpensive and readily available; carbon coating significantly improves the battery's cycle stability, extends its lifespan, and increases and stabilizes its capacity. Attached Figure Description
[0038] Figure 1 Here is a SEM image of the CoS nanosphere material, the precursor precipitate from Example 1.
[0039] Figure 2 SEM image of the precursor precipitate CoS@Ni-MOFs nanospheres prepared in Example 1;
[0040] Figure 3 SEM image of the carbon-encapsulated NiS2 quantum dot composite Co3S4@NiS2 / C prepared in Example 1;
[0041] Figure 4 TEM image of the carbon-encapsulated NiS2 quantum dot composite Co3S4@NiS2 / C prepared in Example 1;
[0042] Figure 5 XRD pattern of the carbon-encapsulated NiS2 quantum dot composite Co3S4@NiS2 / C prepared in Example 1;
[0043] Figure 6 The image shows the XRD pattern of the CoS precipitate nanosphere material from Example 1.
[0044] Figure 7 SEM image of the precursor CoS precipitate nanosphere material prepared in Example 2;
[0045] Figure 8 SEM image of the carbon-encapsulated NiS2 quantum dot composite Co3S4@NiS2 / C prepared in Example 2;
[0046] Figure 9 SEM image of the carbon-encapsulated NiS2 quantum dot composite Co3S4@NiS2 / C prepared in Example 3;
[0047] Figure 10 TEM image of the carbon-encapsulated NiS2 quantum dot composite Co3S4@NiS2 / C prepared in Example 3;
[0048] Figure 11SEM image of the carbon-encapsulated NiS2 quantum dot composite Co3S4@NiS2 / C prepared in Example 4;
[0049] Figure 12 TEM image of the carbon-encapsulated NiS2 quantum dot composite Co3S4@NiS2 / C prepared in Example 4;
[0050] Figure 13 SEM image of the carbon-encapsulated NiS2 quantum dot composite Co3S4@NiS2 / C prepared in Example 5;
[0051] Figure 14 TEM image of the carbon-encapsulated NiS2 quantum dot composite Co3S4@NiS2 / C prepared in Example 5;
[0052] Figure 15 The carbon-encapsulated NiS2 quantum dot composite Co3S4@NiS2 / C prepared in Example 1 was used as a sodium-ion battery anode material at 1 A g. -1 Cyclic stability test results at current density;
[0053] Figure 16 The constant current charge-discharge curve of the carbon-encapsulated NiS2 quantum dot composite Co3S4@NiS2 / C prepared in Example 1 as a sodium-ion battery anode material;
[0054] Figure 17 Rate capability diagram of the carbon-encapsulated NiS2 quantum dot composite Co3S4@NiS2 / C prepared in Example 1 as a sodium-ion battery anode material;
[0055] Figure 18 The carbon-encapsulated NiS2 quantum dot composite material Co3S4@NiS2 / C prepared in Example 1 was used as a sodium-ion battery anode material at 2A g. -1 Cyclic stability test results at current density;
[0056] Figure 19 The carbon-encapsulated NiS2 quantum dot composite Co3S4@NiS2 / C prepared in Example 1 was used as a sodium-ion battery anode material at 10 A g. -1 Cyclic stability test results at current density;
[0057] Figure 20 The carbon-encapsulated NiS2 quantum dot composite Co3S4@NiS2 / C prepared in Example 1 was used as a sodium-ion battery anode material at 1 A g. -1Cyclic stability test results at current density and high temperature (50°C);
[0058] Figure 21 The carbon-encapsulated NiS2 quantum dot composite Co3S4@NiS2 / C prepared in Example 2 was used as a sodium-ion battery anode material at 1 A g. -1 Cyclic stability test results at current density;
[0059] Figure 22 The carbon-encapsulated NiS2 quantum dot composite Co3S4@NiS2 / C prepared in Example 3 was used as a sodium-ion battery anode material at 1 A g. -1 Cyclic stability test results at current density;
[0060] Figure 23 The carbon-encapsulated NiS2 quantum dot composite Co3S4@NiS2 / C prepared in Example 4 was used as a sodium-ion battery anode material at 1 A g. -1 Cyclic stability test results at current density;
[0061] Figure 24 The XRD pattern of the material prepared in Example 5. Detailed Implementation
[0062] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0063] Unless otherwise specified, all test materials and reagents used in the following examples are commercially available.
[0064] Unless otherwise specified in the embodiments, the techniques or conditions described in the literature in this field or in accordance with the product manual may be followed.
[0065] Example 1
[0066] A method for preparing a cobalt tetrasulfide@nickel disulfide / carbon composite material includes the following steps:
[0067] 1) Preparation of the precursor: Weigh 0.146 g Co(NO3)2·6H2O, 0.09 g urea, and 0.02775 g NH4F into a 100 mL beaker, add 40 mL of anhydrous ethanol, and stir magnetically for 10 min to dissolve. Add 0.1878 g of thioacetamide, stir magnetically for 10 min, and then transfer to a 50 mL polytetrafluoroethylene reactor. React at 140 °C for 12 h. After naturally cooling to room temperature, wash four times with deionized H2O by centrifugation, wash twice with ethanol, and vacuum dry at 60 °C for 12 h. Collect the CoS precursor precipitate. Its SEM image is shown below. Figure 1 As shown in the figure, it can be seen that it is a micro-nanosphere with a size of 500 nm.
[0068] 2) Preparation of CoS@Ni-MOFs:
[0069] 0.1 g of CoS precursor, 0.15 g of 1,3,5-pyromellitic acid, 1.033 g of polyvinylpyrrolidone (PVP, M = 58000, K 29-32), and 0.432 g of Ni(NO3)2·6H2O were weighed and added to a mixture of 15 mL ultrapure water and 15 mL DMF. The mixture was magnetically stirred for 20 min, then transferred to a 50 mL polytetrafluoroethylene reactor and reacted at 160 °C for 12 h. After cooling to room temperature, the product was washed four times with deionized water and twice with ethanol, and then vacuum dried at 60 °C for 12 h. The CoS@Ni-MOFs precursor precipitate was collected. Its SEM image is shown below. Figure 2 As shown in the figure, it can be seen that it is a micro-nanosphere with a size of 550nm.
[0070] 3) The dried intermediate product CoS@Ni-MOFs was mixed with sulfur powder at a mass ratio of 1:5 in a ceramic boat and calcined in a nitrogen atmosphere at 350℃ for 2 hours at a heating rate of 2℃ / min. The final product Co3S4@NiS2 / C was obtained, and its SEM image is shown below. Figure 3 As shown in the image, it can be seen that it is an irregularly sized spherical structure. TEM image as follows. Figure 4 As shown.
[0071] The XRD pattern of the Co3S4@NiS2 / C composite material obtained in this embodiment is as follows: Figure 5 As shown, the obtained product is Co3S4@NiS2 / C. The XRD pattern of the CoS precursor material obtained in this embodiment is shown below. Figure 6 As shown.
[0072] Example 2 (as a comparison)
[0073] A method for preparing a cobalt tetrasulfide@nickel disulfide / carbon composite material includes the following steps:
[0074] 1) Preparation of precursors: Weigh 0.146 g Co(NO3)2·6H2O, 0.09 g urea, and 0.02775 g NH4F into a 100 mL beaker, add 40 mL of anhydrous ethanol, and stir magnetically for 20 min to dissolve. Then add 0.1878 g of thioacetamide, stir magnetically for 10 min, and transfer to a 50 mL polytetrafluoroethylene reactor. Place the reactor in an oven at 140 °C for reaction. 20h; After naturally cooling to room temperature, the product was washed four times with deionized H₂O by centrifugation, twice with ethanol, and then vacuum dried at 60°C for 12 hours. The precursor CoS precipitate was collected. Its SEM image is shown below. Figure 7 As shown in the figure, it can be seen that it is a micro-nanosphere with a size of about 500 nm.
[0075] 2) Preparation of CoS@Ni-MOFs:
[0076] 0.15 g of CoS precursor, 0.15 g of 1,3,5-pyromellitic acid, 1.033 g of polyvinylpyrrolidone (PVP, M = 58000, K 29-32), and 0.432 g of Ni(NO3)2·6H2O were weighed and added to a mixture of 15 mL ultrapure water and 15 mL DMF. The mixture was magnetically stirred for 20 min, then transferred to a 50 mL polytetrafluoroethylene reactor and reacted at 160 °C for 12 h. After naturally cooling to room temperature, the product was washed four times with deionized H2O by centrifugation and twice with ethanol. It was then vacuum dried at 60 °C for 12 h, and the CoS@Ni-MOFs precursor precipitate was collected. Its SEM image is shown below. Figure 2 As shown in the figure, it can be seen that it is a micro-nanosphere with a size of 500 nm.
[0077] 3) The dried intermediate product CoS@Ni-MOFs was mixed with sulfur powder (mass ratio 1:5) in a ceramic boat and calcined in a nitrogen atmosphere at 350℃ for 2 hours at a heating rate of 2℃ / min. The final product Co3S4@NiS2 / C was obtained, and its SEM image is shown below. Figure 8 As shown in the figure, it can be seen that it is an irregularly sized spherical structure.
[0078] Figure 7 It can be seen that the reaction time during the synthesis of CoS in Example 2 was relatively long, resulting in more burrs on the surface of the CoS precursor. The individual spheres tended to aggregate into a large mass, leading to poor morphology. When a larger amount of CoS precursor was added, the CoS concentration increased in step 2), and the product formed in the second hydrothermal reaction was an irregular spherical shape with uneven morphology.
[0079] Example 3 (as a comparison)
[0080] A method for preparing a cobalt tetrasulfide@nickel disulfide / carbon composite material includes the following steps:
[0081] 1) The preparation of the precursor is the same as in Example 1;
[0082] 2) Preparation of CoS@Ni-MOFs:
[0083] Weigh 0.1 g of CoS precursor, 0.15 g of 1,3,5-pyromellitic acid, 1.033 g of polyvinylpyrrolidone (PVP, M = 58000, K 29-32), and 0.432 g of Ni(NO3)2·6H2O into a mixed solvent of 15 mL ultrapure water and 15 mL DMF. Stir magnetically for 20 min, then transfer to a 50 mL polytetrafluoroethylene reactor and react at 160 °C for 12 h. After cooling naturally to room temperature, wash four times with deionized H2O by centrifugation, wash twice with ethanol, and dry under vacuum at 60 °C for 12 h. Collect the CoS@Ni-MOFs precursor precipitate.
[0084] 3) The dried intermediate product CoS@Ni-MOFs was mixed with sulfur powder at a mass ratio of... 1:10 The mixture was placed in a ceramic boat and calcined in a nitrogen atmosphere at 350℃ for 2 hours at a heating rate of 2℃ / min, finally yielding the product Co3S4@NiS2 / C, as shown in the SEM image below. Figure 9 As shown, the TEM image is as follows Figure 10 As shown.
[0085] With an increased proportion of sulfur powder, excess sulfur powder will first sublimate and then condense in the tube furnace, adhering to the product surface and forming hard lumps. The final product, Co3S4@NiS2 / C, has very large and numerous surface particles, resulting in a very rough sphere surface, as indicated by TEM (Precision Transformation). Figure 10 As can be seen, the morphology changes are very large. Figure 9 It can be seen that there are many particles on the surface, causing it to become an irregular sphere. Figure 10 The TEM image further confirms its irregular sphere shape.
[0086] Example 4 (as a comparison)
[0087] A method for preparing a cobalt tetrasulfide@nickel disulfide / carbon composite material includes the following steps:
[0088] 1) The preparation of the precursor is the same as in Example 1;
[0089] 2) Preparation of CoS@Ni-MOFs:
[0090] Weigh 0.1 g of CoS precursor, 0.15 g of 1,3,5-pyromellitic acid, 1.033 g of polyvinylpyrrolidone (PVP, M = 58000, K 29-32), and 0.432 g of Ni(NO3)2·6H2O into a mixture of 15 mL ultrapure water and 15 mL DMF. Stir magnetically for 20 min, then transfer to a 50 mL polytetrafluoroethylene reactor and react at 160 °C for 12 h. After cooling naturally to room temperature, wash four times with deionized H2O by centrifugation, wash twice with ethanol, and dry under vacuum at 60 °C for 12 h. Collect the CoS@Ni-MOFs precursor precipitate.
[0091] 3) The dried intermediate product CoS@Ni-MOFs was mixed with sulfur powder at a mass ratio of... 1:20 The mixture was placed in a ceramic boat and calcined in a nitrogen atmosphere at 350℃ for 2 hours at a heating rate of 2℃ / min, finally yielding the product Co3S4@NiS2 / C, as shown in the SEM image below. Figure 11 As shown, the TEM image is as follows Figure 12 As shown.
[0092] Figure 11 It can be seen that as the proportion of sulfur powder further increases, the particles on the surface of the spheres become larger, and almost all the spheres are aggregated together to form a larger, irregular sphere. There is a significant amount of sulfur powder adhering to the surface, and the particles are clearly visible. Figure 12 It can be seen that there are also many small pieces of sulfur powder next to the sphere.
[0093] Example 5 (as a comparison)
[0094] A method for preparing a cobalt tetrasulfide@nickel disulfide / carbon composite material includes the following steps:
[0095] 1) The preparation of the precursor is the same as in Example 1.
[0096] 2) The preparation of the CoS@Ni-MOFs precursor is the same as in Example 1.
[0097] 3) The dried intermediate product CoS@Ni-MOFs and sulfur powder were mixed in a ceramic boat at a mass ratio of 1:5 and calcined in a nitrogen-filled atmosphere at a calcination temperature of [temperature missing]. 550℃ The calcination time was 2 hours, and the heating rate was 2℃ / min. Ultimately, the product Co3S4@NiS2 / C could not be obtained, as shown in the SEM image below. Figure 13 As shown, the TEM image is as follows Figure 14 As shown.
[0098] At a calcination temperature of 550°C, the XRD pattern of the product is... Figure 24 This is not the same substance as in Example 1. Figure 13 , Figure 24It can be seen that although the morphology of the spheres has not changed much, the material composition has changed. The spheres prepared in Example 5 are Co3S4@Ni3S2 / NiS 1.97 / C.
[0099] The underlined data above does not meet the requirements of this invention.
[0100] Performance testing:
[0101] The product of Example 1 was used to prepare sodium batteries as anode materials for sodium-ion batteries, specifically:
[0102] Cobalt tetrasulfide@nickel disulfide / carbon composite material is used as the active material. It is mixed with conductive carbon black and PVDF in a ratio of 7:2:1 and then magnetically stirred for 6-8 hours to disperse it evenly in NMP. The uniformly mixed slurry is coated onto copper foil using a coater and placed in a vacuum drying oven at 60-80℃ for 12-24 hours. After drying, it is pressed into sheets using a tablet press and then cut into small circular electrode sheets using a cutting machine. The electrode sheets are assembled into button batteries in a glove box filled with high-purity argon gas and with water and oxygen values ≤0.01ppm. The electrolyte is NaCF3SO3+DEGDME. The sodium sheet has a purity of Na≥99.99% and a thickness of 0.5mm. After rolling, it is cut to the size of the electrode sheet.
[0103] The specific method for assembling the battery is as follows: Add one drop of electrolyte to the positive electrode shell, then place the electrode plate. Next, add one drop of electrolyte and place the glass fiber. Add three drops of electrolyte to the glass fiber and place a sodium sheet as the counter electrode. Then, place two pieces of nickel foam, add four more drops of electrolyte, cover with the negative electrode shell, and use a hydraulic press to press and seal the battery. Let it stand for 6–12 hours.
[0104] Specific testing procedure: After assembling the sodium-ion half-cell, the following steps were set on the Xinwei tester: first, constant current discharge to 0.3V, then constant current charging to 3V, repeating this cycle a certain number of times. The active material loading on the electrode plates was approximately 1.3 mg / cm³. -2 .
[0105] The test results and data are as follows:
[0106] Figure 15 The carbon-encapsulated NiS2 quantum dot composite Co3S4@NiS2 / C prepared in Example 1 is shown as a sodium-ion battery anode material at 1 A g. -1 Cyclic stability test results at current density; the circuit can cycle stably for more than 1000 cycles at this current density, demonstrating good cyclic stability.
[0107] Figure 16The current density is 0.1 A / g, and the average discharge voltage is around 1.6 V. The second and third curves have a high degree of overlap, indicating good reversibility.
[0108] Figure 17 The graph shows the rate capability of the carbon-encapsulated NiS2 quantum dot composite material Co3S4@NiS2 / C prepared in Example 1 as a sodium-ion battery anode material. As shown in the graph, the composite material can withstand a maximum current density of 10 A / g, indicating good rate performance. Furthermore, it still exhibits high capacity after two cycles of high current rate cycling, demonstrating good electrochemical performance.
[0109] Figure 18 The carbon-encapsulated NiS2 quantum dot composite material Co3S4@NiS2 / C prepared in Example 1 was used as a sodium-ion battery anode material at 2A g. -1 Cyclic stability test results at current density show that the composite material can still be stably cycled for a long time even at higher current densities, exhibiting good cyclic stability.
[0110] Figure 19 The carbon-encapsulated NiS2 quantum dot composite Co3S4@NiS2 / C prepared in Example 1 was used as a sodium-ion battery anode material at 10 A g. -1 Cyclic stability test results at current density show that the composite material can maintain stable long-term cycling even at ultra-high current densities, demonstrating its superior high-current rapid charge and discharge capability.
[0111] Figure 20 The carbon-encapsulated NiS2 quantum dot composite Co3S4@NiS2 / C prepared in Example 1 was used as a sodium-ion battery anode material at 1 A g. -1 Cyclic stability test results at current density and high temperature (50°C) show that the composite material has high temperature resistance, expanding its application scenarios.
[0112] The same performance tests were performed on Examples 2-4, and the results are as follows:
[0113] The cycle performance diagram of Example 2 is shown below. Figure 21 As shown, compared with Example 1, Example 2 had a reduced number of cycles after the hydrothermal reaction was prolonged and the CoS precursor was increased.
[0114] The cycle performance diagram of Example 3 is shown below. Figure 22 As shown, compared with Example 1, the capacity decays faster when the proportion of sulfur powder is increased.
[0115] The cycle performance diagram of Example 4 is shown below. Figure 23As shown, compared with Example 1, the capacity decays faster when the proportion of sulfur powder is further increased.
Claims
1. A method for preparing a cobalt tetrasulfide@nickel disulfide / carbon composite material, characterized in that, The preparation method includes the following steps: 1) Prepare CoS nanosphere precursors via hydrothermal reaction; 2) The CoS nanosphere precursor, organic ligand, surfactant and nickel source were mixed in a solvent and subjected to hydrothermal reaction to obtain the precursor CoS@Ni-MOFs nanospheres; 3) The precursor CoS@Ni-MOF nanospheres were mixed with sulfur powder and calcined under a protective atmosphere to obtain the Co3S4@NiS2 / C composite material; The preparation method of CoS nanospheres in step 1) is as follows: Cobalt source, NH4F and urea are dispersed in a solvent, and then a sulfur source is added. A hydrothermal reaction is then carried out to obtain CoS nanospheres; the hydrothermal reaction is conducted at 130-150℃ for 10-14 hours. The organic ligand mentioned in step 2) is 1,3,5-pyromellitic acid, and the surfactant is polyvinylpyrrolidone; In step 3), the mass ratio of the precursor CoS@Ni-MOFs nanospheres to sulfur powder is 1:5-1:9; the calcination conditions are: calcination at 350℃ for 2 hours; and the heating rate is 2℃ / min.
2. The preparation method according to claim 1, characterized in that, The molar ratio of cobalt source, sulfur source, NH4F and urea in step 1) is 1:4-5.5:1-2:2.5-3.
3. The preparation method according to claim 1, characterized in that, In step 2), the mass ratio of the CoS nanosphere precursor, organic ligand, surfactant and nickel source is 0.08-0.12 : 0.15 : 1.0-1.5 : 0.40-0.
50.
4. The preparation method according to claim 1, characterized in that, In step 2), the solvent is a mixed solution of water and N,N-dimethylformamide.
5. The preparation method according to claim 1, characterized in that, In step 2), the hydrothermal reaction conditions are 150~170℃ for 10~14h.
6. The preparation method according to claim 1, characterized in that, The calcination conditions described in step 2) are: calcination in a tube furnace.
7. A cobalt tetrasulfide@nickel disulfide / carbon composite material prepared by the preparation method according to any one of claims 1-6, characterized in that, The cobalt tetrasulfide@nickel disulfide / carbon composite material has an irregular spherical or blocky structure with a size of 1-2 μm.
8. The application of a cobalt tetrasulfide@nickel disulfide / carbon composite material prepared by the preparation method according to any one of claims 1-6, characterized in that, Sodium-ion battery anodes are prepared using sodium-ion batteries as active materials, thereby enabling the production of sodium-ion batteries.
Citation Information
Patent Citations
ASx / BSy composite heterogeneous electrode material, and preparation method and application thereof
CN113130851A
Negative electrode material, preparation method thereof and sodium ion battery
CN113937281A