A high-efficiency and durable porous geopolymer adsorbent and method thereof
The porous geopolymer adsorbent is prepared by the urea foaming method, which solves the problems of uneven pore size and high cost in the existing technology, and realizes a porous geopolymer adsorbent with uniform pores and stable structure, which has excellent CO2 adsorption performance and Durable performance, suitable for high temperature environments.
Patent Information
- Application Number
- CN202310502308.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-06
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-05-06
AI Technical Summary
In the existing preparation methods of porous geopolymer adsorbents, the pore sizes are uneven, the structure is unstable and the cost is high, which limits its widespread use in CO2 adsorbent applications.
Using urea as a foaming agent, porous geopolymers are prepared at high temperatures through chemical foaming methods. Raw materials such as metakaolin, strong alkali, sodium silicate solution and water-reducing agent are used to form porous geopolymers with uniform pores and stable structure. adsorbent.
A porous geopolymer adsorbent with low cost, uniform pores and stable structure has been realized. It has excellent CO2 adsorption performance and durability, is suitable for high temperature environments, and has a low decomposition rate in acidic media.
Smart Images

Figure CN116474743B_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of adsorbents and relates to a preparation method of an adsorbent and an application thereof. Background Art
[0002] With the development of industrialization, the emission of large amounts of CO2 poses a severe challenge to human survival. It is of great practical significance to study an adsorbent that can effectively absorb CO2.
[0003] Geopolymers are a type of three-dimensional network structure material composed of silicon-oxygen tetrahedrons and aluminum-oxygen tetrahedrons. The raw materials can be natural minerals or industrial wastes containing aluminosilicates. These aluminosilicates can react with strong alkaline solutions at room temperature to 150°C to break and recombine silicon-oxygen and aluminum-oxygen bonds, thereby solidifying and forming a three-dimensional network structure. Geopolymer raw materials are widely available, easy to prepare, and have low energy consumption. At the same time, the molecular sieve-like structure of geopolymers gives them excellent adsorption capacity. In addition, on the basis of preparing geopolymers, they are prepared into porous structures by foaming, which can effectively increase the contact area between the material and CO2 and improve its adsorption capacity. Therefore, porous geopolymers are a very promising CO2 gas adsorbent.
[0004] At present, there have been many studies on the preparation methods of porous geopolymer adsorbents. Chinese patent application number CN112079586A discloses a method for preparing porous geopolymers using hydrogen peroxide. The invention uses hydrogen peroxide to react with some substances in the raw materials to produce bubbles to prepare porous geopolymers. The pores of the material prepared by this method are unevenly distributed and the size is difficult to control; Li Juan et al. (Industrial Technology Innovation, 2022, 9(5): 40-45) used sodium hypochlorite to prepare porous geopolymers, and then added 13X molecular sieves to the porous geopolymer matrix to prepare zeolite-porous geopolymer composites. Porous material; Chinese patent application number CN110694595A prepares a porous geopolymer by hydrogen peroxide, and then impregnates a layer of metal-organic skeleton on its surface. Both methods make the porous geopolymer and other adsorbent materials be compounded into a composite material, and the preparation process is complicated and cumbersome; Chinese patent application number CN112079585B discloses a preparation method for porous geopolymer by microporous foaming, but the silicon carbide used in this method is expensive, which limits its wide application as an adsorbent.
[0005] Therefore, preparing a porous geopolymer adsorbent with uniform pore size, stable structure, high efficiency, durability and low cost is of great significance for practical applications. Summary of the invention
[0006] In view of this, the purpose of the present invention is to provide a novel method for preparing a porous geopolymer adsorbent, wherein urea is used as a foaming agent, and the porous geopolymer is prepared by a chemical foaming method in which urea is decomposed into ammonia at high temperature. The use of urea not only reduces the cost of raw materials, but also makes the prepared porous geopolymer have uniform pores and a stable structure, so that the adsorbent has excellent CO2 adsorption performance and durability.
[0007] In order to achieve the above purpose, the technical solution is as follows:
[0008] A highly efficient and durable porous geopolymer adsorbent comprises the following raw material components by weight: 30-40 parts of metakaolin, 5-10 parts of strong alkali, 40-60 parts of sodium silicate solution, 3-5 parts of water reducing agent and 1-10 parts of foaming agent.
[0009] Preferably, the strong base is selected from one or a mixture of sodium hydroxide, barium hydroxide, lithium hydroxide, and quaternary ammonium hydroxide.
[0010] Preferably, the water reducing agent is selected from one of lignin, naphthalene, melamine and polycarboxylic acid.
[0011] Preferably, the foaming agent is urea.
[0012] Preferably, a weighed strong alkali powder is mixed with a sodium silicate solution to prepare an alkali activator, and after it is cooled to room temperature, a foaming agent is added to the prepared alkali activator solution and stirred evenly, and kaolin and a water reducer are added to form a geopolymer slurry, which is stirred evenly, sealed and solidified, and after curing, a porous geopolymer is obtained, which is demoulded and then ground and sieved to form a powder to obtain a porous geopolymer adsorbent.
[0013] Preferably, the concentration of the sodium silicate solution is 22 wt %.
[0014] Preferably, the curing temperature in the preparation process is 80-120° C., and the curing time is 12-48 hours; the curing temperature is 25-60° C., and the curing time is 3-9 days.
[0015] Preferably, the porous geopolymer is crushed, ground and passed through an 80-mesh sieve, and the adsorbent particle size is less than 200 microns.
[0016] Preferably, the mechanical stirring speed is 300-1500 rpm when the alkaline activator is prepared and mixed, and the mixture is left to stand for 1-3 hours after mixing. The pH value of the prepared alkaline activator is 13.
[0017] Preferably, when urea is added to the prepared alkaline activator solution and stirred evenly, the mechanical stirring speed is 300-1500 rpm; when metakaolin is added to form a geopolymer slurry, the stirring speed is 1500-2500 rpm; and the slurry is placed in a polytetrafluoroethylene or stainless steel mold for sealing and curing.
[0018] Normal temperature refers to 4-38 degrees Celsius.
[0019] Beneficial effects:
[0020] (1) The porous geopolymer adsorbent of the present invention has abundant raw material sources, simple preparation process, low energy consumption, and is environmentally friendly;
[0021] (2) The present invention uses urea as a foaming agent, which is low in cost and produces porous geopolymers with uniform pores, stable structure, strong adsorption performance, easy regeneration, and good reusability;
[0022] (3) The porous geopolymer adsorbent of the present invention has strong high temperature resistance, does not oxidize or decompose at 1000-1200°C, and can be used at a maximum temperature of 1400°C;
[0023] (4) The porous geopolymer adsorbent of the present invention not only has high durability in alkaline media, but also has a low decomposition rate in acidic media. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION
[0025] like Figure 1 As shown, in order to better understand the contents of the present invention, the present invention is further described in detail through specific embodiments below, so that those skilled in the art can implement it according to the text of the description, but the protection scope of the present invention is not limited to the contents.
[0026] Example 1: At 25°C, 20.0g of sodium hydroxide powder was mixed with 163.0g of sodium silicate solution, stirred evenly and then allowed to stand for 1h. After cooling to room temperature, 2.9g of urea was added and mechanically stirred evenly, followed by adding 100.0g of metakaolin and 8.57g of lignin to form a geopolymer slurry, which was stirred until viscous and then placed in a planetary mixer for 10min for mixing. The mixed slurry was poured into a 100mm×100mm×20mm polytetrafluoroethylene mold and sealed. After curing in a 100°C oven for 24h, it was placed in a 40°C oven for curing for 7d, and then the seal was removed, the porous geopolymer product was taken out for grinding, and the porous geopolymer adsorbent powder was obtained by passing through an 80-mesh sieve. The specific surface area and pore structure of the sample were measured using a fully automatic specific surface area and porosity analyzer. The pore size distribution was calculated using the Barrett-Joyner-Halenda (BJH) model. The sample adsorption effect was tested using a static volumetric test. 0.1-0.2 g of dry sample was weighed by the differential method and loaded into an analysis tube. The tube was first installed at the degassing station port, degassed at 100°C for 7 hours, and then manually transferred to the analysis station port for an adsorption performance test. The 24-hour static CO2 adsorption capacity was measured to be 1.95 mmol / g.
[0027] Example 2: At 25°C, 25.0g of sodium hydroxide powder was mixed with 100.0g of sodium silicate solution, stirred evenly and then allowed to stand for 1h. After cooling to room temperature, 25.0g of urea was added and mechanically stirred evenly, followed by adding 100.0g of metakaolin and 10.00g of lignin to form a geopolymer slurry, which was stirred until viscous and then placed in a planetary mixer for 10min for mixing. The mixed slurry was poured into a 100mm×100mm×20mm polytetrafluoroethylene mold and sealed. After curing in an oven at 80°C for 12h, it was placed in an oven at 25°C for curing for 3d, and then the seal was removed, the porous geopolymer product was taken out for grinding, and the porous geopolymer adsorbent powder was obtained by passing through an 80-mesh sieve. The specific surface area and pore structure of the sample were measured using a fully automatic specific surface area and porosity analyzer. The pore size distribution was calculated using the Barrett-Joyner-Halenda (BJH) model. The sample adsorption effect was tested using a static volumetric test. 0.1-0.2 g of dry sample was weighed by the differential method and loaded into an analysis tube. The tube was first installed at the degassing station port, degassed at 100°C for 7 hours, and then manually transferred to the analysis station port for an adsorption performance test. The 24-hour static CO2 adsorption capacity was measured to be 2.18 mmol / g.
[0028] Example 3: At 25°C, 15.0g of sodium hydroxide powder was mixed with 180.0g of sodium silicate solution, stirred evenly and then allowed to stand for 1h. After cooling to room temperature, 15.0g of urea was added and mechanically stirred evenly, followed by adding 100.0g of metakaolin and 16.67g of lignin to form a geopolymer slurry, which was stirred until viscous and then placed in a planetary mixer for 10min for mixing. The mixed slurry was poured into a 100mm×100mm×20mm polytetrafluoroethylene mold and sealed. After curing in a 120°C oven for 48h, it was placed in a 60°C oven for curing for 9d, and then the seal was removed, the porous geopolymer product was taken out for grinding, and the porous geopolymer adsorbent powder was obtained by passing through an 80-mesh sieve. The specific surface area and pore structure of the sample were measured using a fully automatic specific surface area and porosity analyzer. The pore size distribution was calculated using the Barrett-Joyner-Halenda (BJH) model. The sample adsorption effect was tested using a static volumetric test. 0.1-0.2 g of dry sample was weighed by the differential method and loaded into an analysis tube. The tube was first installed at the degassing station port, degassed at 100°C for 7 hours, and then manually transferred to the analysis station port for an adsorption performance test. The 24-hour static CO2 adsorption capacity was measured to be 2.32 mmol / g.
[0029] The weight proportions of the components, curing temperature, curing time, curing temperature and curing time in the above three embodiments are plotted in Table 1 below:
[0030] Table 1
[0031]
[0032] The specific surface area, average pore size, and CO2 gas adsorption capacity of the above three examples are plotted in Table 2 below:
[0033] Table 2
[0034]
[0035] It can be seen from the above table that the porous geopolymer adsorbent foamed with urea has uniform pores, large specific surface area and excellent CO2 adsorption performance.
[0036] The above is only a preferred implementation of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present application. These improvements and modifications should also be regarded as the scope of protection of the present application.
Claims
1. A highly efficient and durable porous geopolymer adsorbent, characterized in that: The raw material components by weight include 30-40 parts of metakaolin, 5-10 parts of strong alkali, 40-60 parts of sodium silicate solution, 3-5 parts of water reducing agent and 1-10 parts of foaming agent, wherein the foaming agent is urea.
2. The highly efficient and durable porous geopolymer adsorbent according to claim 1, characterized in that: The strong base is selected from one or a mixture of sodium hydroxide, barium hydroxide, lithium hydroxide and quaternary ammonium hydroxide.
3. The highly efficient and durable porous geopolymer adsorbent according to claim 2, characterized in that: The water reducing agent is selected from one of lignin, naphthalene, melamine and polycarboxylic acid.
4. The method for preparing a highly efficient and durable porous geopolymer adsorbent according to claim 1, characterized in that: The weighed strong alkali powder is mixed with the sodium silicate solution to prepare an alkali activator. After it is cooled to room temperature, the foaming agent is added to the prepared alkali activator solution and stirred evenly. Kaolin and a water reducer are added to form a geopolymer slurry. After stirring evenly, sealing and curing, a porous geopolymer is obtained after curing, demolding, and then grinding and sieving to form a powder to obtain a porous geopolymer adsorbent.
5. The method for preparing a highly efficient and durable porous geopolymer adsorbent according to claim 4, characterized in that: The concentration of the sodium silicate solution was 22 wt%.
6. The method for preparing a highly efficient and durable porous geopolymer adsorbent according to claim 4, characterized in that: The curing temperature during the preparation process is 80-120° C., and the curing time is 12-48 hours; the curing temperature is 25-60° C., and the curing time is 3-9 days.
7. The method for preparing a highly efficient and durable porous geopolymer adsorbent according to claim 4, characterized in that: The porous geopolymer is crushed, ground and passed through an 80-mesh sieve, and the adsorbent particle size is less than 200 microns.
8. The method for preparing a highly efficient and durable porous geopolymer adsorbent according to claim 4, characterized in that: When preparing the alkaline activator and mixing it evenly, the mechanical stirring speed is 300 to 1500 rpm. After mixing evenly, the mixture is left to stand for 1 to 3 hours. The pH value of the prepared alkaline activator is 13.
9. The method for preparing a highly efficient and durable porous geopolymer adsorbent according to claim 4, characterized in that: When urea is added to the prepared alkaline activator solution and stirred evenly, the mechanical stirring speed is 300 to 1500 rpm; When metakaolin and water reducing agent are added to form geopolymer slurry, the stirring speed is 1500-2500 rpm; the slurry is placed in a polytetrafluoroethylene or stainless steel mold for sealing and curing.