Cross-linkable polymer composition, cross-linked polymer material, metal component and wiring harness

Through the use of cross-linked polymer compositions, the problems of heat resistance and simplicity of coating films in metal surface corrosion protection methods are solved, the formation of uniform coating films with high corrosion resistance and heat resistance is achieved, and the process is simplified. coating process and improves storage stability.

CN116490552BActive Publication Date: 2024-10-01AUTONETWORKS TECH LTD +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180073313.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-11-16
Filing Date
2021-10-28
Publication Date
2024-10-01
Estimated Expiration
2041-10-28

AI Technical Summary

Technical Problem

Existing metal surface anti-corrosion methods are difficult to balance heat resistance and simplicity of coating. The viscosity of grease decreases when heated and it is difficult to form a uniform coating. Curable materials take a long time to cure and are difficult to spread uniformly in non-light irradiated parts. solidify.

Method used

It adopts a cross-linked polymer composition, including component A which liberates metal ions through heat, component B which forms ionic bonding substituents with metal ions, and component C which is an acidic phosphate ester and forms a phosphate ester salt through heat to achieve metal adsorption and Cross-linked to form a coating film with high corrosion resistance and heat resistance.

Benefits of technology

It achieves the formation of a uniform coating film with high corrosion resistance and heat resistance in a short time, can be easily coated on the metal surface, and maintains good storage stability and corrosion resistance at room temperature.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116490552B_ABST
    Figure CN116490552B_ABST
Patent Text Reader

Abstract

Provided are a cross-linked polymer composition and a cross-linked polymer material having high corrosion resistance and heat resistance and capable of easily forming a highly uniform coating film, and a metal component and a wiring harness using the cross-linked polymer composition and the cross-linked polymer material. The cross-linked polymer composition comprises: a component A, wherein the component A releases metal ions by heat; a component B, wherein the component B is composed of an organic polymer having a substituent capable of ionically bonding with the metal ions released from the component A; and a component C, wherein the component C is composed of one or more of acidic phosphates having a hydrocarbon group having 4 or more and 30 or less carbon atoms. The valence of the metal ion released from the component A is set to +y, and the content is set to m mol, the valence of the substituent contained in the component B is set to ‑z, and the content is set to n mol, the valence of the acidic phosphate constituting the component C is set to ‑x, and the content is set to 1 mol, and in g=(m·y‑l·x) / (n·z), g≥0.1.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a cross-linkable polymer composition, a cross-linked polymer material, a metal member, and a wiring harness. Background Art

[0002] Grease is sometimes used in metal equipment and metal parts for the purpose of corrosion protection. For example, Patent Document 1 describes the use of grease containing a perfluoroether base oil, a thickener, barium sulfate or antimony oxide in mechanical parts.

[0003] As a method of imparting corrosion resistance to metal equipment and metal parts, there is also a method of protecting the surface using various curing materials. As curing materials, various curing methods such as photocuring materials, moisture curing materials, anaerobic curing materials, cationic curing materials, anionic curing materials, and thermosetting materials are known. For example, Patent Document 2 describes the use of epoxy curing materials as thermosetting materials.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: International Publication No. 2007 / 052522

[0007] Patent Document 2: Japanese Patent Application Publication No. 2016-098333

[0008] Patent Document 3: Japanese Patent Application Publication No. 2015-151614

[0009] Patent Document 4: Japanese Patent Application Publication No. 2017-179040 Summary of the invention

[0010] Problems to be solved by the invention

[0011] When using grease for corrosion protection of metal surfaces, it is difficult to strike a balance between heat resistance and ease of forming a coating. Grease is a substance in which a thickener is dispersed in a base oil, and its viscosity decreases significantly when heated. Therefore, when applying grease to a metal surface, it is easy to apply by heating, but on the other hand, when heat is applied to the coating film, the grease flows out, so the heat resistance of the grease coating film tends to decrease. By selecting a thickener, the grease can be made less likely to flow out even under high temperature conditions, but in this case, the heating temperature required for applying to the metal surface also becomes higher, making it difficult to form a uniform coating.

[0012] On the other hand, when using various curing materials to protect the metal surface, it is difficult to balance the ease of forming the coating and the uniformity of the coating. Moisture curing materials, cationic curing materials, anionic curing materials, and thermosetting materials usually require a long time to cure, and it cannot be said that a coating can be easily formed. Anaerobic curing materials need to block oxygen during curing, and in this case, it cannot be said that a coating can be easily formed. The curing speed of light-curing materials is relatively fast, but it is difficult to cure parts that are difficult to irradiate with light, and it is difficult to form a coating with high uniformity.

[0013] The problem to be solved by the present disclosure is to provide a crosslinkable polymer composition and a crosslinked polymer material having high corrosion resistance and heat resistance and capable of easily forming a highly uniform coating film, and a metal component and a wiring harness using the crosslinkable polymer composition and the crosslinked polymer material.

[0014] Means for solving problems

[0015] The crosslinkable polymer composition according to the present disclosure has the following configuration.

[0016] The cross-linkable polymer composition comprises:

[0017] A component, wherein the A component releases metal ions by heat;

[0018] A component B, the component B being composed of an organic polymer having a substituent capable of ionically bonding with the metal ion released from the component A; and

[0019] Component C, wherein the component C is composed of one or more of the acidic phosphates represented by the following general formula (C1) and general formula (C2),

[0020] The valence of the metal ion released from the component A is +y, and the content of the metal ion is m mol; the valence of the substituent contained in the component B is -z, and the content of the substituent is n mol; the valence of the acidic phosphate constituting the component C is -x, and the content of the acidic phosphate is 1 mol,

[0021] In g = (m·yl·x) / (n·z), g ≥ 0.1,

[0022] P(=O)(-OR)(-OH)2(C1)

[0023] P(=O)(-OR)2(-OH)(C2)

[0024] Here, R is a hydrocarbon group having 4 to 30 carbon atoms.

[0025] Furthermore, the cross-linked polymer material according to the present disclosure is a cross-linked product of the cross-linkable polymer composition according to the present disclosure, and the component B is cross-linked via the metal ions released from the component A.

[0026] Furthermore, the metal component according to the present disclosure includes a metal substrate and a coating material that covers the surface of the metal substrate, and the coating material is composed of the cross-linked polymer material according to the present disclosure.

[0027] Furthermore, the wiring harness according to the present disclosure includes the cross-linked polymer material according to the present disclosure.

[0028] Effects of the Invention

[0029] According to the crosslinkable polymer composition according to the present disclosure, a coating film having high corrosion resistance and heat resistance and high uniformity can be easily formed. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] [ Figure 1 ] Figure 1 This is a cross-sectional view of a metal member according to one embodiment of the present disclosure.

[0031] [ Figure 2 ] Figure 2 This is a perspective view of a wire harness according to one embodiment of the present disclosure.

[0032] [ Figure 3 ] Figure 3 for Figure 2 Longitudinal section view along line AA. DETAILED DESCRIPTION

[0033] [Description of Embodiments of the Present Disclosure]

[0034] First, embodiments of the present disclosure are listed and described.

[0035] (1) The crosslinkable polymer composition according to the present disclosure has the following configuration.

[0036] The cross-linkable polymer composition comprises:

[0037] A component, wherein the A component releases metal ions by heat;

[0038] A component B, the component B being composed of an organic polymer having a substituent capable of ionically bonding with the metal ion released from the component A; and

[0039] Component C, wherein the component C is composed of one or more of the acidic phosphates represented by the following general formula (C1) and general formula (C2),

[0040] The valence of the metal ion released from the component A is +y, and the content of the metal ion is m mol; the valence of the substituent contained in the component B is -z, and the content of the substituent is n mol; the valence of the acidic phosphate constituting the component C is -x, and the content of the acidic phosphate is 1 mol,

[0041] In g = (m·yl·x) / (n·z), g ≥ 0.1,

[0042] P(=O)(-OR)(-OH)2(C1)

[0043] P(=O)(-OR)2(-OH)(C2)

[0044] Here, R is a hydrocarbon group having 4 to 30 carbon atoms.

[0045] The cross-linkable polymer composition involved in the present disclosure cross-links the B component via the metal ions released from the A component by heat. Therefore, after heating, a coating film with high heat resistance can be formed. In addition, the C component forms a phosphate with the metal ions released from the A component, becoming a metal adsorption component, so that the cross-linkable polymer composition exerts high corrosion resistance. On the other hand, the cross-linkable polymer composition involved in the present disclosure is in a state of high fluidity without heating, so it can be applied to a metal surface with high uniformity. Then, only by heating, a coating film with excellent corrosion resistance and heat resistance is formed as described above, so a coating film with high uniformity can be easily formed. In addition, by making g≥0.1, a sufficient amount of metal ions for cross-linking the B component are released from the A component, so that curing caused by cross-linking can be performed in a short time, forming a coating film with excellent corrosion resistance and heat resistance.

[0046] (2) The component A may have a decomposition point or a phase transition point at 50°C or higher and 200°C or lower. This is because, when preparing the cross-linkable polymer composition or before using the cross-linkable polymer composition, it is easy to suppress the release of metal ions from the component A, and the curing of the cross-linkable polymer composition can be suppressed, so that the coating property at low temperatures such as room temperature is excellent, and the storage stability such as suppressing the quality change during the storage of the cross-linkable polymer composition at low temperatures such as room temperature is excellent. In addition, this is because at an appropriate temperature, due to the decomposition or phase change of the component A, the metal ions are easily released from the component A, and when the cross-linkable polymer composition is used, the curing speed is excellent.

[0047] (3) The component A may be a metal complex. This is because the ligand has an excellent stabilizing effect on metal ions, and can suppress the release of metal ions from the component A during the preparation of the crosslinkable polymer composition and before the use of the crosslinkable polymer composition. In addition, when the crosslinkable polymer composition is used, the metal ions are easily released from the component A by heat.

[0048] (4) The component A may be a metal complex containing a multidentate ligand or a cross-linked ligand. This is because the coordination of the multidentate ligand or the cross-linked ligand is more excellent in stabilizing the metal ions than the non-cross-linked coordination of the monodentate ligand, so when preparing the cross-linkable polymer composition or before using the cross-linkable polymer composition, the release of metal ions from the component A can be further suppressed.

[0049] (5) The component A may be a metal complex containing a β-diketone ligand or an alkoxide ligand. The β-diketone ligand and the alkoxide ligand stably coordinate with the metal ion. In addition, the β-diketone ligand and the alkoxide ligand easily form a multidentate coordination or a cross-linked coordination. In this case, the stabilization effect of the ligand on the metal ion is more excellent compared with the non-cross-linked coordination of the monodentate ligand. When preparing the cross-linkable polymer composition and before using the cross-linkable polymer composition, the release of the metal ion from the component A can be further suppressed.

[0050] (6) The metal of the metal ion released from the component A may be at least one of alkaline earth metals, zinc, titanium, and aluminum. This is because the ions of these metals have a valence of 2 or more, and the crosslinked polymer material composed of the crosslinked product of the crosslinkable polymer composition has excellent stability. In addition, this is because when forming a phosphate ester salt with the component C, it shows high adsorption to the metal surface.

[0051] (7) The substituent of the component B may be an electron-withdrawing group because it is easy to form an ionic bond with the metal ion released from the component A.

[0052] (8) The substituent of the component B may be at least one of a carboxylic acid group, an acid anhydride group, a phosphoric acid group, and a sulfonic acid group. This is because it is easy to form an ionic bond with the metal ion released from the component A.

[0053] (9) The component B may be in a liquid state at 150° C. or lower. This is because the crosslinkable polymer composition can be applied to a metal surface or the like at a relatively low temperature.

[0054] (10) The component A may be contained in an amount of 1 part by mass or more and 30 parts by mass or less per 100 parts by mass of the component B. This is because the crosslinkable polymer composition has excellent crosslinking properties and the effects of a large amount of the component A, such as separation and precipitation, can be easily avoided.

[0055] (11) The component C may be contained in an amount of 1 part by mass or more and 30 parts by mass or less based on 100 parts by mass of the component B. This is because the crosslinkable polymer composition exhibits high corrosion resistance and the effects of a large amount of the component C, such as separation and precipitation of the component C, are easily avoided.

[0056] (12) Furthermore, the cross-linked polymer material of the present disclosure is a cross-linked product of the cross-linkable polymer composition of the present disclosure, and the component B is cross-linked via the metal ions released from the component A. Therefore, the cross-linked polymer material has high corrosion resistance and heat resistance, and can be easily formed into a coating film with high uniformity.

[0057] (13) Furthermore, the metal component of the present disclosure comprises a metal substrate and a coating material coating the surface of the metal substrate, wherein the coating material is composed of the cross-linked polymer material of the present disclosure. Therefore, the metal component has excellent corrosion resistance and maintains a high corrosion resistance even when heated.

[0058] (14) Furthermore, the wire harness of the present disclosure contains the cross-linked polymer material of the present disclosure. Therefore, the wire harness has excellent corrosion resistance and maintains a high corrosion resistance even when heated.

[0059] [Details of the embodiments of the present disclosure]

[0060] Hereinafter, specific examples of the crosslinkable polymer composition, crosslinked polymer material, metal member, and wire harness of the present disclosure will be described with reference to the drawings. It should be noted that the present disclosure is not limited to these examples.

[0061] [1] Cross-linkable polymer composition and cross-linked polymer material

[0062] The crosslinkable polymer composition involved in the present disclosure includes: component A, which releases metal ions by heat; component B, which is composed of an organic polymer having a substituent capable of ionically bonding with the metal ions released from component A; and component C, which is composed of an acidic phosphate having a predetermined structure. The crosslinkable polymer composition involved in the present disclosure is heated to crosslink component B via the metal ions released from component A, thereby causing curing to constitute the crosslinked polymer material involved in the embodiment of the present disclosure. Component C forms a phosphate salt with the metal ions released from component A and functions as a metal adsorption component.

[0063] (1)A component

[0064] Component A is a component that releases metal ions by heat. By heat means that heating is assumed, and a temperature higher than room temperature is assumed. Metal ion release means that metal ions are released from component A by decomposition or phase change of component A. The metal ions released from component A cause crosslinking of component B and formation of a metal salt with component C.

[0065] Component A preferably has a decomposition point or phase transition point at 50°C or more and 200°C or less. This is because, when preparing a cross-linkable polymer composition and before using the cross-linkable polymer composition (before heating), it is easy to suppress the release of metal ions from component A, and the curing of the cross-linkable polymer composition can be suppressed, so that the cross-linkable polymer composition can be easily applied at a low temperature such as room temperature, and the quality change of the cross-linkable polymer composition during storage at a low temperature such as room temperature is suppressed. Such storage stability is excellent. In addition, this is because by decomposing or changing the phase of component A at an appropriate temperature, metal ions are easily released from component A, and when the cross-linkable polymer composition is used, the curing speed is excellent. From the above viewpoints, component A can have a decomposition point or phase transition point at more preferably 60°C or more, and more preferably 70°C or more. In addition, from the above viewpoints, component A can have a decomposition point or phase transition point at more preferably 150°C or less, and more preferably 120°C or less. The decomposition point or phase transition point of component A is represented by the baseline change start temperature measured by differential scanning calorimetry (DSC) (measurement temperature range: 25°C to 200°C, measured in the air). It should be noted that the above phase transition point does not include the melting point, and the above phase transition does not include melting.

[0066] As the metal of the metal ion released from component A, alkaline earth metals, zinc, titanium, aluminum, iron, nickel, copper, zirconium, etc. can be listed. The metal of the above-mentioned metal ion can be at least one of these metals. The metal of the above-mentioned metal ion can be composed of only one of these metals, or it can be composed of two or more. As the metal of the above-mentioned metal ion, it is preferably at least one of alkaline earth metals, zinc, titanium, and aluminum. This is because the metal ions of these metals are valences of more than two valences, and it is easy to crosslink organic polymers, and the stability of the crosslinked polymer material composed of the crosslinked body of the crosslinkable polymer composition is excellent. Moreover, among the above-mentioned preferred metal species, zinc is particularly preferred. This is because the stability of the crosslinked polymer material composed of the crosslinked body of the crosslinkable polymer composition is particularly excellent. In addition, the alkaline earth metals, zinc, titanium, and aluminum listed as preferred substances above are metals of more than two valences, and the ionization tendency is relatively high, so a phosphate salt showing high adsorption to the metal surface can be formed between the C component.

[0067] As component A, metal complexes and the like can be cited. The metal complex is composed of a product in which a metal ion serving as a center is coordinated with a ligand having an unshared electron pair. Component A is preferably a metal complex. This is because the ligand has an excellent stabilizing effect on metal ions, and when preparing a crosslinkable polymer composition and before using the crosslinkable polymer composition, the metal ions can be inhibited from being freed from component A, and when the crosslinkable polymer composition is used, the metal ions are easily freed from component A by heat.

[0068] The ligand of metal complex has a group with a lone electron pair, and the group is coordinated with the metal ion to form a metal complex. As a ligand, the monodentate ligand with a coordination site of 1 and the multidentate ligand with a coordination site of more than 2 can be enumerated. The metal complex generated by the multidentate ligand is due to the chelating effect, and stability is more excellent compared with the metal complex generated by the monodentate ligand. In addition, as a ligand, there is a non-crosslinked ligand of a ligand and a metal ion coordination, a ligand and a crosslinked ligand of more than two metal ion coordinations. The crosslinked ligand is sometimes composed of a monodentate ligand, and sometimes also composed of a multidentate ligand.

[0069] Component A is preferably a metal complex containing a multidentate ligand or a cross-linked ligand. This is because the coordination of the multidentate ligand or the cross-linked ligand is more excellent in stabilizing the metal ions than the non-cross-linked coordination of the monodentate ligand, so when preparing the cross-linkable polymer composition or before using the cross-linkable polymer composition, the release of metal ions from component A can be further suppressed.

[0070] As the ligand of the metal complex, β-diketone ligand (1,3-diketone ligand), alkoxide ligand, etc. can be listed. β-diketone ligand is represented by the following general formula (1). Alkoxide ligand is represented by the following general formula (2). As β-diketone ligand, acetylacetone ligand (acac), 2,2,6,6-tetramethyl-3,5-heptanedione ligand (dpm), 3-methyl-2,4-pentanedione ligand, 3-ethyl-2,4-pentanedione ligand, 3,5-heptanedione ligand, 2,6-dimethyl-3,5-heptanedione ligand, 1,3-diphenyl-1,3-propanedione ligand, etc. can be listed. As alkoxide ligand, methoxide ligand, ethoxide ligand, isopropoxide ligand, n-propoxide ligand, n-butoxide ligand, etc. can be listed.

[0071] [Chemistry 1]

[0072]

[0073] In formula (1), R1, R2, and R3 represent hydrocarbon groups. R1, R2, and R3 may be hydrocarbon groups of the same structure or hydrocarbon groups of different structures. R1, R2, and R3 may be aliphatic hydrocarbon groups or hydrocarbon groups containing aromatic rings. R1, R2, and R3 may be hydrocarbon groups having a carbon number of 1 or more and 10 or less. R3 may be hydrogen. This also includes the case where at least two of R1, R2, and R3 are connected to each other through a ring structure.

[0074] [Chemistry 2]

[0075] R4-O - ...(2)

[0076] In formula (2), R4 represents a hydrocarbon group. R4 may be an aliphatic hydrocarbon group or a hydrocarbon group containing an aromatic ring. R4 may be a hydrocarbon group having 1 to 10 carbon atoms.

[0077] Component A can be a metal complex containing a β-diketone ligand or an alkoxide ligand. β-diketone ligands and alkoxide ligands stably coordinate with metal ions. In addition, this is because β-diketone ligands and alkoxide ligands easily form multidentate coordination or cross-linked coordination. In this case, compared with the non-cross-linked coordination of monodentate ligands, the stabilization effect of the ligand on metal ions is excellent, and when preparing a cross-linkable polymer composition, before using the cross-linkable polymer composition, the metal ions can be further suppressed from being freed from component A.

[0078] (2) Component B

[0079] Component B is a component composed of an organic polymer having a substituent capable of ionically bonding with the metal ions released from component A. As substituents capable of ionically bonding with metal ions, carboxylic acid groups, acid anhydride groups, phosphoric acid groups, sulfonic acid groups, etc. can be cited. The above-mentioned substituents do not include hydroxyl groups. The above-mentioned substituents can be one of the exemplified substituents, or two or more. The above-mentioned substituents can be at least one of the exemplified substituents. This is because it is easy to form ionic bonds with the metal ions released from component A. In addition, the above-mentioned substituents can be electron-withdrawing groups. This is because it is easy to form ionic bonds with the metal ions released from component A.

[0080] The content of the above-mentioned substituent in component B is not particularly limited, but from the viewpoint of ensuring physical properties by crosslinking, it is preferably 0.01% by mass or more and 10% by mass or less. It is more preferably 0.1% by mass or more and 5% by mass or less, and further preferably 0.2% by mass or more and 3% by mass or less. The content of the above-mentioned substituent in component B can be obtained by comparing the size of the substituent characteristic peak in the infrared spectrum with the size of the spectrum peak of the material with known content.

[0081] The organic polymer of component B is an organic polymer such as resin, rubber, and elastomer. Component B may be liquid at room temperature or solid at room temperature, but is preferably liquid below 150°C. This is because the crosslinkable polymer composition can be applied to a metal surface or the like at a relatively low temperature. In addition, component B may be liquid at room temperature. This is because the crosslinkable polymer composition can be applied to a metal surface or the like at room temperature. In addition, this is because the preparation of the crosslinkable polymer composition becomes easy. It should be noted that not only the individual component B, but also the crosslinkable polymer composition as a whole is preferably liquid below 150°C and further at room temperature. In addition, component B preferably has a molecular weight of 1000 or more. This is because even if it is liquid at room temperature, it is easy to solidify by crosslinking. On the other hand, from the viewpoint of being easy to become liquid at room temperature, component B preferably has a molecular weight of 100,000 or less. More preferably, the molecular weight is 50,000 or less. The molecular weight of component B is represented by the number average molecular weight (Mn) obtained by gel permeation chromatography (GPC) analysis.

[0082] As the organic polymer of component B, there can be listed: polyolefin, polybutadiene, polyisoprene, polyacrylate, polymethacrylate, polyurethane, polyester, organopolysiloxane (silicone resin) etc. The substituent of component B can be a substituent introduced into the main chain of the organic polymer, or a substituent introduced into the side chain. As the organic polymer of component B, from the viewpoints of ensuring fluidity at room temperature, polybutadiene and polyisoprene are particularly preferred. In this specification, organic polymer also includes polymers with relatively low polymerization degree such as oligomers.

[0083] (3) Component C

[0084] The component C is composed of one or two or more of the acidic phosphates represented by the following general formula (C1) and general formula (C2).

[0085] P(=O)(-OR)(-OH)2(C1)

[0086] P(=O)(-OR)2(-OH)(C2)

[0087] Here, R is a hydrocarbon group having 4 to 30 carbon atoms.

[0088] Component C forms a metal salt with the metal ions released from component A by heating. The metal salt becomes a metal adsorption component adsorbed on the metal surface, etc. The metal adsorption component exhibits an anticorrosion property to protect the metal surface from corrosion.

[0089] As the hydrocarbon group R constituting the acidic phosphate ester represented by the above formula (C1) and formula (C2), by using a hydrocarbon group having a carbon number of 4 or more and 30 or less, component C shows high compatibility with component B, so component C is difficult to agglomerate in the cross-linkable polymer composition and shows high dispersibility. Even after component C forms a salt with the metal ions released from component A by heat, it is dispersed in component B cured by ionic crosslinking and maintains metal adsorption. From the viewpoint of improving dispersibility, the carbon number of the hydrocarbon group is more preferably 5 or more, and more preferably 6 or more. In addition, it is more preferably 26 or less, and more preferably 22 or less. As the hydrocarbon group R, alkyl, cycloalkyl, alkyl-substituted cycloalkyl, alkenyl, aryl, alkyl-substituted aryl and aralkyl can be listed.

[0090] Examples of the alkyl group include butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl, undecyl, dodecyl, tridecyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, and octadecyl. These alkyl groups may be linear or branched.

[0091] Examples of the cycloalkyl group include cyclopentyl, cyclohexyl, and cycloheptyl. Examples of the alkyl-substituted cycloalkyl group include methylcyclopentyl, dimethylcyclopentyl, methylethylcyclopentyl, diethylcyclopentyl, methylcyclohexyl, dimethylcyclohexyl, methylethylcyclohexyl, diethylcyclohexyl, methylcycloheptyl, dimethylcycloheptyl, methylethylcycloheptyl, and diethylcycloheptyl. There is no particular limitation on the substitution position of the alkyl-substituted cycloalkyl group. The alkyl group may be linear or branched.

[0092] Examples of the alkenyl group include butenyl, pentenyl, hexenyl, heptenyl, octenyl, nonenyl, decenyl, undecenyl, dodecenyl, tridecenyl, tetradecenyl, pentadecenyl, hexadecenyl, heptadecenyl, octadecenyl, etc. These alkenyl groups may be straight-chain or branched.

[0093] As the aryl group, phenyl and naphthyl etc. can be cited. As the aryl group substituted by alkyl, tolyl, xylyl, ethylphenyl, propylphenyl, butylphenyl, pentylphenyl, hexylphenyl, heptylphenyl, octylphenyl, nonylphenyl, decylphenyl, undecylphenyl, dodecylphenyl etc. can be cited. There is no particular restriction on the substitution position of the aryl group substituted by alkyl. The alkyl group can be straight-chain or branched. As the aralkyl group, benzyl, phenylethyl, phenylpropyl, phenylbutyl, phenylpentyl, phenylhexyl etc. can be cited. The alkyl group can be straight-chain or branched.

[0094] From the viewpoint of particularly improving the dispersibility to component B, the hydrocarbon group is preferably an aliphatic hydrocarbon group or an alicyclic hydrocarbon group. More preferably, it is an aliphatic hydrocarbon group. As the aliphatic hydrocarbon group, an alkyl group composed of saturated hydrocarbons and an alkenyl group composed of unsaturated hydrocarbons can be cited. The alkyl group and the alkenyl group as the aliphatic hydrocarbon group can be any structure of a straight chain or a branched chain. However, when the alkyl group is a straight chain alkyl group such as n-butyl or n-octyl, the alkyl groups are easily oriented to each other, and the dispersibility to component B tends to decrease. From this viewpoint, when the hydrocarbon group is an alkyl group, a branched chain alkyl group is preferred compared to a straight chain alkyl group. On the other hand, since the alkenyl group has more than one carbon-carbon double bond structure, even if it is a straight chain, the orientation is not so high. Therefore, the alkenyl group can be a straight chain or a branched chain.

[0095] Specific examples of the acidic phosphate esters include butyl octyl acid phosphate, diisomyristyl acid phosphate, isocetyl acid phosphate, hexyl decyl acid phosphate, isostearyl acid phosphate, isobehenyl acid phosphate, octyl decyl acid phosphate, octyl dodecyl acid phosphate, isobutyl acid phosphate, 2-ethylhexyl acid phosphate, isodecyl acid phosphate, lauryl acid phosphate, tridecyl acid phosphate, stearyl acid phosphate, oleyl acid phosphate, myristyl acid phosphate, palmityl acid phosphate, Palmitate, di(butyl octyl) acid phosphate, diisomyristyl acid phosphate, diisocetyl acid phosphate, di(hexyldecyl) acid phosphate, diisostearyl acid phosphate, diisobehenyl acid phosphate, di(octyldecyl) acid phosphate, di(octyldodecyl) acid phosphate, diisobutyl acid phosphate, di(2-ethylhexyl) acid phosphate, diisodecyl acid phosphate, ditridecyl acid phosphate, dioleyl acid phosphate, dimyristyl acid phosphate, dipalmityl acid phosphate, etc. Among these compounds, stearyl acid phosphate, oleyl acid phosphate, and di(2-ethylhexyl) acid phosphate are preferred from the viewpoints of high corrosion protection when forming a metal salt and dispersibility in component B.

[0096] The cross-linkable polymer composition of the present disclosure may also appropriately contain additives such as diluents, dispersants, and colorants in addition to the above-mentioned components A to C, within the range that does not hinder the function of the material. However, the cross-linkable polymer composition preferably does not contain grease components and various curing materials such as photocurable materials, moisture curable materials, anaerobic curable materials, cationic curable materials, anionic curable materials, and thermosetting materials. In addition, in the cross-linkable polymer composition of the present disclosure, when component B is liquid at 150°C or below or at room temperature, it is preferred that the polymer component that is solid at 150°C or below or at room temperature is not contained. It is further preferred that the cross-linkable polymer composition may contain only component B as a polymer component. In addition, as components that are preferably not contained in the cross-linkable polymer composition, the following compounds of groups (a) to (f) can be listed. That is, the following can be cited: (a) silane coupling agents, (b) epoxy compounds, (c) isocyanates, isothiocyanate compounds, (d) photoradical initiators, thermal radical initiators, (e) chlorine compounds, bromine compounds, and (f) volatile organic solvents. When the crosslinkable polymer composition contains compounds of groups (a) to (d), when heated, it is possible to cause undesirable chemical reactions such as crosslinking of component B and breaking of the main chain of component B caused by reactions different from the crosslinking reaction of the metal ions released from component A. As a result, the heat resistance and re-formability of the crosslinkable polymer composition may not be fully exerted. In addition, when the crosslinkable polymer composition contains compounds of group (e), coloring and corrosive gas generation may occur due to heating. When the crosslinkable polymer composition contains compounds of group (f), ignition and bubble generation may occur when the composition is formed.

[0097] The crosslinkable polymer composition can be easily prepared by mixing components A, B and C to disperse components A and C in component B. When preparing the crosslinkable polymer composition, mixing is preferably performed at room temperature, but heating may be performed as necessary.

[0098] (4) Content of each ingredient

[0099] In the crosslinkable polymer composition according to the present disclosure, the content of each of the components A to C is defined in relation to the valence of each component. Specifically, the valence and content of each component satisfy the following formula (3).

[0100] In g = (m·yl·x) / (n·z), g ≥ 0.1 (3)

[0101] Here, the valence of the metal ion released from component A is set to +y, and the content of the metal ion is set to m moles. In addition, the valence of the substituent capable of bonding with ions contained in component B is set to -z, and the content of the substituent is set to n moles. In addition, the valence of the acidic phosphate constituting component C is set to -x, and the content of the acidic phosphate is set to 1 mole. As metal ions, substituents, and acidic phosphates, when two or more elements with different valences are mixed, in formula (3), each of m·y, l·x, and n·z is the sum of the values ​​calculated for various elements. In the case of acidic phosphates, l·x is calculated for the case of x=2 represented by formula (C1) and the case of x=1 represented by formula (C2), and the value obtained by summing them up becomes the l·x value of the entire acidic phosphate. In addition, the contents of the above-mentioned elements of m moles, n moles, and 1 mole refer to the contents of each element in the entire cross-linkable polymer composition.

[0102] In the cross-linkable polymer composition involved in the present disclosure, the metal ions released from component A by heat are consumed by both the metal ion cross-linking of component B caused by forming ionic bonds with the substituents of component B and the formation of phosphate with component C. Therefore, in order to fully carry out the cross-linking of component B, the metal ions released from component A need to remain even if they are consumed in the formation of phosphate with component C. The g value of the above formula (3) is a value expressed as a ratio of the amount of metal ions released from component A and remaining without being consumed in the formation of phosphate with component C to the amount of substituents present in component B, and the larger the value, the greater the amount of metal ions that can contribute to the cross-linking of component B.

[0103] If g≤0, it means that no metal ions that can contribute to the crosslinking of component B remain, and if g>0, it means that metal ions that can contribute to the crosslinking of component B remain. g≥0.1 means that the amount of metal ions that are not consumed and remain in the formation of the phosphate ester salt with component C is equivalent to more than 10% of the amount of substituents of component B in terms of equivalents. If g=1, metal ions remain in an equivalent number equal to the substituents of component B, but even if ionic crosslinking occurs only in a part of the substituents in component B, the crosslinkable polymer composition has a high viscosity and can form a cured product. Therefore, in order to fully perform ionic crosslinking, it is not necessary to reach the same equivalent number of metal ions as the substituents of component B. If g≥0.1, component B can be fully crosslinked to cure the crosslinkable polymer composition. From the viewpoint of improving curability, g≥0.2 is preferred, and g≥0.5 and g≥1.0 are more preferred. On the other hand, from the viewpoint of avoiding separation and precipitation of component A in the composition before curing, embrittlement of the cross-linked body after curing, and the influence on the corrosion resistance caused by these, g ≤ 2.0 is preferred, and g ≤ 1.5 is more preferred.

[0104] In addition, in the cross-linkable polymer composition, relative to 100 parts by mass of component B, component A may be contained in an amount of more than 1 part by mass and less than 30 parts by mass. By containing more than 1 part by mass of component A, the cross-linking property of component B can be fully obtained, and the metal adsorption property brought by the metal adsorption component formed by component C and metal ions can also be easily obtained, so that a high protective effect is exerted on the metal surface. In addition, by suppressing the content of component A to less than 30 parts by mass, in the state before cross-linking of the cross-linkable polymer composition, it is easy to avoid the separation and precipitation of component A, and even in the state after cross-linking, it is not easy to cause the reduction of the cross-linked body physical properties such as agglomeration and embrittlement of component A and the reduction of the corrosion resistance caused by these phenomena. From these viewpoints, the lower limit of the content of component A is more preferably more than 2 parts by mass, and more preferably more than 5 parts by mass and more than 10 parts by mass. Moreover, the upper limit of the content of component A is more preferably less than 20 parts by mass, and more preferably less than 15 parts by mass.

[0105] In addition, in the crosslinkable polymer composition, relative to 100 parts by mass of component B, a component C of more than 1 part by mass and less than 30 parts by mass can be contained. By containing more than 1 part by mass of component C, the metal adsorption component formed by the metal ions freed from component A and component C shows high metal adsorption, so it is possible to exert a high protective effect on the metal surface. In addition, by suppressing the content of component C to less than 30 parts by mass, in the state before crosslinking of the crosslinkable polymer composition, it is easy to avoid the separation and precipitation of component C, and even in the state after crosslinking, it is not easy to cause the reduction of the crosslinked body properties such as agglomeration and embrittlement of component C and the reduction of the corrosion resistance caused by these phenomena. From these viewpoints, the lower limit of the content of component C is more preferably more than 2 parts by mass, and more preferably more than 5 parts by mass. Moreover, the upper limit of the content of component C is more preferably less than 20 parts by mass, and more preferably less than 15 parts by mass and less than 10 parts by mass.

[0106] (5) Characteristics of cross-linkable polymer composition

[0107] According to the crosslinkable polymer composition of the present disclosure having the above structure, metal ions are released from component A by heat, and the released metal ions are ionically bonded to the substituents of component B, so that the organic polymer of component B is crosslinked via ion bonds. At the same time, the metal ions released from component A form a metal salt of phosphate ester together with component C. Therefore, after heating, the phosphate ester salt is dispersed in the crosslinked body of component B.

[0108] The formation rate of ionic bonds is faster than the formation rate of covalent bonds, so the curing rate of the crosslinkable polymer composition involved in the present disclosure is excellent. In addition, component A is a component that releases metal ions by heat. Until the temperature at which the metal ions are released, the metal ions are not released from component A, and the crosslinking of the organic polymer of component B caused by ionic bonds is not performed. Therefore, the storage stability of the crosslinkable polymer composition involved in the present disclosure is also excellent, and in a state of high fluidity before crosslinking, by applying it on an object such as a metal surface and heating it, a coating film with high uniformity can be easily formed. In addition, the organic polymer of component B in the crosslinkable polymer composition involved in the present disclosure is crosslinked via ionic bonds, and the bonding force is stronger than the van der Waals force, forming a tough crosslinked body. In addition, the crosslinkable polymer composition involved in the present disclosure has excellent heat resistance and excellent chemical resistance because the organic polymer of component B is crosslinked via ionic bonds.

[0109] The phosphate salt formed by the metal ions released from the A component and the C component is highly uniformly dispersed in the crosslinked body of the B component, and exhibits metal adsorption. This metal adsorption exhibits high corrosion resistance on the metal surface. It should be noted that even in the state of acidic phosphate ester that does not form a phosphate salt by ion bonding with metal ions, the C component exhibits a certain degree of metal adsorption, but in the state of forming a phosphate salt together with metal ions, it is more easily adsorbed on the metal surface via ion bonding, and exhibits high corrosion resistance.

[0110] In the crosslinkable polymer composition of the present disclosure, by setting the content ratio of components A to C to g≥0.1, the metal ions released from component A by heat can contribute to both the metal ion crosslinking of component B and the formation of phosphate ester salt with component C. As a result, both the improvement of heat resistance due to the crosslinking of component B and the improvement of corrosion resistance due to the formation of phosphate ester salt are achieved.

[0111] The cross-linkable polymer composition of the present disclosure is easily cross-linked and cured by heat. The cross-linked polymer material of the present disclosure is composed of a cross-linked product of the cross-linkable polymer composition of the present disclosure. In the cross-linked product, the component B in the cross-linkable polymer composition is in a cross-linked state via the metal ions released from the component A.

[0112] The crosslinkable polymer composition of the present disclosure can be used appropriately as a protective material, adhesive material, curing molding material, etc. having corrosion resistance. For example, it can be adhered to the surface of a metal substrate to be protected, and can be used as a corrosion protection for preventing metal corrosion by covering the metal substrate. In addition, as a corrosion protection, it can be used as a corrosion inhibitor for coated wires with terminals, etc.

[0113] [2]Metal components

[0114] Next, the metal components involved in the present disclosure are described. Figure 1 A cross-sectional view of a metal member according to one embodiment is shown in FIG.

[0115] The metal component 10 has a metal substrate 12 and a coating material 14 that covers the surface of the metal substrate 12. The coating material 14 is composed of the cross-linked polymer material involved in the present disclosure, that is, a cross-linked body (cured product) of the cross-linkable polymer composition involved in the present disclosure. The metal component 10 involved in the present disclosure has an excellent corrosion protection effect because the coating material 14 is composed of the cross-linked polymer material of the present disclosure.

[0116] [3] Wiring harness

[0117] Next, the wiring harness involved in the present disclosure is described. The wiring harness involved in the present disclosure includes the cross-linked polymer material involved in the present disclosure. Specifically, for example, the cross-linked polymer material involved in the present disclosure is used in a corrosion inhibitor that covers the electrical connection between the terminal fittings of the covered electric wire with terminals in the wiring harness and the electric wire conductor.

[0118] Here, the covered electric wire with terminal constituting the wiring harness involved in the present disclosure is described. The covered electric wire with terminal is an electric wire having a terminal fitting connected to the conductor end of the insulated electric wire, and the electrical connection portion between the terminal fitting and the electric wire conductor is covered by the cross-linked polymer material involved in the present disclosure (cured product of the cross-linked polymer composition involved in the present disclosure). This structure prevents corrosion at the electrical connection portion.

[0119] Figure 2 is a perspective view of a covered electric wire with a terminal according to one embodiment of the present disclosure, Figure 3 for Figure 2 The longitudinal section of the AA line in Fig. Figure 2 , Figure 3 As shown, in the covered electric wire 1 with terminal, the electric wire conductor 3 of the covered electric wire 2 covered with the insulating coating (insulator) 4 and the terminal fitting 5 are electrically connected via the electrical connection portion 6 .

[0120] The terminal fitting 5 has a tab-shaped connecting portion 51 formed of an elongated flat plate connected to the mating terminal, and an electric wire fixing portion 54 formed by a wire barrel 52 and an insulating barrel 53 and extending from the end of the connecting portion 51. The terminal fitting 5 can be formed (processed) into a predetermined shape by pressing a metal plate.

[0121] In the electrical connection portion 6, the insulating coating 4 at the end of the insulated wire 2 is stripped to expose the wire conductor 3, and the exposed wire conductor 3 is crimped to one side of the terminal fitting 5, thereby connecting the insulated wire 2 to the terminal fitting 5. The wire barrel 52 of the terminal fitting 5 is tightened from the wire conductor 3 of the insulated wire 2 to electrically connect the wire conductor 3 to the terminal fitting 5. In addition, the insulation barrel 53 of the terminal fitting 5 is tightened from the insulating coating 4 of the insulated wire 2.

[0122] In the covered electric wire 1 with a terminal, the range indicated by the dot-dash line is covered with the cured product 7 of the cross-linkable polymer composition involved in the present disclosure. Specifically, the range from the surface of the terminal fitting 5 that is forward of the front end of the portion of the wire conductor 3 exposed from the insulating coating 4 to the surface of the insulating coating 4 that is rearward of the rear end of the portion of the wire conductor 3 exposed from the insulating coating 4 is covered with the cured product 7. That is, the front end 2a side of the covered electric wire 2 is covered with the cured product 7 so that the cured product 7 slightly protrudes from the front end of the wire conductor 3 toward the connecting portion 51 side of the terminal fitting 5. The end edge 5a side of the terminal fitting 5 is covered with the cured product 7 so that the cured product 7 slightly protrudes from the end of the insulating tube 53 toward the insulating coating 4 side of the covered electric wire 2. Moreover, as Figure 3 As shown, the side surface 5b of the terminal fitting 5 is also covered with the cured material 7. It should be noted that the back surface 5c of the terminal fitting 5 may or may not be covered with the cured material 7. The periphery of the cured material 7 is composed of a portion in contact with the surface of the terminal fitting 5, a portion in contact with the surface of the wire conductor 3, and a portion in contact with the surface of the insulating coating 4.

[0123] In this way, the electrical connection portion 6 is covered with the cured material 7 with a predetermined thickness along the shape of the terminal fitting 5 and the outer periphery of the covered electric wire 2. The exposed portion of the wire conductor 3 of the covered electric wire 2 is completely covered by the cured material 7 and is not exposed to the outside. Therefore, the electrical connection portion 6 is completely covered by the cured material 7. Since the cured material 7 has excellent adhesion to any one of the wire conductor 3, the insulating coating 4, and the terminal fitting 5, the cured material 7 is used to prevent moisture and the like from invading the wire conductor 3 and the electrical connection portion 6 from the outside and corroding the metal parts. In addition, since the cured material 7 has excellent adhesion, for example, during the process from manufacturing the wire harness to installing it in the vehicle, even if the wire is bent, it is not easy to form a gap between the cured material 7 and any one of the wire conductor 3, the insulating coating 4, and the terminal fitting 5 at the periphery of the cured material 7, thereby maintaining waterproofness and corrosion resistance.

[0124] The crosslinkable polymer composition according to the present disclosure that forms the cured product 7 is applied within a predetermined range. The crosslinkable polymer composition according to the present disclosure that forms the cured product 7 can be applied by known means such as a dropping method and a coating method.

[0125] The cured product 7 is formed with a predetermined thickness within a predetermined range. The thickness is preferably 0.1 mm or less. If the cured product 7 is too thick, it is difficult to insert the terminal fitting 5 into the connector.

[0126] The wire conductor 3 of the covered electric wire 2 is formed by a stranded wire formed by twisting a plurality of single wires 3a. In this case, the stranded wire may be composed of one metal single wire or two or more metal single wires. In addition, the stranded wire may include single wires formed of organic fibers in addition to metal single wires. It should be noted that being composed of one metal single wire means that all the metal single wires constituting the stranded wire are formed of the same metal material; being composed of two or more metal single wires means that the stranded wire contains metal single wires formed of different metal materials. The stranded wire may also contain a reinforcing wire (tension member) for reinforcing the covered electric wire 2.

[0127] Examples of the material of the metal wire constituting the electric wire conductor 3 include copper, copper alloy, aluminum, aluminum alloy, or materials obtained by applying various plating to these materials. In addition, examples of the material of the metal wire used as a reinforcing wire include copper alloy, titanium, tungsten, stainless steel, etc. In addition, examples of organic fibers used as reinforcing wires include Kevlar, etc. In terms of weight reduction, the metal wire constituting the electric wire conductor 3 is preferably aluminum, aluminum alloy, or materials obtained by applying various plating to these materials.

[0128] Examples of the material of the insulating coating layer 4 include rubber, polyolefin, PVC, and thermoplastic elastomer. These materials may be used alone or in combination of two or more. Various additives may be appropriately added to the material of the insulating coating layer 4. Examples of the additives include flame retardants, fillers, and colorants.

[0129] The material (base material) of the terminal fitting 5 includes various copper alloys, copper, etc. in addition to the commonly used brass. The surface of the terminal fitting 5 may be partially (eg, at the contact) or entirely plated with various metals such as tin, nickel, and gold.

[0130] It should be noted that in Figure 2 In the illustrated covered electric wire with terminal 1, a terminal fitting is crimped and connected to the end of the electric wire conductor, but other known electrical connection methods such as welding may be used instead of crimping.

[0131] Example

[0132] Examples are shown below. The present invention is not limited to the examples. Here, the relationship between the component composition of the crosslinkable polymer composition and the curing rate, heat resistance, and corrosion resistance was studied.

[0133] <Preparation of cross-linkable polymer composition>

[0134] Components A to C were mixed in an agate mortar at room temperature for 5 minutes at the formulations (unit: parts by mass) listed in Table 1 to prepare crosslinkable polymer compositions of samples A1 to A10 and B1 to B8. Components A and C were not added to sample B1, and component C was not added to sample B2.

[0135] The materials used are described below.

[0136] (1)A component

[0137] ·Ca-AA: Calcium(II) acetylacetonate

[0138] ·Zn-AA: Zinc(II) acetylacetonate

[0139] ·Al-IP: Aluminum(III) triisopropoxide

[0140] ·ZnO: Zinc (II) oxide

[0141] ·Ca-St: Calcium (II) stearate

[0142] (2) Component B

[0143] MA5: Maleic anhydride-modified liquid polybutadiene (manufactured by Cray Valley), substituent equivalent weight 2350 g / mol

[0144] UC3510: Liquid polyacrylate with carboxyl groups introduced (manufactured by Toa Gosei Co., Ltd.), substituent equivalent weight 801 g / mol

[0145] X-22-3701E: Carboxyl-modified silicone oil (manufactured by Shin-Etsu Chemical Co., Ltd.), substituent equivalent weight 4000 g / mole

[0146] R134: Liquid polybutadiene (manufactured by Cray Valley Co., Ltd.), without ionic bonding substituents

[0147] (3) C component

[0148] EH-P: di(2-ethylhexyl) acid phosphate (manufactured by SC Organic Chemical Co., Ltd., "Phoslex A-208", molecular weight 322 (average), acid value 172 mgKOH / g)

[0149] ·ST-P: stearyl acid phosphate (manufactured by SC Organic Chemical Co., Ltd., "Phoslex A18", molecular weight 437 (average), acid value 228 mgKOH / g)

[0150] OL-P: Oleyl acid phosphate (manufactured by SC Organic Chemical Co., Ltd., "Phoslex A18D", molecular weight 467 (average), acid value 183 mgKOH / g)

[0151] MT-P: Methyl acid phosphate (manufactured by SC Organic Chemical Co., Ltd., "Phoslex A-1", molecular weight 119 (average), acid value 707 mgKOH / g)

[0152] <Evaluation Method>

[0153] (1) Curing time

[0154] A 50mm×50mm×0.5mm thick copper plate was preheated to 120°C, and 0.1g of each prepared composition was dripped thereon. The moment when each composition was dripped on the heated copper plate was set to 0s (0 seconds), and the time until the dripped composition was cured was taken as the curing time. The time until the composition was cured was set to the moment when the surface of the dripped composition was touched with a spatula and lifted up and the composition no longer drew. When curing was confirmed within 60s, it can be evaluated as excellent curing speed (fast curing).

[0155] (2) Heat resistance

[0156] In the test for evaluating the curing time, for the cured sample, a copper plate was placed vertically in an oven at 155°C for 2 hours, and then the state of the cured product was visually observed. The case where the cured product did not droop was evaluated as "A" with particularly good heat resistance, the case where part of the cured product drooped was evaluated as "B" with good heat resistance, and the case where the cured product completely drooped was evaluated as "C" with poor heat resistance. The measurement conditions such as temperature were in accordance with JIS C60068-2-2.

[0157] (3) Anti-corrosion performance

[0158] The above compositions were applied to a 2 cm portion from one end of a 1 cm × 5 cm copper strip, and cured in an oven at 120°C for 5 minutes. Then, with one end of the coating facing upward, the copper plate was placed vertically in an oven at 155°C for 2 hours, and then returned to room temperature. The obtained sample was used as a test piece for measurement. The coated and cured portion (coating film portion) of the test piece for measurement was used as the cathode electrode, and the separately prepared Al plate was used as the anode electrode. The electrodes were immersed in a 5% NaCl aqueous solution, and the potential difference (corrosion current) was measured. The smaller the potential difference, the more uniform the cured composition on the copper strip exists as a coating, and the stronger the adsorption force on the surface of the copper strip. On the other hand, the larger the potential difference, the more uneven the curing of the composition on the copper strip, or the weaker the adsorption force of the composition on the surface of the copper strip. It should be noted that when an untreated strip copper plate not immersed in a surface protective agent composition is placed vertically in an oven at 155°C and then used as a cathode electrode, the corrosion current value is 80μA. Taking this 80μA value as a reference value, when the current value measured for each sample is less than 1 / 10 of the reference value, it is judged as "A" with particularly high corrosion protection performance (surface protection), and when the current value is more than 1 / 10 and less than 1 / 5 of the reference value, it is judged as "B" with high corrosion protection performance. When the current value is more than 1 / 5 of the reference value, it is judged as "C" with low corrosion protection performance.

[0159] <Evaluation Results>

[0160] In the following Table 1, for samples A1 to A10, B1 to B8, the content of each component (unit: mass parts) is shown in the upper section, and the results of each evaluation are shown in the lower section. The left column in the table represents the equivalent number per unit mass of each component. The unit is mEq / g, and the valence (Eq) of each component per 1g is expressed in milliunits. That is, it is calculated as equivalent number (mEq / g) = valence of each component / molecular weight × 1000. For component C, as a valence, it represents the value obtained by weighted average of the valence (2 valence) of the compound represented by formula (C1) and the valence (1 valence) of the compound represented by formula (C2) according to the content. In addition, in the middle section of the table, as the product of the content of each component and the equivalent number, each value of m·y, n·z, and l·x is calculated, and the g value is calculated based on these values ​​and shown.

[0161]

[0162] The compositions of samples A1 to A10 contain: as component A, a compound that releases metal ions by heat; as component B, an organic polymer having a substituent capable of ionically bonding with metal ions; and as component C, an acidic phosphate represented by the above general formula (C1) and general formula (C2), and the g value defined by their valence and content is g ≥ 0.1. Correspondingly, in any of samples A1 to A10, curing is performed within a short curing time of less than 60 seconds, and good heat resistance and corrosion resistance evaluated as A or B are obtained. It is explained that a part of the metal ions released from component A forms a highly heat-resistant cured product in a short time by cross-linking component B, and another part of the metal ions forms a phosphate ester salt with component C, which imparts high corrosion resistance to the film of the cured product.

[0163] In samples A8 to A10, although sufficiently high corrosion resistance evaluated as B was obtained, the corrosion resistance was not as high as that of samples A1 to A7. In sample A10, the heat resistance was not as high as that of samples A1 to A9, and the curing time was slightly longer. In sample A8, the content of component A was higher than that of samples A1 to A7, and the g value was slightly larger accordingly, which was explained as the physical properties of the crosslinked body being reduced due to the influence of the large amount of component A contained. In sample A9, the content of component B was reduced compared to samples A1 to A7, and the content of component C was increased, which was explained as the form of phosphate ester bonded to metal ions by component C being relatively difficult to form. In sample A10, the content of components A and C was reduced compared to samples A1 to A9, and the g value was also relatively small. Accordingly, it was explained that the crosslinking of component B and the salt formation of component C caused by metal ions were not carried out as efficiently as in the case of samples A1 to A9.

[0164] Since the composition of sample B1 does not contain component A, component B will not be crosslinked by metal ions even if the composition is heated. Therefore, the maleic anhydride-modified liquid polybutadiene of component B remains in the same state and does not cure even if the heating time exceeds 600 seconds. In sample B2, component B is crosslinked due to the contribution of component A, so it cures in a short time and forms a coating film with high heat resistance, but the corrosion protection performance is reduced compared with the case where component C, which is a metal adsorbing component, is not contained.

[0165] In sample B3, zinc oxide, which does not cause the release of metal ions even when heated, is used as component A, and a component that releases metal ions by heat is not used. Therefore, component B cannot be crosslinked with metal ions, and the composition is not cured even if the heating time exceeds 600 seconds. Since no curing is performed, the corrosion protection performance is also reduced. In sample B4, calcium stearate, which is a fatty acid metal salt, is used as component A, and a component that releases metal ions by heat is not used. Even if the fatty acid metal salt is heated, metal oxides are only formed by thermal decomposition, and metal ions are not released even if the composition is heated. Therefore, component B cannot be crosslinked with metal ions, and 500 seconds are required for the curing of the composition. Since the curability of the composition is low, curing cannot be fully carried out, and the corrosion protection performance is also reduced.

[0166] In sample B5, since liquid polybutadiene having no substituted group capable of bonding with ions was used as component B, the composition did not cure even when the heating time exceeded 600 seconds, although it contained component A that freed metal ions. Since no curing occurred, the corrosion protection performance was also reduced.

[0167] In sample B6, as component C, an acidic phosphate ester having a methyl group as a hydrocarbon group having 1 carbon atom was used instead of an acidic phosphate ester having a hydrocarbon group having 4 or more and 30 carbon atoms. In this case, curing by heating proceeds in a short time and good heat resistance is obtained, but the corrosion resistance is reduced. It is believed that since the carbon number of the methyl group contained in the acidic phosphate ester is small, the compatibility of component C and component B is poor, and component C separates and aggregates in the composition, and the adsorption to the metal surface is reduced.

[0168] In samples B7 and B8, both contain more component C than component A, and the g value is g<0.1. Correspondingly, the metal ion crosslinking of component B cannot be fully carried out, and the curing of the composition does not proceed in a short time. Since the curing is not fully carried out, the corrosion resistance is also reduced. In sample B7, g<0, corresponding to the extremely small g value, no curing is observed even if the heating time exceeds 600 seconds, but in sample B8, 0<g<0.1, corresponding to the g value not being as small as sample B7, although it took as long as 280 seconds, the curing of the composition was confirmed. However, the crosslinking of the sample is still considered insufficient, and the corrosion resistance is reduced in sample B8.

[0169] As mentioned above, although the embodiment of this disclosure was described in detail, this invention is not limited to the said embodiment at all, Various changes can be made within the range which does not deviate from the summary of this invention.

[0170] Explanation of symbols

[0171] 1Covered wire with terminal

[0172] 2 coated wire

[0173] 2a Front end of the coated wire

[0174] 3 Wire conductor

[0175] 3a single line

[0176] 4Insulation coating (insulator)

[0177] 5-terminal accessories

[0178] 5a Terminal fitting edge

[0179] 5b Side of terminal fitting

[0180] Back side of 5c terminal fitting

[0181] 51 Connection

[0182] 52 Spools

[0183] 53 Insulation tube

[0184] 54 Wire fixing part

[0185] 6Electrical connection

[0186] 7 cured product

[0187] 10 Metal components

[0188] 12 Metal substrate

[0189] 14. Coating material

Claims

1. A cross-linkable polymer composition comprising: A component, wherein the A component releases metal ions by heat; A component B, the component B being composed of an organic polymer having a substituent capable of ionically bonding with the metal ion released from the component A; and Component C, wherein the component C is composed of one or more of the acidic phosphates represented by the following general formula (C1) and general formula (C2), The valence of the metal ion released from the component A is +y, and the content of the metal ion is m mol; the valence of the substituent contained in the component B is -z, and the content of the substituent is n mol; the valence of the acidic phosphate constituting the component C is -x, and the content of the acidic phosphate is 1 mol, In g = (m·yl·x) / (n·z), g ≥ 0.1, P(=O)(-OR)(-OH)2(C1) P(=O)(-OR)2(-OH)(C2) in, R is a hydrocarbon group having 4 or more and 30 or less carbon atoms, and The metal of the metal ions released from the component A is at least one of alkaline earth metals, zinc, titanium and aluminum.

2. The crosslinkable polymer composition according to claim 1, wherein The component A has a decomposition point or a phase transition point at 50° C. or higher and 200° C. or lower.

3. The crosslinkable polymer composition according to claim 1 or claim 2, wherein: The component A is a metal complex.

4. The crosslinkable polymer composition according to claim 1 or claim 2, wherein The component A is a metal complex containing a multidentate ligand or a cross-linked ligand.

5. The cross-linkable polymer composition according to claim 1 or claim 2, wherein The component A is a metal complex containing a β-diketone ligand or an alkoxide ligand.

6. The crosslinkable polymer composition according to claim 1 or claim 2, wherein: The substituent of the component B is an electron withdrawing group.

7. The cross-linkable polymer composition according to claim 1 or claim 2, wherein: The substituent of the component B is at least one of a carboxylic acid group, an acid anhydride group, a phosphoric acid group, and a sulfonic acid group.

8. The cross-linkable polymer composition according to claim 1 or claim 2, wherein The component B is in a liquid state at 150° C. or lower.

9. The cross-linkable polymer composition according to claim 1 or claim 2, wherein The A component is contained in an amount of 1 part by mass or more and 30 parts by mass or less with respect to 100 parts by mass of the B component.

10. The cross-linkable polymer composition according to claim 1 or claim 2, wherein The C component is contained in an amount of 1 part by mass or more and 30 parts by mass or less with respect to 100 parts by mass of the B component.

11. A cross-linked polymer material, which is a cross-linked product of the cross-linkable polymer composition according to any one of claims 1 to 10, The B component is cross-linked via the metal ions released from the A component. 12 . A metal component comprising a metal substrate and a coating material coating a surface of the metal substrate, wherein the coating material is composed of the cross-linked polymer material according to claim 11 .

13. A wiring harness comprising the cross-linked polymer material according to claim 11.