A constant viscosity carbon black masterbatch and its preparation method and application

By using cardanol ester compounds with carboxyl groups and high-speed jet technology in wet mixing, constant viscosity carbon black masterbatch is prepared, which solves the problems of traditional carbon black masterbatch hardening and filler aggregation, and improves the performance of carbon black in rubber. The dispersion and mechanical properties enable efficient carbon black/rubber composite production.

CN116496554BActive Publication Date: 2024-10-18LIAONING BLACK CAT COMPOSITE NEW MATERIAL TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310411079.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-17
Publication Date
2024-10-18
Estimated Expiration
2043-04-17

AI Technical Summary

Technical Problem

When carbon black-filled rubber composites are prepared by the traditional dry mixing process, it is difficult for carbon black to achieve the best reinforcing effect, and there are problems such as flying dust, serious pollution, and high energy consumption. The carbon black masterbatch is easy to harden during wet mixing. , affecting the subsequent mixing process, and the filler aggregation phenomenon seriously affects the mechanical properties.

Method used

Constant viscosity carbon black masterbatch is used, including carbon black, latex and cardanol ester compounds with carboxyl groups. Cardanol ester compounds are prepared through esterification reaction and combined with high-speed jet mixing technology to improve the dispersion of carbon black in the rubber matrix. properties, inhibit the hardening of the masterbatch and enhance the mechanical properties.

Benefits of technology

It improves the dispersion and mechanical properties of carbon black in rubber, weakens the hardening phenomenon of the masterbatch, extends the storage time, simplifies the mixing process, reduces energy consumption and filler aggregation, and improves the wear resistance and production of composite materials. efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116496554B_ABST
    Figure CN116496554B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of wet mixing of masterbatch, and discloses a constant viscosity carbon black masterbatch, comprising the following raw materials in parts by weight: 10-100 parts of carbon black, 40-160 parts of latex, and 1-25 parts of carboxyl-containing cardanol ester compounds; the preparation process is as follows: carbon black is mixed with water to obtain a carbon black suspension, ground and added with carboxyl-containing cardanol ester compounds to obtain a carbon black slurry; the carbon black slurry and latex collide in a mixing chamber through a high-speed jet, settle together, and obtain a carbon black masterbatch after washing and drying. The present invention can improve the dispersion of fillers while increasing the masterbatch yield, and effectively improve the wear resistance of the rubber, reduce the hysteresis heat generation performance, and effectively inhibit the hardening of the latex, thereby extending the storage time of the masterbatch.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of masterbatch wet mixing, and in particular to a high-performance constant-viscosity carbon black masterbatch and a preparation method and application thereof. Background Art

[0002] Carbon black's small particle size and large specific surface area make it widely used in rubber reinforcement. However, it is difficult to achieve the best reinforcement effect of carbon black when preparing carbon black-filled rubber composites using traditional dry mixing technology, and there are problems such as dust flying, serious pollution and high energy consumption. The introduction of liquid phase mixing technology makes it possible to produce highly dispersed and high-performance carbon black / rubber composites. Since then, wet mixing technology has become one of the research hotspots of filler / rubber mixing technology. A lot of improvement research has been done on continuous liquid phase wet mixing technology at home and abroad, such as modifying carbon black and using fillers, improving shearing and mixing processes, and improving carbon black latex flocculation methods and flocculation processes. The main purpose is to achieve synchronous sedimentation through better affinity adsorption of latex and carbon black, so as to achieve uniform dispersion of carbon black in the latex matrix and reduce the aggregation of fillers.

[0003] In the carbon black / rubber composite product prepared by wet mixing, the rubber phase is not cross-linked, so the carbon black has a significant tendency to aggregate. In actual production, the drying of the masterbatch is a time-consuming procedure in the subsequent processing, and the masterbatch will harden during the later storage process. The hardening of the masterbatch will increase the difficulty of the subsequent mixing process: on the one hand, the aldehyde group in the rubber reacts with the non-rubber component to condense, resulting in an increase in the viscosity of the rubber; on the other hand, during the storage of the rubber, a binding rubber will continue to form, the effective volume of the rubber will decrease, and the viscosity of the rubber will increase. Therefore, before mixing, it is necessary to plasticize it or reduce the Mooney value through an extruder to achieve the Mooney value required for production. After the masterbatch is plasticized, mixing is prone to over-mixing of the rubber, and the Mooney viscosity drops to a very low level, which will not only affect the aging properties of the rubber, but also make the filler more likely to aggregate during the vulcanization process, resulting in increased hysteresis loss.

[0004] Therefore, how to provide a carbon black masterbatch that inhibits the hardening of the masterbatch, improves the dispersion performance of carbon black, and has excellent mechanical properties is a problem that people in this field urgently need to solve. Summary of the invention

[0005] In view of this, the present invention provides a constant viscosity carbon black masterbatch and a preparation method thereof, so as to solve the problems that the traditional masterbatch has too high hardness, is difficult to store, is difficult to mix, and the filler aggregation phenomenon in the existing wet mixing process seriously affects the mechanical properties of the carbon black masterbatch.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0007] A constant viscosity carbon black masterbatch comprises the following raw materials in parts by weight: 10-100 parts of carbon black, 40-160 parts of latex, and 1-25 parts of carboxyl-containing cardanol ester compounds.

[0008] Preferably, in the above-mentioned constant viscosity carbon black masterbatch, the latex includes natural latex and / or synthetic latex.

[0009] Preferably, in the above-mentioned constant viscosity carbon black masterbatch, the carboxyl-containing cardanol ester compound is obtained by esterification reaction of a dicarboxylic acid compound and cardanol.

[0010] Preferably, in the above-mentioned constant viscosity carbon black masterbatch, the carboxyl-containing cardanol ester compound is prepared by the following method:

[0011] An organic solvent is used as a reaction solvent, a dicarboxylic acid compound is mixed with cardanol, an esterification reaction occurs under the catalytic action of a catalyst, and after the reaction is completed, a reduced pressure distillation is performed to obtain a cardanol ester compound with a carboxyl group;

[0012] The reaction temperature of the esterification reaction is 45-70° C., and the reaction time is 2-8 hours.

[0013] Preferably, in the above-mentioned constant viscosity carbon black masterbatch, the molar ratio of the cardanol to the dicarboxylic acid compound is 1:1-2;

[0014] The organic solvent is not limited to any one of dimethyl sulfoxide, chloroform and acetone;

[0015] The catalyst includes, but is not limited to, any one of concentrated sulfuric acid, concentrated hydrochloric acid, zinc oxide, stannous chloride, and dibutyltin dilaurate.

[0016] The present invention also discloses a method for preparing the above-mentioned constant viscosity carbon black masterbatch, comprising the following steps:

[0017] (1) mixing carbon black with water to obtain a carbon black suspension, grinding and adding a carboxyl-containing cardanol ester compound to obtain a carbon black slurry;

[0018] (2) The carbon black slurry and latex collide in a mixing chamber through high-speed jets, settle together, and obtain a carbon black masterbatch after washing and drying.

[0019] Preferably, in the above-mentioned method for preparing constant viscosity carbon black masterbatch, the carbon black suspension in step (1) is prepared by mixing carbon black and water to form a mixed solution with a solid content of 1-10% and then stirring evenly;

[0020] The stirring speed is 100-500 rpm, and the stirring time is 20-60 min;

[0021] The grinding speed is 1000-4000 r / min, and the grinding time is 20-60 min.

[0022] Preferably, in the above-mentioned method for preparing constant viscosity carbon black masterbatch, the latex in step (2) is obtained by diluting concentrated latex with water to a solid content of 10-40%.

[0023] Preferably, in the above-mentioned method for preparing constant viscosity carbon black masterbatch, the flow rate of the carbon black slurry outlet in step (2) is 100-500 m / s and the flow rate is 15-40 kg / min, and the flow rate of the latex outlet is 0.5-5 m / s and the flow rate is 2-12 kg / min;

[0024] The drying temperature is 80-110° C., and the drying time is 1-3 hours.

[0025] In addition, the present invention also provides an application of the above-mentioned constant viscosity carbon black masterbatch or the constant viscosity carbon black masterbatch prepared by any of the above-mentioned methods in vulcanized rubber.

[0026] The present invention provides a constant viscosity carbon black masterbatch and a preparation method thereof. Compared with the prior art, the present invention has the following beneficial effects:

[0027] (1) The carboxyl groups on the carboxyl-containing cardanol ester compounds can be affinity with the oxygen-containing functional groups on the surface of carbon black, and the long aliphatic hydrocarbon chains at the meta position can be combined with the rubber molecular chains, thereby improving the dispersion of carbon black in the rubber matrix, reducing the self-aggregation phenomenon during drying and parking, and improving the wear resistance of the rubber compound through a good filler-rubber cross-linking network. The relative sliding between fillers in the composite material is less, so the hysteresis heat generation is lower;

[0028] (2) Cardanol and dicarboxylic acid compounds undergo esterification reaction in proportion. The carboxyl groups on the carboxyl cardanol ester compounds can break the stability of rubber particles and demulsify them, thus playing the role of latex flocculant. At the same time, it avoids the premature demulsification of latex caused by strong acid. The carbon black and latex are more fully and completely combined, thereby improving the dispersibility and the masterbatch yield.

[0029] (3) Cardanol is used in the preparation of carbon black masterbatch, which can cross-link the molecular chains of latex and introduce the rigid group benzene ring into the latex, thereby improving the mechanical strength of the latex, solving the fatal defects of low elongation and low hardness of wet mixed rubber compared with dry mixed rubber, while satisfying the optimization of rubber physical properties, hysteresis properties and wear resistance;

[0030] (4) During the high-temperature drying process of the masterbatch, the phenolic hydroxyl groups on the benzene ring of cardanol can activate the ortho- and para-position hydrogen atoms, which can react with the aldehyde groups on the latex molecular chain, effectively inhibiting the hardening of the latex, thereby solving the hardening phenomenon of the carbon black masterbatch, extending the storage time of the masterbatch, and facilitating the subsequent mixing of the carbon black masterbatch, simplifying the Mooney reduction procedure of the masterbatch, and reducing the mixing energy consumption and material intake difficulty. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0032] Figure 1 The effect of cardanol oxalate on the Mooney viscosity of the masterbatch in Comparative Example 1 and Examples 1-4;

[0033] Figure 2 is the preparation reaction formula of monocardanol oxalate;

[0034] Figure 3 Schematic diagram of the interaction between cardanol oxalate, carbon black and rubber. DETAILED DESCRIPTION

[0035] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] The embodiment of the present invention provides a high-performance constant-viscosity carbon black masterbatch and a preparation method thereof. The carbon black masterbatch prepared by the method of the present invention can solve the problems of too high hardness of the masterbatch, difficulty in storage and difficulty in mixing; and can improve the flocculation efficiency in the wet compounding process, thereby improving the masterbatch yield, further improving the dispersion of carbon black in rubber, and preparing a carbon black / rubber nanocomposite material with excellent mechanical properties, high wear resistance and low heat generation.

[0037] An embodiment of the present invention provides a constant viscosity carbon black masterbatch, comprising the following raw materials in parts by weight: 10-100 parts of carbon black, 40-160 parts of latex, 1-25 parts of carboxyl cardanol ester compounds and an appropriate amount of water; specifically, for example, the carbon black can be 10 parts, 30 parts, 50 parts, 80 parts, 100 parts, etc., the latex can be 40 parts, 80 parts, 120 parts, 160 parts, etc., the carboxyl cardanol ester compounds can be 1 part, 5 parts, 10 parts, 15 parts, 20 parts, 25 parts, etc., and the addition amount of each raw material can be within the above range.

[0038] The carboxyl groups on the carboxyl-containing cardanol ester compounds can be affinity with the oxygen-containing functional groups on the surface of carbon black, and the long aliphatic hydrocarbon chains at the meta position can combine with the rubber molecular chains, thereby improving the dispersion of carbon black in the rubber matrix, weakening the self-aggregation phenomenon, and thereby improving the wear resistance and various mechanical properties of the rubber and optimizing the hysteresis heat generation performance.

[0039] In some embodiments of the present invention, the latex includes natural latex and / or synthetic latex, wherein the synthetic latex can be styrene-butadiene latex, butadiene latex, butyl latex, chloroprene latex, ethylene-propylene latex, isoprene latex, nitrile latex, acrylic latex, etc.

[0040] Furthermore, the carbon black is carbon black for rubber, such as models such as N115, N134, N219, N220, N234, N326, N330, N339, N375, N351, N550, N660, and N774.

[0041] In some embodiments of the present invention, the carboxyl-containing cardanol ester compound is obtained by esterification reaction between a dicarboxylic acid compound and cardanol; specifically, an organic solvent is used as a reaction solvent, the dicarboxylic acid compound and cardanol are mixed, and an esterification reaction occurs under the catalytic action of a catalyst. After the reaction is completed, the solvent is removed by reduced pressure distillation to obtain the carboxyl-containing cardanol ester compound.

[0042] Furthermore, the reaction temperature of the esterification reaction is 45-70°C, which can be 45°C, 55°C, 65°C, 70°C, etc. The reaction time of the esterification reaction is 2-8h, which can be 2h, 4h, 6h, 8h, etc. The molar ratio of cardanol to the dicarboxylic acid compound is 1:1-2, for example, it can be 1:1, 1:1.2, 1:1.5, 1:2.0, etc., that is, the amount of the dicarboxylic acid compound added is equal to or in excess of the cardanol, because the dicarboxylic acid compound reacts with the cardanol to remove one carboxyl group. The other carboxyl group plays a role in breaking the charge stability of the latex, causing the latex to break and coagulate, promoting the flocculation of carbon black and latex, and at the same time having affinity with carbon black; further, the dicarboxylic acid compound can be oxalic acid, terephthalic acid, naphthalene dicarboxylic acid, 1,4-cyclohexane dicarboxylic acid, diphenyl ether dicarboxylic acid, etc.; the organic solvent can be dimethyl sulfoxide, chloroform, acetone, etc.; the catalyst can be a strong acid catalyst such as concentrated sulfuric acid and concentrated hydrochloric acid, a tin catalyst such as stannous chloride and dibutyltin dilaurate, zinc oxide, etc.

[0043] Cardanol undergoes an esterification reaction with dicarboxylic acid compounds. The carboxyl group on the carboxyl-containing cardanol ester compound can break the stability of the latex and demulsify it, thus playing the role of a latex flocculant. At the same time, it avoids the premature demulsification of the latex caused by strong acid. The carbon black and latex are combined more fully and completely, thereby improving the dispersibility and the masterbatch yield.

[0044] In other embodiments of the present invention, a method for preparing the above-mentioned constant viscosity carbon black masterbatch is disclosed, comprising the following steps:

[0045] Step S100. Mixing carbon black with water to obtain a carbon black suspension, grinding and adding a carboxyl-containing cardanol ester compound to obtain a carbon black slurry;

[0046] Specifically, the carbon black suspension is prepared by the following method: carbon black is mixed with water to prepare a carbon black mixed liquid with a solid content of 1-10%, wherein the solid content can be 1%, 5% or 10%, etc., and the carbon black mixed liquid is stirred and mixed uniformly in a stirrer to obtain a carbon black suspension, wherein the stirring speed of the stirrer is 100-500rpm, and the stirring time is 20-60min.

[0047] Furthermore, the process of grinding and adding carboxyl-containing cardanol ester compounds is specifically as follows: adding the carbon black suspension into a colloid mill for grinding, the rotation speed of the colloid mill is 1000-4000r / min, the grinding time is 20-60min, and during the grinding process, the carboxyl-containing cardanol ester compounds are added and emulsified for 10-30min to obtain a carbon black slurry with good dispersion properties.

[0048] It can be understood that after grinding the carbon black suspension for a period of time, such as 10-30 minutes, the carboxyl cardanol ester compound is added and grinding is continued for 10-30 minutes for emulsification. The carboxyl group on the carboxyl cardanol ester compound can be affinity with the oxygen-containing functional group on the surface of carbon black, and the long aliphatic hydrocarbon chain at the meta position can combine with the rubber molecular chain, thereby improving the dispersion of carbon black in the rubber matrix.

[0049] Step S200. The carbon black slurry and latex collide in a mixing chamber through high-speed jets, settle together, and obtain a carbon black masterbatch after washing and drying.

[0050] Specifically, carbon black slurry and latex collide in a mixing chamber via high-speed jets, the slurry outlet flow rate is set at 100-500 m / s, and the latex outlet flow rate is set at 0.5-5 m / s. The huge speed difference between the slurry flow and the latex flow is utilized to fully mix and disperse the carbon black and latex, and settle together to obtain a carbon black masterbatch wet product with uniform particles. After further washing, the carbon black masterbatch is dried in a forced air drying oven at 80-110°C for 1-3 hours to obtain the carbon black masterbatch.

[0051] During the high-temperature drying process, the phenolic hydroxyl groups on the benzene ring of cardanol can activate the ortho and para hydrogen atoms, which can react with the aldehyde groups on the latex molecular chain, effectively inhibiting the hardening of the latex, thereby solving the hardening phenomenon of the carbon black masterbatch, extending the storage time of the masterbatch, and facilitating the subsequent mixing of the carbon black masterbatch, simplifying the Mooney reduction procedure of the masterbatch, and reducing the mixing energy consumption and material intake difficulty.

[0052] In some embodiments of the present invention, the latex is obtained by diluting concentrated latex with water to a solid content of 10-40%; wherein the solid content of the latex can be 10%, 20%, 30%, 40%, etc.

[0053] In addition, an embodiment of the present invention also provides an application of the constant viscosity carbon black masterbatch or the constant viscosity carbon black masterbatch prepared by the above method in a vulcanized rubber. Since the vulcanized rubber includes the above constant viscosity carbon black masterbatch, the vulcanized rubber prepared therefrom also has excellent mechanical properties, wear resistance and compression heat generation properties, etc., which will not be described in detail.

[0054] The technical solution of the present invention is described below through specific embodiments.

[0055] Example 1

[0056] This embodiment provides a method for preparing a carbon black masterbatch, comprising the following steps:

[0057] (1) Preparation of cardanol ester compounds with carboxyl groups: using dimethyl sulfoxide as solvent and concentrated sulfuric acid as catalyst, cardanol and oxalic acid are mixed in a molar ratio of 1:1 to cause esterification reaction at a temperature of 45-70°C for 2-8 hours. After the reaction is completed, vacuum distillation is performed to obtain monocardanol oxalate; Figure 2 Shown is the reaction formula for the preparation of monocardanol oxalate;

[0058] (2) Preparation of carbon black slurry: 50 parts of carbon black and water were mixed to prepare a mixed solution with a solid content of 3%, and the mixture was stirred in a blender to obtain a carbon black suspension. The blender speed was 300 rpm and the stirring time was 30 min. The carbon black suspension was then added to a colloid mill for grinding. The colloid mill speed was 3000 r / min. The mixture was first ground for 30 min. Then, 1 part of monocardanol oxalate was added and the mixture was ground for 30 min to obtain a carbon black slurry.

[0059] (3) Preparation of natural rubber latex: 100 parts of concentrated natural rubber latex were diluted with water to obtain a natural rubber latex with a solid content of 20%;

[0060] (4) Preparation of carbon black masterbatch: The carbon black slurry and natural rubber latex collide with each other in a mixing chamber through a high-speed jet and settle together to obtain a wet carbon black masterbatch with uniform particles. After washing, the wet carbon black masterbatch is dried in a forced air drying oven at 105° C. for 2 h to obtain the carbon black masterbatch;

[0061] The slurry outlet flow velocity is 350m / s, the flow rate is 22kg / min, the latex outlet flow velocity is 1m / s, the flow rate is 8.8kg / min.

[0062] The carbon black masterbatch of this embodiment is used to prepare the vulcanized rubber, and the steps are as follows: the carbon black masterbatch is mixed with zinc oxide, stearic acid, antioxidant 4020, accelerator CZ, and sulfur in a mass ratio of 150:5:2:1:1.2:2 for rubber refining, and after standing for 8 hours, vulcanization is carried out at 150° C. to obtain the vulcanized rubber.

[0063] Example 2

[0064] This embodiment is substantially the same as embodiment 1, the only difference being that 10 parts of monocardanol oxalate are added.

[0065] Example 3

[0066] This embodiment is substantially the same as embodiment 1, the only difference being that 15 parts of monocardanol oxalate are added.

[0067] Example 4

[0068] This embodiment is substantially the same as embodiment 1, the only difference being that 25 parts of monocardanol oxalate are added.

[0069] Comparative Example 1

[0070] This comparative example provides a method for preparing a carbon black masterbatch, comprising the following steps:

[0071] (1) Preparation of carbon black slurry: 50 parts of carbon black and water were mixed to prepare a mixed solution with a solid content of 3%, and the mixture was stirred in a stirrer to obtain a carbon black suspension. The stirrer speed was 300 rpm and the stirring time was 30 min. The carbon black suspension was then added to a colloid mill for grinding. The colloid mill speed was 3000 r / min and the grinding time was 60 min to obtain a carbon black slurry.

[0072] (2) Preparation of natural rubber latex: 100 parts of concentrated natural rubber latex were diluted with water to obtain a natural rubber latex with a solid content of 20%;

[0073] (3) Preparation of carbon black masterbatch: The carbon black slurry and natural rubber latex collide with each other in a mixing chamber through a high-speed jet and settle together to obtain a wet carbon black masterbatch with uniform particles. After washing, the wet carbon black masterbatch is dried in a forced air drying oven at 105° C. for 2 h to obtain the carbon black masterbatch;

[0074] The carbon black masterbatch of this comparative example is used to prepare a vulcanized rubber, and the steps are as follows: the carbon black masterbatch is mixed with zinc oxide, stearic acid, antioxidant 4020, accelerator CZ, and sulfur in a mass ratio of 150:5:2:1:1.2:2 for rubber refining, and after standing for 8 hours, vulcanizing at 150°C to obtain a vulcanized rubber.

[0075] Comparative Example 2

[0076] The present comparative example provides a method for preparing a carbon black masterbatch, comprising the following steps: adding 100 parts of natural rubber, 50 parts of carbon black (N234), 5 parts of zinc oxide, 2 parts of stearic acid and 1 part of antioxidant 4020 into an internal mixer for mixing, discharging the rubber after the mixing is completed, then adding 1.2 parts of accelerator CZ and 2 parts of sulfur on an open mixer, mixing evenly and producing a rubber sheet, and then standing for 8 hours and vulcanizing at 150° C. using a flat vulcanizer to obtain a vulcanized rubber.

[0077] The yield of the carbon black masterbatch prepared in Examples 1-4 and Comparative Examples 1-2 was calculated, and the properties of the vulcanized rubber were tested. The results are shown in Table 1, wherein the Akron abrasion determination standard is based on GB / T 1689-2014 Determination of wear resistance of vulcanized rubber, the compression heat generation determination standard is based on GB / T 1687-93 Determination of temperature rise and fatigue resistance of vulcanized rubber in flexure test Part 2 Compression flexure test, and the hardness determination standard is based on GB / T 531.1-2008 Vulcanized rubber or thermoplastic rubber indentation hardness test method Part 1: Shore durometer method (Shore hardness).

[0078] Table 1

[0079]

[0080]

[0081] It can be seen from Examples 1-4 and Comparative Example 1 that when no carboxyl-containing cardanol ester compound is added, the wet mixing masterbatch yield is only 84.3%. As the amount of the carboxyl-containing cardanol ester compound increases, the carboxyl group on the carboxyl-containing cardanol ester compound plays a flocculation role, so the masterbatch yield gradually increases;

[0082] It can be seen from Examples 1-4 and Comparative Example 2 that the compression heat generated by the rubber prepared by wet mixing can be reduced by 12.4-36.2% compared with the dry mixing, that is, the addition of carboxyl cardanol ester compounds can improve the dispersion of carbon black in the latex, thereby improving the hysteresis performance of the rubber, and the compression heat is gradually reduced with the increase of the amount of carboxyl cardanol ester compounds, and the wear resistance is improved;

[0083] Comparative Example 1 is a rubber prepared by wet mixing without adding carboxyl-containing cardanol ester compounds. Compared with the dry mixing of Comparative Example 2, the hardness is reduced by 16.2%. The reduction in rubber hardness is not conducive to the manufacture of tires. The embodiment of the present invention can introduce rigid group benzene rings into the rubber by adding carboxyl-containing cardanol ester compounds, thereby increasing the hardness of the rubber.

[0084] In addition, if Figure 1 As shown in the figure, it is the effect of carboxyl cardanol ester compounds on the Mooney viscosity of the masterbatch. It can be seen from the figure that the initial Mooney value of the masterbatch corresponding to Example 1 is the highest, and the hardening phenomenon of the masterbatch is very obvious. The Mooney value increases rapidly in the initial stage. With the increase of the addition amount of carboxyl cardanol ester compounds, the initial Mooney of the masterbatch gradually decreases, and the Mooney change trend is relatively gentle, which is conducive to the further processing and use of the masterbatch.

[0085] Example 5

[0086] This embodiment is basically the same as Embodiment 4, with the only difference being that: in step (1), oxalic acid is replaced by terephthalic acid; in step (2), 50 parts of carbon black are mixed with water to prepare a mixed solution with a solid content of 10%; in step (3), 100 parts of butadiene latex are diluted with water to a butadiene latex with a solid content of 40%.

[0087] Example 6

[0088] This embodiment is basically the same as embodiment 4, with the only difference being that: in step (1), oxalic acid is replaced by diphenyl ether dicarboxylic acid; in step (2), 50 parts of carbon black are mixed with water to prepare a mixed solution with a solid content of 1%; in step (3), 100 parts of concentrated styrene-butadiene latex are diluted with water to a styrene-butadiene latex with a solid content of 10%.

[0089] Comparative Example 3

[0090] This comparative example is basically the same as Example 4, with the only difference being that in step (2), 50 parts of carbon black are mixed with water to prepare a mixed solution with a solid content of 15%.

[0091] Comparative Example 4

[0092] This comparative example is basically the same as Example 4, the only difference being that in step (3), 100 parts of concentrated natural rubber latex are diluted with water to a natural rubber latex with a solid content of 45%.

[0093] Comparative Example 5

[0094] This comparative example is basically the same as Example 4, the only difference being that in step (3), 100 parts of concentrated natural rubber latex are diluted with water to a natural rubber latex with a solid content of 5%.

[0095] The yield of the carbon black masterbatch prepared in Examples 5-6 and Comparative Examples 3-5 was calculated, and the properties of the vulcanized rubber were tested. The results are shown in Table 2.

[0096] Table 2

[0097] Example 4 Example 5 Example 6 Comparative Example 3 Comparative Example 4 Comparative Example 5 Masterbatch yield / % 95.4 93.2 90.5 89.0 89.2 86.2 Compression heat / ℃ 19.0 19.5 19.2 23.5 23.4 24.1 <![CDATA[Abrasion loss by Akron test / cm 3 > 0.270 0.272 0.275 0.295 0.291 0.298

[0098] As can be seen from Table 2, changes in the solid content of carbon black slurry and natural rubber latex during the preparation process will lead to a decrease in the masterbatch yield and a deterioration in the dispersibility of carbon black, which in turn affects the compression heat generation and wear properties of the vulcanized rubber. Especially when the solid content is high, the excessive viscosity of the system is not conducive to the uniform dispersion of carbon black, which in turn causes significant changes in the compression heat generation and wear resistance of the rubber. Therefore, the present invention preferably has a solid content of 1-10% for the carbon black slurry and a solid content of 10-40% for the natural rubber latex.

[0099] Example 7

[0100] This embodiment is basically the same as embodiment 4, the only difference being that the flow velocity of the slurry outlet is 100 m / s, and the flow velocity of the latex outlet is 0.5 m / s.

[0101] Example 8

[0102] This embodiment is basically the same as embodiment 4, the only difference being that the slurry outlet flow velocity is 500 m / s, and the latex outlet flow velocity is 5 m / s.

[0103] Comparative Example 6

[0104] This comparative example is basically the same as Example 4, the only difference being that the slurry outlet flow rate is 350 m / s, and the latex outlet flow rate is 350 m / s.

[0105] Comparative Example 7

[0106] This comparative example is basically the same as Example 4, the only difference being that the slurry outlet flow rate is 1 m / s, and the latex outlet flow rate is 1 m / s.

[0107] Comparative Example 8

[0108] This comparative example is basically the same as Example 4, the only difference being that the slurry outlet flow velocity is 350 m / s, and the latex outlet flow velocity is 10 m / s.

[0109] Comparative Example 9

[0110] This comparative example is basically the same as Example 4, the only difference being that the slurry outlet flow velocity is 80 m / s, and the latex outlet flow velocity is 1 m / s.

[0111] Comparative Example 10

[0112] This comparative example is basically the same as Example 4, the only difference being that the slurry outlet flow velocity is 550 m / s, and the latex outlet flow velocity is 1 m / s.

[0113] The yield of the carbon black masterbatch prepared in Examples 7-8 and Comparative Examples 6-10 was calculated, and the properties of the vulcanized rubber were tested. The results are shown in Table 3.

[0114] Table 3

[0115]

[0116] It can be seen from Examples 4, 7-8 and Comparative Examples 6-10 in Table 3 that since the present invention mainly utilizes the huge speed difference between the slurry flow and the latex flow to fully mix and disperse the carbon black and latex, thereby obtaining a carbon black masterbatch with uniform particles, when the speeds of the slurry flow and the latex flow are consistent or the speed of a certain fluid exceeds the specified range, it will affect the masterbatch production efficiency and the overall performance of the rubber. In particular, when the speeds of the slurry flow and the latex flow are consistent, the production efficiency of the masterbatch will be severely reduced and the overall performance of the rubber will be very poor, resulting in an ineffective utilization.

[0117] In summary, the present invention can improve the dispersion of fillers and increase the masterbatch yield while increasing the wear resistance of the rubber, reducing the hysteresis heat generation, effectively inhibiting the hardening of the latex, and extending the storage time of the masterbatch by introducing carboxyl-containing cardanol ester compounds and strictly limiting the solid content of carbon black slurry and latex, the flow rate of slurry flow and latex flow, etc.

[0118] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the scheme disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.

[0119] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A method for preparing a constant viscosity carbon black masterbatch, characterized in that: The following steps are involved: (1) mixing carbon black with water to obtain a carbon black suspension, grinding and adding a carboxyl-containing cardanol ester compound to obtain a carbon black slurry; (2) the carbon black slurry and latex collide in a mixing chamber through high-speed jets, settle together, and obtain a carbon black masterbatch after washing and drying; The carbon black suspension in step (1) is prepared by mixing carbon black and water to form a mixed solution with a solid content of 1-10% and then stirring the mixture to obtain a uniform mixture; The stirring speed is 100-500 rpm, and the stirring time is 20-60 min; The grinding speed is 1000-4000r / min, and the grinding time is 20-60min; The latex in step (2) is obtained by diluting concentrated latex with water to a solid content of 10-40%; In step (2), the flow rate of the carbon black slurry outlet is 100-500 m / s, and the flow rate of the latex outlet is 0.5-5 m / s; The drying temperature is 60-120°C and the drying time is 1-3h; 10-100 parts of carbon black, 40-160 parts of latex, and 1-25 parts of carboxyl-containing cardanol ester compounds; the latex includes natural latex and / or synthetic latex; the carboxyl-containing cardanol ester compounds are obtained by esterification reaction of dicarboxylic acid compounds and cardanol: using an organic solvent as a reaction solvent, mixing the dicarboxylic acid compounds and cardanol, and causing an esterification reaction under the catalytic action of a catalyst, and after the reaction is completed, distilling under reduced pressure to obtain the carboxyl-containing cardanol ester compounds; the reaction temperature of the esterification reaction is 45-70°C, and the reaction time is 2-8h; The molar ratio of the cardanol to the dicarboxylic acid compound is 1:1-2.

2. Application of the constant viscosity carbon black masterbatch prepared by the method of claim 1 in vulcanized rubber.

Citation Information

Patent Citations

  • Biomass cardanol plasticized chloroprene rubber compound and preparation process thereof

    CN111607138A

  • Application method of cardanol in rubber

    CN114920989A