A kind of compression toughened ultra-high performance concrete and preparation method thereof

By using steel fibers, polymer fibers, metal springs and polymer emulsions in ultra-high performance concrete to form a synergistic toughening structure, the problem of difficulty in improving the compressive toughness of ultra-high performance concrete is solved, and high pressure is achieved The unity of strength and deformation ability and ensure the fluidity and mechanical properties of the material.

CN116535157BActive Publication Date: 2024-11-12SOUTHEAST UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310371107.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-10
Publication Date
2024-11-12
Estimated Expiration
2043-04-10

AI Technical Summary

Technical Problem

Ultra-high performance concrete has difficulties in improving compressive toughness. The existing technology mainly increases the area under the compressive stress-strain curve, but it cannot effectively improve the ratio of peak compressive strength to initial crack compressive strength and peak compressive strain. The compression strain ratio is increased to the initial cracking and the material brittleness increases.

Method used

Using a mixture of steel fibers and polymer fibers, fine cylindrical spiral metal springs and disc metal springs as rigid elastomers, flexible elastomers and polymer emulsions, the matrix high is achieved by forming a polymer network and interwoven structure, combined with a viscosity control agent. Toughness and interface enhancement, coordinated reinforcement of fiber constraints and elastomer energy absorption effects.

Benefits of technology

It significantly improves the compression toughness of ultra-high performance concrete, ensures that the compressive strength does not decrease, the flow is good, the ratio of peak compressive strength to initial cracking and the ratio of peak compressive strain to initial cracking and the compressive strain ratio of peak compressive strain to initial cracking exceeds 1.2. It solves the problem of mechanical properties deterioration caused by polymer toughening, and is suitable for ultra-high performance concrete without coarse aggregates and containing coarse aggregates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116535157B_ABST
    Figure CN116535157B_ABST
Patent Text Reader

Abstract

The present invention discloses a compressive toughening ultra-high performance concrete and a preparation method thereof, and belongs to the technical field of building materials. The raw materials of the compressive toughening ultra-high performance concrete include cementitious materials, rigid elastomers, flexible elastomers, polymer emulsions, fibers, viscosity control agents, water reducers, coarse aggregates, and water; the fibers are a mixture of steel fibers and polymer fibers, and the volume ratio of steel fibers to polymer fibers is 0-1.2:0.5-1.8; the rigid elastomers are metal springs, the flexible elastomers are plastic particles, and the polymer emulsions are one or more of chloroprene latex, styrene-butadiene latex, and nitrile latex in any proportion. The present invention proposes a compressive toughening design method based on matrix-toughening body synergistic toughening, which realizes the all-round compressive performance improvement of the elastic section, microcrack extension section, and main crack extension and destruction stage in the compressive stress-strain curve of ultra-high performance concrete.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and specifically relates to a compressive toughened ultra-high performance concrete and a preparation method thereof. Background Art

[0002] As the most common stress condition for civil engineering structures, compressive loads require concrete to have high compressive strength and excellent compressive toughness, just like the requirements for concrete bending and tensile properties. The compressive toughness of concrete can usually be expressed by the area under the compressive stress-strain curve. The larger the area, the better the toughness. Its compressive stress-strain curve can be roughly divided into three stages: (1) elastic stage, in which the stress-strain curve changes linearly. The maximum stress in the linear stage is the initial crack compressive strength, and the corresponding strain is the initial crack compressive strain; (2) microcrack extension stage, in which the stress-strain curve no longer changes linearly due to the formation and development of microcracks, and eventually a main crack is formed. The maximum stress in this stage is the peak compressive strength, and the corresponding strain is the peak compressive strain; (3) main crack extension and destruction stage, in which the main crack formed by microcracks continues to expand until the specimen is destroyed. However, in the main crack extension stage, the crack width has reached the macroscopic size. At this time, not only the mechanical properties and durability of the concrete itself will decline rapidly, but also the durability and life of the overall structure will be sharply lost. Therefore, the improvement of the compressive toughness of concrete should not only focus on the area under the entire curve, but also should regulate the elastic section and microcrack extension section to make it have a higher ratio of peak compressive strength (σu) to first crack compressive strength (σc) and peak compressive strain (εu) to first crack compressive strain (εc).

[0003] Ultra High Performance Concrete (UHPC) is widely used in the field of bridge engineering due to its ultra-high strength, ultra-high flexural toughness and ultra-high durability. It has become one of the preferred materials for the construction of major national infrastructure projects and national defense security facilities. The ratio of peak flexural strength to first crack flexural strength of ultra-high performance concrete can reach more than 1.5, and the ratio of peak tensile strength to first crack tensile strength can reach more than 1.2, while its peak compressive strength to first crack compressive strength ratio is only 1.0 to 1.2, which is much lower than the peak compressive strength to first crack compressive strength ratio of about 2.0 for ordinary concrete; and the addition of coarse aggregate will further increase the brittleness of the material and reduce the ratio of peak compressive strength to first crack compressive strength. Therefore, how to improve the compressive toughness of ultra-high performance concrete is crucial.

[0004] At present, the compressive toughness of materials is mainly improved by the elastic energy absorption of polymers and the prevention of crack propagation. Patent 201210072871 discloses a high-compression toughened PVC resin composition, which uses chlorinated polyethylene (CPE) as a toughening agent and is prepared by thermoplastic molding. The principle is that its molecular chain contains active groups that can react with the matrix resin, and the toughness is increased by forming a network structure. However, due to the huge difference between the preparation method and the field to which it belongs, it cannot be used for cement-based materials.

[0005] Patent 202110281940.2 discloses a self-healing cement-based composite material and its preparation method and application. PVA fiber is used to achieve higher compressive toughness, showing the effect of "cracked but not broken", and the focus is still on improving the compressive performance after the peak. Patent 201811207141.5 discloses a hybrid fiber concrete and its preparation method and application. It uses a mixture of steel fiber and PVA fiber to improve the compressive toughness of cement-based materials. The improvement of compressive toughness of both is to increase the area under the compressive stress-strain curve, which is not the same as improving the ratio of peak compressive strength to initial crack compressive strength and the ratio of peak compressive strain to initial crack compressive strain. The appendix in patent 201811207141.5 Figure 1 It shows that although the compressive toughness index increases, the curves before the peak value are basically overlapped (the elastic proportional limit does not change), and the slope of the curve from the peak value to the stage where the stress drops to 70% to 75% of the peak value does not change significantly. This is mainly because the speed of bearing capacity reduction is improved after the stress drops rapidly by about 25% to 30% after the peak value (under high stress state, the bearing capacity has dropped rapidly), and the compressive toughness is improved accordingly. In addition, both are for low-strength concrete (compressive strength <50MPa). The higher the material strength, the stronger the brittleness. The compressive strength of ultra-high performance concrete is more than 2.5 times that of the two; and existing studies have also pointed out that the ratio of peak compressive strength to initial crack compressive strength and the ratio of peak compressive strain to initial crack compressive strain cannot be effectively improved by polymer fibers or polymer and steel fiber mixing alone. Summary of the invention

[0006] In view of the current difficulty in improving the compressive toughness of ultra-high performance concrete, the present invention proposes a compressive toughened ultra-high performance concrete and a preparation method thereof, which can effectively improve the compressive toughness of ultra-high performance concrete and ensure that the compressive strength of ultra-high performance concrete has no obvious decrease and the mixture has good working performance.

[0007] To achieve the above object, the technical solution of the present invention is:

[0008] A compressive toughened ultra-high performance concrete, the raw materials of which include the following components and the volume fractions of each component are as follows:

[0009]

[0010]

[0011] The fiber is a mixture of steel fiber and polymer fiber, and the volume ratio of steel fiber to polymer fiber is 0-1.2:0.5-1.8;

[0012] The rigid elastic body is a metal spring, the flexible elastic body is plastic or rubber particles, and the polymer emulsion is one of chloroprene latex, styrene-butadiene latex, and nitrile latex, or a mixture of two or more of them in any proportion.

[0013] The rigid elastomer is one of a fine cylindrical helical metal spring and a butterfly metal spring or a mixture of two of them in any proportion; the fine cylindrical helical spring has a wire diameter of 0.2-0.5 mm, a diameter of 1.5-5 mm, a number of turns of 3-10, and a length of 5-20 mm; the disc spring has an outer diameter of 8-20 mm, an inner diameter of 4-10 mm, a thickness of 0.4-1 mm, and a height of 0.6-1.5 mm. For cylindrical helical metal springs, if the wire diameter, diameter, number of turns, and length are too small, the rigid elastomer itself has a poor compressive toughening effect, and the cement matrix cannot effectively fill the interior of the spring, which also deteriorates the compressive toughening effect; if the wire diameter, diameter, number of turns, and length are too large, it is not conducive to its uniform distribution, and the compressive toughening effect is also poor. Similar to cylindrical helical springs, for disc metal springs, the outer diameter, inner diameter, thickness, and height are too small or too large, which are not conducive to the compressive toughening effect.

[0014] The tensile strength of the flexible elastomer is greater than 20MPa, the elongation at break is greater than 10%, and the particle size is 0.075 to 2.36mm. The tensile strength of UHPC is usually greater than 10MPa, and can even reach more than 15MPa. As a material component in UHPC, the tensile strength of the flexible elastomer should be higher than the tensile strength of the material as a whole, otherwise the mechanical properties of UHPC will be degraded. For the deformation performance of UHPC, steel fiber and organic fiber are the most commonly used toughening materials, and their elongations at break are 0-5% and 5%-10%, respectively. In order to further improve the toughness of UHPC and form a multi-level complementary toughening system with steel fiber and organic fiber, the elongation at break of the flexible elastomer should not be too low. Based on the design concept of the most densely packed UHPC, small-sized particles should be used as much as possible to improve the density of the system. As a substitute for sand, the maximum particle size of the flexible elastomer cannot be too large; if the particle size is too small, the skeleton effect cannot be exerted, and the toughening effect is reduced.

[0015] The plastic can be selected from nylon particles, ABS plastic particles, TPU plastic particles, or a mixture of two or more in any proportion;

[0016] Furthermore, the flexible elastic body is one or a mixture of any two or more of recycled nylon particles, recycled ABS plastic particles, recycled TPU plastic particles, and recycled rubber particles. The large amount of recycled plastic and rubber particles can still ensure the excellent compressive toughness and compressive strength of ultra-high performance concrete, and has excellent green and low-carbon performance.

[0017] The polymer fiber is a mixture of one or more of polypropylene (PP) fiber, polyvinyl alcohol (PVA) fiber, polyester (PET) fiber, and polyoxymethylene (POM) fiber in any proportion; the polymer fiber has a diameter of 0.02-0.4 mm and a length of 4-20 mm; the steel fiber has a diameter of 0.18-0.4 mm and a length of 6-20 mm. Diameter and length are important parameters of the fiber. Too small a diameter makes the fiber difficult to produce and the material selection difficult. Too small a diameter will significantly increase the fiber specific surface area, which is not conducive to fiber dispersion and affects its toughening effect. Too large a fiber diameter will reduce the number of fibers and increase the fiber-matrix interface transition zone, which is not conducive to the toughening effect. For the fiber length, too small a length will reduce its ability to restrain the aggregate and weaken the bridging effect. Too long a length will cause the fibers to entangle and agglomerate, and they cannot be effectively and evenly dispersed, which also deteriorates the toughening effect.

[0018] The cementitious material is composed of cement and admixture, and the volume ratio of the cement to the admixture is 1:0.7-1.5;

[0019] Furthermore, the cement is silicate or ordinary silicate cement of grade 42.5 or above.

[0020] Furthermore, the admixture is silica fume, fly ash, ultrafine mineral powder, and ultrafine limestone powder mixed in a volume ratio of 1:0.5-2:0.75-2.5:0.75-2.5; the specific surface area of ​​the silica fume is greater than 16000m 2 / kg, the average particle size of fly ash is 2-10μm, the ultrafine mineral powder is granulated blast furnace slag powder of grade S95 or above specified in GB / T 18046-2017, and the average particle size of ultrafine limestone powder is 2-10μm.

[0021] The viscosity control agent is a mixture of sodium carbonate, sodium sulfate and sodium benzenesulfonate in a volume ratio of 1:1-3:0.1-0.2;

[0022] The coarse aggregate is one of basalt coarse aggregate, limestone coarse aggregate and granite coarse aggregate or a mixture of two or more of them in any proportion; the particle size of the coarse aggregate is 5 to 16 mm.

[0023] The sand is river sand or quartz sand with a maximum particle size of ≤2.36 mm and a fineness modulus of 2.2 to 2.8.

[0024] The water reducing agent is a polycarboxylic acid high efficiency water reducing agent, and the water reducing rate is ≥30%.

[0025] The compression toughened ultra-high performance concrete of the present invention takes matrix-toughening body synergistic toughening as the design concept, adopts polymer emulsion, and constructs polymer network through adsorption film formation to achieve matrix toughening; introduces micro- and nano-ultrafine powders in cementitious materials to densely fill vacancies and defects in the polymer network, improves matrix density, and plays the role of nanoparticles in promoting hydration, so that the hydration product and the polymer network form an interwoven and interpenetrating structure, thereby reducing the negative impact of polymer emulsion on strength; uses steel fiber and polymer fiber hybrid, especially considers the flexible deformation characteristics of polymer fiber, further exerts the reinforcement and toughening effect of fiber, and the polymer emulsion and micro- and nano-ultrafine powders in the matrix can improve the toughness of the fiber-matrix interface transition zone, Improve the fiber bonding performance, thereby achieving high toughness of the matrix - interface reinforcement - fiber constraint; on this basis, introduce rigid elastomer and flexible elastomer as toughening skeleton, so that the skeleton has both support and energy absorption deformation under pressure, and polymer emulsion and micro- and nano-ultrafine powder can also improve the toughness of the elastomer-matrix interface transition zone, combined with the constraint effect of polymer-steel fiber hybrid on rigid elastomer and flexible elastomer, and the viscosity control agent on the uniform dispersion of rigid elastomer and flexible elastomer, finally achieve the synergistic enhancement and toughening effect of high toughness of the matrix - interface reinforcement - fiber constraint - elastomer energy absorption support, achieve the unity of high compressive strength and deformation capacity, thereby greatly improving the compressive toughness of ultra-high performance concrete.

[0026] On the other hand, the present invention also provides a method for preparing a compression-toughened ultra-high performance concrete, the method for preparing a compression-toughened ultra-high performance concrete specifically comprising the following steps:

[0027] (1) Add cementitious material, viscosity control agent, sand, flexible elastomer and coarse aggregate according to volume ratio and dry mix;

[0028] (2) Continue to add the polymer emulsion, water reducer, and water to form a uniform mixture, and mix well to form a stable flowing slurry;

[0029] (3) Continue to add the rigid elastomer and stir to mix;

[0030] (4) Continue to add fibers and stir to mix well to obtain the compression toughened ultra-high performance concrete.

[0031] Furthermore, the stirring time of step (3) is controlled within 30s to 60s, and the stirring time of step (4) is within 1 to 2min. The stirring time is controlled because too long stirring time is not conducive to uniform dispersion of rigid elastomer and fiber, and will cause temperature rise, which is not conducive to material performance control.

[0032] Compared with the prior art, the beneficial effects of the present invention are:

[0033] (1) The present invention proposes a compressive toughening design method based on the synergistic toughening of the matrix and the toughening body, which achieves an all-round improvement in the compressive performance of ultra-high performance concrete in the elastic section, microcrack extension section, and main crack extension and failure stage in the compressive stress-strain curve.

[0034] (2) The ratio of peak compressive strength to first crack compressive strength of the compression-toughened ultra-high performance concrete of the present invention is greater than 1.2, the ratio of peak compressive strain to first crack compressive strain is greater than 1.2, and the compressive strength is greater than 130 MPa, which solves the problem of mechanical property degradation caused by polymer toughening.

[0035] (3) The compressive toughening ultra-high performance concrete of the present invention not only realizes the compressive toughening of ultra-high performance concrete without coarse aggregate, but also realizes the compressive toughening of ultra-high performance concrete containing coarse aggregate, and the fluidity of the mixture is ≥450mm, which has good practical engineering application value.

[0036] (4) The total volume proportion of cement in the compression-toughened ultra-high performance concrete of the present invention does not exceed 40%, and a large amount of recycled plastic and rubber particles can be used, which has excellent green and low-carbon performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is the compressive stress-strain curve of the compression-toughened ultra-high performance concrete described in Examples 1 to 9 of the present invention.

[0038] Figure 2 The compressive stress-strain curves of the ultra-high performance concrete described in Example 1 and Comparative Examples 1 to 4 of the present invention.

[0039] Figure 3 The compressive stress-strain curves of the ultra-high performance concrete described in Example 9 and Comparative Example 5 of the present invention.

[0040] Figure 4 The attached background technology patent 201811207141.5 Figure 1 . DETAILED DESCRIPTION

[0041] Hereinafter, embodiments of the present invention will be described in detail. However, the present invention may be implemented in many different forms, and the present invention should not be construed as being limited to the specific embodiments set forth herein. On the contrary, these embodiments are provided to explain the principles of the present invention and their practical applications, so that other persons skilled in the art can understand the various embodiments of the present invention and the various modifications suitable for specific intended applications.

[0042] In order to verify the excellent performance of the compression toughened ultra-high performance concrete of the present invention, embodiments 1 to 9 and comparative examples 1 to 5, which include two ultra-high performance concrete systems, one without coarse aggregate and one with coarse aggregate, are provided.

[0043] The raw materials for preparing the compression toughened ultra-high performance concrete in Examples 1-9 and Comparative Examples 1-5 are as follows:

[0044] The cement is Helin PO42.5 cement; the specific surface area of ​​silica fume is 18000m 2 / kg, the average particle size of fly ash is 7.8μm, the ultrafine mineral powder is S95 grade granulated blast furnace slag powder specified in GB / T 18046-2017, and the average particle size of ultrafine limestone powder is 6.510μm; the sand is river sand with a modulus of 2.6; the steel fiber is a copper-plated steel fiber with a diameter of 0.35mm and a length of 20mm; the polymer fiber size is 0.04mm in diameter, 12mm in length and 0.2mm in diameter, 12mm in length; the rigid elastomer is a fine cylindrical helical spring with a wire diameter of 0.35mm, a diameter of 3.5mm, 6 turns, and a length of 15mm, and a disc spring with an outer diameter of 14mm, an inner diameter of 7.2mm, a thickness of 0.8mm, and a height of 1.1mm; the particle size of the flexible elastomer is 0.075-1.18mm; the water reducer is produced by Jiangsu Subote Polycarboxylic acid high-efficiency water-reducing agent, water-reducing rate ≥30%; coarse aggregate is basalt stone with a particle size of 10 to 16 mm.

[0045] The raw materials for preparing the compression toughened ultra-high performance concrete in Examples 1-9 and Comparative Examples 1-5 include the following components and the volume fractions of each component are shown in Table 1. Among them, the rigid elastomer used in Example 1, Examples 4-9, and Comparative Examples 1-5 is a fine cylindrical coil spring, the rigid elastomer used in Example 2 is a butterfly spring, and the rigid elastomer used in Example 3 is a fine cylindrical coil spring with a volume ratio of 1:1 to the butterfly spring.

[0046] Table 1 Raw material components and their volume fractions of Examples 1-9 and Comparative Examples 1-5

[0047]

[0048]

[0049] The compositions of the gelling material, viscosity control agent, fiber and flexible elastomer in the raw materials of Examples 1-9 and Comparative Examples 1-5 are shown in Tables 2-5, respectively.

[0050] Table 2 Composition and volume ratio of cementitious materials of Examples 1-9 and Comparative Examples 1-5

[0051] cement Silica Fume Fly ash Ultrafine mineral powder Ultrafine limestone powder Example 1 1 0.5 0.25 0.375 0.375 Example 2 1 0.5 0.25 0.375 0.375 Example 3 1 0.5 0.25 0.375 0.375 Example 4 1 0.5 0.25 0.375 0.375 Example 5 1 0.154 0.23 0.308 0.308 Example 6 1 0.0875 0.175 0.219 0.219 Example 7 1 0.24 0.24 0.36 0.36 Example 8 1 0.2 0.2 0.3 0.3 Example 9 1 0.0875 0.175 0.219 0.219 Comparative Example 1 1 0.5 0.25 0.375 0.375 Comparative Example 2 1 0.5 0.25 0.375 0.375 Comparative Example 3 1 0.5 0.25 0.375 0.375 Comparative Example 4 1 0.5 0.25 0.375 0.375 Comparative Example 5 1 0.0875 0.175 0.219 0.219

[0052] Table 3 Composition and volume ratio of viscosity control agents of Examples 1-9 and Comparative Examples 1-5

[0053] Sodium sulfate Sodium carbonate Sodium benzenesulfonate Example 1 1 1 0.1 Example 2 1 1 0.1 Example 3 1 1 0.1 Example 4 1 1 0.1 Example 5 2 1 0.15 Example 6 3 1 0.2 Example 7 1 1 0.1 Example 8 2 1 0.15 Example 9 3 1 0.2 Comparative Example 1 1 1 0.1 Comparative Example 2 1 1 0.1 Comparative Example 3 1 1 0.1 Comparative Example 4 1 1 0.1 Comparative Example 5 3 1 0.2

[0054] Table 4 Composition and volume ratio of the fibers of Examples 1-9 and Comparative Examples 1-5

[0055]

[0056]

[0057] Table 5 Composition and volume proportion of the flexible elastomers of Examples 1-9 and Comparative Examples 1-5

[0058] Composition and volume ratio of flexible elastomer Example 1 Recycled rubber particles Example 2 Recycled rubber particles Example 3 Recycled rubber particles Example 4 Rubber Granules Example 5 Recycled ABS plastic particles and recycled rubber particles volume ratio 1:1 Example 6 Recycled nylon particles and recycled TPU plastic particles volume ratio 1:1 Example 7 Recycled ABS plastic particles and recycled TPU plastic particles volume ratio 1:1 Example 8 Recycled nylon particles and recycled ABS plastic particles volume ratio 1:1 Example 9 Recycled TPU plastic granules Comparative Example 1 Recycled rubber particles Comparative Example 2 Recycled rubber particles Comparative Example 3 Recycled rubber particles Comparative Example 4 Recycled rubber particles Comparative Example 5 Recycled TPU plastic granules

[0059] The preparation methods of the compression toughened ultra-high performance concrete in Examples 1-9 and Comparative Examples 1-5 are as follows:

[0060] (1) Add cement and admixtures, viscosity control agent, sand, flexible elastomer, and coarse aggregate, and dry mix for 30 seconds;

[0061] (2) Add a uniform mixture of polymer emulsion, high-efficiency water reducer and water and stir for 3 minutes to form a stable flowing slurry;

[0062] (3) Add rigid elastomer after 20 seconds and stir for 30 seconds;

[0063] (4) Adding fibers after 30 seconds and stirring for 2 minutes to obtain the compressive toughened ultra-high performance concrete.

[0064] Performance Testing

[0065] The fluidity test of the compression-toughened ultra-high performance concrete after mixing was carried out, and the test method referred to GB / T50080~2016 "Standard Test Method for Performance of Ordinary Concrete Mixtures". After the fluidity test was completed, the specimens were formed (100mm×100mm×300m prisms), cured for 28 days under standard conditions, and the compression performance test was carried out to obtain the compressive stress-strain curve. The compression performance test method is: use a high-rigidity press to pre-load the specimen at 50MPa; then, use a loading rate of 1MPa / s to load from 0MPa to 100MPa; finally, continue loading at a loading rate of 0.05mm / min until the bearing capacity of the specimen drops to less than 35% of the peak stress. The test results are as follows: Figures 1 to 3 and as shown in Table 6.

[0066] Table 6 Test results of ultra-high performance concrete compressive characteristic values ​​in the examples and comparative examples

[0067]

[0068] Combination Figure 1 From the test results in Table 6, it can be seen that the compressive properties of the elastic section and microcrack extension section before the peak stress of the compression-toughened ultra-high performance concrete of the present invention are significantly improved, the ratio of peak compressive strength to initial crack compressive strength is 1.21-1.73, and the ratio of peak compressive strain to initial crack compressive strain is 1.33-2.15. For the main crack extension and destruction stage after the peak, no brittle failure occurred in Examples 1-9. And for Examples 1-4 in which the volume of cementitious materials accounts for 45%, when the compressive stress decays to 50% of the peak stress, the strain still increases by about 100%; and when the volume of cementitious materials accounts for only 25% (Examples 7-9), when the compressive stress decays to 50% of the peak stress, the strain also increases by more than 70%. Therefore, the compression-toughened ultra-high performance concrete of the present invention has excellent compressive toughness.

[0069] Compared with the reference group Example 1, the rigid elastomer is not added in Comparative Example 1, but the amount of steel fiber and flexible elastomer is increased. Figure 2 From the test results in Table 6, it can be seen that although Comparative Example 1 has a higher ratio of peak compressive strength to first crack compressive strength and peak compressive strain to first crack compressive strain, the destruction of the toughening skeleton causes a significant decrease in fluidity and peak strength, which deteriorates the mechanical properties and construction performance of the ultra-high performance concrete.

[0070] Compared with the reference group Example 1, in Comparative Example 2, no flexible elastomer is added, but the amount of polymer emulsion, polymer fiber and rigid elastomer is increased. Figure 2 From the test results in Table 6, it can be seen that for Example 2, although the compressive strength is improved, due to the lack of flexible energy-absorbing components, the ratio of its peak compressive strength to the initial crack compressive strength is less than 1.2, that is, after the initial crack, the bearing capacity is less improved, and the compressive toughness of the elastic section and the microcrack extension section is poor.

[0071] Compared with the reference group Example 1, only less polymer emulsion is added in Comparative Example 3, while the amount of rigid elastomer and fiber is increased. Figure 2 From the test results in Table 6, it can be seen that in Comparative Example 3, due to the decrease in matrix toughness, the initial crack strength of the ultra-high performance concrete is improved; and the increase in the amount of rigid body causes the peak strength to increase, and the brittleness of the elastic section and microcrack extension section of the ultra-high performance concrete increases, resulting in a significant decrease in the ratio of peak compressive strength to initial crack compressive strength and the ratio of peak compressive strain to initial crack compressive strain. In addition, the compressive bearing capacity after the peak value also decreases rapidly, and the compressive toughness in the main crack extension and destruction stages deteriorates.

[0072] Compared with the reference group Example 1, an excess amount of polymer emulsion is added in Comparative Example 4. Figure 2As can be seen from the test results in Table 6, due to the increase in polymer, Comparative Example 4 forms a large number of network structures in the ultra-high performance concrete matrix, which makes it have excellent peak compressive strength to first crack compressive strength ratio and peak compressive strain to first crack compressive strain ratio; but the fluidity and mechanical properties decrease the most. From the perspective of mechanical performance indicators, it is basically no longer an ultra-high performance concrete material; and from the perspective of flow performance, it cannot be used in actual engineering applications.

[0073] Compared with the reference group Example 9, the comparative example 5 adds an excess of polymer fibers. Figure 2 As shown in the test results of Table 6, in Comparative Example 5, due to the flexible characteristics of polymer fibers, the entanglement and interlocking effects between the polymer fibers themselves and the steel fibers and coarse aggregates are enhanced, and the packing density of the ultra-high performance concrete is reduced, resulting in a decrease in the fluidity and mechanical properties of the ultra-high performance concrete. The deterioration of the internal pore structure of the ultra-high performance concrete and the increase in defects reduce the ratio of the peak compressive strength to the initial crack compressive strength and the ratio of the peak compressive strain to the initial crack compressive strain, and the compressive bearing capacity after the peak value decreases rapidly. That is, the compressive performance of the elastic section, microcrack extension section, and main crack extension and destruction stage of the ultra-high performance concrete is reduced.

[0074] It can be seen that the compressive toughening ultra-high performance concrete of the present invention achieves the compressive toughening performance of ultra-high performance concrete and coarse aggregate ultra-high performance concrete while ensuring fluidity and ultra-high mechanical properties by giving play to the synergistic effect of polymer matrix toughening, hybrid fiber and rigid and flexible elastomer reinforcement toughening. These components influence each other in combination, and do not exist independently.

Claims

1. A compressive toughened ultra-high performance concrete, characterized in that: The raw materials of the compression toughened ultra-high performance concrete include the following components and the volume fractions of each component are as follows: 25~45 parts of cementitious material; Rigid elastomer 0.25~2 parts; 1.25~10 parts of flexible elastomer; 3-10 parts of polymer emulsion; Fiber 0.75~3 parts; Viscosity control agent 0.05~0.2 parts; Water reducing agent 0.1~0.25 parts; Coarse aggregate 0~25 parts; Sand 11.7~37.5 parts; 10~20 parts water; The fiber is a mixture of steel fiber and polymer fiber, and the volume ratio of steel fiber to polymer fiber is 0-1.2:0.5-1.8; The flexible elastic body is plastic or rubber particles; The rigid elastic body is one of a fine cylindrical helical metal spring and a disc-shaped metal spring, or a mixture of the two in any proportion; the fine cylindrical helical metal spring has a wire diameter of 0.2-0.5 mm, a diameter of 1.5-5 mm, a number of turns of 3-10, and a length of 5-20 mm; the disc-shaped metal spring has an outer diameter of 8-20 mm, an inner diameter of 4-10 mm, a thickness of 0.4-1 mm, and a height of 0.6-1.5 mm; The cementitious material is composed of cement and admixture, and the volume ratio of the cement to the admixture is 1:0.7-1.5; The admixture is silica fume, fly ash, ultrafine mineral powder and ultrafine limestone powder mixed in a volume ratio of 1:0.5~2:0.75~2.5:0.75~2.

5.

2. The compression toughened ultra-high performance concrete according to claim 1, characterized in that: The plastic is one of nylon particles, ABS plastic particles, and TPU plastic particles, or a mixture of two or more of them in any proportion.

3. The compression toughened ultra-high performance concrete according to claim 1, characterized in that: The flexible elastomer is one of recycled nylon particles, recycled ABS plastic particles, recycled TPU plastic particles, and recycled rubber particles, or a mixture of two or more of them in any proportion.

4. The compression toughened ultra-high performance concrete according to claim 1, characterized in that: The polymer fiber is a mixture of one or more of polypropylene fiber, polyvinyl alcohol fiber, polyester fiber and polyoxymethylene fiber in any proportion.

5. The compression toughened ultra-high performance concrete according to claim 1, characterized in that: The viscosity control agent is a mixture of sodium carbonate, sodium sulfate and sodium benzenesulfonate in a volume ratio of 1:1-3:0.1-0.

2.

6. The method for preparing the compressive toughened ultra-high performance concrete according to any one of claims 1 to 5, characterized in that: The specific steps include: (1) Add cementitious material, viscosity control agent, sand, flexible elastomer and coarse aggregate according to volume ratio and mix thoroughly; (2) Continue to add a uniform mixture of polymer emulsion, water reducer and water, and mix well to form a stable flowing slurry; (3) Continue to add rigid elastomer and stir to mix; (4) Continue to add fibers and stir to mix well to obtain the compressive toughened ultra-high performance concrete.

7. The method for preparing a compressively toughened ultra-high performance concrete according to claim 6, characterized in that: The stirring time of step (3) is controlled within 30s to 60s, and the stirring time of step (4) is within 1 to 2min.