A method for preparing multifunctional natural polymer porous material
By introducing a flexible chemical network and preforming a macroporous structure into porous materials, the problem of material structure shrinkage during the freeze-drying process is solved, and the complete morphology and high porosity of the material are achieved, which is suitable for multiple application fields.
Patent Information
- Application Number
- CN202210114412.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-30
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-01-30
AI Technical Summary
It is difficult to prepare complete porous materials with existing technology. During the freeze-drying process, the internal structure of the material causes the skeleton to shrink and the gel structure to collapse due to the growth of ice crystals, resulting in an incomplete porous material structure.
By introducing a flexible chemical network into the preparation of porous materials, a macroporous structure is formed in advance to reduce capillary tension, and a dual method of chemical cross-linking and physical cross-linking is used to form non-covalent interactions to improve the strength and toughness of the material.
It achieves the structural regularity and retention of the pore structure of the material, ensures the complete morphology and high porosity of the material after drying, improves the strength and toughness of the material, and is suitable for the fields of environment, medicine, aerospace and other fields.
Smart Images

Figure CN116554538B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparing environmentally friendly materials, and in particular to a method for preparing a multifunctional natural polymer porous material. Background Art
[0002] The increasing environmental pollution and the gradual shortage of oil resources have made people urgently need new resource substitutes. Cellulose, the most abundant natural polymer in nature, is gradually coming onto the historical stage. Cellulose, which is widely found in materials such as trees, bamboo, cotton and linen, is gaining popularity due to its inexhaustible source and excellent biocompatibility, degradability and other green and environmentally friendly properties. In addition, people have more requirements for the performance of materials, and multifunctional materials are more favored in the rapid development of science and technology. The hydroxyl groups on the cellulose molecular chain have excellent reactivity and can be used for etherification, esterification, graft copolymerization or composited with other materials to form materials with specific functions. For example, continuously etherified cellulose has excellent UV blocking and fluorescence effects (Green Chem., 2021, 23, 479). Water-soluble carboxymethyl cellulose and its derivatives can be used as bio-inks for 3D printing (Carbohydrate Polymers 256 (2021) 117561). Cellulose nanofibers isolated from green algae can be combined with metal-organic frameworks through electrostatic interactions to prepare flexible electrodes for energy storage (J. Mater. Chem. A, 2018, 6, 24050–24057). In addition to cellulose, there is chitin in nature, a natural polymer second only to cellulose in content. Chitin, which is widely found in the shells of crustaceans such as shrimps and crabs, and mollusks such as cuttlefish and squid, has hydroxyl groups similar to cellulose, as well as acetylamino groups that can be used as a nitrogen source for carbon materials; chitosan obtained by deacetylation of chitin contains abundant amino groups and is the only alkaline polysaccharide in nature. Compared with hydroxyl groups, amino groups are not only more reactive, but can also be protonated under acidic conditions to form ammonium ions with cationic properties, which can combine with negatively charged components such as bacterial cell membranes to achieve antibacterial and anti-inflammatory effects, or adhere and aggregate with negatively charged components in red blood cells and platelets to achieve a rapid hemostasis effect, thereby combining with the green and non-toxic properties of the material itself to broaden its application in the field of biomedical materials.
[0003] However, although the large number of hydrogen bonds and high crystallinity between and within natural polymer molecules give the materials excellent physical and chemical properties and wide application potential, and provide new ideas for solving marine and agricultural and forestry wastes, these strong interactions hinder the dissolution and melt processing of polymers in water and common organic solvents. Currently, commonly used solvent systems include LiCl / DMAc system, ionic liquids, alkali / urea system, etc., but LiCl is expensive, difficult to completely recover and easily remains in the regenerated chitin. Ionic liquids need to be kept at 110°C for a long time when dissolving chitin. The alkali / urea system can not only avoid toxicity problems, but also achieve rapid dissolution of polymers, such as KOH / urea solvent for the dissolution of chitin with different degrees of deacetylation (Macromolecules 2020, 53, 13, 5588–5598), (Green Chemistry, 2021, 23); on the other hand, although chitosan can be protonated by acid and quickly dissolved, the mechanical properties of the formed gel are poor, and the acidic environment is prone to toxic residues. The chitosan solution prepared by acid-base combination is stable and has excellent mechanical properties (patent 201710353066.2), which can better utilize the structural characteristics of the polymer itself.
[0004] In terms of material applications, in addition to common hydrogels (Adv. Mater. 2016, 28, 5844), membranes (Adv. Funct. Mater. 2017, 27, 1701100) and silk (Adv. Funct. Mater. 2021, 31, 2104368), structural characteristics such as low density and high porosity also make porous materials a hot topic of research. For example, in the field of hemostatic materials, hydrogels are easy to adhere to the skin and compress nerves and cause nerve damage after swelling. Inorganic particulate hemostatic agents represented by zeolite have severe heat release and can easily burn wounds and even cause blood clots. Porous hemostatic materials not only have a porous structure to accommodate liquid components, but also block the wound after absorbing liquid to achieve the effect of rapid hemostasis. Porous hemostatic materials prepared with natural polymers as raw materials can avoid problems such as biocompatibility with the human body. In addition, in the field of environment, these structural characteristics enable porous materials to better adapt to the environment, and have broad application prospects in seawater desalination, dye adsorption, and water-oil separation. For example, the use of hydrophobic reagents to modify the amino groups on the surface of natural polymers can not only be used in oil-water separation, adsorption, and other fields, but also reduce the influence of hygroscopicity on adsorption efficiency and building peripheral insulation materials. Superelasticity allows the material to easily squeeze out and recycle the absorbed components after the absorption process is completed, improving the recyclability of the material. Composite with reduced graphene oxide can improve the evaporation efficiency of the material for water, and part of the heat adsorbed by the porous structure is also used to heat the water body, thereby improving the photothermal conversion efficiency. The porous structure can also provide a larger surface area for microwave reflection and scattering. Composite with some optoelectronic materials such as MXene can significantly improve the electromagnetic shielding function of the material, and has great application potential in the fields of national defense, aerospace, and flexible electronic devices. In addition, when the material is driven by external force, the internal pore structure will undergo elastic deformation, plastic yielding, and densification to absorb stress and avoid the risk of structural damage. In the preparation of electrode materials, this three-dimensional network structure is conducive to accommodating changes in electrode volume.
[0005] At present, the main methods for preparing porous materials include freeze drying, supercritical, casting, combustion, etc. Among them, freeze drying is the most environmentally friendly and simple method. By changing the pre-freezing temperature or the concentration of the precursor, the pore structure can be adjusted to obtain a series of porous materials with adjustable properties. At present, the precursors used for freeze drying are mostly suspensions such as nanofiber suspensions, but whether it is top-down or bottom-up preparation of natural polymer nanofibers requires a relatively cumbersome process. When directly using hydrogel during freeze drying, the internal structure is too dense, and the volume expansion of ice crystals during the growth process will squeeze the entire gel network, causing the skeleton to shrink and even collapse and rupture of the gel structure after drying, making it difficult to obtain a porous material with a complete structure. In order to maintain the complete morphology of the porous material, low surface tension solvent replacement and annealing such as tert-butyl alcohol are used to reduce the capillary force, and the replacement concentration and annealing temperature need to be optimized according to the experimental conditions. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing a multifunctional natural polymer porous material, which makes full use of the structural characteristics of natural polymers, introduces a flexible chemical network into the prepared porous material to make the material wet elastic, and pre-forms large pores in the flexible chemical network to reduce the capillary tension inside the material during the final freeze-drying, thereby obtaining a porous material with a regular structure.
[0007] The solution adopted by the present invention to achieve the purpose is: a method for preparing a multifunctional natural polymer porous material, comprising the following steps:
[0008] A1. Mixing functional additives, stabilizers, natural polymer materials and alkaline solvents until they are completely dissolved to obtain a natural polymer solution;
[0009] A2, adding a crosslinking agent to the natural polymer solution obtained in step A1, stirring evenly and then placing until a partially chemically crosslinked alkali gel is formed, freezing the alkali gel, and after thawing, soaking the obtained gel in a non-solvent for natural polymer materials for regeneration and then washing with water to obtain a hydrogel;
[0010] A3. Remove the liquid from the hydrogel in step A2 to obtain a multifunctional natural polymer porous material.
[0011] Preferably, in step A1, the natural polymer material is at least one of cellulose, chitin, chitosan, and alginate; the concentration of the natural polymer material in the natural polymer solution is 1wt% to 10wt%; the alkaline solvent is at least one of alkaline hydroxides, alkali metal carbonates, alkaline earth metal carbonates, alkali metal bicarbonates, alkaline earth metal bicarbonates, ammonia water, ammonium carbonate, and an aqueous solution of ammonium bicarbonate; the stabilizer is at least one of urea, thiourea, and polyvinyl alcohol; in the natural polymer solution, the concentration of the alkali is 2wt% to 30wt%, and the concentration of the stabilizer is 0 to 20wt%.
[0012] Preferably, when the natural polymer material is chitosan, the preparation of the natural polymer solution mainly includes the following steps: uniformly mixing the functional additive, the stabilizer, and the weak alkaline aqueous solution, adding chitosan, and stirring to obtain a chitosan solution; or uniformly mixing the functional additive, the dilute acid aqueous solution, and the stabilizer, adding chitosan and stirring evenly, then adding an appropriate amount of alkali to neutralize, and stirring to obtain a chitosan solution.
[0013] Preferably, the weak alkaline aqueous solution is a single bicarbonate aqueous solution or a mixture of multiple bicarbonate aqueous solutions; the dilute acid is a mixture of one or more of an inorganic acid and an organic acid; the concentration of the dilute acid aqueous solution is 1wt% to 4wt%; the neutralizing base is a mixture of any one or more of an alkaline hydroxide, an alkali metal carbonate, an alkaline earth metal carbonate, an alkali metal bicarbonate, an alkaline earth metal bicarbonate, ammonia water, ammonium carbonate, and ammonium bicarbonate; and the concentration of the stabilizer in the chitosan solution is 2wt% to 20wt%.
[0014] The diluted acid is a mixture of one or more of hydrochloric acid, nitric acid, formic acid, acetic acid, lactic acid and citric acid. Generally, the concentration of bicarbonate in the chitosan solution is 2wt% to 10wt%, and the concentration of neutralizing alkali in the chitosan solution is 2wt% to 30wt%.
[0015] Preferably, the chitin or chitosan is obtained by deacetylation of chitin in an aqueous solution of potassium hydroxide or sodium hydroxide and then separating the solid from the mixture.
[0016] The chitin or chitosan is obtained by separating solid from the mixture after deacetylation of chitin in an aqueous solution of potassium hydroxide or sodium hydroxide. The concentration of the aqueous alkali solution is higher than 20wt%, the solid-liquid ratio of chitin to the aqueous alkali solution is 1:(10-20), and the deacetylation temperature is 60°C to 170°C.
[0017] Preferably, in step A1, the functional additive is at least one of inorganic oxides, inorganic nitrides, inorganic carbides, metal oxides, metal carbides, metal nitrides, conductive polymers, one-dimensional nanomaterials, and two-dimensional nanomaterials, and the concentration of the functional additive in the natural polymer solution is 0-20wt%.
[0018] The functional additives include montmorillonite, clay, silicon dioxide, ferroferric oxide, ferric oxide, one-dimensional nanomaterials such as silver nanowires, carbon nanotubes and their derivatives, conductive polymers such as polypyrrole, polythiophene, polyaniline and their derivatives, organic framework compounds, two-dimensional nanomaterials such as graphene and its derivatives, MXene, etc.
[0019] Preferably, the alkaline hydroxide is sodium hydroxide, potassium hydroxide or lithium hydroxide. When sodium hydroxide is used, the concentration of sodium hydroxide in the natural polymer solution is 5wt% to 10wt%. When lithium hydroxide is used, the concentration of lithium hydroxide in the natural polymer solution is 3.8wt% to 6.3wt%. When potassium hydroxide is used, the concentration of potassium hydroxide in the natural polymer solution is 5wt% to 30wt%.
[0020] Preferably, the cross-linking agent is at least one of epoxy compounds, glycidyl ether compounds and acrylate compounds, and the molar ratio of the cross-linking agent to the natural polymer material is 0.1 to 5:1.
[0021] The crosslinking agent is a mixture of one or more of epichlorohydrin, ethylene glycol diglycidyl ether, 1,4-butanediol diglycidyl ether, bisphenol A diglycidyl ether, polypropylene glycol diglycidyl ether, and poly(ethylene glycol) diacrylate.
[0022] Preferably, the non-solvent is a mixed liquid of any one or more of water, saline solution, and low-viscosity organic liquid soluble in water.
[0023] The salt is a salt containing monovalent cations and anions or divalent cations and anions; the water-soluble low-viscosity organic liquid is at least one of alcohols, ketones and esters.
[0024] The salt is potassium salt, sodium salt, magnesium salt, chloride salt, acetate, nitrate, sulfate, carbonate; the alcohol is ethanol; the ketone is acetone; and the ester is methyl formate or ethyl acetate.
[0025] Preferably, the specific method for removing the liquid is carbon dioxide supercritical drying or freeze drying.
[0026] Preferably, the supercritical drying is to replace the hydrogel with anhydrous ethanol or acetone and then dry it with supercritical carbon dioxide; the freeze drying is to replace the hydrogel with a 0-80wt% tert-butyl alcohol-water solution and then freeze dry it.
[0027] Preferably, the method further comprises the following steps: hydrophobically modifying the obtained multifunctional natural polymer porous material to obtain a hydrophobic porous material.
[0028] The hydrophobic modification method is to deposit, graft or coat a hydrophobic compound with low surface chemical energy on the surface of a polymer rich in hydroxyl or amino groups by chemical vapor deposition, chemical grafting or physical coating.
[0029] The compounds with low surface chemical energy include inorganic oxides, silanes, long-chain alkane chlorides, fluorides, etc. The inorganic oxides include titanium dioxide, silicon dioxide, etc.; silanes include dichlorosilane, trichlorosilane, methyltrimethoxysilane, octyltrichlorosilane, hexadecyltrichlorosilane, octadecyltrichlorosilane and octyltrimethoxysilane, etc.; acyl chlorides include undecanoyl chloride, palmitoyl chloride, octadecanoyl chloride, etc.; fluorides include perfluorobenzoyl chloride, perfluorooctanoyl chloride, etc.
[0030] The present invention has the following advantages and beneficial effects:
[0031] (1) The preparation method of the present invention is to prepare a multifunctional porous material that can be manufactured in large size. The present invention first forms a flexible chemical network inside the alkali gel through chemical cross-linking, and pre-forms pores inside the alkali gel by means of the "ice template" method. During the growth of ice crystals, the solute inside the gel will be squeezed by ice crystals and locally aggregated to form pore walls. The area where the ice crystals grow will be occupied by the liquid in the solute after thawing. During the drying process, the macroporous structure in the system significantly reduces the capillary tension, ensuring that the pre-formed pore structure is retained in the dried material, effectively preventing the dense structure inside the material from causing structural shrinkage during drying and causing defects; the macroporous structure can also ensure the uniform distribution of additives, which is helpful for mass-charge transfer. On the other hand, the physical and chemical double cross-linking structure can form non-covalent interactions in the natural polymer-additive region so that the material has both high strength and high toughness. The former forms a physical cross-linking area to bear stress through physical regeneration, and the latter dissipates stress through irreversible covalent cross-linking. The synergistic effect of the two ensures that the material structure can maintain structural integrity when subjected to external stress.
[0032] (2) The natural polymers used in the preparation method of the present invention are all taken from the environment and used in the environment, the solvent system and preparation process used are safe and non-toxic, and the prepared materials can be degraded in the natural environment, which meets the characteristics of "green chemistry". In addition, the materials prepared in the present invention can give full play to the structural characteristics of natural polymers, such as the chelation between amino groups and metal ions, and the abundant hydroxyl groups can form covalent or non-covalent interactions to improve the strength of the material and give the material specific functions. The porous material finally obtained not only maintains the complete morphology, light weight, high specific surface area, high porosity and other structural characteristics, but also can greatly expand the application of the material in the fields of environment, medicine, aerospace, construction, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a sample diagram prepared in Example 1;
[0034] Figure 2 This is a scanning electron microscope image of the material obtained in Example 1. DETAILED DESCRIPTION
[0035] For a better understanding of the present invention, the following examples are provided to further illustrate the present invention, but the present invention is not limited to the following examples.
[0036] In the present invention, the cellulose source may be one or a mixture of pulp separated from trees, bamboo, cotton, grass, hemp and other higher plants, bamboo pulp, cotton pulp, grass pulp, hemp pulp, etc., and refined cellulose separated from animals and bacteria.
[0037] As the source of chitosan, one or more of shrimp shells, crab shells, squid parietal bones, insects or fungal cells can be used. Before preparing chitosan / chitosan with different deacetylation degrees, chitosan is purified by known methods without particular limitation, such as alkali treatment to remove protein, acid treatment to remove minerals such as calcium salts, oxidation decolorization treatment, etc.
[0038] Embodiment 1:
[0039] Add cotton wool to the LiOH-urea mixture and stir to obtain a cellulose solution. The final solution includes 6.3wt% LiOH, 4wt% urea, 2wt% cellulose, and the remainder is water. Add epichlorohydrin at a molar ratio of 0.5:1 between the cross-linking agent and the cellulose anhydroglucose unit AGU. After mixing evenly, pour the solution into a mold to form a partially chemically cross-linked cellulose alkali gel. The gel is then frozen at -40°C, and after thawing, the gel is placed in deionized water for regeneration. Finally, it is washed with water until neutral to obtain a cellulose hydrogel. After replacement with a 20wt% tert-butanol-water solution, it is freeze-dried to obtain a cellulose porous material that can absorb liquid quickly. The product sample prepared in this embodiment is shown in the figure. Figure 1 As shown in the figure, the size of the obtained block material is 7.0cm*3.7cm*0.7cm. It can be seen from the figure that the material after freeze drying has a regular morphology and no obvious shrinkage. Figure 2 As shown, micrometer-scale pore structures can be observed.
[0040] Embodiment 2:
[0041] Montmorillonite is mixed with LiOH-urea aqueous solution, and then bamboo pulp is added and stirred to obtain a cellulose solution. The final solution includes 3.8wt% LiOH, 6wt% urea, 2wt% montmorillonite, 2wt% cellulose, and the balance is water. Epichlorohydrin is added according to the molar ratio of crosslinker to cellulose dehydrated glucose unit AGU of 5:1, and the solution is poured into a mold after mixing evenly to form a partially chemically crosslinked cellulose alkali gel. The gel is then frozen at -40°C, and after thawing, the gel is regenerated in deionized water and washed to neutrality to obtain a cellulose hydrogel. After 80wt% tert-butyl alcohol-water solution replacement and freeze drying, a cellulose / montmorillonite porous material with high strength, excellent heat insulation and flame retardant effects is obtained. When the material is compressed to 80%, its compressive strength is 1.6MPa and its modulus is 7.6MPa. When the material is hydrophobically modified with methyltrimethylsilane, its compressive strength and modulus are increased to 2.2MPa and 9.8MPa, respectively, and the material is a superhydrophobic material.
[0042] Embodiment 3:
[0043] The carbon nanotubes are mixed with a NaOH-thiourea aqueous solution, and then bamboo pulp is added and stirred to obtain a cellulose solution. The final solution includes 10wt% NaOH, 2wt% thiourea, 0.8wt% carbon nanotubes, 2wt% cellulose, and the balance is water. Epichlorohydrin is added according to a molar ratio of 5:1 between the crosslinker and the cellulose anhydroglucose unit AGU, and after mixing evenly, the solution is poured into a mold to form a partially chemically cross-linked cellulose alkali gel. The gel is then frozen at -30°C, and after thawing, the gel is placed in a 15wt% KCl aqueous solution for regeneration for 24 hours, and finally washed with water until neutral to obtain a cellulose hydrogel, and freeze-dried to obtain a cellulose / carbon nanotube porous material with excellent thermal insulation and conductive effects.
[0044] Embodiment 4:
[0045] Silica was mixed with NaOH-urea aqueous solution and then bamboo pulp was added and stirred to obtain a cellulose solution. The final solution included 5wt% NaOH, 8wt% urea, 0.5wt% silica, 2wt% cellulose, and the remainder was water. 1,4-Butanediol diglycidyl ether was added according to the molar ratio of crosslinker to cellulose anhydroglucose unit AGU of 0.5:1, and after mixing evenly, the solution was poured into a mold to form a partially chemically crosslinked cellulose alkali gel. The gel was then frozen at -40°C, and after thawing, the gel was regenerated in a 50wt% ethanol-water solution for 24 hours, and finally washed with water to neutrality to obtain a cellulose hydrogel. After replacement with a 30wt% tert-butyl alcohol-water solution, freeze-dried to obtain an insulating cellulose / silica porous material with better thermal stability than synthetic polymers such as polystyrene.
[0046] Embodiment 5:
[0047] After mixing polypyrrole with KOH aqueous solution, chitosan was added and stirred to obtain chitosan solution. The final solution included 30wt% KOH, 2wt% polypyrrole, 5wt% chitosan, and the balance was water. Ethylene glycol glycidyl ether was added according to the molar ratio of crosslinker to chitosan N-acetylglucosamine unit GlcNAc of 2:1, and after mixing evenly, the solution was poured into a mold to form a partially chemically crosslinked chitosan alkali gel. The gel was then frozen at -70°C, and after thawing, the gel was regenerated with 10wt% NaCl-water solution for 24h, washed with water to neutrality to obtain chitosan hydrogel, and freeze-dried after replacement with 20wt% tert-butyl alcohol-water solution to obtain a conductive chitosan / polypyrrole porous material with excellent biocompatibility. When the material was compressed to 80%, its compressive strength was 1.6MPa and its modulus was 8.3MPa.
[0048] Embodiment 6:
[0049] After mixing MXene with KOH-urea aqueous solution, chitosan was added and stirred to obtain a chitosan solution. The final solution included 20wt% KOH, 4wt% urea, 20wt% MXene, 3wt% chitosan, and the remainder was water. Epichlorohydrin was added according to the molar ratio of the crosslinker to the chitosan N-acetylglucosamine unit GlcNAc of 2:1, and after mixing evenly, the solution was poured into a mold to form a partially chemically cross-linked chitosan alkali gel. The gel was then frozen at -70°C, and after thawing, the gel was regenerated with a 40wt% ethanol-water solution for 24 hours, washed with water to neutrality to obtain a chitosan hydrogel, and freeze-dried to obtain a porous material of chitosan / MXene porous material. The porous material not only has excellent electromagnetic shielding function, but also has photothermal conversion, antibacterial and other functions.
[0050] Embodiment 7:
[0051] Graphene oxide is mixed with KOH-urea aqueous solution and then chitosan is added and stirred to obtain a chitosan solution. The final solution includes 12wt% KOH, 20wt% urea, 4wt% graphene oxide, 10wt% chitosan, and the balance is water. Epichlorohydrin is added according to the molar ratio of crosslinker to chitosan-based glucose unit GlcN of 0.2:1, and after mixing evenly, the solution is poured into a mold to form a partially chemically cross-linked chitosan alkali gel. The gel is then frozen at -70°C, and after thawing, the gel is regenerated with 15wt% NaCl-aqueous solution for 24h, washed with water to neutrality to obtain chitosan hydrogel, and dried by replacing supercritical carbon dioxide with anhydrous ethanol to obtain a chitosan / graphene oxide porous material that can photothermally resist bacteria.
[0052] Embodiment 8:
[0053] After mixing ferroferric oxide with KOH-urea aqueous solution, chitosan is added and stirred to obtain a chitosan solution. The final solution includes 20wt% KOH, 8wt% urea, 1wt% ferroferric oxide, 10wt% chitosan, and the balance is water. Ethylene glycol glycidyl ether is added according to the molar ratio of crosslinker to chitosan glucose unit GlcN of 0.1:1, and after mixing evenly, the solution is poured into a mold to form a partially chemically cross-linked chitosan alkali gel. The gel is then frozen at -70°C, and after thawing, the gel is regenerated with 5wt% ethanol-water solution for 24h, washed with water to neutrality to obtain chitosan hydrogel, and after replacement with 40wt% tert-butyl alcohol-water solution, freeze-dried to obtain a magnetic chitosan / ferroferric oxide porous material, which can use an external magnet to regulate the position of the material and directional adsorption of metal ions in wastewater.
[0054] Embodiment 9:
[0055] After mixing reduced graphene oxide with potassium bicarbonate-urea aqueous solution, chitosan is added and stirred to obtain a chitosan solution, wherein the final solution includes 10wt% potassium bicarbonate, 20wt% urea, 2wt% reduced graphene oxide, 4wt% chitosan, and the balance is water. Ethylene glycol glycidyl ether is added according to the molar ratio of the crosslinker to the chitosan-based glucose unit GlcN of 1:1, and after mixing evenly, the solution is poured into a mold to form a partially chemically cross-linked chitosan alkali gel. The gel is then frozen at -70°C, and after thawing, the gel is regenerated with a 60wt% ethanol-water solution for 24h, washed with water to neutrality to obtain a chitosan hydrogel, and after being replaced with a 40wt% tert-butyl alcohol-water solution, freeze-dried to obtain a chitosan / reduced graphene oxide composite porous material for solar seawater desalination.
[0056] Embodiment 10:
[0057] Silver nanowires are mixed with an ammonium bicarbonate-urea aqueous solution and then chitosan is added and stirred to obtain a chitosan solution. The final solution includes 2wt% ammonium bicarbonate, 16wt% urea, 4wt% silver nanowires, 3wt% chitosan, and the balance is water. Ethylene glycol glycidyl ether is added according to a molar ratio of 1:1 between the crosslinker and the chitosan-based glucose unit GlcN, and after mixing evenly, the solution is poured into a mold to form a partially chemically cross-linked chitosan alkali gel. The gel is then frozen at -40°C, and after thawing, the gel is regenerated with a 60wt% ethanol-water solution for 24 hours, washed with water to neutrality to obtain a chitosan hydrogel, and the conductive chitosan / silver nanowire porous material is obtained by freeze drying after replacement with a 40wt% tert-butyl alcohol-water solution.
[0058] Embodiment 11:
[0059] After mixing titanium dioxide with an acetic acid-urea aqueous solution, chitosan is added and stirred to obtain a chitosan solution, and then potassium bicarbonate is added to the mixed solid for neutralization. The final solution includes 1wt% acetic acid, 2wt% urea, 2wt% titanium dioxide, 1wt% chitosan, 2wt% ammonium bicarbonate, and the balance is water. Ethylene glycol glycidyl ether is added according to a molar ratio of 1:1 between the crosslinker and the chitosan-based glucose unit GlcN, and after mixing evenly, the solution is poured into a mold to form a partially chemically cross-linked chitosan alkali gel. The gel is then frozen at -40°C, and after thawing, the gel is regenerated with a 60wt% ethanol-water solution for 24 hours, washed with water to neutrality to obtain a chitosan hydrogel, and after replacement with a 40wt% tert-butyl alcohol-water solution, freeze-dried to obtain a chitosan / titanium dioxide porous material that can effectively inhibit and kill microorganisms.
[0060] Embodiment 12:
[0061] After mixing MXene with acetic acid-urea aqueous solution, chitosan is added and stirred to obtain chitosan solution, and then potassium bicarbonate-potassium hydroxide mixed solid is added for neutralization. The final solution includes 4wt% acetic acid, 2wt% urea, 10wt% MXene, 2wt% chitosan, 7wt% potassium bicarbonate, 23wt% potassium hydroxide, and the balance is water. Ethylene glycol glycidyl ether is added according to the molar ratio of crosslinker to chitosan-based glucose unit GlcN of 1:1, and after mixing evenly, the solution is poured into a mold to form a partially chemically cross-linked chitosan alkali gel. The gel is then frozen at -40°C, and after thawing, the gel is regenerated with 60wt% ethanol-water solution for 24h, washed with water to neutrality to obtain chitosan hydrogel, and the chitosan / MXene porous material obtained after freeze-drying after replacement with 40wt% tert-butyl alcohol-water solution has not only excellent conductivity, but also dual electrothermal / photothermal responsiveness.
[0062] Comparative Example 1:
[0063] After mixing MXene with KOH aqueous solution, chitosan was added and stirred to obtain chitosan solution, and the final solution included 20wt% KOH, 4wt% urea, 20wt% MXene, 3wt% chitosan, and the balance was water. Epichlorohydrin was added according to the molar ratio of crosslinker to chitosan N-acetylglucosamine unit GlcNAc of 2:1, and after mixing evenly, the solution was poured into a mold to form a partially chemically crosslinked chitosan alkali gel, and then the gel was regenerated with 40wt% ethanol-water solution for 24h, and washed with water until neutral to obtain chitosan hydrogel. During the freeze-drying process, due to the nano-sized porous structure inside the gel, capillary tension will cause the gel to shrink unevenly, and the ice crystal expansion during the freezing process of the hydrogel causes the material to rupture under the action of internal stress, so it is impossible to obtain a uniform and regular chitosan material, and the electromagnetic shielding effect is poor.
[0064] Comparative Example 2:
[0065] After mixing MXene with KOH-urea aqueous solution, chitosan was added and stirred to obtain chitosan solution. The final solution included 20wt% KOH, 4wt% urea, 20wt% MXene, 3wt% chitosan, and the balance was water. After heating the gel, it was frozen at -70°C. During the thawing process, the alkaline gel gradually turned into a solution state and could not maintain the block morphology.
[0066] The above is only a preferred embodiment of the present invention, which certainly cannot be used to limit the scope of rights of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and changes can be made without departing from the principle of the present invention, and these improvements and changes are also regarded as the protection scope of the present invention.
Claims
1. A method for preparing a multifunctional natural polymer porous material, characterized in that: The following steps are involved: A1. Mixing functional additives, stabilizers, natural polymer materials and alkaline solvents until they are completely dissolved to obtain a natural polymer solution; A2, adding a crosslinking agent to the natural polymer solution obtained in step A1, stirring evenly and then placing until a partially chemically crosslinked alkali gel is formed, freezing the alkali gel, and after thawing, soaking the obtained gel in a non-solvent for natural polymer materials for regeneration and then washing with water to obtain a hydrogel; A3, removing liquid from the hydrogel in step A2 to obtain a multifunctional natural polymer porous material; In the step A1, the concentration of the stabilizer in the natural polymer solution is 0-20 wt %, and the concentration of the functional additive in the natural polymer solution is 0-20 wt %.
2. The method for preparing the multifunctional natural polymer porous material according to claim 1, characterized in that: In the step A1, the natural polymer material is at least one of cellulose, chitin, chitosan, and alginate; the concentration of the natural polymer material in the natural polymer solution is 1 wt% to 10 wt%; the alkaline solvent is at least one of alkaline hydroxides, alkali metal carbonates, alkaline earth metal carbonates, alkali metal bicarbonates, alkaline earth metal bicarbonates, ammonia water, ammonium carbonate, and an aqueous solution of ammonium bicarbonate; the stabilizer is at least one of urea, thiourea, and polyvinyl alcohol; and the concentration of the alkali in the natural polymer solution is 2 wt% to 30 wt%.
3. The method for preparing the multifunctional natural polymer porous material according to claim 2, characterized in that: When the natural polymer material is chitosan, the preparation of the natural polymer solution mainly includes the following steps: uniformly mixing the functional additive, the stabilizer, and the weak alkaline aqueous solution, adding chitosan, and stirring to obtain the chitosan solution; or uniformly mixing the functional additive, the dilute acid aqueous solution, and the stabilizer, adding chitosan and stirring to obtain the chitosan solution, and then adding an appropriate amount of alkali to neutralize, and stirring to obtain the chitosan solution.
4. The method for preparing the multifunctional natural polymer porous material according to claim 3, characterized in that: The weak alkali aqueous solution is a single bicarbonate aqueous solution or a mixture of multiple bicarbonate aqueous solutions; the dilute acid is a mixture of one or more inorganic acids and organic acids; the concentration of the dilute acid aqueous solution is 1 wt% to 4 wt%; the neutralizing alkali is a mixture of any one or more of alkaline hydroxides, alkali metal carbonates, alkaline earth metal carbonates, alkali metal bicarbonates, alkaline earth metal bicarbonates, ammonia water, ammonium carbonate, and ammonium bicarbonate; the concentration of the stabilizer in the chitosan solution is 2 wt% to 20 wt%.
5. The method for preparing the multifunctional natural polymer porous material according to claim 2, characterized in that: The chitin or chitosan is obtained by deacetylation of chitin in an aqueous solution of potassium hydroxide or sodium hydroxide and then separating solid from the mixture.
6. The method for preparing the multifunctional natural polymer porous material according to claim 1, characterized in that: In the step A1, the functional additive is at least one of inorganic oxides, inorganic nitrides, inorganic carbides, metal oxides, metal carbides, metal nitrides, conductive polymers, one-dimensional nanomaterials, and two-dimensional nanomaterials.
7. The method for preparing the multifunctional natural polymer porous material according to claim 2, characterized in that: The alkaline hydroxide is sodium hydroxide, potassium hydroxide or lithium hydroxide. When sodium hydroxide is used, the concentration of sodium hydroxide in the natural polymer solution is 5 wt% to 10 wt%. When lithium hydroxide is used, the concentration of lithium hydroxide in the natural polymer solution is 3.8 wt% to 6.3 wt%. When potassium hydroxide is used, the concentration of potassium hydroxide in the natural polymer solution is 5 wt% to 30 wt%.
8. The method for preparing the multifunctional natural polymer porous material according to claim 1, characterized in that: The crosslinking agent is at least one of epoxy compounds, glycidyl ether compounds and acrylate compounds, and the molar ratio of the crosslinking agent to the natural polymer material is 0.1 to 5:
1.
9. The method for preparing the multifunctional natural polymer porous material according to claim 1, characterized in that: The non-solvent is a mixed liquid of any one or more of water, saline solution, and low-viscosity organic liquid soluble in water.
10. The method for preparing the multifunctional natural polymer porous material according to claim 1, characterized in that: The following steps are also included: The obtained multifunctional natural polymer porous material is subjected to hydrophobic modification to obtain a hydrophobic porous material.