Alloyed negative electrode material and preparation method and application thereof

By using alloyed anode materials in lithium battery anode materials, combined with inorganic porous materials and germanium elements, the problems of small capacity and poor cycle of lithium battery anode materials are solved, and high theoretical capacity and cycle stability are achieved, which is suitable for industrial production.

CN116581282BActive Publication Date: 2024-10-22BEIJING IAMETAL NEW ENERGY TECH CO LTD +2
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202310857202.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-13
Publication Date
2024-10-22
Estimated Expiration
2043-07-13

AI Technical Summary

Technical Problem

Existing lithium battery anode materials have problems such as small capacity, poor cycle and low service life during the charge and discharge process, which limits their commercial application.

Method used

An alloyed anode material is used, including germanium elemental and carbon coating layers in inorganic porous materials, prepared through vapor deposition and pyrolytic carbon coating technology to form an anode material with high theoretical capacity, low volume expansion and high conductivity.

Benefits of technology

It achieves high theoretical capacity, low volume expansion and high cycle stability, improves the energy density and service life of lithium batteries, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116581282B_ABST
    Figure CN116581282B_ABST
Patent Text Reader

Abstract

The present invention provides an alloyed negative electrode material and a preparation method and application thereof, and specifically relates to the technical field of negative electrode materials for lithium batteries. The alloyed negative electrode material includes an alloyed composite material as a core layer; and a carbon coating layer that wraps the core layer; the alloyed composite material includes an inorganic porous material and a single germanium substance located in the pores of the inorganic porous material; the germanium substance accounts for 10wt.%-90wt.% in the alloyed negative electrode material. The alloyed negative electrode material provided by the present invention will have a high theoretical capacity (1600 mAh / g), a high diffusion coefficient (100 cm 2 / s) and high conductivity (2.17 s / m) of germanium are used in the negative electrode material. Inorganic porous materials are used to provide space for the contraction and expansion of germanium. The carbon coating layer improves the stability of the core material, synergistically improving the first effect and reversible capacity of the negative electrode material, thereby greatly improving the cycle stability of the negative electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium battery negative electrode materials, and in particular to an alloyed negative electrode material and a preparation method and application thereof. Background Art

[0002] In recent years, negative electrode materials with high specific capacity, such as silicon-based materials, tin-based materials, titanium-based materials, transition metal oxides and various composite negative electrode materials, have gradually been developed and have become an important research direction for improving the energy density of lithium-ion batteries.

[0003] Silicon-based negative electrodes have the disadvantages of large volume change, poor cycle life, and low initial efficiency during the charge and discharge process, which limits their commercial application. Tin-based materials, titanium-based materials, and transition metal oxides also have the defect of small theoretical capacity during the charge and discharge process, which makes their application cost in lithium batteries high.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] One of the purposes of the present invention is to provide an alloyed negative electrode material, aiming to solve the technical problem that the negative electrode material in the prior art cannot take into account the capacity, cycle performance and service life at the same time.

[0006] A second object of the present invention is to provide a method for preparing an alloyed negative electrode material.

[0007] The third object of the present invention is to provide an application of an alloyed negative electrode material in a negative electrode material for a lithium battery.

[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0009] The first aspect of the present invention provides an alloyed negative electrode material, comprising an alloyed composite material as a core layer; and a carbon coating layer wrapping the core layer;

[0010] The alloyed composite material comprises an inorganic porous material and a germanium element located in the pores of the inorganic porous material;

[0011] Wherein, the inorganic porous material includes one of porous ceramics, porous carbon materials, porous silica materials and molecular sieves;

[0012] The germanium single substance accounts for 1wt.%-90wt.% in the alloyed negative electrode material.

[0013] Furthermore, the thickness of the carbon coating layer is 1nm-20nm.

[0014] The porous ceramic material includes at least one of porous alumina, porous zirconia, porous magnesia and porous beryllium oxide.

[0015] Furthermore, it also includes silicon and / or carbon in the pores of the inorganic porous material.

[0016] Further, the product structure includes at least one of nanoparticles, nanowires, nanotubes, nanofibers, nanosheets, films, porous structures and hollow structures.

[0017] The second aspect of the present invention provides a method for preparing the alloyed negative electrode material, comprising the following steps:

[0018] A. obtaining the alloyed composite material by vapor deposition of germanium source gas on a template of an inorganic porous material;

[0019] B. Introducing hydrocarbon gas into the container where the alloyed composite material is located to perform pyrolysis and carbon coating to obtain the alloyed negative electrode material.

[0020] Furthermore, the temperature of the vapor deposition is 300° C.-500° C., and the time is 1 h-4 h.

[0021] The pyrolysis temperature is 550° C.-950° C., and the time is 1 h-3 h.

[0022] The flow rate of the germanium source gas is 40 sccm-80 sccm.

[0023] The flow rate of the hydrocarbon gas is 80 sccm-200 sccm.

[0024] Furthermore, the germanium source gas includes at least one of germane, digermane, dimethylgermane and tetraethylgermane.

[0025] The hydrocarbon gas includes at least one of methane, ethane, ethylene, acetylene, propane and propylene.

[0026] Furthermore, step A also includes depositing silicon source gas and / or carbon source gas simultaneously with vapor deposition of germanium source gas.

[0027] The silicon source gas includes at least one of silane, disilane, methylsilane, dimethylsilane, trimethylsilane, tetramethylsilane, methyldisilane, dimethyldisilane, trimethyldisilane, tetramethyldisilane, hexamethylsilane and ethylsilane.

[0028] The carbon source gas includes at least one of methane, ethane, ethylene, acetylene, propane and propylene.

[0029] Furthermore, the flow rate of the silicon source gas is 40 sccm-80 sccm.

[0030] The flow rate of the carbon source gas is 40 sccm-600 sccm.

[0031] The third aspect of the present invention provides the use of the alloyed negative electrode material in negative electrode materials for lithium batteries.

[0032] Compared with the prior art, the present invention has at least the following beneficial effects:

[0033] The alloyed negative electrode material provided by the present invention has a high theoretical capacity (1600 mAh / g), a high diffusion coefficient (100 cm 2 / s) and high conductivity (2.17 s / m) of germanium are used in the negative electrode material. Inorganic porous materials are used to provide space for the shrinkage and expansion of germanium, and the carbon coating layer improves the stability of the core material. The alloyed negative electrode material has both high theoretical capacity and high conductivity, and the volume expansion is small during the charge and discharge process. In addition, the inorganic porous material weakens the effect of volume change on material performance, synergistically improving the first effect and reversible capacity of the negative electrode material, thereby greatly improving the cycle stability of the negative electrode material.

[0034] The method for preparing the alloyed negative electrode material provided by the present invention has a continuous and simple process, a high degree of mechanization, saves labor costs, and is suitable for large-scale industrial production.

[0035] The alloyed negative electrode material provided by the present invention provides a negative electrode material with better performance for the battery, expands the use places and use conditions of the battery, and promotes the development of downstream industries. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0037] Figure 1 SEM photograph (a), Ge element distribution photograph (b), Si element distribution photograph (c) and C element distribution photograph (d) of the carbon-coated alloyed negative electrode material prepared with alumina porous ceramic powder as a template provided in Example 7. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0039] Hereinafter, the terms "including", "having" and their cognates, which may be used in various embodiments of the present invention, are intended only to indicate specific features, numbers, steps, operations, elements, components or combinations of the foregoing items, and should not be understood as first excluding the existence of one or more other features, numbers, steps, operations, elements, components or combinations of the foregoing items or adding the possibility of one or more features, numbers, steps, operations, elements, components or combinations of the foregoing items.

[0040] Furthermore, the terms “first”, “second”, “third”, etc. are merely used for distinguishing descriptions and are not to be understood as indicating or implying relative importance.

[0041] The first aspect of the present invention provides an alloyed negative electrode material, comprising an alloyed composite material as a core layer; and a carbon coating layer wrapping the core layer;

[0042] The alloyed composite material comprises an inorganic porous material and a germanium element located in the pores of the inorganic porous material;

[0043] Wherein, the inorganic porous material includes one of porous ceramics, porous carbon materials, porous silica materials and molecular sieves;

[0044] The germanium single substance accounts for 1wt.%-90wt.% in the alloyed negative electrode material.

[0045] The alloyed negative electrode material provided by the present invention has a high theoretical capacity (1600 mAh / g), a high diffusion coefficient (100 cm 2 / s) and high conductivity (2.17 s / m) of germanium are used in the negative electrode material. Inorganic porous materials are used to provide space for the shrinkage and expansion of germanium, and the carbon coating layer improves the stability of the core material. The alloyed negative electrode material has both high theoretical capacity and high conductivity, and the volume expansion is small during the charge and discharge process. In addition, the inorganic porous material weakens the effect of volume change on the material performance, and synergistically improves the first effect and reversible capacity of the negative electrode material, thereby greatly improving the cycle stability of the negative electrode material. When used as the negative electrode of a lithium-ion battery, the alloyed negative electrode material can undergo an alloying reaction with lithium ions to store lithium, and has an ultra-high theoretical specific capacity.

[0046] When the proportion of germanium in the alloyed negative electrode material is less than 1wt.%, the germanium cannot be effectively connected and contacted, so the electronic conductivity of the composite alloyed negative electrode material cannot be effectively improved, and the rate performance of the material is reduced. In addition, when the proportion of germanium is too low, the specific capacity of the composite material cannot be effectively improved, and the energy density of the battery is reduced. When the proportion of germanium in the alloyed negative electrode material is greater than 90wt.%, the inorganic porous material used for support cannot form a stable structure and fixed distribution of pores, and thus cannot buffer the volume expansion and contraction of the alloy material during the charging and discharging process, resulting in rapid collapse of the composite material and rapid decay of the electrochemical performance.

[0047] Typically but not limiting, the proportion of germanium in the alloyed negative electrode material is 1 wt.%, 2 wt.%, 5 wt.%, 10 wt.%, 20 wt.%, 40 wt.%, 60 wt.%, 80 wt.% or 90 wt.%.

[0048] Furthermore, the thickness of the carbon coating layer is 1nm-20nm. When the thickness of the carbon coating layer is less than 1nm, a stable and complete carbon coating layer cannot be effectively formed on the surface of the deposited alloying material, resulting in the instability of the material to air. After contact with air, a violent oxidation reaction will occur, resulting in material failure. At the same time, the stability of the material to water will be reduced, causing gas production and pole piece peeling when the electrode slurry is made; when the thickness of the carbon coating layer is greater than 20nm, the carbon layer will hinder the rapid transmission of lithium ions, causing the rate performance of the composite material to decrease, and rapid charging and discharging cannot be achieved. In addition, if the proportion of carbon material is too high, the specific capacity of the material will be reduced, and the energy density of the battery will be reduced. Typically but not restrictive, the thickness of the carbon coating layer is 1nm, 3nm, 5nm, 7nm, 9nm, 11nm, 13nm, 15nm, 17nm, 19nm or 20nm.

[0049] The porous ceramic material includes at least one of porous alumina, porous zirconia, porous magnesia and porous beryllium oxide.

[0050] Furthermore, it also includes silicon and / or carbon in the pores of the inorganic porous material.

[0051] Further, the product structure includes at least one of nanoparticles, nanowires, nanotubes, nanofibers, nanosheets, films, porous structures and hollow structures.

[0052] The second aspect of the present invention provides a method for preparing the alloyed negative electrode material, comprising the following steps:

[0053] A. obtaining the alloyed composite material by vapor deposition of germanium source gas on a template of an inorganic porous material;

[0054] B. Introducing hydrocarbon gas into the container where the alloyed composite material is located to perform pyrolysis and carbon coating to obtain the alloyed negative electrode material.

[0055] The method for preparing the alloyed negative electrode material provided by the present invention has a continuous and simple process, a high degree of mechanization, saves labor costs, and is suitable for large-scale industrial production.

[0056] The present invention uses chemical vapor deposition technology to achieve the particle size control and morphology control of the alloyed material. The size of the formed nanoparticles can be controlled by adjusting the deposition conditions to grow alloyed materials with different morphologies. The gaseous material can also be introduced into the interior or surface of the inorganic porous material to cause it to be cracked in the pores and surface of the template to form an alloyed negative electrode material with a porous structure and a special morphology.

[0057] Furthermore, the temperature of the vapor deposition is 300°C-500°C, and the time is 1h-4h. The chemical vapor deposition is formed by cracking the gas source of the germanium material under high temperature conditions, and the high temperature conditions are above the cracking temperature of the gas source of the germanium material. The vapor deposition equipment can be a rotary furnace, a fluidized bed deposition furnace, or a horizontal bed vibration furnace. When there are multiple gas sources for vapor deposition, the temperature of vapor deposition is greater than the cracking temperature of all gas sources, thereby ensuring the vapor deposition of various materials.

[0058] Typically, but not limiting, the vapor deposition temperature is 300° C., 350° C., 400° C., 450° C. or 500° C.; and the time is 1 h, 2 h, 3 h or 4 h.

[0059] The pyrolysis temperature is 550°C-950°C, and the time is 1h-3h. Typically but not limiting, the pyrolysis temperature of hydrocarbon gas is 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C or 950°C, and the time is 1h, 2h or 3h.

[0060] The flow rate of the germanium source gas is 40sccm-1000sccm. When the flow rate of the germanium source gas is less than 40sccm, the deposition rate of germanium is too low, and germanium is deposited as individual particles, which cannot form an effective continuous deposition layer, increasing the risk of oxidation and making batch preparation too difficult; when the flow rate of the germanium source gas is greater than 1000sccm, the germanium gas cannot be effectively cracked, resulting in a decrease in the utilization rate of germanium and an increase in manufacturing costs. Typically but not restrictively, the flow rate of the germanium source gas is 40sccm, 100sccm, 500sccm, 800sccm or 1000sccm.

[0061] The flow rate of the hydrocarbon gas is 80sccm-200sccm. When the flow rate of the hydrocarbon gas is less than 80sccm, a continuous coating layer cannot be formed on the surface of the alloyed composite negative electrode material, and carbon coating cannot be effectively performed; when the flow rate of the hydrocarbon gas is greater than 200sccm, the cracking rate of acetylene is reduced, and incomplete cracking of acetylene will cause more hydrocarbons to appear on the surface of the alloyed negative electrode material, increasing the resistivity of the material. Typically but not restrictively, the flow rate of the hydrocarbon gas is 80sccm, 100sccm, 150sccm, 180sccm or 200sccm.

[0062] Furthermore, the germanium source gas includes at least one of germane, digermane, dimethylgermane and tetraethylgermane.

[0063] The hydrocarbon gas includes at least one of methane, ethane, ethylene, acetylene, propane and propylene.

[0064] Furthermore, step A also includes depositing silicon source gas and / or carbon source gas simultaneously with vapor deposition of germanium source gas.

[0065] The silicon source gas includes at least one of silane, disilane, methylsilane, dimethylsilane, trimethylsilane, tetramethylsilane, methyldisilane, dimethyldisilane, trimethyldisilane, tetramethyldisilane, hexamethylsilane and ethylsilane.

[0066] The carbon source gas includes at least one of methane, ethane, ethylene, acetylene, propane and propylene.

[0067] Furthermore, the flow rate of the silicon source gas is 40sccm-1000sccm. When the flow rate of the silicon source gas is less than 40sccm, the deposition rate of silicon is too low, silicon is deposited as individual particles, and an effective continuous deposition layer cannot be formed, which increases the risk of oxidation and makes batch preparation too difficult; when the flow rate of the silicon source gas is greater than 1000sccm, the silane gas cannot be effectively cracked, resulting in a decrease in the utilization rate of silane and an increase in manufacturing costs. Typically but not restrictively, the flow rate of the silicon source gas is 40sccm, 100sccm, 200sccm, 500sccm or 1000sccm.

[0068] It should be noted that during the deposition process, the gas flow rate of the germanium source gas, the silicon source gas and the carbon source gas is related to the mass ratio of germanium, silicon and carbon in the alloyed negative electrode material finally formed. In the implementation process of the present invention, alloyed negative electrode materials with different germanium, silicon and carbon contents are obtained by adjusting the flow rate and time of the germanium source gas, the silicon source gas and the carbon source gas.

[0069] The flow rate of the carbon source gas is 40 sccm-600 sccm.

[0070] The third aspect of the present invention provides the use of the alloyed negative electrode material in negative electrode materials for lithium batteries.

[0071] The alloyed negative electrode material provided by the present invention provides a negative electrode material with better performance for the battery, expands the use places and use conditions of the battery, and promotes the development of downstream industries.

[0072] The present invention is further described below by specific examples and comparative examples, but it should be understood that these examples are only used for more detailed description and should not be understood as limiting the present invention in any form. The raw materials used in the examples and comparative examples of the present invention, if no specific conditions are specified, are carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially.

[0073] Example 1

[0074] This embodiment provides an alloyed negative electrode material, and the preparation method is as follows:

[0075] 1. Add 100 g of porous alumina ceramic powder (Jiangxi Baohong Nanotechnology Co., Ltd. / LA50) into a fluidized bed chemical vapor deposition equipment and heat it to 370 °C. Under nitrogen protection, introduce germane gas and ethylene gas into the fluidized bed chemical vapor deposition equipment at the same time, wherein the flow rate of germane gas is controlled to 500 sccm, and the flow rate of ethylene gas is controlled to 100 sccm. After co-deposition for 1 h, stop introducing germane gas and ethylene gas.

[0076] 2. Take out the deposited material, use a jet mill to crush it to Dv50=10 um, then add it to a rotary coating furnace, heat it to 850 °C under nitrogen protection, and introduce acetylene gas at a gas flow rate of 100 sccm for gas phase coating. After 2 hours, stop introducing acetylene to obtain carbon-coated alloyed negative electrode material powder particles made with alumina porous ceramic powder as a template.

[0077] Example 2

[0078] This embodiment provides an alloyed negative electrode material. The difference from Example 1 is that 100 g of porous silica powder (Jiangsu Huimai Powder Technology Co., Ltd.) is used to replace 100 g of alumina porous ceramic powder, and finally a carbon-coated alloyed negative electrode material powder particle made with porous silica powder as a template is obtained. The remaining raw materials and steps are the same as those in Example 1 and will not be repeated here.

[0079] Example 3

[0080] This embodiment provides an alloyed negative electrode material. The difference from Example 1 is that 100g of porous carbon microspheres (Guangdong Hanyan Activated Carbon Technology Co., Ltd. / HY-001) are used to replace 100g of alumina porous ceramic powder, and finally carbon-coated alloyed negative electrode material powder particles prepared with porous carbon microspheres as templates are obtained. The remaining raw materials and steps are the same as those in Example 1 and will not be repeated here.

[0081] Example 4

[0082] This embodiment provides an alloyed negative electrode material, and the preparation method is as follows:

[0083] 1. Add 100 g of alumina porous ceramic powder into a fluidized bed chemical vapor deposition equipment and heat it to 370°C. Under nitrogen protection, introduce tetraethylgermane gas and ethylene gas into the fluidized bed chemical vapor deposition equipment at the same time, wherein the flow rate of tetraethylgermane gas is controlled to 300 sccm. After deposition for 3 h, stop introducing tetraethylgermane gas.

[0084] 2. Same as Example 1.

[0085] Example 5

[0086] This embodiment provides an alloyed negative electrode material, and the preparation method is as follows:

[0087] 1. The temperature of the fluidized bed chemical vapor deposition equipment was raised to 370 °C. Under the condition of nitrogen protection, germane gas and ethylene gas were simultaneously introduced into the fluidized bed chemical vapor deposition equipment. The flow rate of the germane gas was controlled to be 500 sccm, and the flow rate of the ethylene gas was controlled to be 500 sccm. After 3 h of co-deposition, the introduction of the germane gas and the ethylene gas was stopped.

[0088] 2. Under nitrogen protection, the heating temperature was raised to 850 °C, and acetylene gas was introduced at a gas flow rate of 100 sccm for gas phase coating. After 2 h, the acetylene was stopped to obtain a carbon-coated, spontaneously grown nano-scale fibrous alloyed negative electrode material.

[0089] Example 6

[0090] This embodiment provides an alloyed negative electrode material, and the preparation method is as follows:

[0091] 1. Add 100 g of alumina porous ceramic powder into a fluidized bed chemical vapor deposition equipment and heat it to 370°C. Under nitrogen protection, introduce germane gas into the fluidized bed chemical vapor deposition equipment, wherein the flow rate of germane gas is controlled to 500 sccm and the introduction of germane gas is stopped after deposition for 1 h.

[0092] 2. Take out the deposited material, use a jet mill to crush it to Dv50=10 um, then add it to a rotary coating furnace, heat it to 850 °C under nitrogen protection, and introduce acetylene gas at a gas flow rate of 100 sccm for gas phase coating. After 2 hours, stop introducing acetylene to obtain carbon-coated alloyed negative electrode material powder particles made with alumina porous ceramic powder as a template.

[0093] Example 7

[0094] This embodiment provides an alloyed negative electrode material, and the preparation method is as follows:

[0095] 1. Add 100 g of alumina porous ceramic powder into a fluidized bed chemical vapor deposition equipment and heat it to 370 ° C. Under nitrogen protection, introduce tetraethylgermane gas and tetramethylsilane gas into the fluidized bed chemical vapor deposition equipment at the same time, wherein the flow rate of tetraethylgermane gas is controlled to 500 sccm, and the flow rate of tetramethylsilane gas is controlled to 400 sccm. After co-deposition for 1 h, stop the introduction of tetraethylgermane gas and tetramethylsilane gas.

[0096] 2. Same as Example 1.

[0097] The carbon-coated alloyed negative electrode material powder particles prepared using alumina porous ceramic powder as a template obtained in Example 7 were subjected to SEM and element distribution detection, and the obtained photos are as follows: Figure 1 As shown. Figure 1 (b) Figure 1 (c) and Figure 1 As can be seen in (d), germanium, silicon and carbon elements are evenly deposited on the template, the elements are evenly distributed, and no obvious agglomeration occurs.

[0098] Comparative Example 1

[0099] This comparative example provides a silicon-carbon negative electrode material, and the preparation method is as follows:

[0100] 1. Add 100 g of alumina porous ceramic powder into a fluidized bed chemical vapor deposition equipment and heat it to 370°C. Under nitrogen protection, introduce silane gas and ethylene gas into the fluidized bed chemical vapor deposition equipment at the same time, wherein the flow rate of silane gas is controlled to 500 sccm, and the flow rate of ethylene gas is controlled to 40 sccm. After 3 h of co-deposition, stop introducing silane gas and ethylene gas.

[0101] 2. Take out the above deposited material, use a jet mill to crush it to Dv50=10 um, then add it to a rotary coating furnace, heat it to 850 °C under nitrogen protection, and pass acetylene gas at a gas flow rate of 100 sccm for gas phase coating. After 2 hours, stop passing acetylene to obtain carbon-coated silicon-carbon negative electrode material powder particles made with alumina porous ceramic powder as a template.

[0102] Comparative Example 2

[0103] This comparative example provides a silicon-carbon negative electrode material, and the preparation method is as follows:

[0104] 1. Under nitrogen protection, silane gas and ethylene gas were simultaneously introduced into the fluidized bed chemical vapor deposition equipment, wherein the flow rate of silane gas was controlled to 500 sccm, and the flow rate of ethylene gas was controlled to 40 sccm. After 3 h of co-deposition, the introduction of silane gas and ethylene gas was stopped.

[0105] 2. Take out the deposited material, use a jet mill to crush it to Dv50=10 um, then add it to a rotary coating furnace, heat it to 850 °C under nitrogen protection, and introduce acetylene gas at a gas flow rate of 100 sccm for gas phase coating. After 2 hours, stop introducing acetylene to obtain carbon-coated, template-free silicon-carbon negative electrode material powder particles.

[0106] Comparative Example 3

[0107] This comparative example provides an alloyed negative electrode material, and the preparation method is as follows:

[0108] 1. Under nitrogen protection, germane gas and ethylene gas were introduced into the fluidized bed chemical vapor deposition equipment at the same time, wherein the flow rate of germane gas was controlled to be 500 sccm, and the flow rate of ethylene gas was controlled to be 100 sccm. After co-deposition for 1 h, the introduction of germane gas and ethylene gas was stopped.

[0109] 2. Take out the deposited material, use a jet mill to crush it to Dv50=10 um, then add it to a rotary coating furnace, heat it to 850 °C under nitrogen protection, and introduce acetylene gas at a gas flow rate of 100 sccm for gas phase coating. After 2 hours, stop introducing acetylene to obtain carbon-coated, template-free alloyed negative electrode material powder particles.

[0110] Test Example 2

[0111] The negative electrode materials provided in Examples 1-7 and Comparative Examples 1-3 are assembled into batteries in the following steps:

[0112] 1. Pole sheet preparation: The negative electrode material, conductive agent (Super-P), and polyacrylic acid (PAA) binder are mixed in a mass ratio of 80:10:10 to prepare a slurry. After stirring and mixing, the slurry is coated on the copper foil current collector. After drying at room temperature, the slurry is placed in a vacuum oven and further dried at 60°C under vacuum conditions for 12 hours to obtain a pole sheet.

[0113] 2. Battery assembly: The above-obtained electrode pieces are cut into circular pieces with a diameter of 10 mm and an active material loading of 1.3 mg / cm 2 ; Metal lithium sheet was used as the counter electrode, 1 mol / L LiPF6 (the solvent was a mixture of ethylene carbonate and diethyl carbonate in a volume ratio of 1:1, with 5% volume of fluoroethylene carbonate added) as the electrolyte, and a polypropylene microporous membrane was used to assemble a 2032-type button cell in an argon atmosphere glove box, with 50 μL of electrolyte added to each cell.

[0114] The obtained 2032 type button battery was subjected to electrical performance test: the charge and discharge cut-off voltages were 1.5V and 0.005V, respectively, and then the battery was activated at a rate of 0.05C and the charge and discharge cycle test was performed at a rate of 0.5C.

[0115] The results are shown in Table 1 below.

[0116] Table 1 Electrical performance data

[0117]

[0118] It can be seen from Table 1 that different templates have little effect on the deposition of germanium, and the capacity efficiency and capacity retention rate after 100 cycles are at similar levels; the material obtained by the simultaneous cracking of tetraethylgermane and ethylene has low capacity and efficiency, but a high capacity retention rate; increasing the amount of germanium deposited can effectively increase the capacity of the material, but too much germanium deposition will reduce the first coulombic efficiency and capacity retention rate of the material; compared with only germanium deposition, the capacity and first coulombic efficiency of the simultaneous germanium / carbon deposition have decreased, but the capacity retention rate is higher; simultaneous multi-deposition of germanium / silicon / carbon, due to the higher specific capacity of silicon, can achieve higher capacity and first coulombic efficiency with less deposition amount, and the capacity retention rate is higher; in addition, the capacity retention rate of the material co-deposited with silicon and carbon is lower than that of the material co-deposited with germanium and carbon; when deposited without the aid of a template, silicon and carbon may form silicon carbide, resulting in reduced capacity, efficiency and capacity retention rate, while germanium and carbon can exert normal capacity and have a higher capacity retention rate due to their low cracking temperature.

[0119] Finally, it should be noted that the above-described embodiments are only specific implementations of the present invention, which are used to illustrate the technical solutions of the present invention, rather than to limit them. The protection scope of the present invention is not limited thereto. Although the present invention is described in detail with reference to the above-described embodiments, ordinary technicians in the field should understand that any technician familiar with the technical field can still modify the technical solutions recorded in the above-described embodiments within the technical scope disclosed by the present invention, or can easily think of changes, or make equivalent replacements for some of the technical features therein; and these modifications, changes or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention, and should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be based on the protection scope of the claims.

Claims

1. A method for preparing an alloyed negative electrode material, It is characterized in that The preparation method is as follows: S1. Add 100 g of porous alumina ceramic powder into a fluidized bed chemical vapor deposition device and heat it to 370° C. Under nitrogen protection, introduce tetraethylgermane gas and tetramethylsilane gas into the fluidized bed chemical vapor deposition device at the same time, wherein the flow rate of tetraethylgermane gas is controlled to 500 sccm, and the flow rate of tetramethylsilane gas is controlled to 400 sccm. After co-deposition for 1 h, the introduction of tetraethylgermane gas and tetramethylsilane gas is stopped; S2. Take out the deposited material, crush it to Dv50=10 μm using a jet mill, then add it to a rotary coating furnace, heat it to 850°C under nitrogen protection, and introduce acetylene gas at a gas flow rate of 100 sccm for gas phase coating. After 2 hours, stop introducing acetylene to obtain carbon-coated alloyed negative electrode material powder particles made with alumina porous ceramic powder as a template.

Citation Information

Patent Citations

  • Lithium battery silicon-carbon negative electrode composite material and preparation method thereof

    CN110649254A

  • Carbon-silicon negative electrode material and preparation method thereof

    CN112054171A

  • Three-dimensional porous silicon-carbon composite material and preparation method and application thereof

    CN113078318A

  • Silicon-based negative electrode material and preparation method and application thereof

    CN114956046A

  • Low-expansion silicon-carbon negative electrode material and preparation method thereof

    CN115986075A