Method for producing slurry for insulating protective layer of secondary battery and device for producing slurry for insulating protective layer of secondary battery
By adjusting the mixing ratio by adjusting the particle size and compression correction curve and premixing the insulating material and bonding material in the powder mixer, the problems of powder aggregation and electrostatic adhesion of the insulating protective layer of lithium ion secondary battery are solved, and the slurry is realized Stability of composition and efficient manufacturing.
Patent Information
- Application Number
- CN202310097740.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2022-02-14
- Filing Date
- 2023-02-08
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-02-08
AI Technical Summary
In the slurry manufacturing method for the insulating protective layer of the existing lithium-ion secondary battery, powders of boehmite insulating material and PVDF bonding material are prone to aggregation and electrostatic adhesion, resulting in a deviation in mixing ratio and powder clogging.
By making the correction curve of the particle size and compression relationship between the insulating material and the bonding material, the mixing ratio is measured and adjusted, and the insulating material and bonding material are mixed in advance in the powder mixer to generate a uniform mixed powder and with sliding properties The slurry mixer is placed in the optimized hopper and solvent is added to make the slurry.
The composition deviation of the insulating protective layer slurry is effectively suppressed, the electrostatic adhesion and aggregation is prevented, the uniform mixing and flowability of the powder is ensured, and the stability and efficient manufacturing of the insulating protective layer are ensured.
Smart Images

Figure CN116589892B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method and an apparatus for producing a slurry for an insulating protective layer of a secondary battery, and more particularly to a method and an apparatus for producing a slurry for an insulating protective layer of a secondary battery having a small deviation in slurry composition. Background Art
[0002] Secondary batteries such as lithium-ion secondary batteries are light in weight and can obtain high energy density, so they are also preferably used as high-output power supplies for vehicles. In such secondary batteries, the storage elements with a structure in which the positive and negative electrodes are insulated by separators are stacked in a battery shell. In addition, the storage element sometimes has a wound electrode body formed by winding the laminate in a cylindrical or elliptical column shape. Usually, the positive and negative electrodes of such an electrode body are designed in a manner that the dimension in the width direction of the negative electrode composite material layer is wider than the dimension in the width direction of the positive electrode composite material layer. The negative electrode composite material layer is opposite to the positive electrode current collector with the metal exposed through the separator. In this case, usually due to the separator, there is no short circuit between the positive electrode and the negative electrode. However, due to the precipitation of metal in the negative electrode or the intrusion of metal fine powder, etc., penetrating the separator, a short circuit may occur between the positive electrode and the negative electrode, thereby generating heat. For the purpose of preventing such a short circuit, a scheme is disclosed in which an insulating protective layer containing an inorganic filler is provided on the surface of the positive electrode current collector along the end of the positive electrode active material layer.
[0003] Such an insulating protective layer of a secondary battery is formed by mixing insulating material particles and a binder for binding the particles together, adding a solvent to the mixture to prepare a slurry, and applying the slurry to a predetermined position of an electrode to form the insulating protective layer.
[0004] As shown in Patent Document 1, inorganic ceramics such as boehmite are used as particles of such insulating material for high insulation. In addition, the insulating protective layer is unstable when only ceramics are used, so resins such as PVDF (polyvinylidene fluoride) are used as a bonding material for bonding them.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2018-198218 Summary of the invention
[0008] Problems to be solved by the invention
[0009] Fig.13This is a block diagram of a manufacturing device for insulating protective layer slurry of lithium ion secondary battery in the prior art. In the existing slurry manufacturing method using such a manufacturing device, the insulating material I and the bonding material B are fed into a powder feeding device 101 having a hopper 2i for an insulating material I such as boehmite and a hopper 2b for a bonding material B such as PVDF to be bonded thereto. After that, these powder materials are respectively fed out by a conveyor 4 such as an electromagnetic feeder, a solvent E is added to the powder material, and a slurry is generated in a slurry kneading machine 5.
[0010] Fig.14 Schematic diagram of a boehmite hopper 2i of a conventional apparatus for manufacturing a slurry for an insulating protective layer of a lithium ion secondary battery. In the prior art, since the particle size of the powder of the insulating material I such as boehmite is small, the particles of the powder are easily agglomerated. Fig.14 As shown, bridging may occur due to aggregation in the hopper 2i or the pipe 6i of the powder feeding device 101, resulting in powder clogging.
[0011] Fig.15 1 is a schematic diagram of a PVDF hopper 2b of a prior art device for manufacturing a slurry for insulating protective layer of a lithium ion secondary battery. In addition, in the prior art, a resin such as PVDF (polyvinylidene fluoride) as a binder material B is easily charged with static electricity, such as Figure 3 As shown, there is a problem that static electricity easily adheres to the hopper 2b, the pipe 6b, etc. of the powder feeding device 101.
[0012] Therefore, there is a problem that the binder B, which is PVDF (polyvinylidene fluoride), and boehmite do not form a predetermined mixing ratio, and the composition of the powder material varies.
[0013] The problem to be solved by the method for producing a slurry for an insulating protective layer of a secondary battery and the apparatus for producing a slurry for an insulating protective layer of a secondary battery of the present invention is to suppress the variation in the composition of the slurry for an insulating protective layer of a secondary battery.
[0014] Means for solving problems
[0015] According to one aspect of the present disclosure, a method for manufacturing a slurry for an insulating protective layer of a secondary battery comprises: using a plurality of groups of particle sizes and compression degrees of insulating materials to prepare an insulating material calibration curve indicating the relationship between the particle sizes and compression degrees of the insulating material; using a plurality of groups of particle sizes and compression degrees of binding materials to prepare a binding material calibration curve indicating the relationship between the particle sizes and compression degrees of the binding material; measuring the particle size of the insulating material to be introduced; measuring the particle size of the binding material to be introduced; based on the measured particle size of the insulating material and the measured particle size of the binding material, referring to the insulating material calibration curve and the binding material calibration curve, determining an optimal mixing weight ratio so that the compression degree of a mixed powder of the insulating material and the binding material becomes a set compression degree; mixing the insulating material and the binding material according to the determined mixing weight ratio to generate a mixed powder of the insulating material and the binding material; introducing the generated mixed powder of the insulating material and the binding material into a powder introducing device; and adding a solvent to the mixed powder introduced by the powder introducing device to manufacture a slurry.
[0016] In a method for manufacturing a slurry for an insulating protective layer of a secondary battery according to another aspect of the present disclosure, when a powder feeding device has a funnel-shaped metal hopper with a surface roughness Ra=0.02 [μm] or less, an inner wall of the hopper has an inclination angle θ of 60 to 70 [°] relative to the horizontal, and an inner diameter Dh of a discharge port at the bottom of the hopper is 100 to 200 [mm], the average particle size Di (d50) of the particles of the insulating material is greater than 1.0 [μm] and less than 3.0 [μm], the average particle size Db (d50) of the particles of the binding material is greater than 50 [μm] and less than 150 [μm], and the mixing weight ratio [w%] of the binding material in the total of the insulating material and the binding material is in the range of 15 [w%] or more.
[0017] According to another aspect of the present disclosure, a manufacturing device for a slurry for an insulating protective layer of a secondary battery comprises a slurry kneading machine and a powder feeding device for feeding raw materials into the slurry kneading machine, and a control device for controlling the powder feeding device and the slurry kneading machine. The powder feeding device comprises: a powder mixer for feeding powder of insulating material and powder of bonding material to generate a uniform mixed powder; and a hopper for feeding the mixed powder generated in the powder mixer into the slurry kneading machine.
[0018] Effects of the Invention
[0019] According to the method for producing a slurry for an insulating protection layer of a secondary battery and the apparatus for producing a slurry for an insulating protection layer of a secondary battery of the present invention, it is possible to suppress the variation in the composition of the slurry for an insulating protection layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a block diagram of an apparatus for producing a slurry for an insulating protective layer of a lithium ion secondary battery according to the present embodiment.
[0021] Figure 2 It is a schematic diagram of a hopper of the manufacturing apparatus of the slurry for insulating protection layer of the lithium ion secondary battery of this embodiment.
[0022] Figure 3 Schematic diagram showing a state in which the surface of PVDF particles is covered with boehmite particles.
[0023] Figure 4 This is a flowchart of a method for producing a slurry for an insulating protective layer of a lithium ion secondary battery according to the present embodiment.
[0024] Figure 5 This is a flowchart of the process of preparing a calibration curve in the method for producing the slurry for the insulating protection layer of the lithium ion secondary battery according to the present embodiment.
[0025] Figure 6 This is a table showing the mixing weight ratio of PVDF to the total of PVDF and boehmite and the amount of boehmite required in coating so as not to cause electrostatic adhesion of PVDF.
[0026] Figure 7 This is a graph showing the mixing weight ratio of PVDF to the mixed powder of PVDF and boehmite and the amount of boehmite required in coating in order to prevent electrostatic adhesion of PVDF.
[0027] Figure 8 This is a table showing the relationship between the mixing weight ratio of PVDF to the total of PVDF and boehmite and the degree of compression.
[0028] Fig. 9 This is a graph showing the relationship between the mixing weight ratio of PVDF to the total of PVDF and boehmite and the degree of compression.
[0029] Fig.10 This is a graph showing the relationship between the particle size of PVDF and the degree of compressibility of PVDF.
[0030] Fig.11 This is a graph showing the relationship between the particle size of boehmite and the compressibility of boehmite.
[0031] Fig.12 This is a graph showing the relationship between the particle size of PVDF and the amount of boehmite.
[0032] Fig.13 This is a block diagram of a conventional apparatus for producing a slurry for an insulating protective layer of a lithium-ion secondary battery.
[0033] Fig.14 This is a schematic diagram of a hopper for boehmite in a conventional apparatus for producing a slurry for an insulating protective layer of a lithium ion secondary battery.
[0034] Fig.15 This is a schematic diagram of a PVDF hopper of a conventional apparatus for producing a slurry for an insulating protective layer of a lithium ion secondary battery. DETAILED DESCRIPTION
[0035] (Overview of this embodiment)
[0036] The following reference Figures 1 to 12 The manufacturing method of the insulating protective layer slurry of the secondary battery of the present invention is described by the manufacturing method of the insulating protective layer slurry of the lithium ion secondary battery. In the present embodiment, as a secondary battery, a lithium ion secondary battery is used as an example for description, as an insulating material I, boehmite is used as an example for description, as a bonding material B, polyvinylidene fluoride (PVDF) is used as an example for description, but it is not limited to these.
[0037] (Principle of this embodiment)
[0038] <Problems of the present embodiment>
[0039] In the prior art, Fig.13 As shown in FIG. 2 , the insulating material I is put into the hopper 2i alone, and the bonding material B is put into the hopper 2b alone. The particle size of boehmite is small, and boehmite has the property of being easily agglomerated. Therefore, Fig.14 As shown, in the hopper 2i, the insulating material I (boehmite) agglomerates, increases in apparent size, and generates bridges. Therefore, blockage or stagnation occurs in a portion of the hopper 2i or the pipe 6i, and sometimes the entire amount of the insulating material I input cannot reach the slurry kneading machine 5.
[0040] On the other hand, since the surface of PVDF particles is easily charged, Fig.15 As shown, the binder B (PVDF) directly contacts the inner wall of the hopper 2b, and the PVDF may be electrostatically attached to the inner wall of the hopper 2b. Therefore, a blockage or retention occurs in the hopper 2b or a part of the pipe 6b, and sometimes the entire amount of the binder B cannot reach the slurry kneading machine 5.
[0041] Since these phenomena occur randomly, there is a problem that the mixing of the insulating material I and the adhesive material B is different each time.
[0042] <Overview of the Manufacturing Apparatus of the Insulating Protective Layer Slurry S of the Present Embodiment>
[0043] Figure 1: This is a block diagram of a manufacturing device for an insulating protective layer slurry S of a lithium ion secondary battery of the present embodiment. The manufacturing device for an insulating protective layer slurry S of a lithium ion secondary battery of the present embodiment includes a powder feeding device 1 for feeding raw materials into a slurry kneading machine 5, and a slurry kneading machine 5. The powder feeding device 1 includes a powder mixer 3 for feeding powder of an insulating material I and powder of a bonding material B to generate a uniform mixed powder M. In addition, the powder feeding device 1 includes a hopper 2 for feeding the mixed powder M generated in the powder mixer 3 into the slurry kneading machine 5. The mixed powder M fed into the hopper 2 is fed into the slurry kneading machine 5. The mixed powder M fed into the slurry kneading machine 5 is kneaded with a solvent E such as an organic solvent to generate a slurry S for an insulating protective layer. The manufacturing device for the slurry S for an insulating protective layer of the present embodiment includes a control device 7 with a computer, and implements the manufacturing method of the slurry S for an insulating protective layer of the present embodiment.
[0044] The manufacturing device (control device 7) of the insulating protective layer slurry S in the present disclosure can be constructed as a computer system including one or more processors; and a non-temporary memory (non-temporary computer-readable storage medium) storing a command (computer program) that can be executed by the processor to make the processor execute the control according to any one of the embodiments and modifications (for example, the flowchart (S1 to S6, S11 to S14) of the manufacturing method of the insulating protective layer slurry S, etc.). The processor may include a dedicated hardware circuit such as a CPU (Central Processing Unit), a GPU (Graphics Processing Unit), an integrated circuit for a specific purpose (ASIC: Application Specific Integrated Circuit), or a combination thereof. The non-temporary computer-readable storage medium can be used to store the desired program code in the form of a RAM (Random Access Memory), a ROM (Read Only Memory), an optical disk storage device such as a CD-ROM, a magnetic disk storage device, a magnetic storage device, a flash memory, or a command or data structure, and includes any other medium that can be accessed by a computer.
[0045] In this embodiment, in such a manufacturing device, the powder of the insulating material I and the powder of the bonding material B are mixed at a predetermined mixing weight ratio [w %] to generate a mixed powder M. Therefore, the manufacturing device of this embodiment is characterized in that the mixed powder M at the predetermined mixing weight ratio [w %] is charged into the hopper 2.
[0046] <Main Functions and Effects of the Present Embodiment>
[0047] Figure 3 Schematic diagram showing a state in which the surface of PVDF particles as the binding material B in this embodiment is covered with particles of boehmite as the insulating material I. In this embodiment, before being put into the hopper 2, the powder of the insulating material I and the powder of the binding material B are pre-mixed by the powder mixer 3 to generate a mixed powder M. As a result of such mixing, in the mixed powder M, the insulating material I with a smaller particle size is attached to the binding material B with a larger particle size in a manner that the surface is appropriately covered by static electricity. Therefore, it is possible to suppress the surface of the binding material B from being electrostatically attached to the inner surface of the hopper 2.
[0048] On the other hand, the insulating material I having a small particle size is dispersed by adhering to the surface of the binder B, and aggregation thereof can be suppressed.
[0049] In the case of this embodiment, a common single hopper 2 is used as the hopper 2 for the insulating material I and the hopper 2 for the binding material B, and the mixed powder M is not easily electrostatically attached, and agglomeration due to agglomeration is also suppressed. Therefore, the total amount of the insulating material I and the binding material B for the slurry kneading machine 5 can be smoothly and without omission into the slurry kneading machine 5. Therefore, the deviation of the composition of the slurry S for the insulating protective layer of the lithium ion secondary battery can be suppressed.
[0050] Hereinafter, the method for producing the slurry for the insulating protection layer of the lithium ion secondary battery according to the present embodiment will be described in detail.
[0051] <Manufacturing device of insulating protective layer slurry S>
[0052] The manufacturing apparatus of the slurry S for insulating protective layer includes a powder feeding device 1 and a slurry kneading machine 5. The powder feeding device 1 includes a powder mixer 3 and a hopper 2. Each of them will be described in detail below.
[0053] <Powder mixer 3>
[0054] The powder mixer 3 receives the powder of the insulating material I and the powder of the bonding material B and generates a uniform mixed powder M. The powder mixer 3 is a circular device in a plan view, and comprises: a large material input opening 31 located at the top; a bottom surface 32 that closes the bottom; and a cylindrical side surface 33. The powder mixer 3 has a vertical drive shaft 35 at its center for rotating a stirring blade 34 for stirring. The stirring blade 34 is rotated by a driving unit 36 to stir the powder inside. The powder mixer 3 is not limited to the illustrated equipment, and a propeller or the like may be used to stir instead of the stirring blade 34. In addition, the powder mixer 3 may also have a cylindrical drum with a horizontal or inclined drive shaft to rotate the container itself.
[0055] Although not shown in the figure, the powder mixer 3 includes a discharge port provided on the bottom surface 32, and the mixed powder M is charged into the hopper 2. Alternatively, the powder mixer 3 may be tilted as a whole to charge the mixed powder M into the hopper 2.
[0056] <Hopper 2>
[0057] Figure 2 Schematic diagram of the hopper 2 of the manufacturing device for the insulating protective layer of the lithium ion secondary battery of the present embodiment. The hopper 2 puts the mixed powder M generated by mixing in the powder mixer 3 into the slurry kneading machine 5. The upper part 22 of the hopper 2 has a cylindrical shape. An opening 21 is opened at the upper end of the upper part 22. The lower part 23 of the hopper 2, which is continuous from the upper part 22, has a hollow inverted frustum shape that narrows in a tapered manner. A circular discharge port 24 is opened at the lower end of the lower part 23.
[0058] The hopper 2 is made of stainless steel such as SUS304, and has a surface roughness Ra of 0.02 [μm] or less. If the surface roughness exceeds Ra = 0.02 [μm], the sliding with the mixed powder M deteriorates, which is not ideal; however, in the case of existing equipment, it can be used even if it is outside the numerical range.
[0059] The inner wall of the lower portion 23 of the hopper 2 has an inclination angle θ of 60 to 70 [°] relative to the horizontal. In addition, the inner diameter Dh of the discharge port 24 at the bottom of the hopper 2 is 100 to 200 [mm]. These values can also be used even if they are outside the numerical range in the case of existing equipment.
[0060] <Piping 6>
[0061] The discharge port 24 at the bottom of the hopper 2 may be provided with a pipe 6 having the same inner diameter.
[0062] <Slurry mixer 5>
[0063] The slurry kneading machine 5 receives the mixed powder M introduced into the hopper 2 and kneads the mixed powder M with a solvent E such as an organic solvent to produce an insulating protective layer slurry S. The type of the kneading machine is not particularly limited as long as the mixed powder M and the solvent E can be uniformly kneaded.
[0064] <Insulation Material I>
[0065] As the insulating material I, particles having high insulation and heat resistance, low cost, stable quality and uniformity are preferred.
[0066] Examples of the insulating material I include inorganic ceramics such as silicon dioxide (SiO2), aluminum oxide (Al2O3), titanium dioxide (TiO2), lithium titanate (Li4Ti5O 12), oxides such as zirconium oxide (ZrO2) or barium titanate (BaTiO3), or hydroxides such as boehmite (Al2O3·3H2O), etc.
[0067] In particular, aluminum oxide (Al2O3) and lithium titanate (Li4Ti5O 12 ), barium titanate (BaTiO3) or boehmite (Al2O3·3H2O). In this embodiment, boehmite is exemplified as the insulating material I, but the present invention is not limited thereto.
[0068] The average particle size Di (d50) of the particles of the insulating material I of the present embodiment is, for example, not less than 1.0 [μm] and not more than 3.0 [μm]. The average particle size Di (d50) of the insulating material I is relatively small, so it is easy for the insulating material I to aggregate. In the present embodiment, the aggregation of the insulating material I that is easy to aggregate can be suppressed. Here, the "particle size" or "average particle size" in the present application refers to the median diameter (d50) in the frequency distribution measured by the laser diffraction method unless otherwise stated.
[0069] The insulating material I may be used alone or in combination of two or more.
[0070] <Bonding Material B>
[0071] The binding material B (binder) stably binds the particles of the insulating material I. Among the binding materials B, particles having high insulation and heat resistance, low cost, stable quality, and uniformity are preferred.
[0072] In this embodiment, polyvinylidene fluoride (hereinafter sometimes referred to as "PVDF") is exemplified as the bonding material B. Resins such as PVDF have strong bonding strength. On the other hand, PVDF is easily charged and has the problem of being easily attached to the hopper 2, piping 6, etc. of the powder feeding device 1 due to static electricity. In this embodiment, the problem caused by the charging of the bonding material B is solved.
[0073] It should be noted that the binder B is not limited to PVDF, and examples of the binder B that is similarly easily charged include carboxymethyl cellulose (CMC), polymethyl methacrylate (PMMA), and the like.
[0074] In addition, polyethylene (PE), polypropylene (PP), tetrafluoroethylene (PTFE) and the like can be cited as the binder B. The invention of this embodiment can also be applied to such a binder B.
[0075] The average particle size Db (d50) of the PVDF particles as the binder B in this embodiment is, for example, 50 [μm] or more and 150 [μm] or less. Thus, compared with the average particle size Di (d50) of the particles of the insulating material I, which is 1.0 [μm] or more and 3.0 [μm] or less, the average particle size Db (d50) of the binder B is relatively large.
[0076] <Mixed powder M>
[0077] The mixed powder M is obtained by uniformly mixing the powder of the insulating material I and the powder of the binding material B using a powder mixer 3 .
[0078] It should be noted that, in addition to the insulating material I and the binding material B, the mixed powder M may also contain, for example, a dispersant or a thickener. However, in the description of this embodiment, for the sake of convenience, the description of other components is omitted, and the mixed powder M is described as a mixture of the insulating material I and the binding material B in a mixed weight ratio [w%).
[0079] <Mixing of mixed powder M>
[0080] In the mixed powder M of the present embodiment, that is, the total of the insulating material I and the binder B, the mixing weight ratio [w %] of the insulating material I is in the range of 15 [w %] or more.
[0081] On the other hand, the mixing weight ratio [w%] of the insulating material I in the total of the insulating material I and the adhesive material B is in the range of 80 [w%] or less. Preferably, the mixing weight ratio [w%] of the insulating material I in the total of the insulating material I and the adhesive material B is in the range of 25 [w%] or less.
[0082] <Function of insulating protective layer>
[0083] The purpose of the present embodiment is to be the most suitable method for manufacturing the insulating protective layer slurry for forming the insulating protective layer of the lithium ion secondary battery. The function of the insulating protective layer is to suppress the situation that the foreign matter such as metal powder existing between the pole plates or the metal precipitated on the pole plates penetrates the separator and produces a small short circuit. Therefore, high insulation performance and high mechanical strength are required for the insulating protective layer. From such an aspect, materials such as boehmite can be appropriately used. Therefore, it is a prerequisite that the insulating protective layer contains sufficient insulating material I.
[0084] Therefore, it is preferable that the mixing weight ratio [w %] of boehmite as the insulating material I in the mixed powder M of the present embodiment is higher.
[0085] <Stabilization of the insulating protective layer>
[0086] The purpose of adding the binder B to the particles of the insulating material I is to stabilize the insulating protective layer formed. From this perspective, the mixing weight ratio [w%] of PVDF as the binder B in this embodiment is preferably 15 [w%] or more. If the mixing weight ratio [w%] of PVDF is less than 15 [w%], boehmite as the insulating material I is likely to fall off from the insulating protective layer formed.
[0087] On the other hand, when the mixing weight ratio [w%] of PVDF is 25 [w%] or more, the mixing weight ratio [w%] of boehmite as the insulating material I is relatively reduced. In addition, when the slurry is applied, the viscosity is too high, making it difficult to apply uniformly.
[0088] <Required amount of boehmite to suppress static electricity adhesion>
[0089] Figure 6 It indicates the mixing weight ratio [w %] of PVDF to the total of PVDF and boehmite and the amount of boehmite required in coating so as not to cause electrostatic adhesion of PVDF.
[0090] For PVDF as the binder B and boehmite as the insulating material I in this embodiment, the following is obtained: Figure 3 The amount of particles of insulating material I shown in the figure is required to cover the particles of bonding material B. Figure 6 As shown, if boehmite is 100% and PVDF is 0%, the amount of boehmite required to coat the surface of the PVDF is of course 0 [w%] of the mixed powder M. If PVDF is 10%, the amount of boehmite used to coat the surface of the PVDF is 2.54 [w%] of the mixed powder M. Since boehmite is contained in the mixed powder M at 90 [w%], a sufficient amount can be ensured. In this way, if PVDF is 70%, the amount of boehmite used to coat the surface of the PVDF is 17.75 [w%] of the mixed powder M. Since boehmite is contained in the mixed powder M at 30 [w%], a sufficient amount can still be ensured. In addition, if PVDF is 80%, the amount of boehmite used to coat the surface of the PVDF is 20.29 [w%] of the mixed powder M. In this case, since boehmite is contained in the mixed powder M at 20 [w%], a substantially sufficient amount is ensured to effectively suppress electrostatic adhesion. Furthermore, if PVDF is 90%, the amount of boehmite used to coat the surface of the PVDF is 22.82 [w%] of the mixed powder M. However, since the mixed powder M contains only 10 [w%] of boehmite, the amount used to coat the surface of the PVDF with boehmite cannot be ensured.
[0091] Thus, by Figure 6As shown in the table, the mixing weight ratio [w%] of the binder B in the total of the insulating material I and the binder B is preferably within a range of 80 [w%] or less. In other words, boehmite is preferably 20 [w%] or more of the mixed powder M.
[0092] Figure 7 FIG. L2 shows the mixing weight ratio of the mixed powder of PVDF and boehmite and the required amount of boehmite in coating to prevent electrostatic adhesion of PVDF. FIG. L2 shows the mixing weight ratio [w %] and the required amount of boehmite required for coating PVDF. Figure 7 Lieutenant General Figure 6 As can be seen from this, in order to perform coating without causing electrostatic adhesion of PVDF, the required amount of boehmite can be confirmed to be 20 [w%] or more of the mixed powder M.
[0093] Therefore, in the present embodiment, from the viewpoint of suppressing electrostatic adhesion, the boehmite content in the mixed powder M is preferably 20 [w %] or more.
[0094] <Compression C>
[0095] Fig.10 This is a graph showing the relationship between the particle size Db [μm] of PVDF and the compression degree C [%] of PVDF. Fig.11 This is a graph showing the relationship between the particle size Di [μm] of boehmite and the compression degree C [%] of boehmite.
[0096] Here, when "ρtapped" is used as the "tapped bulk density" and "ρbulk" is used as the "loose bulk density", "compression degree C[%]" is defined as compression degree C[%] = {(ρtapped-ρbulk) / ρtapped}×100. From the perspective of compression degree C[%], the smaller the particle size of the powder, the smaller the tapped bulk density ρtapped (density when pressed tightly). That is, the smaller the particle size, the higher the compression degree C[%]. In addition, if the compression degree C[%] increases, the fluidity becomes worse.
[0097] <Mixed weight ratio [%] and compression degree C [%]>
[0098] Fig.12 This is a graph showing the relationship between the particle size Db [μm] of PVDF and the amount of boehmite. As mentioned above, the particle size Di [μm] of boehmite is smaller than the particle size Db [μm] of PVDF. Thus, since the compression C [%] increases as the particle size Db [μm] decreases, the compression C [%] increases as the amount of boehmite with a small particle size Di [μm] increases. Fig.12As shown, it is assumed that the particle size Di [μm] of boehmite is the same. At this time, the mixing weight ratio [%] of boehmite used to maintain a certain compression degree C [%] of the mixed powder M is taken into consideration. It can be seen that when the particle size Db [μm] of PVDF is small, the mixing weight ratio [%] of boehmite is relatively high; when the particle size Db [μm] of PVDF is large, the mixing weight ratio [%] of boehmite is relatively low. That is, even if the particle size Db [μm] of PVDF changes, the set compression degree C [%] can be achieved by changing the mixing weight ratio [%] of boehmite.
[0099] <Adjustment of Compression Degree C [%] of Mixed Powder M in the Present Embodiment>
[0100] Figure 8 This is a table showing the relationship between the mixing weight ratio [w%] of PVDF of the present embodiment to the mixed powder M which is the total of PVDF and boehmite and the compression degree C [%] of the mixed powder M. In addition, Fig. 9 FIG. L3 is a graph showing the relationship between the mixing weight ratio [w %] of PVDF to the total of PVDF and boehmite and the compression degree C [%] of the mixed powder M.
[0101] First, when PVDF is 0%, that is, when PVDF is not added to boehmite, the compression C[%] of the mixed powder M is the compression C[%] of the boehmite itself, which is 53.1[%] in the present embodiment. In this state, the compression C[%] of the boehmite is too high, agglomeration occurs, and the fluidity deteriorates. Therefore, as described in the problem of the prior art, bridges due to agglomeration are generated in the hopper 2 and the piping 6, and the total amount of the mixed powder M cannot be smoothly fed into the slurry kneading machine 5.
[0102] On the other hand, for reference, when PVDF is 100%, that is, the mixed powder M is entirely PVDF and there is no boehmite in the mixed powder M, the compression C[%] of the mixed powder M is the compression C[%] of PVDF itself, which is 9.7[%] in the present embodiment. In this state, the compression C[%] of the mixed powder M is low and agglomeration is likely to occur. Therefore, there is no problem if only fluidity is considered, but since boehmite as the insulating material I is not included, an insulating protective layer cannot be formed.
[0103] Here, according to the study by the present inventors, it is found that in the present embodiment, the compression degree C[%] of the mixed powder M without causing bridges due to aggregation in the hopper 2 and the pipe 6 is about 47[%].
[0104] Therefore, next, when PVDF is 10 [w %], the compression C [%] of the mixed powder M is 48.8 [%], and the compression C [%] is improved. However, in this state, the compression C [%] of the mixed powder M is still too high, agglomeration occurs, and the fluidity deteriorates.
[0105] Furthermore, when PVDF is 15 [w %], the compression C [%] of the mixed powder M is 46.6 [%], which is lower than the target compression C [%] = 47 [%]. In this state, the compression C [%] of the mixed powder M is sufficiently reduced, the generation of bridges caused by agglomeration can be suppressed, and the deterioration of fluidity can be effectively suppressed.
[0106] Therefore, if Fig. 9 As shown, in the mixed powder M, when PVDF is 15 [w %] or more and boehmite is less than 85 [w %], it is preferable from the viewpoint of the compression degree C [%] of the mixed powder M.
[0107] <Method for producing slurry for insulating protective layer>
[0108] Figure 4 1 is a flow chart of a method for producing a slurry for an insulating protective layer of a lithium ion secondary battery according to the present embodiment. Figure 4 A method for producing the insulating protective layer slurry for the lithium ion secondary battery according to the present embodiment will be described.
[0109] The method for manufacturing a slurry for an insulating protective layer includes a calibration curve preparation step (S1), a particle size measurement step (S2), a mixing weight ratio determination step (S3), a powder mixing step (S4), a powder feeding device feeding step (S5), and a slurry manufacturing step (S6).
[0110] <Calibration curve preparation step (S1)>
[0111] The calibration curve preparation step (S1) includes an insulating material calibration curve preparation step of preparing an insulating material calibration curve representing the relationship between the particle size [μm] and the compression C [%] of the insulating material I having different particle sizes [μm]. In addition, the calibration curve preparation step (S1) includes an adhesive material calibration curve preparation step of preparing an adhesive material calibration curve representing the relationship between the particle size [μm] and the compression C [%] of the adhesive material B according to the relationship between the particle size [μm] and the compression C [%] of the adhesive material B having different particle sizes [μm].
[0112] The "calibration curve" here refers to a graph showing the relationship between different particle sizes [μm] and the compression C [%] corresponding to the particle sizes [μm], which is derived from data previously measured experimentally. In one example, multiple groups of particle sizes [μm] and compression C [%] of a powder (insulating material I or bonding material B) are measured experimentally in advance, and a "calibration curve" is derived using the measured multiple groups. Therefore, the compression C [%] of the powder can be estimated by measuring the particle size [μm] and referring to the calibration curve for the measured particle size [μm].
[0113] <Details of Calibration Curve Creation Step (S1)>
[0114] Figure 5 This is a flowchart of a calibration curve preparation process of the method for producing a slurry for an insulating protective layer of a lithium ion secondary battery according to the present embodiment. The calibration curve preparation step (S1) of the present embodiment includes the following process.
[0115] The calibration curve preparation step (S1) includes a bulk density measurement step (S11), a compression degree calculation step (S12), and a calibration curve calculation step (S14) performed after these steps are completed.
[0116] <Bulk Density Measurement Step (S11)>
[0117] The bulk density measuring step (S11) includes an insulating material bulk density measuring step for measuring the bulk density of the powder of the insulating material I and a bonding material bulk density measuring step for measuring the bulk density of the powder of the bonding material B. As the processes, only the measurement objects are different, so they are described together.
[0118] Here, “bulk density ρ” refers to the density at the apparent volume [g / cm 3 ] In addition, “bulk density ρ” uses “loose bulk density ρbulk (Aerated Bulk Density)” and “tapped bulk density ρtapped (Packed Bulk Density)”. “Loose bulk density ρbulk” is also called sparse packing density, and is a value with a relatively large void ratio (Void) or void ratio (Porosity) when lightly packed. “Tapped bulk density ρtapped” is also called dense packing density, and is a value with a relatively small void ratio (Void) or void ratio (Porosity) when densely packed. Regarding the measurement method, the mass [g] and volume [cm 3 ], divide the measured mass [g] by the measured volume [cm 3 ].
[0119] In the insulating material bulk density measuring step of measuring the bulk density ρ of the powder of the insulating material I, the mass [g] of the powder of the insulating material I is divided by the volume [cm 3 ], and measure the "insulating material bulk density ρi". In one example, the "insulating material bulk density ρi" includes the "tapped bulk density" and "loose bulk density" of the powder of the insulating material I. In the step of measuring the bulk density ρ of the powder of the bonding material B, the mass [g] of the powder of the bonding material B is divided by the volume [cm 3 ], and measure the "binder bulk density ρb". In one example, the "binder bulk density ρb" includes the "tapped bulk density" and "loose bulk density" of the powder of the binder B.
[0120] <Compression Degree Calculation Step (S12)>
[0121] The compression degree calculation step (S12) includes an insulating material compression degree calculation step and an adhesive material compression degree calculation step. The insulating material compression degree calculation step and the adhesive material compression degree calculation step differ only in the calculation objects as processes, so they are described together.
[0122] In the "insulating material compression calculation step", the compression C [%] of the powder of the insulating material I is calculated based on the bulk density ρi of the powder of the insulating material I measured in the "bulk density measurement step (S11)".
[0123] As described above, when "ρtapped" is used as the "tapped bulk density" and "ρbulk" is used as the "loose bulk density", the "compression degree C [%]" can be calculated by "compression degree C [%] = {(ρtapped-ρbulk) / ρtapped} × 100".
[0124] The "binder material compression calculation step" is also performed using the same process to calculate the compression C [%] of the powder of the binder material B.
[0125] <Measurement at different particle sizes>
[0126] The bulk density measurement step (S11) and the compression calculation step (S12) are performed using the above process. In this process, the purpose of this step is to obtain the relationship between the particle size [μm] and the compression C [%] of the insulating material I, and the relationship between the particle size [μm] and the compression C [%] of the bonding material B. Therefore, it is necessary to plot the combination of "particle size [μm]" and "compression C [%]" on the graph to analyze the relationship between "particle size [μm]" and "compression C [%]". In addition, in the bulk density measurement step (S11) and the compression calculation step (S12), it is necessary to perform measurements of different particle sizes [μm] more than three times.
[0127] Therefore, in step (S13), it is determined whether these measurements are performed three times or more. If they are less than three times (S13: NO), the process returns to the bulk density measurement step (S11) and performs measurements at different particle sizes [μm]. In addition, if these measurements are performed three times or more (S13: YES), the process proceeds to the calibration curve calculation step (S14).
[0128] <Calibration Curve Calculation Step (S14)>
[0129] The calibration curve calculation step (S14) includes an "insulating material calibration curve calculation step" and a "bonding material calibration curve calculation step". In the "insulating material calibration curve calculation step", a calibration curve is calculated based on the particle size [μm] and compression C [%] of the powder of the insulating material I. In the "bonding material calibration curve calculation step", a calibration curve is calculated based on the particle size [μm] and compression C [%] of the powder of the bonding material B.
[0130] The “insulating material correction curve calculation step” and the “adhesive material correction curve calculation step” differ only in the objects, and the processes are the same, so they are described together.
[0131] In the bulk density measurement step (S11) and the compression calculation step (S12) of the "insulating material correction curve calculation step", the measurement of different particle sizes [μm] is performed more than 3 times. The correction curve calculation step (S14) is a process for obtaining the relationship between the particle size [μm] and the compression C [%] of the insulating material I, and the relationship between the particle size [μm] and the compression C [%] of the bonding material B. Therefore, a graph is plotted on the graph for the combination of "particle size [μm]" and "compression C [%]" measured in the bulk density measurement step (S11) and the compression calculation step (S12). Based on multiple points representing the relationship between "particle size [μm]" and "compression C [%]" plotted on the graph like this, a graph connecting these plotting points is made. If there are 3 drawing points, the graph is generated in the form of a quadratic curve. It should be noted that the drawing points can also be 2 points. If there are 2 points, the graph is generated in the form of a linear function. When a plurality of plot points are taken, the relationship between "particle size [μm]" and "compression degree C [%]" is determined by regression analysis using the least square method or the like. These relationships are stored in a computer (not shown).
[0132] The "insulating material calibration curve" and "bonding material calibration curve" are derived using the above process. If the particle size Di [μm] (d50) of insulating material I is measured using the "insulating material calibration curve", the compression C [%] of insulating material I can be immediately known. Similarly, if the particle size Db [μm] (d50) of bonding material B is measured using the "bonding material calibration curve", the compression C [%] of bonding material B can be immediately known.
[0133] <Particle Size Measurement Step (S2)>
[0134] The particle size measuring step (S2) includes an "insulating material measuring step" for measuring the particle size Di (d50) of the inserted insulating material I, and a "bonding material measuring step" for measuring the particle size Db (d50) of the inserted bonding material B. In one example, in the "insulating material measuring step", the particle size Di (d50) of the inserted insulating material I is measured in advance before the insulating material I is inserted into the powder inserting device. In one example, in the "bonding material measuring step", the particle size Db (d50) of the inserted bonding material B is measured in advance before the bonding material B is inserted into the powder inserting device.
[0135] The “insulating material measurement step” and the “adhesive material measurement step” differ only in the measurement objects, and the processes are common, so they are described together.
[0136] The average particle size Di of the particles of the insulating material I and the average particle size Db of the binder B introduced are both average median diameters determined by a laser diffraction method.
[0137] <Mixing Weight Ratio Determination Step (S3)>
[0138] In the mixing weight ratio determination step (S3), the average particle size Di of the particles of the insulating material I and the average particle size Db of the bonding material B obtained in the particle size measurement step (S2) are converted into compression degrees C [%]. The conversion into compression degrees C [%] is performed with reference to the "insulating material calibration curve" and "bonding material calibration curve" calculated in the calibration curve calculation step (S14).
[0139] The mixing weight ratio [w %] of the insulating material I and the bonding material B is determined in such a way that the compression degree C [%] of the mixed powder M becomes the set compression degree C [%] according to the compression degree C [%] of the insulating material I and the bonding material B. Here, for example, Fig. 9As shown, based on the calculated compression C[%] of the insulating material I and the bonding material B, a graph L3 is prepared showing the compression C[%] of the mixed powder M when the mixing weight ratio [w%] of the bonding material B is 0[w%] to 100[w%]. And, the mixing weight ratio [w%] of the insulating material I and the bonding material B of the mixed powder M is determined so that the compression C[%] of the mixed powder M is less than the compression C[%] at which bridging does not occur.
[0140] <Powder Mixing Step (S4)>
[0141] In the powder mixing step (S4), the insulating material I and the bonding material B are introduced into the powder mixing device from the opening 31 at the mixing weight ratio [w %] of the insulating material I and the bonding material B determined in the mixing weight ratio determination step (S3). Figure 1 In the powder mixer 3 shown, powder mixing is performed. At this time, the insulating material I and the binding material B are mixed in a dry state without adding a solvent to the insulating material I and the binding material B. In the powder mixer 3, the driving shaft 35 is rotated by the driving unit 36, and the insulating material I and the binding material B are uniformly mixed by the stirring blade 34.
[0142] <Powder feeding device feeding step (S5)>
[0143] In the powder feeding device feeding step (S5), the insulating material I and the bonding material B are mixed in the powder mixing step (S4) to form a uniform mixed powder M, which is fed into the hopper 2 of the powder feeding device 1. When feeding, the discharge port (not shown) provided on the bottom surface 32 of the powder mixer 3 is opened, and the mixed powder M is dropped by gravity. The powder mixer 3 may also be tilted. In addition, the mixed powder M may be sucked into the hopper 2 by an air pressure pump. In this case, the mixed powder M will not agglomerate and will not cause electrostatic adhesion, so it can be smoothly fed into the hopper 2.
[0144] In order to make the feeding smoother, the powder mixer 3 or the pipe 6 may be vibrated by a vibrator or the like. In addition, the mixed powder M may be conveyed by an electromagnetic feeder or the like during the feeding.
[0145] <Slurry manufacturing step (S6)>
[0146] like Figure 1 As shown, the mixed powder M introduced into the hopper 2 is introduced into the slurry kneading machine 5 through the pipe 6. In the slurry manufacturing step (S6), the solvent E is added to the mixed powder M by the slurry kneading machine 5 and kneaded to manufacture the slurry S for the insulating protective layer.
[0147] (Effects of Implementation Methods)
[0148] In this embodiment, before being put into the hopper 2, the powder of the insulating material I and the powder of the bonding material B are mixed in advance by the powder mixer 3 to generate a mixed powder M. As a result of such mixing, in the mixed powder M, the particles of the insulating material I with a smaller particle size are attached in a manner that appropriately covers the surface of the particles of the bonding material B with a larger particle size. Therefore, electrostatic adhesion on the surface of the particles of the bonding material B is suppressed.
[0149] On the other hand, the particles of the insulating material I having a small particle size are dispersed by adhering to the surfaces of the particles of the binding material B, and aggregation thereof is suppressed.
[0150] In the case of this embodiment, a common single hopper 2 is used for the insulating material I and the binding material B, and the mixed powder M is not easily electrostatically attached, and agglomeration due to agglomeration is also suppressed, so the total amount of the insulating material I and the binding material B can be smoothly and without omission into the slurry kneading machine 5. Therefore, the deviation of the composition of the slurry S for the insulating protective layer of the lithium ion secondary battery can be suppressed.
[0151] (Effects of Embodiments)
[0152] (1) According to the method for producing a slurry for an insulating protective layer of a lithium ion secondary battery of the present embodiment, it is possible to suppress the variation in the composition of the slurry S for an insulating protective layer.
[0153] (2) By mixing the powders, the insulating material I which is not easily charged is adsorbed and applied to the surface of the binding material B which is easily charged, thereby preventing the mixed powder M from adhering to the hopper 2 and the pipe 6 due to static electricity.
[0154] (3) By mixing the powders, the insulating material I having a small particle size is attached to the surface of the easily charged binder B and dispersed, thereby suppressing the aggregation of the insulating material I.
[0155] (4) The mixed powder M optimized by mixing the insulating material I and the bonding material B in an optimal ratio can reduce the compression C [%] and ensure the fluidity of the powder.
[0156] (5) The hopper 2 of the powder feeding device 1 is a funnel-shaped metal hopper with a surface roughness Ra of 0.02 [μm] or less, the inner wall of the hopper 2 has an inclination angle θ of 60 to 70 [°] relative to the horizontal, and the inner diameter Dh of the discharge port at the bottom of the hopper 2 is 100 to 200 [mm].
[0157] Therefore, the mixed powder M can smoothly slide down in the hopper 2 without being attached, and the entire amount thereof can be fed into the slurry kneading machine 5 .
[0158] (6) Since the mixed powder M is prepared by mixing the insulating material I and the bonding material B, a common single hopper 2 can be used for the insulating material I and the bonding material B. Therefore, it is not necessary to prepare a plurality of hoppers, nor is it necessary to use equipment for transporting between the plurality of hoppers.
[0159] (7) The mixing weight ratio [w%] of the adhesive material B in the total of the insulating material I and the adhesive material B is set to 15 [w%] or more. Therefore, the peeling and falling of the insulating material I can be effectively suppressed.
[0160] (8) The mixing weight ratio [w%] of the adhesive material B in the total of the insulating material I and the adhesive material B is set to 15 [w%] or more. Therefore, the aggregation of the insulating material I can be suppressed, and the bridging of the insulating material I in the hopper 2 can be effectively suppressed.
[0161] (9) The mixing weight ratio [w%] of the above-mentioned adhesive material B in the total of the insulating material I and the adhesive material B is set to 80 [w%] or less. Therefore, the surface of the adhesive material B can be coated with the insulating material I, and static electricity adhesion can be effectively suppressed.
[0162] (10) The mixing weight ratio [w%] of the adhesive material B in the total of the insulating material I and the adhesive material B is set to 25 [w%] or less. Therefore, the insulating property of the insulating protective layer can be improved while effectively suppressing the intrusion of metals and the like.
[0163] (11) The calibration curve preparation step (S1) includes an insulating material calibration curve preparation step and a bonding material calibration curve preparation step. In the insulating material calibration curve preparation step, an insulating material calibration curve is prepared to show the relationship between the particle size Di and the compression degree C[%] of a plurality of powders having different particle sizes Di of the insulating material I. In the bonding material calibration curve preparation step, a bonding material calibration curve is prepared to show the relationship between the particle size Db and the compression degree C[%] of a plurality of powders having different particle sizes Db of the bonding material B. Therefore, by referring to the insulating material calibration curve L5 and the bonding material calibration curve L4, the compression degree C[%] of the insulating material I and the bonding material B to be put in can be obtained by measuring the particle sizes thereof.
[0164] (12) The calibration curve preparation step (S1) includes a bulk density measurement step (S11) and a compression degree calculation step (S12). By repeating these steps, the insulating material calibration curve L5 and the adhesive material calibration curve L4 can be prepared.
[0165] (Other examples)
[0166] In the present embodiment, a lithium ion secondary battery is described as an example of a secondary battery, but the present invention is not limited to the lithium ion secondary battery, and can be applied to other secondary batteries having an insulating protective layer as long as the present invention can be applied.
[0167] In this embodiment, boehmite is exemplified as the insulating material I, but boehmite may be replaced with other insulating materials I such as alumina. In addition, in this embodiment, PVDF is exemplified as the binder B, but other easily charged resins may be used as the binder B.
[0168] The hopper 2 illustrated in this embodiment is a preferred example, and an existing hopper can be used. In this case, it is needless to say that a person skilled in the art can optimize the obtained compression degree C [%] and the like to suit the hopper.
[0169] The numerical values and ranges shown in the present embodiment are merely examples and can be optimized by those skilled in the art.
[0170] · Figure 4 , Figure 5 The flowchart shown is an example, and those skilled in the art may add to, delete, change, or replace the order of the process to implement it.
[0171] The present invention can be implemented by those skilled in the art by adding, deleting, or changing the configuration thereof without departing from the scope of the claims.
[0172] (Note)
[0173] The following describes the technical ideas that can be grasped by the present disclosure. It should be noted that, not for the purpose of limitation but to assist understanding, the constituent elements recorded in the supplementary notes are given reference symbols corresponding to the constituent elements in the embodiments. The reference symbols are shown in the form of examples to assist understanding, and the constituent elements recorded in each supplementary note should not be limited to the constituent elements represented by the reference symbols.
[0174] (Note 1)
[0175] A method for producing a slurry for an insulating protective layer of a secondary battery, comprising:
[0176] Using a plurality of sets of particle sizes and compression degrees of the insulating material (I), an insulating material calibration curve (S1) is prepared that represents the relationship between the particle size and compression degree of the insulating material;
[0177] Using a plurality of sets of particle sizes and compression degrees of the binder (B), a binder calibration curve (S1) is prepared that indicates the relationship between the particle size and compression degree of the binder;
[0178] Measuring the particle size (S2) of the insulating material to be put into the device;
[0179] Measuring the particle size (S2) of the bonding material to be input;
[0180] Based on the measured particle size of the insulating material and the measured particle size of the bonding material, an optimal mixing weight ratio is determined with reference to the insulating material calibration curve and the bonding material calibration curve so that the compression degree of the mixed powder of the insulating material and the bonding material becomes a set compression degree (S3);
[0181] The insulating material and the bonding material are mixed according to the determined mixing weight ratio to generate a mixed powder of the insulating material and the bonding material (S4);
[0182] The generated mixed powder of the insulating material and the bonding material is fed into a powder feeding device (1) (S5); and
[0183] A solvent is added to the mixed powder introduced by the powder introducing device to produce a slurry (S6).
[0184] (Note 2)
[0185] The method for producing a slurry for an insulating protective layer of a secondary battery according to Supplement 1 further comprises:
[0186] The mixed powder is fed into the slurry kneading machine (5) by the powder feeding device (S6),
[0187] The production of the above slurry includes:
[0188] In the slurry kneading machine, a solvent is added to the mixed powder introduced by the powder introducing device to produce a slurry.
[0189] (Note 3)
[0190] The method for producing a slurry for an insulating protective layer of a secondary battery according to Appendix 1 or 2, wherein:
[0191] The preparation of the above insulation material correction curve includes:
[0192] Determining the bulk density of the insulating material powder (S11);
[0193] Calculating the degree of compression of the insulating material powder based on the bulk density of the insulating material powder obtained by the above measurement (S12); and
[0194] The insulating material calibration curve is calculated according to the particle size and compression degree of the insulating material powder (S14).
[0195] The preparation of the above bonding material calibration curve includes:
[0196] Determining the bulk density of the powder of the bonding material (S11);
[0197] Calculating the compression degree of the powder of the bonding material based on the bulk density of the powder of the bonding material obtained by the above measurement (S12); and
[0198] The bonding material calibration curve is calculated according to the particle size and compression degree of the bonding material powder (S13).
[0199] (Note 4)
[0200] The method for producing a slurry for an insulating protective layer of a secondary battery according to Appendix 1 or 2, wherein the insulating material is boehmite.
[0201] (Note 5)
[0202] The method for producing a slurry for an insulating protective layer of a secondary battery according to Appendix 1 or 2, wherein the binder is polyvinylidene fluoride.
[0203] (Note 6)
[0204] The method for producing a slurry for an insulating protective layer of a secondary battery according to Appendix 1 or 2, wherein:
[0205] When the powder feeding device has a funnel-shaped metal hopper (2) with a surface roughness Ra of 0.02 [μm] or less, the inner wall of the hopper has an inclination angle θ of 60 to 70 [°] relative to the horizontal, and the inner diameter Dh of the discharge port at the bottom of the hopper is 100 to 200 [mm],
[0206] The average particle size Di (d50) of the particles of the insulating material is 1.0 [μm] or more and 3.0 [μm] or less, and the average particle size Db (d50) of the particles of the bonding material is 50 [μm] or more and 150 [μm] or less,
[0207] The mixing weight ratio [w %] of the above-mentioned adhesive material in the total of the above-mentioned insulating material and the above-mentioned adhesive material is in the range of 15 [w %] or more.
[0208] (Note 7)
[0209] The method for producing a slurry for an insulating protective layer of a secondary battery according to Supplementary Note 6, wherein a mixing weight ratio [w %] of the above-mentioned binder in the total of the above-mentioned insulating material and the above-mentioned binder is within a range of 80 [w %] or less.
[0210] (Note 8)
[0211] The method for producing a slurry for an insulating protective layer of a secondary battery as described in Supplementary Note 6, wherein a mixing weight ratio [w %] of the above-mentioned binder in the total of the above-mentioned insulating material and the above-mentioned binder is in a range of 25 [w %] or less.
[0212] Description of Reference Numerals
[0213] 1. 101…Powder feeding device
[0214] 2…Hopper
[0215] 2i…Hopper for insulating materials
[0216] 2b…Hopper for bonding material
[0217] 21…Opening
[0218] 22…upper part
[0219] 23…lower part
[0220] 24…Discharge port
[0221] 3…Powder mixer
[0222] 31…Opening
[0223] 32…Bottom
[0224] 33…Side
[0225] 34…Stirring blade
[0226] 35…Drive shaft
[0227] 36…Driver
[0228] 4…Conveyor
[0229] 5…Slurry mixer
[0230] 6, 6i, 6b...Piping
[0231] I…Insulating material (boehmite)
[0232] B…Binder (polyvinylidene fluoride (PVDF))
[0233] M…Mixed powder
[0234] E…Solvent
[0235] S...(for insulation protective layer) paste
[0236] ρ…Bulk density
[0237] L1~L6…curve graph
[0238] θ…Inclination angle (the inner wall of the hopper relative to the horizontal)
[0239] Dh…Inner diameter (of the discharge port at the bottom of the hopper)
[0240] Di(d50)…average particle size (of insulating materials)
[0241] Db(d50)…average particle size (of binder material)
Claims
1. A method for producing a slurry for an insulating protective layer of a secondary battery, the method comprising: Using a plurality of sets of particle sizes and compression degrees of insulating materials, creating an insulating material calibration curve representing the relationship between the particle sizes and compression degrees of the insulating materials; Using a plurality of sets of particle sizes and compression degrees of the binder material, creating a binder material calibration curve representing the relationship between the particle size and compression degree of the binder material; Determining the particle size of the insulating material added; Determining the particle size of the input bonding material; Based on the measured particle size of the insulating material and the measured particle size of the bonding material, an optimal mixing weight ratio is determined with reference to the insulating material calibration curve and the bonding material calibration curve so that the compression degree of the mixed powder of the insulating material and the bonding material becomes a set compression degree; In the powder mixer of the manufacturing device, the insulating material and the bonding material are mixed according to the determined mixing weight ratio to generate a mixed powder of the insulating material and the bonding material; Putting the generated mixed powder of the insulating material and the bonding material into the hopper of the manufacturing device; as well as In the slurry kneading machine of the manufacturing device, a solvent is added to the mixed powder introduced through the hopper to manufacture a slurry, The preparation of the insulation material correction curve includes: Determining the bulk density of the insulating material powder; calculating the degree of compression of the insulating material powder based on the measured bulk density of the insulating material powder; and The insulation material calibration curve is calculated according to the particle size and compression degree of the insulation material powder. The preparation of the bonding material calibration curve includes: Determining the bulk density of the powder of the bonding material; calculating the compressibility of the powder of the bonding material based on the measured bulk density of the powder of the bonding material; and The bonding material calibration curve is calculated according to the particle size and compression degree of the bonding material powder.
2. The method for producing a slurry for an insulating protective layer of a secondary battery according to claim 1, characterized in that: The insulating material is boehmite.
3. The method for producing a slurry for an insulating protective layer of a secondary battery according to claim 1, characterized in that: The bonding material is polyvinylidene fluoride.
4. The method for producing a slurry for an insulating protective layer of a secondary battery according to claim 1, characterized in that: The hopper is made of a funnel-shaped metal with a surface roughness Ra of 0.02 μm or less, the inner wall of the hopper has an inclination angle θ of 60 to 70° relative to the horizontal, and the inner diameter Dh of the discharge port at the bottom of the hopper is 100 to 200 mm. The particles of the insulating material have an average particle size Di of d50 of 1.0 μm or more and 3.0 μm or less, and the particles of the bonding material have an average particle size Db of d50 of 50 μm or more and 150 μm or less, The mixing weight ratio of the adhesive material in the total of the insulating material and the adhesive material is in a range of 15w% or more.
5. The method for producing a slurry for an insulating protective layer of a secondary battery according to claim 4, characterized in that: The mixing weight ratio of the adhesive material in the total of the insulating material and the adhesive material is in a range of 80w% or less.
6. The method for producing a slurry for an insulating protective layer of a secondary battery according to claim 4, characterized in that: The mixing weight ratio of the adhesive material in the total of the insulating material and the adhesive material is in a range of 25w% or less.