A high-strength, dirt-resistant TPU material and preparation method thereof
By using cross-linking agents containing organosilicon oxygen segments in TPU materials for cross-linking, the problems of low density and insufficient dirt resistance of TPU materials are solved, and materials with high specific gravity, high strength and good hydrophobicity are realized, improving the overall performance of the material.
Patent Information
- Application Number
- CN202310541888.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-15
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-05-15
AI Technical Summary
The low density of existing TPU materials results in poor texture, and common modification methods can lead to a decrease in tensile strength, making it difficult to simultaneously improve the material's high specific gravity and dirt resistance.
A cross-linking agent containing organosilicone segments and terminated by isocyanate is used to react with the hydroxyl and urethane bonds in TPU to achieve a large number of grafting and cross-linking of organosilicone segments and introduce a micro-crosslinked structure. Improve the molecular weight and physical properties of materials.
It significantly improves the dirt resistance and physical properties of the material, enhances the hydrophobicity and sweat resistance, avoids delamination caused by the introduction of fillers, and improves the overall performance of the material.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermoplastic polyurethane elastomer (TPU) composite materials, and in particular to a high-strength and dirt-resistant TPU material and a preparation method thereof. Background Art
[0002] As people's living standards continue to improve and the level of social intelligence continues to improve, smart wearable products are pouring into people's lives. In the field of smart wearables, high-density materials often give people a sense of luxury, especially in the wristband and watch industry. High-density wristbands can fit the wrist better when worn, giving people a sense of comfort, the so-called "wrist pressure feeling"; at the same time, in the field of wearables, colors are gradually diversified. Some light-colored products will produce obvious color spots due to long-term contact with the skin or contamination with oil, which greatly affects the product's ornamental value.
[0003] In the field of smart wearables, the commonly used high-density material is fluororubber, but fluororubber is a thermosetting material with poor low-temperature resistance, complex processing and extremely high price, which greatly limits its application.
[0004] Thermoplastic polyurethane elastomer (TPU) is a type of elastomer that can be plasticized by heating, has a wide range of hardness, high strength, high modulus, and high wear resistance. It is widely used in the field of wearables, but the density of TPU is 1.1-1.2g / cm 3 In order to increase its density, a large amount of fillers need to be added. The introduction of a large amount of fillers will inevitably cause the physical properties of the material to fluctuate. Therefore, a certain amount of cross-linking agent needs to be introduced to make the material have higher mechanical properties and obtain high-strength, high-specific gravity and dirt-resistant TPU material.
[0005] The patent specification with publication number CN113416408A discloses a method for preparing a modified TPU material. Inorganic fillers such as barium sulfate with a particle size of 0.2-0.7 μm are modified with an ethanol solution of a silane coupling agent and then blended with TPU for extrusion granulation to solve the problem of poor texture caused by low density of TPU materials. However, the mechanical properties of the modified TPU materials, such as tensile strength, are reduced.
[0006] The patent specification with the publication number CN113637139A discloses a method for preparing a silicone-modified TPU composition, which involves the following steps: adding a reactive hydroxy silicone modifier to the molten TPU under the protection of an inert atmosphere, and continuously stirring during the mixing process until the NCO reaches the theoretical value, thereby obtaining a reactive hydroxy silicone-modified TPU. This patented technology is to graft silicone onto both ends of TPU by reacting the hydroxyl groups of the reactive hydroxy silicone modifier with the isocyanate groups at both ends of TPU. This modification method has a small amount of silicone grafted and it is difficult for the silicone itself to crosslink with TPU. As described in the patent specification, the silicone-containing chain segments in the silicone-modified TPU are incompatible with the TPU body and will migrate to the surface of TPU to form a silicone layer. Summary of the invention
[0007] The present invention provides a high-strength and dirt-resistant TPU material. A cross-linking agent containing an organic silicon oxygen chain segment and terminated by isocyanate is added to the TPU. The cross-linking agent reacts with hydroxyl groups and carbamate bonds in the TPU through isocyanate groups to achieve a large amount of grafting and cross-linking of the organic silicon oxygen chain segments on the TPU, which can significantly improve the dirt resistance of the material and introduce a micro-cross-linking structure, significantly increase the molecular weight of the material, and further improve the physical properties and dirt resistance of the composite material.
[0008] The specific technical solutions are as follows:
[0009] A high-strength, dirt-resistant TPU material, the raw material composition includes, by weight:
[0010] TPU 30-70 parts,
[0011] 5-20 parts of cross-linking agent;
[0012] The crosslinking agent contains an organic silicon oxygen segment and is terminated by an isocyanate group.
[0013] The TPU raw material in the high-strength and dirt-resistant TPU material of the present invention can be conventional hydroxyl-terminated TPU.
[0014] The cross-linking agent contains a large number of Si-O segments, which can give the material good hydrophobicity, so that the product has good resistance to hand sweat and other properties during wearing and use, thereby improving the product's resistance to dirt.
[0015] The high-strength and dirt-resistant TPU material, the cross-linking agent can be obtained by reacting silicone diol with diisocyanate.
[0016] The organosilicon diol may be selected from one or more of dimethylsilanediol, cycloethyl-methyl-silanediol, propylmethylsilanediol, dicyclopentylsilanediol, diphenylsilanediol, polyether siloxane diol, and dihydroxy polydimethylsiloxane.
[0017] The molecular weight of the polyether siloxane diol and the dihydroxy polydimethylsiloxane is preferably 500-4000 g / mol.
[0018] The diisocyanate may be selected from one or more of toluene diisocyanate, diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, xylylene diisocyanate, 3,3'-dimethyl-4,4'-biphenyl diisocyanate, cyclohexane dimethylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, and 3,3'-dimethyl-4,4'-diphenylmethane diisocyanate.
[0019] In a preferred example, the high-strength and dirt-resistant TPU material, the preparation method of the cross-linking agent comprises: reacting silicone diol and diisocyanate at a molar ratio of 1:2-3 at 100-130° C. and a vacuum degree of 100-500 Pa to obtain the cross-linking agent. The reaction time is adjustable, for example, it can be 0.5-3 hours.
[0020] In a preferred example, the raw material composition of the high-strength and dirt-resistant TPU material also includes 30-70 parts by mass of barium sulfate.
[0021] More preferably, the average particle size of the barium sulfate is less than 1 micron.
[0022] In a preferred example, the raw material composition of the high-strength and dirt-resistant TPU material also includes 0.5-2 parts by mass of silicone lubricant.
[0023] More preferably, the molecular weight of the silicone lubricant is 30000-60000 g / mol.
[0024] The present invention also provides a method for preparing the high-strength and dirt-resistant TPU material, wherein the high-strength and dirt-resistant TPU material is obtained by melting TPU and a cross-linking agent under a protective atmosphere.
[0025] The protective atmosphere refers to an atmosphere that will not participate in or affect the melting reaction, for example, it can be a dry nitrogen atmosphere.
[0026] In a preferred example, the method for preparing the high-strength and dirt-resistant TPU material adopts a twin-screw extruder to carry out the melt reaction, wherein TPU is added through the main feed port and a cross-linking agent is added through the exhaust port.
[0027] In a preferred embodiment, in the method for preparing the high-strength and dirt-resistant TPU material, 30-70 parts by weight of barium sulfate is added to the main feed port. Further preferably, the average particle size of the barium sulfate is less than 1 micron.
[0028] In a preferred embodiment, in the method for preparing the high-strength and dirt-resistant TPU material, 0.5-2 parts by mass of silicone lubricant is also added to the main feeding port. Further preferably, the molecular weight of the silicone lubricant is 30,000-60,000 g / mol.
[0029] In a preferred example, in the method for preparing the high-strength and dirt-resistant TPU material, the aspect ratio of the twin-screw extruder is 44-56:1.
[0030] In a preferred example, in the preparation method of the high-strength and dirt-resistant TPU material, the twin-screw extruder has 13 heating zones, and the temperatures of the heating zones from the main feeding port to the die are as follows: the temperature of the first heating zone is 130-160°C, the temperature of the second heating zone is 140-170°C, the temperature of the third heating zone is 140-170°C, the temperature of the fourth heating zone is 140-170°C, the temperature of the fifth heating zone is 130-160°C, the temperature of the sixth heating zone is 130-160°C, the temperature of the seventh heating zone is 120-150°C, the temperature of the eighth heating zone is 100-130°C, the temperature of the ninth heating zone is 100-130°C, the temperature of the tenth heating zone is 100-130°C, the temperature of the eleventh heating zone is 100-130°C, the temperature of the twelfth heating zone is 100-130°C, and the temperature of the thirteenth heating zone is 140-170°C; the exhaust port is in the sixth heating zone.
[0031] In a preferred example, in the method for preparing the high-strength and dirt-resistant TPU material, the rotation speed of the twin-screw extruder is 200-300 rpm.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] 1) The cross-linking agent of the present invention contains a large amount of Si-O segments, which can give the material good hydrophobicity, so that the product has good sweat resistance and other properties during wearing and use, thereby improving the product's anti-fouling performance.
[0034] 2) The advantage of the composite material of the present invention over the traditional anti-fouling TPU is that if the TPU containing silicone is directly synthesized by in-situ reaction of silicone diol, its heat resistance and stability are poor and its physical properties are low. After the secondary blending process, the performance of this TPU containing silicone will be further reduced. Therefore, the present invention uses ordinary TPU to introduce Si-O bonds during the blending process. The cross-linking agent containing Si-O bonds reacts with the hydroxyl and carbamate bonds in TPU through the isocyanate end group in the screw, which can not only improve the anti-fouling performance of the material, but also introduce a micro-cross-linking structure, increase the molecular weight of the material, and then improve the physical properties and anti-fouling performance of the blended material. However, the hydroxyl-terminated silicone modifier used in the prior art cannot react with the carbamate bonds in the TPU segment to form an internal cross-linking structure.
[0035] 3) A small amount of high molecular weight silicone lubricant can be introduced into the material of the present invention. The introduction of Si-O crosslinking agent greatly improves the compatibility of TPU and silicone, avoiding the phenomenon of material stratification caused by the introduction of silicone. The selection of high molecular weight silicone lubricant with a molecular weight of 30000-60000 g / mol can not only further improve the material's smoothness and dirt resistance, but also avoid the problem of precipitation migration because it is a high molecular weight substance.
[0036] 4) The material of the present invention can use barium sulfate with an average particle size of less than 1 micron as a high specific gravity filler. The surface of the material filled with it is more delicate, and it has lower hiding power than metal oxides such as zinc oxide, antimony trioxide, molybdenum oxide, etc., and its color is light white. Different color products can be prepared according to actual color requirements. Moreover, it is a strong metal acid salt, and its stability is much higher than that of metal oxides, and it is more skin-friendly, and is more suitable for the preparation of wearable products. DETAILED DESCRIPTION
[0037] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention.
[0038] The operating methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturers.
[0039] Unless otherwise specified, the amount of each component in the following examples and comparative examples refers to parts by mass. The preparation method of the cross-linking agent is as follows: dihydroxy polydimethylsiloxane and diisocyanate are put into a reaction kettle, a vacuum device is turned on, and the reaction is carried out at 115° C. and a vacuum degree of 300 Pa for 1.5 hours to obtain a cross-linking agent A; in the cross-linking agent A, the molecular weight of the dihydroxy polydimethylsiloxane is 1000 g / mol, the diisocyanate is diphenylmethane diisocyanate (MDI), and the molar ratio of the dihydroxy polydimethylsiloxane to the MDI is 1:2.
[0040] In the following embodiments and comparative examples, the twin-screw extruder has 13 heating zones, and the temperatures of the heating zones from the main feed port to the die are: the temperature of the first heating zone is 130-160°C, the temperature of the second heating zone is 140-170°C, the temperature of the third heating zone is 140-170°C, the temperature of the fourth heating zone is 140-170°C, the temperature of the fifth heating zone is 130-160°C, the temperature of the sixth heating zone is 130-160°C, the temperature of the seventh heating zone is 120-150°C, the temperature of the eighth heating zone is 100-130°C, the temperature of the ninth heating zone is 100-130°C, the temperature of the tenth heating zone is 100-130°C, the temperature of the eleventh heating zone is 100-130°C, the temperature of the twelfth heating zone is 100-130°C, and the temperature of the thirteenth heating zone is 140-170°C. The exhaust port is in the sixth heating zone. The screw speed of the twin-screw extruder is 250rpm. The screw length-diameter ratio of the twin-screw extruder is 50: 1. The main feed port and exhaust port of the twin-screw extruder are protected by dry nitrogen.
[0041] In the above cross-linking agent preparation method, when other conditions remain unchanged, dihydroxy polydimethylsiloxane is replaced by polyether siloxane diol to obtain cross-linking agent B; in cross-linking agent B, the molecular weight of polyether siloxane diol is 1000g / mol, the diisocyanate is diphenylmethane diisocyanate (MDI), and the molar ratio of polyether siloxane diol to MDI is 1:2.
[0042] In the following embodiments and comparative examples, the density test adopts the determination of density of non-foamed plastics - Part 1 - immersion method, liquid pycnometer method and titration method GB-T1033.1-2008; the tensile strength and elongation at break test adopt the standard test method for tensile properties of vulcanized rubber and thermoplastic elastomer rubber GB-T 528-2009, wherein the gauge length is 25 mm, the tensile rate is 500 mm / min, and the test specimens are 5 dumbbell-shaped specimens with a thickness of 2±0.1 mm and a width of 6±0.1 mm, and the median value is taken; the above test environments are all carried out at 23±1°C and 50±5%RH; the contact angle test adopts the standard test method for measuring the surface tension of solid coatings, substrates and pigments using contact angle ASTM D7490-2013.
[0043] Example 1
[0044] 1. Weigh 0.8 parts of silicone (molecular weight 50000 g / mol) and 50 parts of TPU particles, mix them and place them on a particle loss-in-weight scale, and place 50 parts of barium sulfate (average particle size 0.7 μm) on a powder loss-in-weight scale.
[0045] 2. Place 5 parts of crosslinking agent A in a side-feed hot melt adhesive machine. Keep the temperature of the side-feed hot melt adhesive machine and the adhesive hose at 60°C.
[0046] 3. Set the mass ratio of the pellet loss-in-weight scale, powder loss-in-weight scale and side-fed hot melt adhesive machine to 50.8:50:5 and feed them into the twin-screw extruder. The pellet loss-in-weight scale and powder loss-in-weight scale correspond to the main feeding port, and the side-fed hot melt adhesive machine corresponds to the exhaust port.
[0047] 4. After exiting the die, the product is granulated by drawing and drying at 100℃.
[0048] The high-strength, dirt-resistant TPU material prepared in this embodiment has a density of 1.83 g / cm 3 , the tensile strength is 13.18MPa, the elongation at break is 812.17%, and the water contact angle is 74.76°.
[0049] Example 2
[0050] 1. Weigh 0.8 parts of silicone (molecular weight 50000 g / mol) and 50 parts of TPU particles, mix them and place them on a particle loss-in-weight scale, and place 50 parts of barium sulfate (average particle size 0.7 μm) on a powder loss-in-weight scale.
[0051] 2. Place 15 parts of crosslinking agent A in a side-feed hot melt adhesive machine. Keep the temperature of the side-feed hot melt adhesive machine and the adhesive hose at 60°C.
[0052] 3. Set the mass ratio of the pellet loss-in-weight scale, powder loss-in-weight scale and side-fed hot melt adhesive machine to 50.8:50:15 and feed them into the twin-screw extruder. The pellet loss-in-weight scale and powder loss-in-weight scale correspond to the main feeding port, and the side-fed hot melt adhesive machine corresponds to the exhaust port.
[0053] 4. After exiting the die, the product is granulated by drawing and drying at 100℃.
[0054] The high-strength, dirt-resistant TPU material prepared in this embodiment has a density of 1.78 g / cm 3 , the tensile strength is 17.07MPa, the elongation at break is 707.73%, and the water contact angle is 82.1°.
[0055] Example 3
[0056] 1. Weigh 0.8 parts of silicone (molecular weight 50000 g / mol) and 50 parts of TPU particles, mix them and place them on a particle loss-in-weight scale, and place 50 parts of barium sulfate (average particle size 0.7 μm) on a powder loss-in-weight scale.
[0057] 2. Place 15 parts of crosslinking agent B in a side-feed hot melt adhesive machine. Keep the temperature of the side-feed hot melt adhesive machine and the adhesive hose at 60°C.
[0058] 3. Set the mass ratio of the pellet loss-in-weight scale, powder loss-in-weight scale and side-fed hot melt adhesive machine to 50.8:50:15 and feed them into the twin-screw extruder. The pellet loss-in-weight scale and powder loss-in-weight scale correspond to the main feeding port, and the side-fed hot melt adhesive machine corresponds to the exhaust port.
[0059] 4. After exiting the die, the product is granulated by drawing and drying at 100℃.
[0060] The high-strength, dirt-resistant TPU material prepared in this embodiment has a density of 1.77 g / cm 3 , the tensile strength is 19.26MPa, the elongation at break is 731.52%, and the water contact angle is 80.03°.
[0061] Example 4
[0062] 1. Weigh 50 parts of TPU particles and place them on a particle loss-in-weight scale, and 50 parts of barium sulfate (average particle size of 0.7 μm) and place them on a powder loss-in-weight scale.
[0063] 2. Place 10 parts of crosslinking agent A in a side-feed hot melt adhesive machine. Keep the temperature of the side-feed hot melt adhesive machine and the adhesive hose at 60°C.
[0064] 3. Set the mass ratio of the pellet loss-in-weight scale, powder loss-in-weight scale and side-fed hot melt adhesive machine to 50:50:10 and feed them into the twin-screw extruder. The pellet loss-in-weight scale and powder loss-in-weight scale correspond to the main feeding port, and the side-fed hot melt adhesive machine corresponds to the exhaust port.
[0065] 4. After exiting the die, the product is granulated by drawing and drying at 100℃.
[0066] The high-strength, dirt-resistant TPU material prepared in this embodiment has a density of 1.79 g / cm 3 , the tensile strength is 17.63MPa, the elongation at break is 715.92%, and the water contact angle is 78.8°.
[0067] Comparative Example 1
[0068] 1. Weigh 50 parts of TPU particles and place them on a particle loss-in-weight scale, and 50 parts of barium sulfate (average particle size of 0.7 μm) and place them on a powder loss-in-weight scale.
[0069] 2. Set the mass ratio of the pellet loss-in-weight scale and the powder loss-in-weight scale to 50:50 and feed them into the twin-screw extruder. The pellet loss-in-weight scale and the powder loss-in-weight scale correspond to the main feeding port.
[0070] 3. After exiting the die, the product is granulated by drawing and drying at 100℃ to obtain the product.
[0071] The TPU material prepared in this comparative example has a density of 1.85 g / cm 3, tensile strength is 9.51MPa, elongation at break is 893.5%, and water contact angle is 66.8°.
[0072] Comparative Example 2
[0073] 1. Weigh 0.8 parts of silicone (molecular weight 50000 g / mol) and 50 parts of TPU particles, mix them and place them on a particle loss-in-weight scale, and place 50 parts of barium sulfate (average particle size 0.7 μm) on a powder loss-in-weight scale.
[0074] 2. Set the mass ratio of the pellet loss-in-weight scale and the powder loss-in-weight scale to 50.8:50 and feed them into the twin-screw extruder. The pellet loss-in-weight scale and the powder loss-in-weight scale correspond to the main feeding port.
[0075] 3. After exiting the die, the product is granulated by drawing and drying at 100℃ to obtain the product.
[0076] The TPU material prepared in this comparative example has a density of 1.85 g / cm 3 , the tensile strength is 9.33MPa, the elongation at break is 887.42%, and the water contact angle is 68.3°.
[0077] Comparative Example 3
[0078] 1. Weigh 50 parts of NCO-terminated (R value greater than 1) TPU particles and place them on a particle loss-in-weight scale, and 50 parts of barium sulfate (average particle size of 0.7 μm) and place them on a powder loss-in-weight scale.
[0079] 2. Place 10 parts of dihydroxy polydimethylsiloxane (molecular weight 1000 g / mol) in a side-feed hot melt adhesive machine. The temperature of the side-feed hot melt adhesive machine and the adhesive hose is maintained at 60°C.
[0080] 3. Set the mass ratio of the pellet loss-in-weight scale, powder loss-in-weight scale and side-fed hot melt adhesive machine to 50:50:10 and feed them into the twin-screw extruder. The pellet loss-in-weight scale and powder loss-in-weight scale correspond to the main feeding port, and the side-fed hot melt adhesive machine corresponds to the exhaust port.
[0081] 4. After exiting the die, the product is granulated by drawing and drying at 100℃.
[0082] The TPU material prepared in this comparative example has a density of 1.83 g / cm 3 The tensile strength is 9.52MPa, the elongation at break is 638.29%, and the product has obvious stratification and surface oil precipitation. The water contact angle after wiping the surface is 68.51°.
[0083] Comparative Example 4
[0084] 1. Weigh 50 parts of NCO-terminated (R value greater than 1) TPU particles and place them on a particle loss-in-weight scale, and 50 parts of barium sulfate (average particle size of 0.7 μm) and place them on a powder loss-in-weight scale.
[0085] 2. Place 10 parts of dihydroxy polydimethylsiloxane (molecular weight 1000 g / mol) in a side-feed hot melt adhesive machine. The temperature of the side-feed hot melt adhesive machine and the adhesive hose is maintained at 60°C.
[0086] 3. Set the mass ratio of the pellet loss-in-weight scale, powder loss-in-weight scale and side-fed hot melt adhesive machine to 50:50:10 and feed them into the twin-screw extruder. The pellet loss-in-weight scale and powder loss-in-weight scale correspond to the main feeding port, and the side-fed hot melt adhesive machine corresponds to the exhaust port.
[0087] 4. After exiting the die head, the pellets are drawn and granulated, and dried at 100°C. The obtained TPU pellets are fully mixed with ammonium persulfate at a mass ratio of 100:6 and placed in the feeding hopper of the twin-screw extruder. The pellets are fed into the twin-screw extruder through the self-feeding port for melt vulcanization and cross-linking processing.
[0088] 5. After exiting the die, the product is granulated by drawing and then dried at 100℃ to obtain the product.
[0089] The TPU material prepared in this comparative example has a density of 1.86 g / cm 3 The tensile strength is 12.17MPa, the elongation at break is 453.42%, and the product has obvious stratification and surface oil precipitation. The water contact angle after wiping the surface is 70.9°.
[0090] In addition, it should be understood that after reading the above description of the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.
Claims
1. A high-strength, dirt-resistant TPU material, characterized in that: In parts by mass, the raw material composition includes: TPU 30-70 parts, 5-20 parts of cross-linking agent; The cross-linking agent contains an organic silicon oxygen chain segment and is terminated by isocyanate groups; the cross-linking agent reacts with hydroxyl groups and urethane bonds in TPU via isocyanate groups; The cross-linking agent is obtained by reacting an organosilicon diol with a diisocyanate; The organosilicon diol is selected from one or more of dimethylsilanediol, cycloethyl-methyl-silanediol, propylmethylsilanediol, dicyclopentylsilanediol, diphenylsilanediol, polyether siloxane diol, and dihydroxy polydimethylsiloxane; The molecular weight of the polyether siloxane diol and the dihydroxy polydimethylsiloxane is 500-4000 g / mol; The preparation method of the cross-linking agent comprises: reacting an organosilicon diol with a diisocyanate in a molar ratio of 1:2-3 under the conditions of 100-130° C. and a vacuum degree of 100-500 Pa to obtain the cross-linking agent.
2. The high-strength, dirt-resistant TPU material according to claim 1, characterized in that: The diisocyanate is selected from one or more of toluene diisocyanate, diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, xylylene diisocyanate, 3,3'-dimethyl-4,4'-biphenyl diisocyanate, cyclohexane dimethylene diisocyanate, 4,4'-dicyclohexylmethane diisocyanate and 3,3'-dimethyl-4,4'-diphenylmethane diisocyanate.
3. The high-strength, dirt-resistant TPU material according to claim 1, characterized in that: The raw material composition of the high-strength and dirt-resistant TPU material also includes 30-70 parts by mass of barium sulfate; The average particle size of the barium sulfate is less than 1 micron.
4. The high-strength, dirt-resistant TPU material according to claim 1, characterized in that: The raw material composition of the high-strength and dirt-resistant TPU material also includes 0.5-2 parts by mass of silicone lubricant; The molecular weight of the silicone lubricant is 30000-60000 g / mol.
5. The method for preparing the high-strength and dirt-resistant TPU material according to claim 1 or 2, characterized in that: The high-strength and dirt-resistant TPU material is obtained by melting and reacting TPU and a cross-linking agent under a protective atmosphere.
6. The preparation method according to claim 5, characterized in that: The melt reaction is carried out using a twin-screw extruder, wherein TPU is added through the main feed port and a cross-linking agent is added through the exhaust port.
7. The preparation method according to claim 6, characterized in that: 30-70 parts by weight of barium sulfate is also added to the main feed port; The average particle size of the barium sulfate is less than 1 micron.
8. The preparation method according to claim 6, characterized in that: 0.5-2 parts by mass of silicone lubricant is also added to the main feeding port; The molecular weight of the silicone lubricant is 30000-60000 g / mol.
9. The preparation method according to claim 6, characterized in that: The aspect ratio of the twin-screw extruder is 44-56:1; The twin-screw extruder has 13 heating zones, and the temperatures of the heating zones from the main feeding port to the die are as follows: the temperature of the first heating zone is 130-160°C, the temperature of the second heating zone is 140-170°C, the temperature of the third heating zone is 140-170°C, the temperature of the fourth heating zone is 140-170°C, the temperature of the fifth heating zone is 130-160°C, the temperature of the sixth heating zone is 130-160°C, the temperature of the seventh heating zone is 120-150°C, the temperature of the eighth heating zone is 100-130°C, the temperature of the ninth heating zone is 100-130°C, the temperature of the tenth heating zone is 100-130°C, the temperature of the eleventh heating zone is 100-130°C, the temperature of the twelfth heating zone is 100-130°C, and the temperature of the thirteenth heating zone is 140-170°C; the exhaust port is in the sixth heating zone; The rotation speed of the twin-screw extruder is 200-300 rpm.
Citation Information
Patent Citations
Modified TPU material as well as preparation method and application thereof
CN113416408A
Organic silicon modified TPU composition and preparation method thereof
CN113637139A
Silane terminated polyurethane oligomer and its preparation method
CN103910847A
Anti-fingerprint oil-resistant TPU (Thermoplastic Polyurethane) film and preparation method thereof
CN108034223A