A kind of moisture-heat resistant polyurethane thermal conductive structural adhesive and preparation method thereof
By using polyurethane structural glue that combines modified diol with polyether polyol and isocyanate, the problem of aging of polyurethane structural glue in humid and heat environment is solved, good thermal conductivity and shear strength are achieved, and new energy is ensured. Reliable operation and safety of the battery.
Patent Information
- Application Number
- CN202310563912.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-18
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2043-05-18
AI Technical Summary
The aging of existing polyurethane structural glue in humid and hot environments can easily lead to a decrease in bond strength and mechanical strength, and is prone to unsafe accidents such as circuit breakers and leakage, which cannot meet the requirements of new energy batteries.
A polyurethane structural glue composed of a modified diol containing benzene ring and amide bond at both ends and a polyether polyol is prepared by amidation reaction of the modified diol and combined with isocyanate. A polyurethane thermally conductive structural adhesive with good moisture and heat aging resistance is formed.
This polyurethane thermal conductivity structural adhesive has good thermal conductivity, shear strength and anti-humidity and heat aging properties, and can provide reliable structural bonding in new energy batteries to ensure the safe operation of new energy vehicles.
Smart Images

Figure SMS_2 
Figure SMS_3 
Figure QLYQS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyurethane structural adhesives, and in particular relates to a moisture-heat resistant polyurethane thermal conductive structural adhesive and a preparation method thereof. Background Art
[0002] With the improvement of environmental awareness, rising oil prices and government support, new energy vehicles have gradually become a hot spot in the market. The battery of new energy vehicles is equivalent to the engine of traditional fuel vehicles and is the "heart" of new energy vehicles. More than 80% of the volume of new energy vehicle batteries is composed of organic chemical materials, including structural adhesive materials, thermal conductive materials, insulating materials, heat insulating materials and sealing materials, among which structural adhesive materials are responsible for bonding cells to cells, cells to foam, cells to module shells, etc., and play a key role in realizing the integration of cells and modules.
[0003] Generally speaking, in order to ensure the normal and stable operation of the battery, the structural adhesive needs to have both good thermal conductivity and bonding functions. For example, patent CN111995979B discloses a room temperature fast-curing polyurethane thermal conductive structural adhesive, in which component A is composed of the following mass percentages: polyether diol 2-10%, chain extender 2-10%, polyether triol 2-10%, thermal conductive filler 30-80%, flame retardant 5-20%, dehydrator 0.1-1.0%, catalyst 0.1-1.0%; component B is composed of the following mass percentages: polyether diol 15-40%, 4,4'-diphenylmethane diisocyanate 5-12%, thermal conductive filler 30-80%, flame retardant 5-20%. Patent CN111303820B discloses a two-component polyurethane structural adhesive for power battery bonding and a preparation method thereof. The polyurethane structural adhesive includes component A and component B; component A includes 40 to 65 parts of polymethylene polyphenyl isocyanate, 30 to 50 parts of aluminum hydroxide, 2 to 5 parts of hydrophobic fumed silica, and 0 to 5 parts of plasticizer; component B includes 40 to 65 parts of bio-based polyol, 1 to 4 parts of fumed silica, 25 to 50 parts of flame retardant, 1 to 5 parts of adhesion promoter and 0.01 to 0.5 parts of catalyst; the bio-based polyol is selected from one or more of rapeseed oil-modified polyol, castor oil-modified polyol, soybean oil-modified polyol and palm oil-modified polyol; the adhesion promoter is prepared by reacting aminophenylsilane with a silane modifier.
[0004] The above-mentioned polyurethane structural adhesive not only has excellent shear resistance, but also has good thermal conductivity. It can be used in new energy power battery modules to effectively transfer heat and structurally bond battery PACK packages. However, polyurethane structural adhesives are very sensitive to the aging effects caused by humid and hot environments. Batteries are sometimes in humid and hot working conditions for a long time. Aging causes the bonding strength and mechanical strength to decrease, and unsafe and unstable accidents such as circuit breaking and leakage are prone to occur. Therefore, simply requiring polyurethane structural adhesives to have good bonding strength and thermal conductivity cannot meet the requirements for their use in new energy batteries. They must also have good resistance to moisture and heat. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a moisture-heat resistant polyurethane thermal conductive structural adhesive and a preparation method thereof. The present invention provides a modified diol containing a benzene ring and an amide bond at both ends, and the polyurethane structural adhesive prepared by compounding the modified diol with a polyol raw material of the modified diol and a polyether polyol has good resistance to moisture-heat aging, providing safety guarantee for the reliable operation of new energy vehicles.
[0006] To achieve the above object, the present invention adopts the following specific technical solutions:
[0007] A polyurethane thermal conductive structural adhesive, comprising components A and B.
[0008] The A component includes the following raw materials: mixed alcohol, small molecule chain extender, modified thermal conductive filler, catalyst, the mixed alcohol is compounded by modified diol and polyether polyol, the structural formula of the modified diol is shown in the following formula I:
[0009] Formula I:
[0010] ;
[0011] Wherein, n is an integer of 4-12 (such as 5, 6, 8, 10, 11), R1 and R2 are independently selected from C1-C4 alkylene (such as methylene, ethylene, propylene, butylene);
[0012] The B component includes the following raw materials: isocyanate and modified thermal conductive filler.
[0013] A polyurethane heat-conductive structural adhesive comprises components A and B, wherein the weight ratio of component A to component B is 1:1-1.2.
[0014] The A component comprises the following raw materials in parts by weight: 30-40 parts of polyol, 0.5-2 parts of small molecule chain extender, 40-80 parts of modified thermal conductive filler, and 0.1-0.5 parts of catalyst; the compounding mass ratio of the modified diol to the polyether polyol is 5.5-7.5:1;
[0015] The B component includes the following raw materials in parts by weight: 20-32 parts of isocyanate and 40-80 parts of modified thermal conductive filler.
[0016] The modified diol is prepared by amidation reaction of amino-polyethylene glycol-amino (H2N-PEG-NH2) and hydroxybenzoic acid ester derivatives, and the molar ratio of the two is 1:2.07-2.15.
[0017] In the amino-polyethylene glycol-amino, the polymer of polyethylene glycol is 4-12, specifically selected from one or a combination of two or more of amino-tetrapolyethylene glycol-amino, amino-pentapolyethylene glycol-amino, amino-hexapolyethylene glycol-amino, amino-heptapolyethylene glycol-amino, amino-octapolyethylene glycol-amino, amino-nonapolyethylene glycol-amino, amino-decapolyethylene glycol-amino, amino-undecaprolactone and amino-dodecaprolactone.
[0018] The hydroxybenzoate derivatives are selected from methyl 4-(hydroxymethyl)benzoate, methyl 4-(1-hydroxyethyl)benzoate, methyl 4-(2-hydroxyethyl)benzoate, methyl 4-(3-hydroxy-2-methylpropyl)benzoate, methyl 4-(3-hydroxypropyl)benzoate, methyl 4-(3-hydroxybutyl)benzoate, methyl 4-(4-hydroxybutyl)benzoate, and methyl 4-(4-hydroxybutyl)benzoate, or a combination of two or more thereof.
[0019] The modified diol is prepared by a method comprising the steps of:
[0020] Amino-polyethylene glycol-amino, hydroxybenzoate derivatives and solvent are added into a reaction kettle, the temperature is raised to a reflux state and the reflux state is maintained for reaction, and finally a modified diol is obtained by vacuum distillation.
[0021] The solvent is selected from one or a combination of two or more of methanol, ethanol, water, isopropanol, chloroform and acetone; the reaction time under the reflux state is 5-8h.
[0022] The modifier of the modified thermally conductive filler is one or a combination of two or more of an aminosilane coupling agent, a hydroxyl silane coupling agent, an epoxy silane coupling agent, and an isocyanate silane coupling agent, preferably an aminosilane coupling agent; the thermally conductive filler is selected from one or a combination of two or more of aluminum oxide, aluminum hydroxide, aluminum nitride, boron nitride, and magnesium oxide.
[0023] There is no particular limitation on the preparation method of the modified thermally conductive filler. The method commonly used in the art can be used. Acid solution is added dropwise to a mixture of a coupling agent, water and ethanol to adjust the pH value, the mixture is first placed at room temperature for hydrolysis, the hydrolyzate is added to ethanol, the thermally conductive filler is added, the temperature is increased and the reaction is carried out at a constant temperature, and finally the modified thermally conductive filler is obtained by filtering, washing, drying and grinding. Furthermore, the volume ratio of the coupling agent, water and ethanol in the hydrolyzate is 1-2:1-2:8, and the pH value is adjusted to 3-4. The volume ratio of the hydrolyzate to ethanol is 1-2:20, the mass ratio of the hydrolyzate to the thermally conductive filler is 1-2:20, the room temperature placement time is 1-3h, the temperature is increased to 60-80°C, and the constant temperature reaction time is 3-5h.
[0024] The aminosilane coupling agent is selected from the group consisting of 4-aminobutyltriethoxysilane, 4-amino-3,3-dimethylbutyltrimethoxysilane, N-(2-aminoethyl)-11-aminoundecyltrimethoxysilane, N-[3-(trimethoxysilyl)propyl]n-butylamine, N-methyl-3-aminopropyltrimethoxysilane, 11-aminoundecyltrimethoxysilane, (3-aminopropyl)trimethoxysilane, 11-aminoundecyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-[3-trimethoxysilyl]propyl]-1,6-hexanediamine, and N-ethyl-3-trimethoxysilane-2-methylpropylamine, or a combination of two or more thereof.
[0025] The thermal conductive filler is selected from one or a combination of two or more of aluminum oxide, aluminum hydroxide, aluminum nitride, boron nitride and magnesium oxide.
[0026] The small molecule chain extender is selected from one or a combination of two or more of ethylene glycol, diethylene glycol, 1,4-butanediol, and 1,6-hexanediol.
[0027] The catalyst is an organic tin catalyst, selected from one or a combination of two or more of dibutyltin dilaurate, stannous octoate, and dibutyltin mercaptan.
[0028] The functionality of the polyether polyol is 2-4, and the number average molecular weight is 800-1600 g / mol. The polyether polyol is not particularly limited, and any polyether polyol commonly used in the art can be selected from, but not limited to, one or a combination of two or more of polypropylene glycol, polypropylene oxide triol, and polyoxypropylene tetraol.
[0029] The functionality of the isocyanate is 2-3, and is selected from one or a combination of two or more of 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, diphenylmethane diisocyanate, and triphenylmethane triisocyanate.
[0030] The present invention also provides a method for preparing the polyurethane thermal conductive structural adhesive, comprising the following steps:
[0031] (S1) Weighing the raw material mixed alcohol of component A, small molecule chain extender, and modified thermal conductive filler, adding them into a mixing kettle, vacuum mixing until uniform, then adding a catalyst, vacuum mixing until uniform, and discharging to obtain component A;
[0032] (S2) Weigh the raw materials of component B, isocyanate and modified thermal conductive filler, add them into a mixing kettle, mix them in vacuum until they are uniform, and discharge the materials to obtain component B.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] The present invention provides a modified diol having a benzene ring and an amide bond at both ends, and a polyurethane structural adhesive prepared by using a mixed alcohol raw material compounded with the modified diol and a polyether polyol has good resistance to moisture and heat aging, and does not reduce other mechanical properties of the structural adhesive, providing safety guarantee for the reliable operation of new energy vehicles. The polyurethane thermal conductive structural adhesive of the present invention has good thermal conductivity, shear strength and moisture and heat aging resistance, and can be used for structural bonding of new energy batteries. DETAILED DESCRIPTION
[0035] The present invention will be further described below in conjunction with specific embodiments, but is not limited to the contents of the specification. Unless otherwise specified, the "parts" described in the embodiments of the present invention are all parts by weight. The reagents used are all commercially available reagents in the art.
[0036] Amino-tetraethylene glycol-amino, amino-decaethylene glycol-amino, and amino-dodecaethylene glycol-amino were purchased from Xi'an Kaixin Biotechnology Co., Ltd.
[0037] Al2O3, spherical alumina, average particle size 8-10 μm, Nippon Electric Chemical Industry Co., Ltd.
[0038] Polypropylene oxide triol was purchased from Guangzhou Qixu Chemical Co., Ltd. with a number average molecular weight of 1100 g / mol.
[0039] Preparation of modified thermally conductive filler:
[0040] Preparation Example a1
[0041] To a mixture of N-[3-trimethoxysilyl]propyl]-1,6-hexanediamine, water and ethanol in a volume ratio of 1:1:8, 10 wt% dilute hydrochloric acid solution was added dropwise to adjust the pH to 3, and the mixture was allowed to stand at room temperature for 1 hour for hydrolysis. 10 mL of the hydrolyzed solution was added to 100 mL of ethanol, and then 100 g of Al2O3 was added. The temperature was raised to 80°C and the reaction was kept at a constant temperature for 3 hours. Finally, the mixture was filtered, washed with ethanol 3 times, dried and ground to obtain the modified thermal conductive filler.
[0042] Preparation Example a2
[0043] The rest is the same as Preparation Example a1, except that an equal volume of 3-(2,3-epoxypropyloxy)propyloxysilane is used instead of N-[3-trimethoxysilyl]propyl]-1,6-hexanediamine.
[0044] Preparation of modified diols
[0045] Preparation Example b1
[0046] 1 mol of amino-tetraethylene glycol-amino and 2.15 mol of methyl 4-(hydroxymethyl)benzoate were added to 700 mL of ethanol solvent, the temperature was raised to reflux state and maintained at reflux state for reaction for 8 hours, and finally the modified diol was obtained by vacuum distillation.
[0047] Preparation Example b2
[0048] The rest is the same as Preparation Example b1, except that an equimolar amount of amino-dodecaethylene glycol-amino is used to replace amino-tetraethylene glycol-amino.
[0049] Preparation Example b3
[0050] The rest is the same as Preparation Example b1, except that methyl 4-(4-hydroxybutyl)benzoate is used in an equal molar amount to replace methyl 4-(hydroxymethyl)benzoate.
[0051] Preparation Example b4
[0052] The rest is the same as Preparation Example b1, except that an equimolar amount of amino-decaethylene glycol-amino is used to replace amino-tetraethylene glycol-amino.
[0053] Preparation of polyurethane thermal conductive structural adhesive
[0054] Example 1
[0055] Mixed alcohol: prepared by mixing the modified diol prepared in Preparation Example b1 and polypropylene oxide triol at a mass ratio of 7.5:1;
[0056] S1: Weigh 40 parts of mixed alcohol, 1 part of ethylene glycol, and 80 parts of the modified thermal conductive filler prepared in Preparation Example a1 into a mixing kettle, mix them in vacuum until uniform, then add 0.5 parts of dibutyltin dilaurate and mix them in vacuum until uniform, and then discharge to obtain component A;
[0057] S2: Weigh 32 parts of 2,4-toluene diisocyanate as the raw material of component B and 80 parts of the modified thermal conductive filler prepared in Preparation Example a1, add them into a mixing kettle, heat to 70° C., mix in vacuum until uniform, and obtain component B.
[0058] The weight ratio of component A to component B is 1:1.
[0059] Embodiment 2-4
[0060] The rest is the same as Example 1, except that the modified diols used correspond to Preparation Examples b2-b4 respectively.
[0061] Example 5
[0062] The rest is the same as Example 1, except that the mixed alcohol is a compound of the modified diol prepared in Preparation Example b1 and polypropylene oxide triol in a mass ratio of 5.5:1.
[0063] Example 6
[0064] The mixed alcohol is a compound of the modified diol prepared in Preparation Example b1 and polypropylene oxide triol in a mass ratio of 7.5:1;
[0065] S1: Weigh 30 parts of mixed alcohol, 1 part of ethylene glycol, and 40 parts of the modified thermal conductive filler prepared in Preparation Example a1 into a mixing kettle, mix them in vacuum until uniform, then add 0.5 parts of dibutyltin dilaurate and mix them in vacuum until uniform, and then discharge to obtain component A;
[0066] S2: Weigh 20 parts of 2,4-toluene diisocyanate as the raw material of component B and 40 parts of the modified thermal conductive filler prepared in Preparation Example a1, add them into a mixing kettle, heat to 70°C, mix in vacuum until uniform, and discharge to obtain component B. The weight ratio of component A to component B is 1:1.
[0067] Comparative Example 1
[0068] The rest is the same as Example 1, except that the mixed alcohol is replaced by polypropylene oxide triol.
[0069] The polyurethane thermal conductive structural adhesives prepared in the above Examples 1-6 and Comparative Example 1 were subjected to the following performance tests:
[0070] Thermal conductivity: Thermal conductivity was measured according to ASTM D5470.
[0071] Damp-heat aging: In the damp-heat aging box, the temperature is 85℃, the humidity is 85%, and the aging time is 1000h.
[0072] Shear strength: Referring to the standard GB / T 7124-2008 Determination of tensile shear strength of adhesives (rigid material to rigid material), the single lap tensile shear strength of PET film and PET film, 30003 aluminum alloy and 30003 aluminum alloy was tested. The tensile speed was 2mm / min, and the number of specimens was 5. The maximum shear failure load was recorded as the failure load. The test results were expressed as the arithmetic mean of the tensile shear strength. The tensile shear strength was calculated by dividing the failure load by the shear area. The shear strength loss rate was % before and after the test of wet heat aging.
[0073] Table 1
[0074]
[0075] It can be seen from Table 1 that the polyurethane structural adhesive raw material prepared by the present invention has good thermal conductivity, shear strength and resistance to moisture and heat aging, can be used for structural bonding of new energy batteries, and can provide safety guarantee for the reliable operation of new energy vehicles.
[0076] The above detailed description is a specific description of one feasible embodiment of the present invention. The embodiment is not intended to limit the patent scope of the present invention. Any equivalent implementation or modification that does not deviate from the present invention should be included in the scope of the technical solution of the present invention.
Claims
1. A polyurethane thermal conductive structural adhesive, characterized in that: Including components A and B, The A component comprises the following raw materials in parts by weight: 30-40 parts of mixed alcohol, 0.5-2 parts of small molecule chain extender, 40-80 parts of modified thermal conductive filler, and 0.1-0.5 parts of catalyst. The mixed alcohol is a compound of modified diol and polyether polyol in a mass ratio of 5.5-7.5:
1. The structural formula of the modified diol is shown in Formula I below: Formula I: ; Wherein, n is an integer of 4-12, and R1 and R2 are independently selected from C1-C4 alkylene groups; The B component includes the following raw materials in parts by weight: 20-32 parts of isocyanate, 40-80 parts of modified thermal conductive filler; the functionality of the isocyanate is 2-3; The weight ratio of component A to component B is 1:1-1.2; The modifier of the modified thermally conductive filler is one or a combination of two or more of an aminosilane coupling agent, a hydroxyl silane coupling agent, an epoxy silane coupling agent, and an isocyanate silane coupling agent; the thermally conductive filler is selected from one or a combination of two or more of aluminum oxide, aluminum hydroxide, aluminum nitride, boron nitride, and magnesium oxide.
2. The polyurethane thermal conductive structural adhesive according to claim 1, characterized in that: The modified diol is prepared by amidation reaction of amino-polyethylene glycol-amino and hydroxybenzoate derivatives, and the molar ratio of the two is 1:2.07-2.
15.
3. The polyurethane thermal conductive structural adhesive according to claim 2, characterized in that: The amino-polyethylene glycol-amino group is selected from one or a combination of two or more of amino-tetrapolyethylene glycol-amino, amino-pentapolyethylene glycol-amino, amino-hexapolyethylene glycol-amino, amino-heptapolyethylene glycol-amino, amino-octapolyethylene glycol-amino, amino-nonapolyethylene glycol-amino, amino-decapolyethylene glycol-amino, amino-undecaprolactone and amino-dodecaprolactone; the hydroxybenzoate derivative is selected from one or a combination of two or more of methyl 4-(hydroxymethyl)benzoate, methyl 4-(1-hydroxyethyl)benzoate, methyl 4-(2-hydroxyethyl)benzoate, methyl 4-(3-hydroxy-2-methylpropyl)benzoate, methyl 4-(3-hydroxypropyl)benzoate, methyl 4-(3-hydroxybutyl)benzoate, methyl 4-(4-hydroxybutyl)benzoate and methyl 4-(4-hydroxybutyl)benzoate.
4. The polyurethane thermal conductive structural adhesive according to claim 1, characterized in that: The modified diol is prepared by a method comprising the steps of: Amino-polyethylene glycol-amino, hydroxybenzoate derivatives and solvent are added into a reaction kettle, the temperature is raised to a reflux state and the reflux state is maintained for reaction, and finally a modified diol is obtained by vacuum distillation.
5. The polyurethane thermal conductive structural adhesive according to claim 4, characterized in that: The solvent is selected from one or a combination of two or more of methanol, ethanol, water, isopropanol, chloroform and acetone; the reaction time under the reflux state is 5-8h.
6. The polyurethane thermal conductive structural adhesive according to claim 1, characterized in that: The functionality of the polyether polyol is 2-4, and the number average molecular weight is 800-1600 g / mol.
7. The polyurethane thermal conductive structural adhesive according to claim 1, characterized in that: The isocyanate is selected from one or a combination of two or more of 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, diphenylmethane diisocyanate, and triphenylmethane triisocyanate.
8. The method for preparing the polyurethane thermal conductive structural adhesive according to any one of claims 1 to 7, comprising the following steps: (S1) weighing the raw material mixed alcohol of component A, small molecule chain extender, and modified thermal conductive filler, adding them to a mixing kettle, vacuum mixing until uniform, then adding a catalyst, vacuum mixing until uniform, and discharging to obtain component A; (S2) Weighing the raw materials of component B, isocyanate and modified thermal conductive filler, adding them into a mixing kettle, mixing them in vacuum until they are uniform, and discharging the materials to obtain component B.