Preparation method and application of a 3D printable hydrogel precursor liquid and a highly conductive and elastic hydrogel
By using the reaction and freeze-thaw cycle technology of polyvinyl alcohol, ethylene glycol, EDOT and other materials in the hydrogel, a highly conductive and highly elastic hydrogel is formed, which solves the problem of difficult to balance mechanical properties and conductive properties in the existing technology. Efficient preparation of hydrogels with excellent stretch and conductive properties is achieved, which is suitable for wearable devices and human movement detection.
Patent Information
- Application Number
- CN202310754767.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-26
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-06-26
AI Technical Summary
It is difficult to efficiently prepare hydrogel materials with both stable mechanical properties and high electrical conductivity using existing technology, especially the problem of decreased electrical conductivity when frozen at low temperatures.
The 3D printable hydrogel precursor liquid is prepared using a mixed reaction of polyvinyl alcohol, ethylene glycol, EDOT, acrylamide, initiator and N,N'-methylenebisacrylamide, and freeze-thaw cycle technology Forming a highly conductive and highly elastic hydrogel, PEDOT can be evenly interspersed in the PVA/PAM dual network system.
An antifreeze hydrogel material with high stretchability and high conductivity was obtained, which can maintain conductive properties at low temperatures and build complex structures through 3D printing technology, which is suitable for wearable devices and human movement detection.
Smart Images

Figure CN116655953B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of functional hydrogels, and in particular to a preparation method and application of a 3D printable hydrogel precursor liquid and a highly conductive and elastic hydrogel. Background Art
[0002] As artificial intelligence technology matures, flexible electronic devices have attracted widespread attention and research in artificial intelligence, electronic skin, human health monitoring and human-computer interaction. In flexible wearable electronic devices, sensors are an important component that can convert external physical or environmental stimuli into detectable electrical signals. Flexible wearable sensors also have excellent flexibility, high sensitivity and fast sensing functions. They can be installed on clothes or even directly attached to the surface of human skin to achieve long-term monitoring of human movement and physiological activities, such as joint bending, speaking, breathing, pulse and skin temperature. Hydrogels have broad application prospects in the field of flexible electronics due to their excellent flexibility, ion transport and adjustable mechanical properties. In recent years, conductive hydrogel electronic materials designed with hydrogel as the matrix have developed rapidly and have shown broad application prospects in the field of flexible electronics such as electronic skin, flexible sensors and flexible supercapacitors. Conductive hydrogels are an emerging class of hydrogels that combine a hydrophilic matrix and a conductive filler, such as metal nanoparticles, conductive polymers or carbon-based materials, adding new properties to the essence of hydrogels, including flexibility, stretchability, conductivity, etc. Among them, poly(3,4-ethylenedioxythiophene) (PEDOT), a derivative of polythiophene, is an ideal candidate material for the development of bioelectronic devices. It is attractive because of its high conductivity and good biocompatibility in the oxidized state, excellent conductivity, and excellent electrochemical stability. Therefore, compounding polymer hydrogel with PEDOT material can not only improve the mechanical properties of the hydrogel, but also give the hydrogel excellent conductive properties. These properties make it one of the most promising candidate materials for flexible wearable electronic devices among the many new flexible materials that have emerged in recent years.
[0003] However, the conductive hydrogels reported so far have problems such as poor mechanical properties and loss of conductivity when frozen at low temperatures. The methods and properties of the prepared hydrogels are often unsatisfactory. For example, Peng Y et al. introduced PEDOT, PAA and glycerol into the PVA hydrogel network by in-situ polymerization and two-step immersion, and successfully prepared a high-strength antifreeze and moisture-proof hydrogel strain sensor. The resulting composite hydrogel has good conductivity (~0.95S / m) and high mechanical strength (~3.6MPa). The gel remains flexible and stretchable at low temperatures and responds well to multiple strains and subtle human movements. Their research shows that EDOT can be evenly dispersed in PVA solution, but this method of first polymerization and then two immersions results in more complicated steps, and the immersion method will lead to a decrease in conductive and mechanical properties (Peng Y, Pi M, Zhang X, et al. High strength, antifreeze, and moisturizing conductive hydrogel for human-motion detection [J]. Polymer, 2020, 196: 122469.). Sun et al. used physically cross-linked gelatin, chemically cross-linked PAM and PEDOT:PSS as raw materials and used a double network method to prepare stretchable conductive hydrogel as a conductive element. The conductive element has an ultra-wide strain sensing range (0% to 2850%), a short response time (200ms) and excellent durability and repeatability (1200 cycles), and a sensitivity of 1.58, which can effectively identify complex human body movements. The study is a hydrogel prepared by a rigid network gelatin and a flexible network PAM double network and a conductive material PEDOT:PSS. The presence of this double network gives the hydrogel good stretchability, but the presence of PSS in the conductive material PEDOT:PSS weakens the conductive properties of PEDOT (H.Sun, Y.Zhao, C.Wang, et al. Ultra-stretchable, durable and conductive hydrogel with hybrid double network as high performance strain sensor and stretchabletriboelectric nanogenerator [J]. Nano Energy, 2020, 76: 105035-105047.). Peng W et al. prepared a double network organic hydrogel by doping conductive ZnSO4 into polyvinyl alcohol-polyacrylamide (PVA-PAM) double network hydrogel and then immersing it in a mixed solvent of ethylene glycol (EG) and H2O.The hydrogel has high electrical conductivity (0.44S / m), excellent fatigue resistance, outstanding moisturizing ability and excellent antifreeze ability, but the use of ionic liquid conductivity is prone to the risk of ion leakage when the hydrogel is deformed (Peng W, Han L, Gao Y, et al. Flexible organohydrogel ionic skin with Ultra-Low temperature freezing resistance and Ultra-Durable moisture retention [J]. Journal of Colloid and Interface Science, 2022, 608: 396-404.).
[0004] Therefore, how to efficiently prepare hydrogel materials that have both stable mechanical properties and high conductive properties has become an urgent problem that needs to be solved by technicians in this field. Summary of the invention
[0005] In view of this, the present invention provides a 3D printable hydrogel precursor liquid and a preparation method and application of a highly conductive and elastic hydrogel, the purpose of which is to solve the technical problem that the prior art cannot efficiently prepare a hydrogel material with both stable mechanical properties and high conductive properties.
[0006] In order to achieve the above object, the present invention adopts the following technical solution:
[0007] The present invention provides a method for preparing a 3D printable hydrogel precursor liquid, comprising the following steps:
[0008] Polyvinyl alcohol solution, ethylene glycol aqueous solution, EDOT, acrylamide, initiator, N,N'-methylenebisacrylamide and tetramethylethylenediamine are mixed and reacted to obtain a 3D printable hydrogel precursor liquid.
[0009] Furthermore, the volume ratio of the polyvinyl alcohol solution, the ethylene glycol aqueous solution and tetramethylethylenediamine is 8-12 mL: 10-20 mL: 8-12 μL;
[0010] The mass ratio of EDOT, acrylamide, initiator and N,N'-methylenebisacrylamide is 0.25-1.5 g: 4-5 g: 0.9-3.4 g: 0.001-0.01 g;
[0011] The mass volume ratio of the EDOT and ethylene glycol aqueous solution is 0.25-1.5 g:10-20 mL.
[0012] Furthermore, the mass concentration of the PVA solution is 10-20%; the mass concentration of the ethylene glycol aqueous solution is 30-50%.
[0013] Furthermore, the reaction temperature is 50-90° C., and the reaction time is 6-12 hours.
[0014] Furthermore, the initiator is ammonium persulfate and / or potassium persulfate.
[0015] The present invention provides a 3D printable hydrogel precursor liquid prepared by the above preparation method.
[0016] The present invention also provides a method for preparing a highly conductive and highly elastic hydrogel using the above-mentioned 3D printable hydrogel precursor liquid, comprising the following steps:
[0017] The 3D printable hydrogel precursor liquid is subjected to freeze-thaw cycles to obtain a highly conductive and elastic hydrogel; the number of freeze-thaw cycles is ≥3.
[0018] The invention provides a high-conductivity and high-elasticity hydrogel prepared by the above-mentioned preparation method.
[0019] The present invention also provides the use of the highly conductive and highly elastic hydrogel prepared by the above method in electrocardiographic electrodes or wearable devices.
[0020] It can be seen from the above technical solution that compared with the prior art, the beneficial effects of the present invention are as follows:
[0021] (1) The present invention prepares an antifreeze double network hydrogel by in-situ polymerization, realizes the uniform interpenetration of PEDOT in the PVA / PAM double network system composed of rigid PVA and flexible PAM, thereby simultaneously improving the tensile properties and conductive properties of the hydrogel, and obtaining an antifreeze hydrogel material with high elongation and high conductivity, which can be used in wearable devices;
[0022] (2) The present invention introduces a binary solvent of water / ethylene glycol and uses a simple one-pot method to complete the gelation of the precursor solution, and then achieves efficient preparation of the hydrogel through freeze-thaw cycles;
[0023] (3) The 3D printable hydrogel precursor liquid prepared by the present invention exhibits excellent fluidity, which is crucial for constructing complex structures by 3D printing. A simplified 3D printed hydrogel sensor model was prepared on a flexible substrate, which has the potential to be applied in detecting human body movements. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 A shape diagram of the 3D printable hydrogel precursor liquid prepared in Example 1 printed by 3D printing;
[0025] Figure 2 A comparison chart of the conductive properties of the highly conductive and highly elastic hydrogels prepared in Examples 1 to 6;
[0026] Figure 3 A comparison chart of the tensile properties of the highly conductive and highly elastic hydrogels prepared in Examples 1 to 6;
[0027] Figure 4 The stress-strain curve of the highly conductive and highly elastic hydrogel prepared in Example 1 after continuous compression for 20 times;
[0028] Figure 5 This is a DSC test curve of the highly conductive and highly elastic hydrogel prepared in Example 1;
[0029] Figure 6 This is a diagram showing the effect of using the highly conductive and highly elastic hydrogel prepared in Example 1 in an ECG electrode;
[0030] Figure 7 This is a diagram showing the effect of using the highly conductive and highly elastic hydrogel prepared in Example 1 in a wearable sensor at different movement amplitudes;
[0031] Figure 8 A diagram showing a device for monitoring ECG signals and recording ECG waveforms using the highly conductive and highly elastic hydrogel prepared in Example 1 as an electrode;
[0032] Fig. 9 This is a picture showing the effect of using the highly conductive and highly elastic hydrogel prepared in Example 1 as a sensor to detect cheek muscle movements;
[0033] Fig.10 This is a diagram showing the effect of using the highly conductive and highly elastic hydrogel prepared in Example 1 as a sensor to detect repeated frowning-brow center movements;
[0034] Fig.11 This is a diagram showing the effect of using the highly conductive and highly elastic hydrogel prepared in Example 1 as a sensor to detect repeated frowning-eyebrow movements;
[0035] Fig.12 This is a diagram showing the effect of using the highly conductive and highly elastic hydrogel prepared in Example 1 as a sensor to detect the hand clenching and expanding motion;
[0036] Fig.13 This is a diagram showing the effect of using the highly conductive and highly elastic hydrogel prepared in Example 1 as a sensor to detect finger bending;
[0037] Fig.14 This is a diagram showing the effect of using the highly conductive and highly elastic hydrogel prepared in Example 1 as a sensor to detect arm bending;
[0038] Fig.15 This is a diagram showing the effect of using the highly conductive and highly elastic hydrogel prepared in Example 1 as a sensor to detect knee bending;
[0039] Fig.16 This is a diagram showing the effect of using the highly conductive and highly elastic hydrogel prepared in Example 1 as a sensor to detect wrist bending. DETAILED DESCRIPTION
[0040] The present invention provides a method for preparing a 3D printable hydrogel precursor liquid, comprising the following steps:
[0041] Polyvinyl alcohol solution, ethylene glycol aqueous solution, EDOT, acrylamide, initiator, N,N'-methylenebisacrylamide and tetramethylethylenediamine are mixed and reacted to obtain a 3D printable hydrogel precursor liquid.
[0042] In the present invention, polyvinyl alcohol (C2H4O) n It is a water-soluble polymer material. There are O atoms in the highly polar hydroxyl group (-OH) in the molecular chain. It has strong adhesion, good mechanical properties and biocompatibility, and can form a three-dimensional network structure through self-crosslinking. Polyacrylamide (C3H5NO) n It is a linear organic high molecular polymer with a large number of amide groups on the molecular chain, which can form associative hydrogen bonds with surrounding molecules. It has active chemical properties, a typical three-dimensional network structure, good adhesion and thickening properties, no toxic side effects, and stable performance. Double network gel can achieve the complementary advantages of polyvinyl alcohol (PVA) and polyacrylamide (PAM). The two network ratios are reasonably adjusted and combined with the amount of solvent. The mixed solvent of water and ethylene glycol is used to replace the pure water solvent. The strong hydrogen bonding between water and ethylene glycol makes the water molecules firmly fixed in the hydrogel network to prevent the freezing and volatilization of water molecules. The conductive material is prepared by in-situ polymerization to overcome stress concentration and obtain a hydrogel with improved basic performance, achieving a stable balance between multiple properties, thereby constructing a stable high-performance double network hydrogel carrier transport system. Compared with single network structure hydrogels, double cross-linked networks can provide more energy dissipation.
[0043] PEDOT has the following characteristics: (1) high conductivity, which can reach about 1000S / cm after doping; (2) good solubility, and the solubility of polythiophene increases with the increase of substituted alkyl; (3) stable chemical properties, and its chemical properties are not easily affected by environmental changes under acidic or alkaline conditions; (4) can be used as an electrode material. The introduction of EDOT (3,4-ethylenedioxythiophene) can enhance the mechanical properties of hydrogels on the one hand, and at the same time, it also provides hydrogels with excellent conductivity.
[0044] In the present invention, the volume ratio of the polyvinyl alcohol solution, the ethylene glycol aqueous solution and tetramethylethylenediamine is 8-12 mL: 10-20 mL: 8-12 μL, preferably 9-11 mL: 14-17 mL: 9-11 μL, and more preferably 10 mL: 15 mL: 10 μL;
[0045] The mass ratio of EDOT, acrylamide, initiator and N,N'-methylenebisacrylamide is 0.25-1.5g:4-5g:0.9-3.4g:0.001-0.01g, preferably 0.5-1.25g:4.2-4.8g:1.46-2.9g:0.002-0.008g, more preferably 0.75-1.0g:4.4-4.6g:1.94-2.43g:0.004-0.006g;
[0046] The mass volume ratio of the EDOT and ethylene glycol aqueous solution is 0.25-1.5 g:10-20 mL, preferably 0.5-1.25 g:14-17 mL, and more preferably 0.75-1.0 g:15 mL.
[0047] In the present invention, the mass concentration of the PVA solution is 10-20%, preferably 13-17%, and more preferably 14.27%; the mass concentration of the ethylene glycol aqueous solution is 30-50%, preferably 35-45%, and more preferably 40%.
[0048] In the present invention, the reaction temperature is 50 to 90° C., preferably 60 to 80° C., and more preferably 70 to 75° C.; the reaction time is 6 to 12 h, preferably 7 to 11 h, and more preferably 8 to 10 h.
[0049] In the present invention, the initiator is ammonium persulfate and / or potassium persulfate, preferably ammonium persulfate.
[0050] The present invention provides a 3D printable hydrogel precursor liquid prepared by the above preparation method.
[0051] The present invention also provides a method for preparing a highly conductive and highly elastic hydrogel using the above-mentioned 3D printable hydrogel precursor liquid, comprising the following steps:
[0052] The 3D printable hydrogel precursor liquid is subjected to freeze-thaw cycles to obtain a highly conductive and elastic hydrogel; the number of freeze-thaw cycles is ≥3, preferably ≥4, and more preferably ≥5.
[0053] The invention provides a high-conductivity and high-elasticity hydrogel prepared by the above-mentioned preparation method.
[0054] The present invention also provides the use of the highly conductive and highly elastic hydrogel prepared by the above method in electrocardiographic electrodes or wearable devices.
[0055] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0056] Example 1
[0057] PVA powder was dissolved in deionized water, and magnetically stirred at 90°C for 3 hours until completely dissolved to obtain a polyvinyl alcohol solution with a mass concentration of 14.27%, and then the polyvinyl alcohol solution was cooled to room temperature. 10 mL of polyvinyl alcohol solution was added to 15 mL of 40% ethylene glycol aqueous solution and stirred for 10 minutes to mix evenly, and then 0.25 g of EDOT, 4.9 g of acrylamide, 0.98 g of ammonium persulfate and 0.002 g of N, N'-methylenebisacrylamide were added. 10 μL of tetramethylethylenediamine was added during the stirring and mixing process, and then reacted at 50°C for 6 hours to obtain a 3D printable hydrogel precursor liquid.
[0058] Figure 1 The shape diagram of the 3D printable hydrogel precursor liquid prepared in this embodiment is printed by 3D printing. Figure 1 It can be seen that the 3D printable hydrogel precursor liquid prepared by the present invention has good fluidity.
[0059] The 3D printable hydrogel precursor liquid was freeze-thawed for 5 times to obtain a highly conductive and elastic hydrogel.
[0060] Example 2
[0061] The steps were the same as those in Example 1, except that the amount of EDOT used was 0.5 g and the amount of ammonium persulfate used was 1.46 g to prepare a highly conductive and elastic hydrogel.
[0062] Example 3
[0063] The steps were the same as those in Example 1, except that the amount of EDOT used was 0.75 g and the amount of ammonium persulfate used was 1.94 g to prepare a highly conductive and elastic hydrogel.
[0064] Example 4
[0065] The steps were the same as those in Example 1, except that the amount of EDOT used was 1.0 g and the amount of ammonium persulfate used was 2.43 g to prepare a highly conductive and elastic hydrogel.
[0066] Example 5
[0067] The steps were the same as those in Example 1, except that the amount of EDOT used was 1.25 g and the amount of ammonium persulfate used was 2.90 g to prepare a highly conductive and elastic hydrogel.
[0068] Example 6
[0069] The steps were the same as those in Example 1, except that the amount of EDOT used was 1.5 g and the amount of ammonium persulfate used was 3.39 g to prepare a highly conductive and elastic hydrogel.
[0070] Figure 2 The conductive properties of the highly conductive and highly elastic hydrogels prepared in Examples 1 to 6 are compared. Figure 2 It can be obtained that the highly conductive and highly elastic hydrogel prepared by the present invention has a relatively high conductivity, which can reach up to 32.29 S / m.
[0071] Figure 3 The tensile properties of the highly conductive and highly elastic hydrogels prepared in Examples 1 to 6 are compared. Figure 3 It can be obtained that the highly conductive and highly elastic hydrogel prepared by the present invention has excellent stretchability, which can reach up to 1050%.
[0072] Figure 4 The stress-strain curve of the highly conductive and highly elastic hydrogel prepared in Example 1 after 20 consecutive compressions is shown in FIG. Figure 4 It can be seen that the highly conductive and highly elastic hydrogel prepared by the present invention has excellent stability.
[0073] Figure 5 This is the DSC test curve of the highly conductive and highly elastic hydrogel prepared in Example 1. Figure 5 It can be seen that the hydrogel prepared by the present invention can work in harsh environments, and the antifreeze performance can reach -42°C.
[0074] Figure 6 The effect diagram of the use of the highly conductive and highly elastic hydrogel prepared in Example 1 in an ECG electrode shows that it can detect heart rate changes very well.
[0075] Figure 7 The effect diagram of the use of the highly conductive and highly elastic hydrogel prepared in Example 1 in a wearable sensor under different movement amplitudes shows that it has a good response and can detect the movement of various parts of the human body.
[0076] Figure 8 The highly conductive and highly elastic hydrogel prepared in Example 1 is used as an electrode to monitor ECG signals and record ECG waveforms. Figure B is an ECG test signal diagram, Figure C is a local enlarged diagram of the ECG test signal, and Figure D is an ECG test signal peak mark diagram. Figure 8It can be seen that the hydrogel electrode can accurately reflect the beating of the human heart when it is at rest. The existence of P wave, QRS complex and T wave can be clearly and continuously seen from the spectrum, and the heartbeat waveform can be clearly and continuously output. The hydrogel as an electrocardiogram sensor electrode has sufficient flexibility, fits seamlessly with the skin and does not fall off, and can accurately reflect the beating of the human heart.
[0077] The muscle movements caused by cheek bulging were monitored by attaching the two ends of the hydrogel-based sensor to a person's cheek. When the wearable sensor was attached to the volunteer's face, the cyclical bulging and relaxation of the face could be detected with a repeatable and stable signal ( Fig. 9 By attaching the hydrogel-based sensor to the forehead, regular and repeatable resistance signals evoked during alternating normal and frowning movements can be collected ( Fig.10 and Fig.11 Our hydrogel sensor can not only monitor the subtle muscle movements mentioned above, but also track the bending movements produced by major joints such as wrists, knuckles, elbows, and knees. For example, the resistance signal caused by hand bending can be collected by fixing the hydrogel-based sensor on the surface of the palm ( Fig.12 ), fixed on the wrist to collect wrist flexion ( Fig.16 ) induced resistance signals. In addition, by adhering the hydrogel-based sensor to the right index finger, the resistance response induced during the bending-release cycle of the index finger from 30° to 90° was collected ( Fig.13 Similar elbow and knee movements were tracked by attaching hydrogel-based sensors to the corresponding joints (flexed and extended to varying degrees) ( Fig.14 ). The reproducibility of the resistance signal at a specific joint bending angle demonstrates the good working stability of the hydrogel-based sensor. As the bending angle increases, the resistance output increases, which is attributed to the increase in the deformation length of the hydrogel. The identification of joint motion angles helps to achieve remote real-time manipulation of robot movements, demonstrating the prospects of this hydrogel-based sensor in artificial intelligence and human-computer interaction. By fixing the hydrogel, the human body's motion state can be monitored - based on the sensor on the knee, such as Fig.15 These results indicate that exercise behavior can be converted into real-time resistance signals by the hydrogel sensor prepared by the present invention, which is helpful for realizing exercise monitoring.
[0078] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a 3D printable hydrogel precursor liquid, characterized in that: The following steps are involved: The polyvinyl alcohol solution, the ethylene glycol aqueous solution, EDOT, acrylamide, an initiator, N,N'-methylenebisacrylamide and tetramethylethylenediamine are mixed and reacted to obtain a 3D printable hydrogel precursor liquid; The volume ratio of the polyvinyl alcohol solution, the ethylene glycol aqueous solution and tetramethylethylenediamine is 8-12 mL: 10-20 mL: 8-12 μL; The mass ratio of EDOT, acrylamide, initiator and N,N'-methylenebisacrylamide is 0.25-1.5 g: 4-5 g: 0.9-3.4 g: 0.001-0.01 g; The mass volume ratio of the EDOT and ethylene glycol aqueous solution is 0.25-1.5 g:10-20 mL; The reaction temperature is 50-90°C and the reaction time is 6-12h; The initiator is ammonium persulfate and / or potassium persulfate.
2. The preparation method according to claim 1, characterized in that: The mass concentration of the PVA solution is 10-20%; the mass concentration of the ethylene glycol aqueous solution is 30-50%.
3. A 3D printable hydrogel precursor liquid prepared by the preparation method according to claim 1 or 2.
4. A method for preparing a highly conductive and highly elastic hydrogel using the 3D printable hydrogel precursor liquid according to claim 3, characterized in that: The following steps are involved: The 3D printable hydrogel precursor liquid is subjected to freeze-thaw cycles to obtain a highly conductive and elastic hydrogel; the number of freeze-thaw cycles is ≥3.
5. The highly conductive and highly elastic hydrogel prepared by the preparation method according to claim 4.
6. Use of the highly conductive and highly elastic hydrogel according to claim 5 in electrocardiographic electrodes or wearable devices.