Preparation method of ultra-thin bionic coating and its product and application
By adjusting the pH value in the buffer solution, an ultra-thin bionic coating in an acidic environment is formed, which solves the problems of uneven and unstable bionic coating of mussels, and achieves efficient and uniform coating preparation and high enzyme loading. Acid resistance.
Patent Information
- Application Number
- CN202310661022.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-06
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-06-06
AI Technical Summary
The mussel bionic coating has problems such as unevenness, long reaction time and unstable, which leads to uneven and unstable deposition on the surface of the material, affecting its application range and performance.
By adjusting the pH value to an acidic environment in a buffer solution, the reaction system of polyphenol compounds and amino compounds is carried out under acidic conditions, forming an ultra-thin bionic coating with a thickness of 0.5-1.5 nm, overcoming uneven and unstable Disadvantages, the preparation of bionic coatings with short reaction time, thin coating thickness and uniform coating are achieved.
A ultra-thin bionic coating with short reaction time, thin coating thickness, uniform stability is obtained, which can adhere evenly to the surface of porous materials without affecting light transmission performance, and achieve high enzyme loading during enzyme immobilization. High activity and strong acid resistance.
Smart Images

Figure BDA0004268987090000101 
Figure BDA0004268987090000111 
Figure BDA0004268987090000151
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of material surface / interface modification, and relates to a preparation method of an ultra-thin bionic coating, a product and an application thereof. Background Art
[0002] Surface coatings have been widely used to change the physical / chemical properties of materials, give materials the ability to be functionalized, or enhance their anti-pollution and anti-corrosion properties. Lee et al. used dopamine as a building monomer and prepared polydopamine coatings that can be applied to almost all inorganic and organic materials under weakly alkaline oxygen-containing conditions (Lee H, Dellatore SM, Miller WM, et al. Mussel-inspired surface chemistry for multifunctional coatings [J]. Science, 2007, 318 (5849): 426-430). In recent years, due to the high price of dopamine and the possibility of neurotoxicity, a system of mussel biomimetic coatings constructed from phenolamine binary components has gradually been derived.
[0003] The presence of a large number of phenolic hydroxyl groups and their oxidation products, quinone groups and amino groups, on the mussel biomimetic coating gives it a strong nonspecific adhesion ability. At the same time, these active groups also allow it to act as a medium for secondary reactions, so it has become one of the most commonly used surface modification methods. Compared with other carrier activation methods, the mussel biomimetic coating can easily modify the surface of materials such as microspheres, polymer separation membranes and screens, and achieve a higher enzyme loading and expand the application range of biological enzymes.
[0004] However, the surface modification based on mussel biomimetic coatings still faces some challenges: the electrostatic interaction between phenolic hydroxyl groups and amino groups easily leads to the rapid aggregation of phenolamine components. Under the joint promotion of covalent and non-covalent effects, a large number of aggregates will quickly form in the coating solution, resulting in the particles deposited on the surface of the substrate being too large and uneven in size; secondly, due to the uneven coating formation process, the coating thickness can only be increased by increasing the coating time to achieve the purpose of obtaining a complete coating, but because the coating is too thick, the unstable non-covalent interaction between the coatings will cause it to partially fall off, reducing the stability of the coating. Therefore, the current mussel biomimetic coatings still have the limitations of unevenness, long reaction time and instability.
[0005] In order to solve the above problems, many studies have proposed strategies to enhance the oxidative environment in the coating solution, including adding chemical oxidants and biological oxidants to the coating solution to further accelerate the coating deposition rate under the initiation of oxidants. Wei et al. increased the deposition rate of polydopamine coating from 2.1 nm / h to 35 nm / h by adding ammonium persulfate oxidant (Wei, Q.; Zhang, F.; Li, J.; Li, B.; Zhao, C. Oxidant-Induced Dopamine Polymerization for Multifunctional Coatings. Polym. Chem. 2010, 1 (9), 1430); Qiu et al. used laccase to accelerate the oxidation of phenolic hydroxyl groups, which also promoted the rapid formation of the coating (Qiu, W.-Z.; Zhong, Q.-Z.; Du, Y.; Lv, Y.; Xu, Z.-K. Enzyme-Triggered Coatings of Tea Catechins / Chitosan for Nanofiltration Membranes with High Performance. Green Chem. 2016, 18 (23), 6205–6208). The addition of oxidants enhances the covalent interaction between phenolic amine components and improves the stability of the main structure of the coating. However, the excellent adhesion of mussel biomimetic coatings comes from the presence of a large number of phenolic hydroxyl groups. The process of its formation is first adhesion and then gradual deposition. Excessive oxidation will weaken its interfacial adhesion. In addition, oxidants will cause the particle size of aggregates in the coating solution to increase further, so enhancing the oxidative environment cannot solve its uneven and unstable defects. In addition, the current standard for evaluating the coating formation speed is too single, and only the coating thickness is taken into consideration. The uniformity of the coating should also be included in the measurement criteria. Summary of the invention
[0006] In view of the deficiencies of the prior art, the object of the present invention is to provide a method for preparing an ultra-thin bionic coating and its product and application.
[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a method for preparing an ultra-thin bionic coating, the preparation method comprising:
[0009] A buffer solution containing polyphenol compounds is mixed with an alcohol solution containing amino compounds, and simultaneously or subsequently contacted with a matrix material to deposit on the surface of the matrix material, thereby obtaining an ultrathin bionic coating attached to the surface of the matrix material; the buffer solution is an acidic buffer solution.
[0010] The present invention creatively adjusts the reaction system of polyphenol compounds and amino compounds to an acidic environment, that is, adjusts the pH value of the buffer solution to acidic, thereby overcoming the drawbacks of unevenness, long reaction time and instability of the bionic coating, and simply and efficiently obtains a bionic coating with short reaction time, thin and uniform coating thickness and good stability. The "ultra-thin" involved in the present invention means that the thickness of the bionic coating is only 0.5-1.5nm.
[0011] Preferably, the polyphenol compound comprises any one of catechol, pyrogallol, gallic acid, tannic acid, catechin, catechin gallate or gallocatechin.
[0012] Preferably, the amino compound includes any one or a combination of at least two of ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, 3-aminopropyltriethoxysilane, 3-(2-aminoethylamino)propyltriethoxysilane or polyethyleneimine.
[0013] Preferably, the matrix material is selected from inorganic materials, metallic materials or organic materials.
[0014] One of the advantages of the bionic coating involved in the present invention is its excellent interface adhesion, which makes it have a wide range of applications and can be adhered and deposited on almost all types of materials, which are not particularly limited here, and typically include inorganic materials, metal materials, and organic materials.
[0015] Preferably, the buffer solution is selected from any one of acetic acid-sodium acetate buffer solution, citric acid-sodium citrate buffer solution, glycine-hydrochloric acid buffer solution or disodium hydrogen phosphate-sodium dihydrogen phosphate, or a combination of at least two thereof.
[0016] Preferably, the pH value of the buffer solution is 3-6, such as pH=3, pH=3.2, pH=3.5, pH=3.7, pH=4.0, pH=4.2, pH=4.5, pH=5, pH=5.5, pH=5.8, pH=6.0, etc. Other specific values within this numerical range can be selected and will not be described one by one here. A further preferred pH value is 3-4.5.
[0017] In the preparation method of the present invention, the pH value of the buffer solution is controlled within the range of 3-6, which can shorten the formation time of the bionic coating, make the coating thinner and more uniform, and improve the stability. When the pH value is lower than 3, the oxidation of phenolic hydroxyl groups may be directly inhibited, and the phenolamine coating cannot be formed; and when the pH value is higher than 6, the oxidation rate of phenolic hydroxyl groups is too fast, which will cause the adhesion of the fixed coating to deteriorate, and the electrostatic interaction between phenolic hydroxyl groups and amino groups is strong, and the aggregate particle size in the coating solution is too large, resulting in uneven and thick deposited coatings and poor stability. Furthermore, the effect is better when the pH value is controlled within the range of 3-4.5.
[0018] Preferably, the concentration of the polyphenol compound in the buffer solution is 0.5-5 g / L, for example, 0.5 g / L, 1 g / L, 1.5 g / L, 2 g / L, 2.5 g / L, 3 g / L, 3.5 g / L, 4 g / L, 4.5 g / L, 5 g / L, etc.
[0019] Preferably, the concentration of the amino compound in the alcohol solution is 5-10 g / L, for example, 5 g / L, 5.5 g / L, 6 g / L, 6.5 g / L, 7 g / L, 7.5 g / L, 8 g / L, 8.5 g / L, 9 g / L, 9.5 g / L, 10 g / L, etc.
[0020] Preferably, the volume ratio of the buffer solution containing polyphenol compounds to the alcohol solution containing amino compounds is (3-10):1, for example 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1, 10:1, etc., and the more preferred volume ratio is (7-9):1.
[0021] Other specific point values within the above numerical range can be selected and will not be described in detail here.
[0022] In the preparation method involved in the present invention, the addition ratio of polyphenol compounds to amino compounds also affects the properties of the prepared bionic coating. Therefore, by adjusting the ratio of phenolamines, more phenolic hydroxyl groups and quinone groups are given to the coating surface while ensuring that the coating reaches a certain degree of crosslinking.
[0023] Preferably, the alcohol solution comprises any one of anhydrous methanol, anhydrous ethanol or anhydrous 1-propanol, or a combination of at least two thereof.
[0024] Preferably, the contacting method includes direct mixing and contacting with the matrix material, or spin coating, spray coating, or flowing through the matrix material.
[0025] Preferably, the contacting is carried out at a temperature of 10-35°C, such as 10°C, 15°C, 20°C, 22°C, 24°C, 25°C, 30°C, 35°C, etc., preferably 20-25°C.
[0026] Preferably, the contact time is 5-60 min, for example, 5 min, 10 min, 15 min, 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min, 60 min, etc., preferably 25-35 min.
[0027] Other specific point values within the above numerical range can be selected and will not be described in detail here.
[0028] In a second aspect, the present invention provides an ultra-thin bionic coating prepared according to the method for preparing the ultra-thin bionic coating described in the first aspect.
[0029] In a third aspect, the present invention provides a method for preparing the ultrathin bionic coating according to the first aspect or an application of the ultrathin bionic coating according to the second aspect in preparing dye adsorption materials, membrane separation materials, catalytic materials, biopharmaceutical materials or anti-pollution materials.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] The present invention creatively adjusts the reaction system of the polyphenol compound and the amino compound to an acidic environment, that is, adjusts the pH value of the buffer solution to acidity, thereby overcoming the drawbacks of unevenness, long reaction time and instability of the bionic coating, and simply and efficiently obtains a bionic coating with short reaction time, thin and uniform coating thickness and good stability. The bionic coating prepared by the present invention has a thickness of only 0.5-1.5 nm, can be uniformly adhered and modified on the pore surface of the porous material, does not affect the light transmission performance of the light-transmitting matrix material, and can achieve high enzyme loading, high activity, strong acid resistance and stability when used for enzyme immobilization. DETAILED DESCRIPTION
[0032] In order to further explain the technical means and effects adopted by the present invention, the technical solution of the present invention is further described below in conjunction with the preferred embodiments of the present invention, but the present invention is not limited to the scope of the embodiments.
[0033] The 3-(2-aminoethylamino)propyltriethoxysilane involved in the following examples is a product purchased from Aladdin with a model number of 5089-72-5; tannic acid is a product purchased from Sigma with a model number of 1401-55-4; tetraethylenepentamine is a product purchased from Aladdin with a model number of 4961-41-5; and gallic acid is a product purchased from Sigma with a model number of 149-91-7.
[0034] Example 1
[0035] This embodiment provides a method for preparing a bionic coating, which is as follows:
[0036] Silicon wafer is selected as the matrix material, and the raw materials are tannic acid and 3-(2-aminoethylamino)propyltriethoxysilane.
[0037] Tannic acid was dissolved in 20 mL of 50 mM acetic acid-sodium acetate buffer (pH=3.6) to obtain a tannic acid buffer with a concentration of 2 g / L, and 3-(2-aminoethylamino)propyltriethoxysilane was dissolved in anhydrous ethanol (analytical grade) to obtain a 3-(2-aminoethylamino)propyltriethoxysilane ethanol solution with a concentration of 10 g / L; the tannic acid buffer and the 3-(2-aminoethylamino)propyltriethoxysilane ethanol solution were then mixed at a solution volume ratio of 8:1 to obtain a mixed solution; a silicon wafer was placed in the mixed solution, stirred at 150 rpm for 30 min at 25° C., and then rinsed with deionized water to obtain an ultrathin bionic coating attached to the surface of the matrix material.
[0038] Example 2
[0039] This embodiment provides a method for preparing a bionic coating, which is as follows:
[0040] Silicon wafer is selected as the matrix material, and the preparation raw materials are gallic acid and 3-(2-aminoethylamino)propyltriethoxysilane.
[0041] Gallic acid was dissolved in 20 mL of 50 mM acetic acid-sodium acetate buffer (pH=3.6) to obtain a gallic acid buffer with a concentration of 2 g / L, 3-(2-aminoethylamino)propyltriethoxysilane was dissolved in anhydrous ethanol (analytical grade) to obtain a 3-(2-aminoethylamino)propyltriethoxysilane ethanol solution with a concentration of 10 g / L; then the gallic acid buffer and the 3-(2-aminoethylamino)propyltriethoxysilane ethanol solution were mixed at a solution volume ratio of 7:1 to obtain a mixed solution; a silicon wafer was placed in the above mixed solution, stirred at 150 rpm for 25 minutes at 25°C, and then rinsed with deionized water to obtain an ultra-thin bionic coating attached to the surface of the matrix material.
[0042] Example 3
[0043] This embodiment provides a method for preparing a bionic coating, which is as follows:
[0044] Silicon wafer is selected as the matrix material, and the raw materials are tannic acid and tetraethylenepentamine.
[0045] Tannic acid was dissolved in 20 mL of 50 mM acetic acid-sodium acetate buffer (pH=3.6) to obtain a tannic acid buffer with a concentration of 2 g / L, and tetraethylene pentamine was dissolved in anhydrous ethanol (analytical grade) to obtain a tetraethylene pentamine ethanol solution with a concentration of 10 g / L; the tannic acid buffer and the tetraethylene pentamine ethanol solution were then mixed at a solution volume ratio of 9:1 to obtain a mixed solution; a silicon wafer was placed in the above mixed solution, stirred at 150 rpm for 35 min at 20°C, and then rinsed with deionized water to obtain an ultrathin bionic coating attached to the surface of the matrix material.
[0046] Example 4
[0047] This embodiment provides a method for preparing a bionic coating, which is as follows:
[0048] Silicon wafers were selected as the matrix material, and the raw materials for preparation were tannic acid and 3-(2-aminoethylamino)propyltriethoxysilane. The only difference from Example 1 was that the acetic acid-sodium acetate buffer solution was replaced with a citric acid-sodium citrate buffer solution with a pH of 3.6, and the other raw materials and process parameters remained unchanged.
[0049] Example 5
[0050] This embodiment provides a method for preparing a bionic coating, which is as follows:
[0051] Silicon wafer was selected as the matrix material, and the raw materials for preparation were tannic acid and 3-(2-aminoethylamino)propyltriethoxysilane. The only difference from Example 1 was that the pH of the acetic acid-sodium acetate buffer was 5.0, and other raw materials and process parameters remained unchanged.
[0052] Example 6
[0053] This embodiment provides a method for preparing a bionic coating, which is as follows:
[0054] Silicon wafer was selected as the matrix material, and the raw materials for preparation were tannic acid and 3-(2-aminoethylamino)propyltriethoxysilane. The only difference between the embodiment 1 and the embodiment 1 was that the pH of the acetic acid-sodium acetate buffer was 6.0, and the other raw materials and process parameters remained unchanged.
[0055] Comparative Example 1
[0056] This comparative example provides a method for preparing a biomimetic coating, which is as follows:
[0057] Silicon wafer was selected as the matrix material, and the raw materials for preparation were tannic acid and 3-(2-aminoethylamino)propyltriethoxysilane. The only difference from Example 1 was that the buffer solution was replaced with a Tris-HCl buffer solution with a pH of 8.5, and the other raw materials and process parameters remained unchanged.
[0058] Test Example 1
[0059] The thickness and uniformity of the bionic coatings prepared in Examples 1-6 and Comparative Example 1 were measured. The spectroscopic ellipsometer was used to measure the bionic coatings of each group at three incident angles of 65°, 70° and 75° to the surface normal. The measurements were performed at 10 points to confirm the uniformity of the bionic coating thickness, and the average value was given. The results are shown in Table 1.
[0060] Table 1
[0061] Group Thickness(nm) Example 1 1.17±0.03 Example 2 0.88±0.06 Example 3 0.79±0.07 Example 4 0.92±0.08 Example 5 1.51±0.12 Example 6 3.59±0.32 Comparative Example 1 46.25±1.30
[0062] It can be seen from the data in Table 1 that, compared with Comparative Example 1, when the preparation method of the present invention is used, i.e., the pH of the reaction system is adjusted to 3-6, the bionic coating obtained can ensure good uniformity while ensuring a very thin thickness, and the effect is better when the pH is 3-4.5. In addition, the phenolamine monomer and the buffer solution used in the preparation of the coating have little effect on the thickness of the coating, indicating that the preparation method of the ultra-thin bionic coating developed by the present invention is applicable to a wide range of polyphenols and amino-containing substances, and is not limited by the buffer system.
[0063] Example 7
[0064] This embodiment provides a method for preparing a bionic coating, which is as follows:
[0065] PES-50kDa ultrafiltration membrane was selected as the matrix material, and the raw materials for preparation were tannic acid and 3-(2-aminoethylamino)propyltriethoxysilane.
[0066] Tannic acid was dissolved in 20 mL of 50 mM acetic acid-sodium acetate buffer (pH=3.6) to obtain a tannic acid buffer with a concentration of 2 g / L, 3-(2-aminoethylamino)propyltriethoxysilane was dissolved in anhydrous ethanol (analytical grade) to obtain a 3-(2-aminoethylamino)propyltriethoxysilane ethanol solution with a concentration of 10 g / L; the tannic acid buffer and the 3-(2-aminoethylamino)propyltriethoxysilane ethanol solution were then mixed at a solution volume ratio of 8:1 to obtain a mixed solution; a PES-50 kDa ultrafiltration membrane was placed in the above mixed solution, stirred at 150 rpm for 30 min at 25° C., and then rinsed with deionized water to obtain an ultrathin bionic coating attached to the surface of the matrix material.
[0067] Example 8
[0068] This embodiment provides a method for preparing a bionic coating, which is as follows:
[0069] PES-50kDa ultrafiltration membrane was selected as the matrix material, and the raw materials for preparation were tannic acid and 3-(2-aminoethylamino)propyltriethoxysilane. The only difference between it and Example 7 was that the pH of the acetic acid-sodium acetate buffer was 5.0, and other raw materials and process parameters remained unchanged.
[0070] Example 9
[0071] This embodiment provides a method for preparing a bionic coating, which is as follows:
[0072] PES-50kDa ultrafiltration membrane was selected as the matrix material, and the raw materials for preparation were tannic acid and 3-(2-aminoethylamino)propyltriethoxysilane. The only difference between it and Example 7 was that the pH of the acetic acid-sodium acetate buffer was 6.0, and other raw materials and process parameters remained unchanged.
[0073] Comparative Example 2
[0074] This comparative example provides a method for preparing a biomimetic coating, which is as follows:
[0075] PES-50kDa ultrafiltration membrane was selected as the matrix material, and the raw materials for preparation were tannic acid and 3-(2-aminoethylamino)propyltriethoxysilane. The only difference from Example 7 was that the buffer solution was replaced with a Tris-HCl buffer solution with a pH of 8.5, and the other raw materials and process parameters remained unchanged.
[0076] Test Example 2
[0077] Investigate the changes in pore size distribution of PES-50kDa ultrafiltration membrane before and after coating modification:
[0078] Neutral molecular dextran (molecular weight 5, 10, 20, 40, 70 kDa, respectively) was dissolved in deionized water to prepare a 1 g / L feed solution to test the changes in pore size distribution before and after the modification of the PES-50 kDa ultrafiltration membrane coating in Examples 7-9 and Comparative Example 2. The effective filtration area was 4.52 cm 2 The dead-end filtration device was used to evaluate the retention performance of the ultrafiltration membrane for dextran. Before each test, the ultrafiltration membrane was pre-pressed with deionized water in the filtration mode of 1 mL / min for 15 minutes to maintain the ultrafiltration membrane structure. The flow rate was set to 0.2 mL / min, and the filtration was terminated after collecting 2 mL of permeate. The concentration of dextran in the permeate and retentate was then measured by liquid chromatography, and the concentration of the raw material solution was calculated by the material conservation formula, which is: C0V0=C P V P +C R V R ,
[0079] Among them, C0, C P and C Rare the glucan concentrations of the raw liquid, permeate and retentate, V0, V P and V R are the volumes of feed solution, permeate and retentate respectively.
[0080] The retention rate (R, %) is calculated as follows:
[0081]
[0082] Stocks diameter of dextran (d S The relationship between the molecular weight of dextran (Mw, g / mol) is:
[0083] d s =0.066×M W 0.46
[0084] The pore size and pore size distribution are calculated based on the solute transport method, which ignores the spatial and hydrodynamic interactions between the solute and the membrane pores. The formula is:
[0085]
[0086] The Stokes size of dextran when the rejection rate was 50% (μs) was taken as the average effective pore size (μp).
[0087] The results are shown in Table 2.
[0088] Table 2
[0089] Group Average pore size (nm) PES-50kDa 4.14 Example 7 2.34 Example 8 2.71 Example 9 3.14 Comparative Example 2 3.90
[0090] It can be seen from the data in Table 2 that, compared with the comparative example, when the preparation method involved in the present invention is adopted, that is, when the pH of the reaction system is adjusted to 3-6, especially when the pH is lower than 5, the size of the aggregates in the obtained bionic coating is smaller, so that they can fully enter the pores and fully modify the pores, making the pore size smaller.
[0091] Example 10
[0092] This embodiment provides a method for preparing a bionic coating, which is as follows:
[0093] Polystyrene cuvettes were selected as matrix materials, and the raw materials were tannic acid and 3-(2-aminoethylamino)propyltriethoxysilane.
[0094] Tannic acid was dissolved in 20 mL of 50 mM acetic acid-sodium acetate buffer (pH=3.6) to obtain a tannic acid buffer with a concentration of 2 g / L, and 3-(2-aminoethylamino)propyltriethoxysilane was dissolved in anhydrous ethanol (analytical grade) to obtain a 3-(2-aminoethylamino)propyltriethoxysilane ethanol solution with a concentration of 10 g / L; the tannic acid buffer and the 3-(2-aminoethylamino)propyltriethoxysilane ethanol solution were then mixed at a solution volume ratio of 8:1 to obtain a mixed solution; a polystyrene cuvette was placed in the mixed solution, stirred at 150 rpm for 30 min at 25° C., and then rinsed with deionized water to obtain an ultra-thin bionic coating attached to the surface of the matrix material.
[0095] Embodiment 11
[0096] This embodiment provides a method for preparing a bionic coating, which is as follows:
[0097] A polystyrene cuvette was selected as the matrix material, and the raw materials for preparation were tannic acid and 3-(2-aminoethylamino)propyltriethoxysilane. The only difference between the embodiment 10 and the embodiment 10 was that the pH of the acetic acid-sodium acetate buffer was 5.0, and the other raw materials and process parameters remained unchanged.
[0098] Example 12
[0099] This embodiment provides a method for preparing a bionic coating, which is as follows:
[0100] A polystyrene cuvette was selected as the matrix material, and the raw materials for preparation were tannic acid and 3-(2-aminoethylamino)propyltriethoxysilane. The only difference between the embodiment 10 and the embodiment 10 was that the pH of the acetic acid-sodium acetate buffer was 6.0, and the other raw materials and process parameters remained unchanged.
[0101] Comparative Example 3
[0102] This comparative example provides a method for preparing a biomimetic coating, which is as follows:
[0103] A polystyrene cuvette was selected as the matrix material, and the raw materials for preparation were tannic acid and 3-(2-aminoethylamino)propyltriethoxysilane. The difference between the embodiment 10 was that the buffer solution was replaced with a Tris-HCl buffer solution with a pH of 8.5, and the other raw materials and process parameters remained unchanged.
[0104] Test Example 3
[0105] The transmittance of the polystyrene cuvettes before and after the coating modification in Examples 10-12 and Comparative Example 3 was tested at 340 nm using an ultraviolet-visible spectrophotometer. The results are shown in Table 3.
[0106] Table 3
[0107] Group Light transmittance (%) Polystyrene cuvettes 100 Example 10 99.9 Embodiment 11 99.5 Example 12 99.0 Comparative Example 3 94.7
[0108] It can be seen from the data results in Table 3 that, compared with the comparative example, when the preparation method involved in the present invention is adopted, that is, when the pH of the reaction system is adjusted to 3-6, especially when the pH is lower than 5, the bionic coating obtained is thinner and more uniform, and has less impact on the light transmittance of the optical material.
[0109] Example 13
[0110] This embodiment provides a method for preparing a bionic coating, which is as follows:
[0111] Nylon microfiltration membrane was selected as the matrix material, and the raw materials for preparation were tannic acid and 3-(2-aminoethylamino)propyltriethoxysilane.
[0112] Tannic acid was dissolved in 20 mL of 50 mM acetic acid-sodium acetate buffer (pH=3.6) to obtain a tannic acid buffer with a concentration of 2 g / L, 3-(2-aminoethylamino)propyltriethoxysilane was dissolved in anhydrous ethanol (analytical grade) to obtain a 3-(2-aminoethylamino)propyltriethoxysilane ethanol solution with a concentration of 10 g / L; the tannic acid buffer and the 3-(2-aminoethylamino)propyltriethoxysilane ethanol solution were then mixed at a solution volume ratio of 8:1 to obtain a mixed solution; a nylon microfiltration membrane was placed in the mixed solution, stirred at 150 rpm for 30 min at 25° C., and then rinsed with deionized water to obtain an ultrathin bionic coating attached to the surface of a matrix material.
[0113] Embodiment 14
[0114] This embodiment provides a method for preparing a bionic coating, which is as follows:
[0115] Nylon microfiltration membrane was selected as the matrix material, and the raw materials for preparation were tannic acid and 3-(2-aminoethylamino)propyltriethoxysilane. The only difference between it and Example 13 was that the pH of the acetic acid-sodium acetate buffer was 5.0, and other raw materials and process parameters remained unchanged.
[0116] Embodiment 15
[0117] This embodiment provides a method for preparing a bionic coating, which is as follows:
[0118] Nylon microfiltration membrane was selected as the matrix material, and the raw materials for preparation were tannic acid and 3-(2-aminoethylamino)propyltriethoxysilane. The only difference between it and Example 13 was that the pH of the acetic acid-sodium acetate buffer was 6.0, and other raw materials and process parameters remained unchanged.
[0119] Comparative Example 4
[0120] This comparative example provides a method for preparing a biomimetic coating, which is as follows:
[0121] Nylon microfiltration membrane was selected as the matrix material, and the raw materials for preparation were tannic acid and 3-(2-aminoethylamino)propyltriethoxysilane. The only difference between it and Example 13 was that the buffer solution was replaced with a Tris-HCl buffer solution with a pH of 8.5, and the other raw materials and process parameters remained unchanged.
[0122] Test Example 4
[0123] The biomimetic coating modified nylon membranes prepared in Examples 13-15 and Comparative Example 4 were used for enzyme immobilization:
[0124] Glucose oxidase was dissolved in 20 mL of 10 mM acetic acid-sodium acetate buffer (pH = 5.0) to obtain a glucose oxidase solution with a concentration of 0.125 g / L. The coated modified nylon membrane of each group was placed in the enzyme solution, stirred at 150 rpm for 2 h at 25°C, and then washed with 10 mM acetic acid-sodium acetate buffer (pH = 5.0) to obtain immobilized glucose oxidase.
[0125] (1) Determination of enzyme loading:
[0126] The amount of immobilized enzyme was calculated by mass balance, and the protein concentration was monitored with a UV-visible spectrophotometer at 595 nm using the Bradford method.
[0127] Mass balance equation:
[0128] M I =C T ×V T -C P ×V P -C W ×V W Among them, M I is the protein loading; C T , C P and C W are the protein concentrations in the initial enzyme solution, the remaining enzyme solution, and the washing solution, respectively; V T 、V p and V W are the volumes of initial enzyme solution, remaining enzyme solution and washing solution respectively.
[0129] (2) Characterization of enzyme activity:
[0130] Phenol, 4-aminoantipyrine, horseradish peroxidase and glucose were dissolved in acetic acid-sodium acetate buffer (10mM, pH=5.0) to prepare substrate solutions, in which their concentrations were 40mM, 0.4mM, 0.015g / L, and 100mM, respectively; then the immobilized enzyme was added to 20mL of the above substrate solution under the action of a magnetic stirrer, and the change in the absorbance of the solution at 505nm was recorded. One unit of catalytic activity (U) is defined as the amount of enzyme that consumes 1μmol H2O2 per minute under the assay conditions (25℃, pH 5.0);
[0131] (3) Immobilized enzyme stability test:
[0132] The immobilized enzyme with the initial enzyme activity measured in step (2) was rinsed with ethanol and then immersed in a 100 mM citric acid-sodium citrate buffer solution at pH 3.0 for 2 h. The residual enzyme activity and the enzyme activity of the immersion solution were then measured to characterize its stability.
[0133] The results are shown in Table 4.
[0134] Table 4
[0135]
[0136] It can be seen from the data in Table 4 that, compared with the comparative example, when the pH of the reaction system is adjusted to 3-6 by the preparation method of the present invention, especially when the pH is lower than 5, the bionic coating obtained can achieve a higher enzyme loading when used for enzyme immobilization, and by comparing the data of the initial enzyme activity, the residual enzyme activity and the enzyme activity of the immersion liquid of each group, it can be seen that the bionic coating obtained by the preparation method of the present invention has better acid resistance and stability.
[0137] The applicant declares that the present invention uses the above-mentioned embodiments to illustrate the preparation method of the ultra-thin bionic coating of the present invention, its products and applications. However, the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
[0138] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0139] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
Claims
1. A method for preparing an ultra-thin bionic coating, characterized in that: The preparation method comprises: A buffer solution containing a polyphenol compound is mixed with an alcohol solution containing an amino compound, and simultaneously or subsequently contacted with a matrix material to deposit on the surface of the matrix material, thereby obtaining an ultrathin bionic coating attached to the surface of the matrix material; The buffer solution is an acidic buffer solution; the pH value of the buffer solution is 3-4.5; The thickness of the ultra-thin bionic coating is 0.5-1.5 nm; The polyphenol compound includes any one or a combination of at least two of catechol, pyrogallol, gallic acid, tannic acid, catechin, catechin gallate or catechin gallate; The amino compound includes any one of ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexamine, 3-aminopropyltriethoxysilane, 3-(2-aminoethylamino)propyltriethoxysilane or polyethyleneimine, or a combination of at least two thereof; The concentration of the polyphenol compound in the buffer solution is 0.5-5 g / L; The concentration of the amino compound in the alcohol solution is 5-10 g / L; The volume ratio of the buffer solution containing polyphenol compounds to the alcohol solution containing amino compounds is (3-10):
1.
2. The method for preparing the ultra-thin bionic coating according to claim 1, characterized in that: The matrix material is selected from inorganic materials or organic materials.
3. The method for preparing the ultra-thin bionic coating according to claim 1, characterized in that: The buffer solution is selected from any one of acetic acid-sodium acetate buffer solution, citric acid-sodium citrate buffer solution, glycine-hydrochloric acid buffer solution or disodium hydrogen phosphate-sodium dihydrogen phosphate, or a combination of at least two thereof.
4. The method for preparing the ultra-thin bionic coating according to claim 1, characterized in that: The volume ratio of the buffer solution containing the polyphenol compound to the alcohol solution containing the amino compound is (7-9):
1.
5. The method for preparing the ultra-thin bionic coating according to claim 1, characterized in that: The alcohol solution includes any one of anhydrous methanol, anhydrous ethanol or anhydrous 1-propanol, or a combination of at least two of them.
6. The method for preparing the ultra-thin bionic coating according to claim 1, characterized in that: The contacting method includes direct mixing and contacting with the matrix material, or spin coating, spray coating, and flowing through the matrix material.
7. The method for preparing the ultra-thin bionic coating according to claim 1, characterized in that: The contacting is carried out at a temperature of 10-35°C.
8. The method for preparing the ultra-thin bionic coating according to claim 7, characterized in that: The contacting is carried out at a temperature of 20-25°C.
9. The method for preparing the ultra-thin bionic coating according to claim 1, characterized in that: The contact time is 5-60 minutes.
10. The method for preparing the ultra-thin bionic coating according to claim 9, characterized in that: The contact time is 25-35 minutes.
11. An ultra-thin bionic coating prepared by the method for preparing an ultra-thin bionic coating according to any one of claims 1 to 10.
12. A method for preparing an ultrathin bionic coating according to any one of claims 1 to 10 or use of the ultrathin bionic coating according to claim 11 in preparing dye adsorption materials, membrane separation materials, catalytic materials, biopharmaceutical materials or anti-pollution materials.