A low-dose powder coating leveling agent and its preparation method and use method
By using isooctyl acrylate and silica in powder coating leveling agents, optimizing the formula and preparation process of the leveling agent solves the problems of large usage, high cost and uneven leveling performance in the existing technology, and achieves It achieves low-dose, high-efficiency, and environmentally friendly leveling effects.
Patent Information
- Application Number
- CN202310762829.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-27
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2043-06-27
AI Technical Summary
Existing powder coating leveling agents are used in large amounts and are costly, and they also have problems with uneven leveling performance and odor pollution.
Isooctyl acrylate is used as the synthetic monomer, combined with silica as the adsorption carrier, and through a specific mass ratio formula and preparation process, the amount of leveling agent used is reduced, the leveling effect is improved, and odor emissions are reduced.
It significantly reduces the amount of leveling agent used, improves the leveling effect, reduces the environmental burden of the production process and use process, and has a simple process and low cost, making it suitable for large-scale production.
Smart Images

Figure CN116715987B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings (IPC classification number C08F220 / 00), and in particular to a low-dose powder coating leveling agent and a preparation method and a use method thereof. Background Art
[0002] When curing, thermosetting powder coatings will produce defects such as orange peel and pores due to uneven flow, resulting in uneven surface of the coated object. The best way to solve this problem is to add powder coating leveling agent into the formula, which can reduce the melt viscosity of the powder coating system, increase the fluidity of the molten coating before curing, and increase the density of the directional molecular structure in the system, making the surface tension more uniform, and promoting the coating to form a flat, smooth and uniform coating film during the drying process, reducing the possibility of orange peel formation.
[0003] Chinese Patent No. 201811303876.8 discloses a multifunctional leveling agent for powder coatings, which increases the softening points of the leveling agent and the brightener by adding a high softening point substance α-methylstyrene, and then mixes them in proportion to obtain a material with suitable elasticity and toughness, so that the leveling agent and the brightener can better achieve their respective functions. Chinese Patent No. 201410139372.2 discloses a reactive high-activity leveling agent for epoxy powder coatings, which promotes the compatibility of epoxy resin and substrate by introducing polar groups such as hydroxyl groups and acid anhydrides. However, some of the above-mentioned prior arts still have problems such as high usage of butyl acrylate, high dosage of leveling agent, and high cost. Therefore, the development of a low-cost, low-dosage, and high-efficiency leveling agent has great market prospects. Summary of the invention
[0004] The first aspect of the present invention provides a low-dose powder coating leveling agent, wherein the raw materials for preparing the leveling agent include: synthetic monomers, adsorption carriers, catalysts, molecular weight regulators, and solvents, wherein the synthetic monomers include butyl acrylate and isooctyl acrylate in a mass ratio of (1-5):2.
[0005] In some embodiments, the relative molecular mass of the leveling agent is 5000-20000, and the molecular weight distribution is 1.5-5.
[0006] In some embodiments, the synthetic monomer further comprises at least one of hydroxyethyl acrylate, hydroxypropyl acrylate, methyl methacrylate, methyl acrylate, ethyl acrylate, lauryl methacrylate, octadecyl methacrylate, butyl methacrylate, and ethyl methacrylate.
[0007] Furthermore, the synthetic monomers include butyl acrylate, isooctyl acrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, methyl acrylate, and ethyl acrylate.
[0008] Furthermore, the mass ratio of butyl acrylate, isooctyl acrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, methyl acrylate and ethyl acrylate is (1-5):2:(0.5-2):(0.5-2):(1-2):(1-2).
[0009] Preferably, the mass ratio of butyl acrylate, isooctyl acrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, methyl acrylate and ethyl acrylate is (1-5):2:(0.5-2):(0.5-2):0.7:0.7.
[0010] Most preferably, the mass ratio of butyl acrylate, isooctyl acrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, methyl acrylate and ethyl acrylate is 3:2:0.5:1:0.7:0.7.
[0011] The applicant found in the research that when the synthetic monomers are butyl acrylate, isooctyl acrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, methyl acrylate, and ethyl acrylate, the synthesized polyacrylates have better loading capacity with the adsorption carrier, and are easier to precipitate from the white carbon black when the powder coating is heated and cured. Its molecular structure can reduce the surface tension of the coating, thereby causing the coating to form a flat and smooth film during the drying and film-forming process. In particular, the introduction of isooctyl acrylate can reduce the dosage of the leveling agent, or the leveling effect is better at the same dosage. The reason may be that isooctyl acrylate can increase the C chain length and steric hindrance of the polymer side chain, so that the alkyl long chain can be better dispersed to the surface, achieving a better leveling effect. When the proportion of the synthetic monomers is adjusted or the type is changed, the problem of decreased leveling performance will occur. The reason may be that the inappropriate ratio leads to uneven distribution of the long chain groups of isooctyl acrylate, resulting in the inability of the leveling agent to be evenly dispersed to the coating surface, which in turn causes the uneven distribution of the leveling agent on the coating surface, resulting in different leveling performance in different places, resulting in a decrease in leveling.
[0012] In the prior art, butyl acrylate is often added in a large amount in the formula of the leveling agent, and the unreacted butyl acrylate has a strong odor, which causes a great burden on the human body and the environment. The applicant unexpectedly discovered in the experiment that the odor of the leveling agent can be reduced by introducing isooctyl acrylate, making the production link and the use process more environmentally friendly.
[0013] In some embodiments, the adsorption carrier includes at least one of white carbon black, mesoporous silica, and molecular sieve.
[0014] In some embodiments, the packing density of the adsorption carrier is 40-60 g / L, and the specific surface area is 320000±25 cm 2 / g.
[0015] Furthermore, the adsorption carrier is white carbon black, purchased from Dongguan Xinke Chemical, HL-200.
[0016] The polyacrylate synthesized in the present invention is a flowable viscous fluid at room temperature. The applicant has found that mixing it with white carbon black not only improves its compatibility in powder coatings, but also enables the coating to flow evenly.
[0017] Furthermore, the catalyst can be selected from the types commonly used in the art, including but not limited to azobisisobutyronitrile.
[0018] Furthermore, the molecular weight regulator can be selected from commonly used types in the art, including but not limited to chain transfer agent TPMS, which can be purchased from Wuxi Yiyuan New Material Technology Co., Ltd.
[0019] Furthermore, the solvent can be selected from commonly used types in the art, including but not limited to ethoxyethanol.
[0020] The second aspect of the present invention provides a method for preparing a low-dose powder coating leveling agent, comprising the following steps:
[0021] S1. Add solvent to container 1, replace with inert gas and heat;
[0022] S2. Add the synthetic monomer, catalyst and molecular weight regulator into container 2 and mix well to obtain a mixture;
[0023] S3. The mixture is added dropwise to a hot solvent and kept warm, and the solvent is removed after cooling to obtain a prepolymer;
[0024] S4. Add the adsorption carrier into the prepolymer and stir evenly to obtain the leveling agent.
[0025] In some embodiments, the mass ratio of the synthetic monomer to the solvent is (1-5): (1-5).
[0026] In some embodiments, the dripping time in S3 is 3-6 hours.
[0027] In some embodiments, the mass ratio of the prepolymer to the adsorption carrier is (1-3):1.
[0028] In the present invention, the mass ratio of the prepolymer to the adsorption carrier has a significant influence on the leveling effect of the leveling agent. If the content of the adsorption carrier is too high, the content of the effective ingredient will decrease and the amount of the auxiliary agent used will increase. If the amount added is too small, the adsorption amount of the adsorption carrier will exceed the adsorption amount of the adsorption carrier, and the white carbon black will not be able to completely adsorb all the leveling agents, resulting in the adsorption product agglomerating and sticky, and cannot be added to the powder coating system. The leveling effect is best only when the mass ratio of the two is (1-3): 1. The reason may be that the amount of the two added just meets the adsorption limit of the white carbon black.
[0029] The third aspect of the present invention provides a method for using a low-dose leveling agent for powder coatings, wherein the addition amount of the leveling agent is 1-20wt% of the total amount of the powder coatings.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] 1. The creative introduction of isooctyl acrylate in the present invention can reduce the dosage of the leveling agent, or achieve a better leveling effect at the same dosage, and can also reduce the odor of the leveling agent, making the production process and the use process more environmentally friendly.
[0032] 2. By introducing an adsorption carrier, especially white carbon black, as much effective ingredient as possible can be adsorbed and the adsorption carrier has no effect on other properties of the powder coating.
[0033] 3. The preparation process of the present invention is simple, the raw materials are readily available, the preparation cost is low, and it is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is the infrared spectrum of the leveling agent prepared in Example 1. Peaks 3443, 2960, 2934, and 2874 in the figure indicate the generation of polyacrylic acid substances; and peaks 1105, 637, and 473 are generated by silicon dioxide (white carbon black).
[0035] Figure 2 This is the GPC picture of the leveling agent prepared in Example 1. It can be seen from the figure that the number average molecular weight of the leveling agent is 5223 and the molecular weight distribution is 3.72. DETAILED DESCRIPTION
[0036] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] Example 1
[0038] The first aspect of this embodiment provides a low-dose powder coating leveling agent, wherein the raw materials for preparing the leveling agent include: a synthetic monomer, an adsorption carrier, a catalyst, a molecular weight regulator, and a solvent.
[0039] The synthetic monomers are butyl acrylate, isooctyl acrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, methyl acrylate and ethyl acrylate, and the mass ratio is 3:2:0.5:1:0.7:0.7.
[0040] The adsorption carrier is white carbon black with a filling density of 40-60 g / L and a specific surface area of 320000±25 cm 2 / g.
[0041] The catalyst is azobisisobutyronitrile.
[0042] The molecular weight regulator is a chain transfer agent TPMS.
[0043] The solvent is ethoxyethanol.
[0044] The second aspect of this embodiment provides a method for preparing a low-dose powder coating leveling agent, comprising the following steps:
[0045] S1. Add 500 mL of solvent to container 1, replace the gas with nitrogen and heat to 115°C;
[0046] S2. 500 g of synthetic monomer, 1 g of catalyst, and 1 g of molecular weight regulator were added to container 2 and mixed to obtain a mixture;
[0047] S3. The mixture was added dropwise to a solvent at 115°C and kept warm for 3h, cooled to 90°C and the solvent was removed in vacuo to obtain a prepolymer, and the addition time was 5h;
[0048] S4. Add the adsorption carrier into the prepolymer and stir evenly to obtain the leveling agent.
[0049] The mass ratio of the prepolymer to the adsorption carrier is 62:38.
[0050] Example 2
[0051] The first aspect of this embodiment provides a low-dose powder coating leveling agent. The specific implementation method is the same as that of Example 1, except that the synthetic monomers are butyl acrylate, isooctyl acrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, methyl acrylate, and ethyl acrylate, and the mass ratio is 1:2:0.5:1:0.7:0.7.
[0052] The second aspect of this embodiment provides a method for preparing a low-dose powder coating leveling agent, and the specific implementation method is the same as that of embodiment 1, except that:
[0053] Example 3
[0054] The first aspect of this embodiment provides a low-dose powder coating leveling agent. The specific implementation method is the same as that of Example 1, except that the synthetic monomers are butyl acrylate, isooctyl acrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, methyl acrylate, and ethyl acrylate, and the mass ratio is 5:2:2:2:0.7:0.7.
[0055] The second aspect of this embodiment provides a method for preparing a low-dose powder coating leveling agent, and the specific implementation method is the same as that of embodiment 1, except that:
[0056] Comparative Example 1
[0057] The first aspect of this comparative example provides a low-dose powder coating leveling agent, and the specific implementation method is the same as Example 1, except that the synthetic monomers are butyl acrylate, isooctyl acrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, methyl acrylate, and ethyl acrylate, and the mass ratio is 3:4:0.25:0.25:3:1.
[0058] The second aspect of this comparative example provides a method for preparing a low-dose powder coating leveling agent, and the specific implementation method is the same as that of Example 1.
[0059] Comparative Example 2
[0060] The first aspect of this comparative example provides a low-dose powder coating leveling agent. The specific implementation method is the same as that of Example 1, except that the synthetic monomers are butyl acrylate, ethyl methacrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, methyl acrylate, and ethyl acrylate in a mass ratio of 3:2:0.5:1:0.7:0.7, that is, ethyl methacrylate is used to replace isooctyl acrylate.
[0061] The second aspect of this comparative example provides a method for preparing a low-dose powder coating leveling agent, and the specific implementation method is the same as that of Example 1.
[0062] Comparative Example 3
[0063] The first aspect of this comparative example provides a low-dose powder coating leveling agent, and the specific implementation method is the same as that of Example 1, except that the synthetic monomers are butyl acrylate, isooctyl acrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, lauryl methacrylate, and octadecyl methacrylate, and the mass ratio is 3:2:0.5:1:0.7:0.7.
[0064] The second aspect of this comparative example provides a method for preparing a low-dose powder coating leveling agent, and the specific implementation method is the same as that of Example 1.
[0065] Comparative Example 4
[0066] The first aspect of this comparative example provides a low-dose powder coating leveling agent, and the specific implementation method is the same as that of Example 1, except that the adsorption carrier is a molecular sieve with a particle size of 6-13nm and a specific surface area of 500m 2 / g, purchased from Zhongke Leiming (Beijing) Technology Co., Ltd., model molecular sieve SBA-15.
[0067] The second aspect of this comparative example provides a method for preparing a low-dose powder coating leveling agent, and the specific implementation method is the same as that of Example 1.
[0068] Comparative Example 5
[0069] The first aspect of this comparative example provides a low-dose powder coating leveling agent, and the specific implementation manner is the same as that of Example 1, except that it does not contain an adsorption carrier.
[0070] The second aspect of this comparative example provides a method for preparing a low-dose powder coating leveling agent, and the specific implementation method is the same as that of Example 1.
[0071] Comparative Example 6
[0072] The first aspect of this comparative example provides a low-dose powder coating leveling agent, and the specific implementation method is the same as that of Example 1.
[0073] The second aspect of this comparative example provides a method for preparing a low-dose powder coating leveling agent. The specific implementation method is the same as that of Example 1, except that the mass ratio of the prepolymer to the adsorption carrier is 130:38.
[0074] Performance Testing
[0075] Storage stability: The powder coating leveling agent prepared in the examples and comparative examples was sealed and placed at room temperature (25° C.) for 7 days to observe whether it agglomerated or not, and to open the bag and smell whether there was any obvious odor.
[0076] Coating appearance: The leveling agent was added to the powder coating (purchased from Guangdong Golisi Chemical Co., Ltd., GS low-temperature series powder coating) according to the following formula. After premixing, it was melt-extruded through an extruder, roller-rolled, and crushed and sieved to obtain acrylic resin powder coating. The powder spraying process was electrostatic spray gun spraying. The coating thickness was about 0.5 mm. The substrate was tinplate sheet that had been degreased and rusted. It was baked under curing conditions of 165°C×10 min to obtain an acrylic resin powder coating. The coating appearance was observed and recorded.
[0077] Formula: Powder coating GS-01 400g
[0078] Curing agent DDDA 100g
[0079] Leveling agent 6g
[0080]
[0081]
[0082] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A low-dose powder coating leveling agent, characterized in that: The raw materials for preparing the leveling agent include: synthetic monomers, adsorption carriers, catalysts, molecular weight regulators, and solvents; The synthetic monomers include butyl acrylate, isooctyl acrylate, hydroxyethyl acrylate, hydroxypropyl acrylate, methyl acrylate, and ethyl acrylate in a mass ratio of (1-5):2:(0.5-2):(0.5-2):0.7:0.7; The adsorption carrier is white carbon black, with a filling density of 40-60 g / L and a specific surface area of 320000±25 cm² / g; The catalyst is azobisisobutyronitrile; The molecular weight regulator is a chain transfer agent TPMS; The solvent is ethoxyethanol; The preparation method of the low-dose powder coating leveling agent comprises the following steps: S1. Add solvent to container 1, replace with inert gas and heat; S2. Add the synthetic monomer, catalyst and molecular weight regulator into container 2 and mix well to obtain a mixture; S3. The mixture is added dropwise to a hot solvent and kept warm, and the solvent is removed after cooling to obtain a prepolymer; S4. Add the adsorption carrier to the prepolymer and stir evenly to obtain a leveling agent; The mass ratio of the prepolymer to the adsorption carrier is 62:
38.
2. The low-dose powder coating leveling agent according to claim 1, characterized in that: The relative molecular mass of the leveling agent is 5000-20000, and the molecular weight distribution is 1.5-5.
3. The low-dose powder coating leveling agent according to claim 2, characterized in that: The mass ratio of the synthetic monomer to the solvent is (1-5): (1-5).
4. The low-dose powder coating leveling agent according to claim 3, characterized in that: The dropping time in S3 is 3-6 hours.
5. A method for using the low-dose powder coating leveling agent according to any one of claims 1 to 4, characterized in that: The added amount of the leveling agent is 1-20wt% of the total amount of the powder coating.