Negative electrode active materials and their preparation methods, secondary batteries and electrical devices
By distributing crystalline and amorphous silicon-based materials in the porous structure of the matrix material, the problem of volume effect of silicon-based materials during charge and discharge is solved, and a negative electrode active material with high capacity, high initial coulombic efficiency and low volume expansion is realized, thereby improving the energy density and cycle performance of secondary batteries.
Patent Information
- Application Number
- CN202280005823.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-02
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-11-02
AI Technical Summary
The capacity of existing graphite anode materials has approached the theoretical value. Silicon-based materials have a volume effect during charge and discharge, which leads to low initial coulombic efficiency, poor cycle performance, and poor storage performance of secondary batteries.
The substrate material has a multi-pore structure, with silicon-based material mainly located in the pore structure of the substrate material. By controlling the distribution of crystalline and amorphous silicon-based materials, crystalline silicon-based material is located in the inner region and amorphous silicon-based material is located in the outer region, forming a high-capacity, high-first-coulombic-efficiency negative electrode active material.
It achieves high capacity, high initial coulombic efficiency and low volume expansion, and the secondary battery has high energy density, long cycle life and long storage life.
Smart Images

Figure CN116724415B_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of battery technology, specifically relating to a negative electrode active material and its preparation method, a secondary battery and an electrical device. Background Technology
[0002] In recent years, rechargeable batteries have been widely used in energy storage power systems such as hydropower, thermal power, wind power, and solar power plants, as well as in power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, and many other fields. The rapid development of rechargeable batteries has placed higher demands on energy density. Graphite is the most commonly used negative electrode active material in rechargeable batteries, but its capacity utilization is already close to its theoretical specific capacity of 372 mAh / g. Silicon has attracted widespread attention due to its theoretical specific capacity of up to 4200 mAh / g and its relatively low cost. However, silicon exhibits a significant volume effect during charge and discharge, easily causing particle breakage and pulverization, which in turn leads to poor initial coulombic efficiency, cycle performance, and storage performance of rechargeable batteries. Summary of the Invention
[0003] The purpose of this application is to provide a negative electrode active material and its preparation method, a secondary battery and an electrical device, wherein the negative electrode active material has high capacity, high initial coulombic efficiency and low volume expansion, and enables the secondary battery to achieve high energy density, high initial coulombic efficiency, long cycle life and long storage life.
[0004] This application provides a negative electrode active material, the negative electrode active material comprising a matrix material and a silicon-based material, the matrix material comprising a plurality of porous structures, at least a portion of the silicon-based material being located within the porous structures of the matrix material, the silicon-based material comprising crystalline silicon-based material, a region defined as the area formed by extending from the outer surface of the negative electrode active material toward the interior of the particle at a distance of 0.5 times the length between any point on the outer surface of the particle and the particle core, is denoted as the outer region, and a region inside the outer region is denoted as the inner region, in a cross-sectional image of the negative electrode active material, the total cross-sectional area of the crystalline silicon-based material in the outer region is smaller than the total cross-sectional area of the crystalline silicon-based material in the inner region.
[0005] The negative electrode active material provided in this application includes a matrix material with multiple pore structures and at least a portion of silicon-based material located in the pore structures of the matrix material. The silicon-based material includes crystalline silicon-based material, and in a cross-sectional image of the negative electrode active material, the total cross-sectional area of the crystalline silicon-based material in the outer region is smaller than the total cross-sectional area of the crystalline silicon-based material in the inner region. Thus, the crystalline silicon-based material is mainly located in the inner region of the negative electrode active material. Consequently, the negative electrode active material provided in this application can have high capacity, high initial coulombic efficiency, and low volume expansion, and can enable secondary batteries to achieve high energy density, high initial coulombic efficiency, long cycle life, and long storage life.
[0006] In any embodiment of this application, the cross-sectional image of the negative electrode active material includes a cross-sectional image passing through the particle core of the negative electrode active material.
[0007] In any embodiment of this application, in the cross-sectional image of the negative electrode active material, the ratio α1 of the total cross-sectional area of the crystalline silicon-based material in the outer region to the total cross-sectional area of the crystalline silicon-based material in the inner region is (0-50):100, and can be optionally (0-10):100. By ensuring that the crystalline silicon-based material is mainly located in the inner region of the negative electrode active material, the improvement effect of the crystalline silicon-based material on the initial coulombic efficiency can be fully utilized, while avoiding significant adverse effects on the cycle performance and storage performance of the secondary battery.
[0008] In any embodiment of this application, the silicon-based material further includes amorphous silicon-based material. Optionally, in a cross-sectional image of the negative electrode active material, the total cross-sectional area of the amorphous silicon-based material in the outer region is greater than the total cross-sectional area of the amorphous silicon-based material in the inner region. By placing the amorphous silicon-based material primarily in the outer region of the negative electrode active material, the role of the amorphous silicon-based material in improving cycle performance and reducing volume expansion can be fully utilized.
[0009] In any embodiment of this application, the ratio α2 of the total cross-sectional area of the amorphous silicon-based material in the inner region to the total cross-sectional area of the amorphous silicon-based material in the outer region is (0-0):100, and can be optionally (0-10):100. The outer region of the negative electrode active material mainly contains amorphous silicon-based material, and contains no or a small amount of crystalline silicon-based material. This allows the crystalline silicon-based material to fully utilize its role in improving the initial coulombic efficiency, while also fully utilizing the amorphous silicon-based material to improve cycle performance and reduce volume expansion.
[0010] In any embodiment of this application, in the outer region of the cross-sectional image of the negative electrode active material, the ratio β1 of the total cross-sectional area of the crystalline silicon-based material to the total cross-sectional area of the amorphous silicon-based material is (0-25):100, optionally (0-5):100, and more preferably, the total cross-sectional area of the crystalline silicon-based material is 0. The outer region of the negative electrode active material mainly contains amorphous silicon-based material, and contains no or a small amount of crystalline silicon-based material. This allows the crystalline silicon-based material to fully exert its effect on improving the initial coulombic efficiency, while also fully leveraging the amorphous silicon-based material's effect on improving cycle performance and reducing volume expansion.
[0011] In any embodiment of this application, in the internal region of the cross-sectional image of the negative electrode active material, the ratio β2 of the total cross-sectional area of the crystalline silicon-based material to the total cross-sectional area of the amorphous silicon-based material is 100:(0-250), optionally 100:(0-100). The internal region of the negative electrode active material may contain only crystalline silicon-based material, or it may contain a mixture of crystalline silicon-based material and amorphous silicon-based material. Furthermore, by further adjusting the total cross-sectional area of the crystalline silicon-based material to the total cross-sectional area of the amorphous silicon-based material within a suitable range, the effect of the crystalline silicon-based material on improving the first coulombic efficiency can be better utilized.
[0012] In any embodiment of this application, in the cross-sectional image of the negative electrode active material, the ratio γ1 of the total cross-sectional area of the crystalline silicon-based material to the total cross-sectional area of the negative electrode active material is greater than 0 and less than or equal to 25%, and can be selected as 5%-20%. When the total cross-sectional area of the crystalline silicon-based material is within the above range, the effect of the crystalline silicon-based material on improving the initial coulombic efficiency can be fully utilized, while avoiding its significant adverse impact on the cycle performance and storage performance of the secondary battery.
[0013] In any embodiment of this application, in the cross-sectional image of the negative electrode active material, the ratio γ2 of the total cross-sectional area of the amorphous silicon-based material to the total cross-sectional area of the negative electrode active material is greater than or equal to 35% and less than 100%, and can be selected as 40%-60%. When the total cross-sectional area of the amorphous silicon-based material is within the above range, the effect of the amorphous silicon-based material on improving cycle performance and reducing volume expansion can be fully utilized, while avoiding a significant adverse impact on the initial coulombic efficiency of the secondary battery.
[0014] In any embodiment of this application, the mass percentage of the crystalline silicon-based material in the silicon-based material is greater than 0 and less than or equal to 40 wt%, and can be selected as 10 wt%-30 wt%. When the content of the crystalline silicon-based material is within the above range, the effect of the crystalline silicon-based material on improving the initial coulombic efficiency can be fully utilized, while avoiding its significant adverse impact on the cycle performance and storage performance of the secondary battery.
[0015] In any embodiment of this application, at least a portion of the silicon-based material is located within the porous structure of the substrate material, and there are voids between the silicon-based material and the substrate material. When there are voids between the silicon-based material and the substrate material, these voids can serve as spaces to accommodate the volume expansion of the silicon-based material, buffering the stress generated during the expansion process.
[0016] In any embodiment of this application, the grain size of the crystalline silicon-based material is greater than 0 and less than or equal to 10 nm, and can be selected as 2 nm-8 nm. When the crystalline silicon-based material has a suitable grain size, it can improve the initial coulombic efficiency of the secondary battery while avoiding significant adverse effects on the cycle performance and storage performance of the secondary battery.
[0017] In any embodiment of this application, the crystalline silicon-based material includes one or more of crystalline elemental silicon, silicon oxide, silicon-carbon materials, silicon-nitrogen composites, and silicon alloy materials. Optionally, the crystalline silicon-based material includes crystalline elemental silicon.
[0018] In any embodiment of this application, the amorphous silicon-based material includes one or more of amorphous elemental silicon, silicon oxide, silicon-carbon materials, silicon-nitrogen composites, and silicon alloy materials. Optionally, the amorphous silicon-based material includes amorphous elemental silicon.
[0019] In any embodiment of this application, the silicon-based material includes vapor-deposited silicon-based material, and optionally includes vapor-deposited elemental silicon.
[0020] In any embodiment of this application, the porosity of the matrix material is 30%-60%, optionally 40%-50%. When the porosity of the matrix material is within the above range, it is beneficial to accommodate sufficient silicon-based material, thereby improving the energy density of the secondary battery.
[0021] In any embodiment of this application, the matrix material includes one or more of carbon materials, graphite materials, and transition metal oxide materials.
[0022] In any embodiment of this application, the matrix material includes a carbon material, which comprises one or more of activated carbon, biomass carbon, pyrolytic carbon, and resin carbon. This not only alleviates the volume expansion of silicon-based materials and improves their conductivity, but also promotes the transport of active ions and increases the specific capacity of the negative electrode active material. Furthermore, compared to graphite materials, carbon materials have a more uniform porous structure, which is beneficial for the dispersion of silicon-based materials.
[0023] In any embodiment of this application, the negative electrode active material further includes a coating layer located on at least a portion of the surface of the substrate material. The coating layer is located on the outer side of the negative electrode active material, thereby further preventing direct contact between the silicon-based material and the electrolyte, reducing the reactivity of the silicon-based material after contact with air, thus reducing electrolyte side reactions, reducing active ion consumption, and improving the cycle performance of the secondary battery.
[0024] In any embodiment of this application, the coating layer comprises one or more of carbon materials, conductive polymers, metal oxides, and metal sulfides.
[0025] In any embodiment of this application, the coating layer comprises a carbon material, optionally including one or more of hard carbon, soft carbon, graphene, carbon fibers, and carbon nanotubes. When the coating layer comprises a carbon material, it helps to improve the conductivity of the silicon-based material.
[0026] In any embodiment of this application, the thickness of the coating layer is 0 nm-200 nm, and can be selected as 10 nm-150 nm. When the thickness of the coating layer is within the above range, it is beneficial for the negative electrode active material to have high specific capacity and low volume expansion.
[0027] In any embodiment of this application, the negative electrode active material includes carbon and silicon.
[0028] In any embodiment of this application, the mass percentage of carbon in the negative electrode active material is 40wt%-60wt%, and optionally 45wt%-50wt%.
[0029] In any embodiment of this application, the mass percentage of silicon in the negative electrode active material is 38wt%-58wt%, and optionally 40wt%-55wt%.
[0030] When the content of carbon and / or silicon in the negative electrode active material is within the above range, it is beneficial for the negative electrode active material to achieve both high specific capacity and high conductivity.
[0031] In any embodiment of this application, the negative electrode active material further includes other elements, including one or more of oxygen, metal elements, and nitrogen.
[0032] In any embodiment of this application, the sum of the mass percentages of other elements in the negative electrode active material is 0wt%-20wt%, and optionally 0wt%-10wt%.
[0033] In any embodiment of this application, the pore volume of the negative electrode active material is 0.001 cm³. 3 / g-.02cm 3 / g, can be selected as 0.01cm 3 / g-0.02cm 3 / g. When the pore volume of the negative electrode active material is within the above range, the internal voids of the negative electrode active material are within a suitable range. On the one hand, this can improve the specific capacity and initial coulombic efficiency of the negative electrode active material, and on the other hand, it can buffer the stress generated during the expansion of silicon-based materials.
[0034] In any embodiment of this application, the average particle size Dv50 of the negative electrode active material is 4 μm-12 μm. When the average particle size Dv50 of the negative electrode active material is within the above range, it helps to reduce surface activity, reduce interfacial side reactions, reduce SEI film formation consumption, and also helps to improve the active ion and electron transport performance, thereby further improving the cycle performance of the secondary battery.
[0035] In any embodiment of this application, the BET specific surface area of the negative electrode active material is 1 m². 2 / g-15m 2 / g.
[0036] When the BET specific surface area of the negative electrode active material is within the above range, it helps to reduce surface activity, reduce interfacial side reactions, reduce SEI film formation consumption, and improve the first coulombic efficiency and cycle performance of the secondary battery.
[0037] A second aspect of this application provides a method for preparing a negative electrode active material, comprising the following steps: providing a matrix material including a plurality of porous structures; dispersing a silicon-based material into the porous structures of the matrix material to obtain the negative electrode active material, wherein the negative electrode active material includes the matrix material and the silicon-based material, the matrix material including a plurality of porous structures, at least a portion of the silicon-based material being located in the porous structures of the matrix material, the silicon-based material including crystalline silicon-based material, a region defined by extending from the outer surface of the negative electrode active material to the interior of the particle at a distance of 0.5 times the length between any point on the outer surface of the particle and the particle core is denoted as the outer region, and a region inside the outer region is denoted as the inner region, wherein in a cross-sectional image of the negative electrode active material, the total cross-sectional area of the crystalline silicon-based material in the outer region is smaller than the total cross-sectional area of the crystalline silicon-based material in the inner region.
[0038] In any embodiment of this application, the porosity of the matrix material is 30%-60%, optionally 40%-50%. When the porosity of the matrix material is within the above range, it is beneficial for the deposition process to proceed smoothly, and it is also beneficial for the negative electrode active material to have a suitable silicon content, a suitable specific surface area, and / or a suitable pore volume.
[0039] In any embodiment of this application, the matrix material includes one or more of carbon materials, graphite materials, and transition metal oxide materials.
[0040] In any embodiment of this application, the matrix material includes a carbon material, which includes one or more of activated carbon, biomass carbon, pyrolytic carbon, and resin carbon.
[0041] In any embodiment of this application, the average particle size Dv50 of the substrate material is 4μm-12μm. When the average particle size Dv50 of the substrate material is within the above range, it is beneficial for the deposition process to proceed smoothly, and it is also beneficial for the negative electrode active material to have a suitable silicon content, a suitable specific surface area, and / or a suitable pore volume.
[0042] In any embodiment of this application, the step of dispersing silicon-based material into the porous structure of the matrix material includes the following steps: placing the matrix material comprising multiple porous structures as a substrate in a reactor, introducing a first mixed gas containing silicon source gas and depositing at a first temperature T1 for a first time t1, and stopping the introduction of the first mixed gas after the deposition is completed; after the temperature inside the reactor drops to a second temperature T2, introducing a second mixed gas containing silicon source gas and depositing at the second temperature T2 for a second time t2, and obtaining the negative electrode active material after the deposition is completed, wherein the silicon-based material includes crystalline silicon-based material and amorphous silicon-based material, and in the cross-sectional image of the negative electrode active material, the total cross-sectional area of the crystalline silicon-based material in the outer region is smaller than the total cross-sectional area of the crystalline silicon-based material in the inner region, and the total cross-sectional area of the amorphous silicon-based material in the outer region is larger than the total cross-sectional area of the amorphous silicon-based material in the inner region.
[0043] In any embodiment of this application, before introducing the first mixed gas containing silicon source gas, the method further includes the step of placing a matrix material comprising multiple porous structures as a substrate in a reactor, and performing purging and preheating treatment using a protective gas. Optionally, the preheating temperature is 200℃-300℃. This facilitates the removal of residual moisture in the matrix material, thereby promoting the subsequent successful deposition and formation of crystalline silicon-based materials.
[0044] In any embodiment of the present application, the volume proportion V1 of the silicon source gas in the first mixed gas is greater than the volume proportion V2 of the silicon source gas in the second mixed gas. This facilitates the adjustment of the distribution regions of the crystalline silicon-based material and the amorphous silicon-based material, so that the crystalline silicon-based material is mainly located in the inner region of the negative electrode active material, and the amorphous silicon-based material is mainly located in the outer region of the negative electrode active material. As a result, not only can the crystalline silicon-based material fully exert its effect of improving the initial Coulombic efficiency, but also the amorphous silicon-based material can fully exert its effects of improving the cycle performance and reducing the volume expansion.
[0045] In any embodiment of the present application, T1>T2. By adjusting the first temperature during deposition to be higher than the second temperature, it is beneficial to adjust the distribution regions of the crystalline silicon-based material and the amorphous silicon-based material, so that the crystalline silicon-based material is mainly located in the inner region of the negative electrode active material, and the amorphous silicon-based material is mainly located in the outer region of the negative electrode active material. As a result, not only can the crystalline silicon-based material fully exert its effect of improving the initial Coulombic efficiency, but also the amorphous silicon-based material can fully exert its effects of improving the cycle performance and reducing the volume expansion.
[0046] In any embodiment of the present application, t1<t2. By adjusting the first time during deposition to be shorter than the second time, it is beneficial to adjust the content and distribution region of the crystalline silicon-based material.
[0047] In any embodiment of the present application, the first mixed gas includes a silicon source gas and a protective gas, and optionally, the volume proportion V1 of the silicon source gas in the first mixed gas is 10%-50%.
[0048] In any embodiment of the present application, the total gas flow rate of the first mixed gas is 0.5L / min-20L / min.
[0049] In any embodiment of the present application, the first temperature T1 is 500°C-700°C.
[0050] In any embodiment of the present application, the first time t1 is 0.5h-8h, optionally 0.5h-4h.
[0051] By adjusting at least one of the composition ratio of the first mixed gas, the total gas flow rate of the first mixed gas, the first temperature, and the first time within the above ranges, it is beneficial to form the crystalline silicon-based material, and also beneficial to adjust parameters such as the distribution region, grain size, and deposition amount of the crystalline silicon-based material.
[0052] In any embodiment of the present application, the second mixed gas includes a silicon source gas and a protective gas, and optionally, the volume proportion V2 of the silicon source gas in the second mixed gas is 5%-20%.
[0053] In any embodiment of this application, the second mixed gas includes a silicon source gas, a carbon source gas, and a protective gas. Optionally, the volume percentage V2 of the silicon source gas in the second mixed gas is 5%-20%, and the volume percentage of the carbon source gas is 5%-10%.
[0054] In any embodiment of this application, the total gas flow rate of the second mixed gas is 0.5 L / min to 20 L / min.
[0055] In any embodiment of this application, the second temperature T2 is 400℃-500℃.
[0056] In any embodiment of this application, the second time t2 is 2h-16h, and can be selected as 4h-16h.
[0057] By adjusting at least one of the composition ratio of the second mixed gas, the total gas flow rate of the second mixed gas, the second temperature, and the second time to be within the above range, it is beneficial to form amorphous silicon-based materials, and also beneficial to adjust parameters such as the distribution area and deposition amount of the amorphous silicon-based materials.
[0058] In any embodiment of this application, the total gas flow rate of the second mixture is the same as the total gas flow rate of the first mixture.
[0059] In any embodiment of this application, the method further includes the step of forming a coating layer on at least the surface of the obtained negative electrode active material, the coating layer comprising one or more of carbon materials, conductive polymers, metal oxides and metal sulfides.
[0060] In any embodiment of this application, the step of forming the coating layer includes the following steps: placing the obtained negative electrode active material in a reactor, introducing a third mixed gas containing carbon source gas, and depositing it at a third temperature T3 for a third time t3 to obtain a carbon-coated negative electrode active material. This facilitates the formation of a uniform carbon layer.
[0061] In any embodiment of this application, the third mixed gas includes a carbon source gas and a protective gas. Optionally, the volume percentage V3 of the carbon source gas in the third mixed gas is 10%-50%.
[0062] In any embodiment of this application, the total gas flow rate of the third mixed gas is 0.5 L / min to 20 L / min.
[0063] In any embodiment of this application, the third temperature T3 is 600℃-700℃.
[0064] In any embodiment of this application, the third time t3 is 0.5h-2h.
[0065] By adjusting at least one of the composition ratio of the third mixed gas, the total gas flow rate of the third mixed gas, the third temperature, and the third time to be within the above range, it is beneficial to form a coating layer of appropriate thickness and avoid the coating layer being too thick, which would reduce the initial coulombic efficiency and / or specific capacity of the negative electrode active material.
[0066] A third aspect of this application provides a secondary battery, including a negative electrode sheet, wherein the negative electrode sheet comprises the negative electrode active material described in the first aspect of this application or the negative electrode active material prepared by the method described in the second aspect of this application.
[0067] The fourth aspect of this application provides an electrical device that includes the secondary battery of the third aspect of this application.
[0068] The negative electrode active material provided in this application possesses high capacity, high initial coulombic efficiency, and low volume expansion, and also enables the secondary battery to achieve high energy density, high initial coulombic efficiency, long cycle life, and long storage life. The power device of this application includes the secondary battery provided in this application, and therefore possesses at least the same advantages as the aforementioned secondary battery. Attached Figure Description
[0069] To more clearly illustrate the technical solutions of the embodiments of this application, the accompanying drawings used in the embodiments of this application will be briefly described below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on the drawings without creative effort.
[0070] Figure 1 This is a schematic diagram of a cross-sectional image of the negative electrode active material of this application.
[0071] Figure 2 This is a schematic diagram of one embodiment of the battery cell of this application.
[0072] Figure 3 This is an exploded view of one embodiment of the battery cell of this application.
[0073] Figure 4 This is a schematic diagram of one embodiment of the battery module of this application.
[0074] Figure 5 This is a schematic diagram of one embodiment of the battery pack of this application.
[0075] Figure 6 yes Figure 5 An exploded view of an embodiment of the battery pack shown.
[0076] Figure 7This is a schematic diagram of one embodiment of an electrical device that uses a secondary battery as a power source, as described in this application.
[0077] In the accompanying drawings, the figures may not be drawn to scale. The reference numerals are explained as follows: 1 Battery pack, 2 Upper casing, 3 Lower casing, 4 Battery module, 5 Battery cell, 51 Casing, 52 Electrode assembly, 53 Cover plate, 100 Negative electrode active material, 101 External region, 102 Internal region, O Particle core. Detailed Implementation
[0078] The following detailed description, with appropriate reference to the accompanying drawings, discloses the negative electrode active material of this application, its preparation method, and embodiments of secondary batteries and power-consuming devices comprising the same. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided for the purpose of enabling those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.
[0079] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0080] Unless otherwise specified, all embodiments and optional embodiments of this application may be combined with each other to form new technical solutions, and such technical solutions should be considered to be included in the disclosure of this application.
[0081] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions, and such technical solutions shall be deemed to be included in the disclosure of this application.
[0082] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the mention that the method may also include step (c) indicates that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0083] Unless otherwise specified, the terms "comprising" and "including" as used in this application can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.
[0084] Unless otherwise specified, the term "or" is inclusive in this application. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, the condition "A or B" is satisfied by any of the following conditions: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0085] Unless otherwise specified, in this application, the terms "first," "second," etc., are used to distinguish different objects, rather than to describe a specific order or primary / secondary relationship.
[0086] In this application, the terms "multiple" or "various" refer to two or more kinds.
[0087] In this application, "mainly located in" a specific region (e.g., an internal region or an external region) means that at least half of the corresponding material (e.g., a crystalline silicon-based material or an amorphous silicon-based material) is located in that specific region, and also includes the case where all of the corresponding material (e.g., a crystalline silicon-based material or an amorphous silicon-based material) is located in that specific region (e.g., an internal region or an external region).
[0088] Unless otherwise stated, the terms used in this application have the common meanings as commonly understood by those skilled in the art.
[0089] Unless otherwise stated, the values of the parameters mentioned in this application can be determined using various testing methods commonly used in the art, for example, according to the testing methods given in the embodiments of this application.
[0090] Silicon possesses a theoretical specific capacity as high as 4200 mAh / g, which can significantly improve the energy density of secondary batteries. Silicon also has a voltage plateau slightly higher than graphite, making it less prone to dendrite formation on the negative electrode and improving the safety performance of secondary batteries. Furthermore, silicon is widely distributed in the Earth's crust, abundant in resources, and inexpensive, thus reducing the production cost of secondary batteries. Therefore, materials containing silicon (hereinafter referred to as silicon-based materials) have become highly promising negative electrode active materials.
[0091] However, silicon-based materials also have some drawbacks. Unlike carbon-based materials such as graphite, silicon-based materials react with metals (such as lithium and sodium) through alloying reactions during charging and discharging. This results in a significant volume effect, making the particles prone to breakage and pulverization, which in turn leads to pulverization of the negative electrode film and loss of electrical contact with the current collector. Furthermore, the volume effect of silicon-based materials causes repeated damage and reconstruction of the solid electrolyte interphase (SEI) film on the particle surface, further increasing the irreversible consumption of active ions and ultimately affecting the capacity of the secondary battery. Therefore, when silicon-based materials are used as negative electrode active materials, they typically suffer from high irreversible capacity, low initial coulombic efficiency, and large volume expansion, resulting in significant actual capacity loss and poor cycle life in secondary batteries.
[0092] In addition, silicon is a semiconductor material with low intrinsic conductivity. When used as a negative electrode active material, it can affect the capacity volatilization of the secondary battery or require an additional amount of conductive agent, which reduces the actual coating weight of the negative electrode active material and affects the energy density of the secondary battery.
[0093] Currently, the main modification methods for addressing the above problems include the following aspects.
[0094] (1) Reducing the size of silicon-based materials to the nanoscale can alleviate their volume effect. However, the inventors of this application have found that the high specific surface area of nano-silicon-based materials can further exacerbate interfacial side reactions, increase the irreversible consumption of active ions, and reduce the first coulombic efficiency.
[0095] (2) Prepare porous silicon-based materials to mitigate the volume effect by utilizing their own deformation. However, the inventors of this application have found that when using porous silicon-based materials, the volume effect cannot be effectively mitigated, and the improvement on the first coulomb efficiency is also limited.
[0096] (3) Coating the surface of silicon-based materials with a conductive carbon layer increases the conductivity of silicon-based materials and alleviates the volume effect. However, the inventors of this application have found that when the conductive carbon layer is too thin, the coating is incomplete, which leads to rapid capacity decay and short cycle life of the secondary battery; when the conductive carbon layer is too thick, its rigidity is too strong, and the secondary battery is more prone to breakage and pulverization during charging and discharging, thus limiting the improvement of the first coulombic efficiency.
[0097] Therefore, none of the above modification methods can enable secondary batteries to simultaneously achieve high energy density, high initial coulombic efficiency, low volume expansion, and long cycle life.
[0098] In view of this, the inventors of this application have proposed a novel negative electrode active material through extensive research, which has high capacity, high initial coulombic efficiency and low volume expansion, and enables secondary batteries to achieve high energy density, high initial coulombic efficiency, long cycle life and long storage life.
[0099] Negative electrode active materials
[0100] A first aspect of this application provides a negative electrode active material. The negative electrode active material includes a matrix material and a silicon-based material. The matrix material includes a plurality of porous structures, and at least a portion of the silicon-based material is located within the porous structures of the matrix material. The silicon-based material includes crystalline silicon-based material. An outer region is defined as the area formed by extending from the outer surface of the negative electrode active material towards the interior of the particle, a distance equal to 0.5 times the length between any point on the outer surface of the particle and the particle core. The region inside the outer region is defined as the inner region. In a cross-sectional image of the negative electrode active material, the total cross-sectional area of the crystalline silicon-based material in the outer region is smaller than the total cross-sectional area of the crystalline silicon-based material in the inner region.
[0101] In this application, a cross-section of the negative electrode active material particles can be prepared using dual-beam focused ion beam microscopy (DIB-SEM). This cross-section passes through the central region of the negative electrode active material, optionally through the particle core. The cross-sectional image characteristics of the negative electrode active material can then be observed using transmission electron microscopy (TEM) or high-resolution transmission electron microscopy (HRTEM). When observing the cross-sectional image of the negative electrode active material, crystalline silicon-based materials will produce lattice fringes, thereby easily distinguishing between crystalline and amorphous silicon-based materials.
[0102] In this application, the cross-sectional image of the negative electrode active material includes a cross-sectional image passing through the particle core of the negative electrode active material.
[0103] In this application, "particle core" refers to the intersection of the longest diameter (or longest diagonal) and the shortest diameter (or shortest diagonal) of the negative electrode active material particle.
[0104] Figure 1 This is a schematic diagram of a cross-sectional image of the negative electrode active material 100 of this application, and the cross-sectional image passes through the particle core O of the negative electrode active material 100. Figure 1 As shown, the negative electrode active material 100 includes an outer region 101 and an inner region 102 located inside the outer region 101. The intersection of the longest diameter (or longest diagonal) and the shortest diameter (or shortest diagonal) of the negative electrode active material particle is the particle core O. The length between any point P on the outer surface of the particle and the particle core O is denoted as Rn. The region formed by extending from the outer surface of the negative electrode active material particle into the particle interior at a distance of 0.5 times the length Rn between any point P on the outer surface of the particle and the particle core O is denoted as the outer region 101.
[0105] It should be noted that "length Rn" here refers to the distance from any point on the outer surface of the particle to the particle core. When the negative electrode active material has a regular or irregular morphology other than an ideal sphere, the length Rn is a variable value, meaning that the distance from different positions on the outer surface of the particle to the particle core is a constantly changing value. Consequently, the distance extended from different positions on the outer surface of the particle into the particle is also a constantly changing value. Therefore, the area enclosed by all points on the outer surface of the negative electrode active material particle by extending the corresponding distance (i.e., 0.5Rn) into the particle and the outer surface of the particle together constitutes the external region.
[0106] In this application, the description that "the total cross-sectional area of the crystalline silicon-based material in the outer region is less than the total cross-sectional area of the crystalline silicon-based material in the inner region" is not limited to the outer region necessarily containing crystalline silicon-based material. When the outer region does not contain crystalline silicon-based material, and the total cross-sectional area of the crystalline silicon-based material in the outer region is 0, it is also considered to satisfy the condition that "the total cross-sectional area of the crystalline silicon-based material in the outer region is less than the total cross-sectional area of the crystalline silicon-based material in the inner region".
[0107] The negative electrode active material provided in this application includes a matrix material with multiple pore structures and at least a portion of silicon-based material located in the pore structures of the matrix material. The silicon-based material includes crystalline silicon-based material, and in a cross-sectional image of the negative electrode active material, the total cross-sectional area of the crystalline silicon-based material in the outer region is smaller than the total cross-sectional area of the crystalline silicon-based material in the inner region. Thus, the crystalline silicon-based material is mainly located in the inner region of the negative electrode active material. Consequently, the negative electrode active material provided in this application can have high capacity, high initial coulombic efficiency, and low volume expansion, and can enable secondary batteries to achieve high energy density, high initial coulombic efficiency, long cycle life, and long storage life.
[0108] This is because crystalline silicon-based materials help improve the initial coulombic efficiency of secondary batteries. However, crystalline silicon-based materials have large volume expansion and poor structural stability, which is detrimental to improving the cycle performance and reducing the volume expansion of secondary batteries. By placing the crystalline silicon-based material mainly in the internal region of the negative electrode active material, the effect of crystalline silicon-based materials in improving the initial coulombic efficiency can be fully utilized, while avoiding its significant adverse impact on the cycle performance and storage performance of secondary batteries. Therefore, the negative electrode active material provided in this application can have high capacity, high initial coulombic efficiency, and low volume expansion, and can also enable secondary batteries to achieve high energy density, high initial coulombic efficiency, long cycle life, and long storage life.
[0109] In some embodiments, the silicon-based material further includes amorphous silicon-based materials.
[0110] In some embodiments, the silicon-based material includes crystalline silicon-based material and amorphous silicon-based material. In a cross-sectional image of the negative electrode active material, the total cross-sectional area of the crystalline silicon-based material in the outer region is smaller than the total cross-sectional area of the crystalline silicon-based material in the inner region, and the total cross-sectional area of the amorphous silicon-based material in the outer region is larger than the total cross-sectional area of the amorphous silicon-based material in the inner region.
[0111] In this application, the description that "the total cross-sectional area of the amorphous silicon-based material in the outer region is greater than the total cross-sectional area of the amorphous silicon-based material in the inner region" is not limited to the inner region necessarily containing amorphous silicon-based material. When the inner region does not contain amorphous silicon-based material, and the total cross-sectional area of the amorphous silicon-based material in the inner region is 0, it is also considered that "the total cross-sectional area of the amorphous silicon-based material in the outer region is greater than the total cross-sectional area of the amorphous silicon-based material in the inner region" is satisfied.
[0112] The silicon-based material of this application includes both crystalline and amorphous silicon-based materials. The crystalline silicon-based material is mainly located in the internal region of the negative electrode active material, while the amorphous silicon-based material is mainly located in the external region of the negative electrode active material. As a result, the negative electrode active material provided by this application can have high capacity, high initial coulombic efficiency and low volume expansion, and can enable the secondary battery to achieve high energy density, high initial coulombic efficiency, long cycle life and long storage life.
[0113] This is because crystalline silicon-based materials help improve the initial coulombic efficiency of secondary batteries. However, crystalline silicon-based materials have large volume expansion and poor structural stability, which is detrimental to improving the cycle performance and reducing the volume expansion of secondary batteries. Amorphous silicon-based materials have small volume expansion, which is beneficial to improving the cycle performance and reducing the volume expansion of secondary batteries. However, amorphous silicon-based materials have lower initial coulombic efficiency, resulting in a large actual capacity loss in secondary batteries. By placing crystalline silicon-based materials mainly in the internal region of the negative electrode active material and amorphous silicon-based materials mainly in the external region of the negative electrode active material, the role of crystalline silicon-based materials in improving initial coulombic efficiency can be fully utilized, as well as the role of amorphous silicon-based materials in improving cycle performance and reducing volume expansion. Therefore, the negative electrode active material provided in this application can have high capacity, high initial coulombic efficiency, and low volume expansion, and can also enable secondary batteries to achieve high energy density, high initial coulombic efficiency, long cycle life, and long storage life.
[0114] In some embodiments, in the cross-sectional image of the negative electrode active material, the ratio α1 of the total cross-sectional area of the crystalline silicon-based material in the outer region to the total cross-sectional area of the crystalline silicon-based material in the inner region is (0-50):100, optionally (0-40):100, (0-30):100, (0-20):100, (0-15):100, (0-10):100, (0-5):100. In some embodiments, in the cross-sectional image of the negative electrode active material, the ratio α1 of the total cross-sectional area of the crystalline silicon-based material in the outer region to the total cross-sectional area of the crystalline silicon-based material in the inner region may be 0, that is, the aforementioned outer region of the negative electrode active material does not contain crystalline silicon-based material.
[0115] By placing the crystalline silicon-based material primarily within the internal region of the negative electrode active material, the positive impact of the crystalline silicon-based material on the initial coulombic efficiency can be fully realized, while avoiding significant adverse effects on the cycle performance and storage performance of the secondary battery.
[0116] In some embodiments, in the cross-sectional image of the negative electrode active material, the ratio α2 of the total cross-sectional area of the amorphous silicon-based material in the inner region to the total cross-sectional area of the amorphous silicon-based material in the outer region is (0-30):100, optionally (0-25):100, (0-20):100, (0-15):100, (0-10):100, or (0-5):100. In some embodiments, in the cross-sectional image of the negative electrode active material, the ratio α2 of the total cross-sectional area of the amorphous silicon-based material in the inner region to the total cross-sectional area of the amorphous silicon-based material in the outer region may be 0, that is, the aforementioned inner region of the negative electrode active material does not contain amorphous silicon-based material.
[0117] By placing the amorphous silicon-based material primarily in the external region of the negative electrode active material, the role of the amorphous silicon-based material in improving cycle performance and reducing volume expansion can be fully utilized.
[0118] In some embodiments, in the outer region of the cross-sectional image of the negative electrode active material, the ratio β1 of the total cross-sectional area of the crystalline silicon-based material to the total cross-sectional area of the amorphous silicon-based material is (0-25):100, optionally (0-20):100, (0-15):100, (0-10):100, (0-5):100. More preferably, the total cross-sectional area of the crystalline silicon-based material is 0, that is, the aforementioned outer region of the negative electrode active material does not contain crystalline silicon-based material. The outer region of the negative electrode active material mainly contains amorphous silicon-based material, and contains no or a small amount of crystalline silicon-based material. This allows for the full utilization of the crystalline silicon-based material's role in improving the initial coulombic efficiency, as well as the full utilization of the amorphous silicon-based material's role in improving cycle performance and reducing volume expansion.
[0119] In some embodiments, in the internal region of the cross-sectional image of the negative electrode active material, the ratio β2 of the total cross-sectional area of the crystalline silicon-based material to the total cross-sectional area of the amorphous silicon-based material is 100:(0-250), optionally 100:(0-100), 100:(0-80), 100:(0-60), 100:(0-40), 100:(0-30), 100:(0-20), 100:(0-10), or 100:(0-5). The internal region of the negative electrode active material may contain only crystalline silicon-based material, or it may contain a mixture of crystalline and amorphous silicon-based materials. By further adjusting the total cross-sectional area of the crystalline silicon-based material to the total cross-sectional area of the amorphous silicon-based material within a suitable range, the effect of the crystalline silicon-based material on improving the first coulombic efficiency can be better utilized.
[0120] In some embodiments, in the cross-sectional image of the negative electrode active material, the ratio γ1 of the total cross-sectional area of the crystalline silicon-based material to the total cross-sectional area of the negative electrode active material is greater than 0 and less than or equal to 25%, for example, it can be a range of any values consisting of 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, or higher. Optionally, the ratio γ1 of the total cross-sectional area of the crystalline silicon-based material to the total cross-sectional area of the negative electrode active material is 5%-20%, 8%-20%, 10%-20%, 12%-20%, or 12%-18%.
[0121] When the total cross-sectional area of crystalline silicon-based materials is within the above range, it can fully leverage the role of crystalline silicon-based materials in improving the initial coulombic efficiency, while avoiding significant adverse effects on the cycle performance and storage performance of secondary batteries.
[0122] In some embodiments, in the cross-sectional image of the negative electrode active material, the ratio γ2 of the total cross-sectional area of the amorphous silicon-based material to the total cross-sectional area of the negative electrode active material is greater than or equal to 35% and less than 100%, and can be selected as 40%-65%, 40%-60%, 40%-55%, or 40%-50%.
[0123] When the total cross-sectional area of amorphous silicon-based materials is within the above range, the effect of amorphous silicon-based materials on improving cycle performance and reducing volume expansion can be fully utilized, while avoiding a significant adverse impact on the initial coulombic efficiency of secondary batteries.
[0124] In some embodiments, the mass percentage of the crystalline silicon-based material in the silicon-based material is greater than 0 and less than or equal to 40 wt%, for example, it can be a range consisting of any value of 5 wt%, 10 wt%, 15 wt%, 20 wt%, 25 wt%, 30 wt%, 35 wt%, 40 wt%, or more. Optionally, the mass percentage of the crystalline silicon-based material in the silicon-based material is 5 wt%-40 wt%, 5 wt%-35 wt%, 10 wt%-35 wt%, or 10 wt%-30 wt%.
[0125] When the content of crystalline silicon-based materials is within the above range, it can fully leverage the role of crystalline silicon-based materials in improving the initial coulombic efficiency, while avoiding significant adverse effects on the cycle performance and storage performance of the secondary battery.
[0126] In some embodiments, at least a portion of the silicon-based material is located within the porous structure of the substrate material, and there are voids between the silicon-based material and the substrate material. When there are voids between the silicon-based material and the substrate material, these voids can serve as spaces to accommodate the volume expansion of the silicon-based material, buffering the stress generated during the expansion process.
[0127] In some embodiments, the grain size of the crystalline silicon-based material is greater than 0 and less than or equal to 10 nm, for example, it can be a range of any values including 2 nm, 3 nm, 4 nm, 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, or higher. Optionally, the grain size of the crystalline silicon-based material is 2 nm-10 nm or 2 nm-8 nm.
[0128] Larger grain sizes in crystalline silicon-based materials can improve the initial coulombic efficiency of secondary batteries, but are detrimental to their cycle performance and storage capacity. Therefore, when crystalline silicon-based materials have a suitable grain size, they can improve the initial coulombic efficiency of secondary batteries while avoiding significant adverse effects on their cycle performance and storage capacity.
[0129] The grain size of crystalline silicon-based materials is a term known in the art and can be determined using instruments and methods known in the art. For example, it can be tested using a high-resolution transmission electron microscope.
[0130] In some embodiments, the crystalline silicon-based material includes one or more of crystalline elemental silicon, silicon oxide, silicon-carbon materials, silicon-nitrogen composites, and silicon alloy materials. Optionally, the crystalline silicon-based material includes crystalline elemental silicon (also known as crystalline silicon).
[0131] In some embodiments, the amorphous silicon-based material includes one or more of amorphous elemental silicon, silicon oxide, silicon-carbon materials, silicon-nitrogen composites, and silicon alloy materials. Optionally, the amorphous silicon-based material includes amorphous elemental silicon (also known as amorphous silicon or amorphous silicon).
[0132] In some embodiments, the silicon-based material includes vapor-deposited silicon-based material, optionally including vapor-deposited elemental silicon, wherein the vapor-deposited elemental silicon includes vapor-deposited crystalline silicon and vapor-deposited amorphous silicon.
[0133] The matrix material includes multiple porous structures, and at least a portion of the silicon-based material is located within the porous structure of the matrix material. This allows the matrix material to effectively mitigate the volume expansion of the silicon-based material and prevent the silicon-based material or the negative electrode active material from breaking or pulverizing.
[0134] In some embodiments, the porosity of the matrix material is 30%-60%, for example, it can be a range consisting of any value of 30%, 35%, 40%, 45%, 50%, 55%, 60%, or higher. Optionally, the porosity of the matrix material is 40%-50%.
[0135] When the porosity of the matrix material is within the above range, it is beneficial to accommodate sufficient silicon-based material, which in turn helps to improve the energy density of the secondary battery.
[0136] In some embodiments, the matrix material includes one or more of carbon materials, graphite materials, and transition metal oxide materials. These matrix materials all include multiple porous structures, which can alleviate the volume expansion of silicon-based materials and, in addition, improve the conductivity of silicon-based materials.
[0137] In some embodiments, the matrix material comprises a transition metal oxide material. Transition metal oxide materials have a controllable and tunable pore structure and more uniform pore size, which is beneficial for the uniform dispersion of silicon-based materials. Optionally, the molecular formula of the transition metal oxide is M. x O y 0 < x ≤ 2, 0 < y ≤ 3, and M includes one or more elements selected from Ni, Co, Mn, Ti, and Cu. For example, the transition metal oxide includes one or more elements selected from NiO, Ni2O3, CoO, Co2O3, MnO, Mn2O3, TiO, TiO2, Ti2O3, Cu, Cu2O, and CuO.
[0138] In some embodiments, the matrix material includes graphite materials, such as natural graphite. This not only alleviates the volume expansion of silicon-based materials and improves their conductivity, but also promotes the transport of active ions and increases the specific capacity of the negative electrode active material.
[0139] In some embodiments, the matrix material comprises a carbon material, which includes one or more of activated carbon, biomass carbon, pyrolytic carbon, and resin carbon. This not only alleviates the volume expansion of silicon-based materials and improves their conductivity, but also promotes the transport of active ions and increases the specific capacity of the negative electrode active material. Furthermore, compared to graphite materials, carbon materials have a more uniform porous structure, which is beneficial for the dispersion of silicon-based materials.
[0140] In some embodiments, the negative electrode active material further includes a coating layer located on at least a portion of the surface of the substrate material. The coating layer is located on the outer side of the negative electrode active material, thereby further preventing direct contact between the silicon-based material and the electrolyte, reducing the reactivity of the silicon-based material upon contact with air, thus reducing electrolyte side reactions, decreasing active ion consumption, and improving the cycle performance of the secondary battery. Furthermore, the coating layer can also buffer the volume expansion of the silicon-based material, which also helps improve the storage performance of the secondary battery.
[0141] In some embodiments, the coating layer comprises one or more of carbon materials, conductive polymers, metal oxides, and metal sulfides.
[0142] In some embodiments, the carbon material includes one or more of hard carbon, soft carbon, graphene, carbon fiber, and carbon nanotubes.
[0143] In some embodiments, the conductive polymer includes one or more of polyaniline, polypyrrole, and polythiophene.
[0144] In some embodiments, the metal oxide includes one or more of iron oxide, zinc oxide, tin oxide, copper oxide, and titanium oxide.
[0145] In some embodiments, the metal sulfide includes one or more of tin sulfide, molybdenum sulfide, titanium sulfide, iron sulfide, and copper sulfide.
[0146] In some embodiments, the coating layer comprises a carbon material, optionally including one or more of hard carbon, soft carbon, graphene, carbon fiber, and carbon nanotubes. Thus, in addition to preventing direct contact between the silicon-based material and the electrolyte and buffering the volume expansion of the silicon-based material, the coating layer can also contribute to the capacity and improve the specific capacity of the negative electrode active material.
[0147] In addition, when the coating layer includes carbon materials, it also helps to improve the conductivity of silicon-based materials.
[0148] In some embodiments, the thickness of the coating layer is 0 nm-200 nm, optionally 10 nm-200 nm, 10 nm-180 nm, or 10 nm-150 nm. A coating layer thickness within these ranges is beneficial for the negative electrode active material to have high specific capacity and low volume expansion. In this application, when the coating layer thickness is 0 nm, it indicates that the negative electrode active material does not have a coating layer.
[0149] In some embodiments, the negative electrode active material includes carbon and silicon.
[0150] In some embodiments, the carbon content in the negative electrode active material is 40 wt%-60 wt%, for example, it can be any range consisting of 40 wt%, 42 wt%, 44 wt%, 46 wt%, 48 wt%, 50 wt%, 52 wt%, 54 wt%, 56 wt%, 58 wt%, 60 wt%, or more. Optionally, the carbon content in the negative electrode active material is 45 wt%-50 wt%.
[0151] In some embodiments, the silicon content in the negative electrode active material is 38 wt%-58 wt%, for example, it can be any range consisting of 40 wt%, 42 wt%, 44 wt%, 46 wt%, 48 wt%, 50 wt%, 52 wt%, 54 wt%, 56 wt%, 58 wt%, or higher. Optionally, the silicon content in the negative electrode active material is 40 wt%-55 wt%.
[0152] When the content of carbon and / or silicon in the negative electrode active material is within the above range, it is beneficial for the negative electrode active material to achieve both high specific capacity and high conductivity.
[0153] The carbon content in the negative electrode active material can be tested according to GB / T 20123-2006 / ISO 15350:2000, using an HCS-140 infrared carbon-sulfur analyzer. The silicon content in the negative electrode active material can be tested according to GB / T20975.5-2020.
[0154] In some embodiments, the negative electrode active material includes, in addition to carbon and silicon, other elements, including one or more of oxygen, metals, and nitrogen. The distribution area of these other elements is not specifically limited; for example, they may be located in at least one of the coating layer, the silicon-based material, and the matrix material.
[0155] In some embodiments, the sum of the mass percentages of other elements in the negative electrode active material is 0 wt%-20 wt%, optionally 0 wt%-10 wt% or 0 wt%-5 wt%. In this application, when the sum of the mass percentages of other elements in the negative electrode active material is 0 wt%, it means that the negative electrode active material does not include elements other than carbon and silicon.
[0156] In some embodiments, the pore volume of the negative electrode active material is 0.001 cm³ / g-0.02 cm³ / g, optionally 0.01 cm³ / g-0.02 cm³ / g. When the pore volume of the negative electrode active material is within the above range, the internal porosity of the negative electrode active material is within a suitable range. On the one hand, this can improve the specific capacity and initial coulombic efficiency of the negative electrode active material; on the other hand, it can also buffer the stress generated during the expansion of the silicon-based material.
[0157] In this application, the pore volume of the negative electrode active material has a meaning known in the art and can be determined using instruments and methods known in the art. For example, it can be tested according to GB / T 21650.2-2008. The testing instrument can be a TRISTAR II 3020 specific surface area and porosity analyzer from Micromeritics, USA.
[0158] In some embodiments, the average particle size Dv50 of the negative electrode active material is 4 μm-12 μm. When the average particle size Dv50 of the negative electrode active material is within the above range, it helps to reduce surface activity, reduce interfacial side reactions, reduce SEI film formation consumption, and also helps to improve the active ion and electron transport performance, thereby further improving the cycle performance of the secondary battery.
[0159] In this application, the average particle size Dv50 of the negative electrode active material has a meaning known in the art, which represents the particle size corresponding to a cumulative volume distribution percentage of 50% of the material, and can be measured using instruments and methods known in the art.
[0160] For example, according to GB / T 19077-2016, a laser particle size analyzer can be used for convenient determination. The testing instrument can be the Mastersizer 3000 laser particle size analyzer from Malvern Instruments Ltd., UK.
[0161] In some embodiments, the BET specific surface area of the negative electrode active material is 1 m². 2 / g-15m 2 / g. When the BET specific surface area of the negative electrode active material is within the above range, it helps to reduce surface activity, reduce interfacial side reactions, reduce SEI film formation consumption, and improve the first coulombic efficiency and cycle performance of the secondary battery.
[0162] In this application, the BET specific surface area of the negative electrode active material has a meaning known in the art and can be measured using instruments and methods known in the art. For example, it can be measured using the nitrogen adsorption specific surface area analysis method according to GB / T 19587-2017, and calculated using the BET (Brunauer Emmett Teller) method. The nitrogen adsorption specific surface area analysis can be performed using a TRISTAR II 3020 specific surface area and porosity analyzer from Micromeritics, Inc., USA.
[0163] Preparation method
[0164] The second aspect of this application provides a method for preparing a negative electrode active material, which can prepare the negative electrode active material of the first aspect of this application.
[0165] The method includes the following steps: providing a matrix material comprising multiple pore structures; dispersing a silicon-based material into the pore structures of the matrix material to obtain a negative electrode active material, wherein the negative electrode active material comprises a matrix material and a silicon-based material, the matrix material comprising multiple pore structures, at least a portion of the silicon-based material being located within the pore structures of the matrix material, the silicon-based material comprising crystalline silicon-based material, a region defined by extending from the outer surface of the negative electrode active material toward the interior of the particle at a distance 0.5 times the length between any point on the outer surface of the particle and the particle core is designated as the outer region, and a region inside the outer region is designated as the inner region, wherein in a cross-sectional image of the negative electrode active material, the total cross-sectional area of the crystalline silicon-based material in the outer region is smaller than the total cross-sectional area of the crystalline silicon-based material in the inner region.
[0166] In some embodiments, the porosity of the substrate material is 30%-60%, optionally 40%-50%. A porosity within this range is beneficial for the smooth progress of the deposition process and also helps the negative electrode active material to have suitable silicon content, suitable specific surface area, and / or suitable pore volume. If the porosity of the substrate material is too low, some silicon-based material is easily deposited on the surface of the substrate material, affecting the initial coulombic efficiency of the negative electrode active material. If the porosity of the substrate material is too high, insufficient silicon-based material deposition can lead to an excessively large specific surface area of the negative electrode active material, thereby increasing interfacial side reactions, increasing irreversible consumption of active ions, and reducing the initial coulombic efficiency of the negative electrode active material.
[0167] In some embodiments, the average particle size Dv50 of the substrate material is 4 μm-12 μm. When the average particle size Dv50 of the substrate material is within the above range, it is beneficial for the deposition process to proceed smoothly, and it is also beneficial for the negative electrode active material to have a suitable silicon content, a suitable specific surface area, and / or a suitable pore volume. When the average particle size Dv50 of the substrate material is too small, the deposition effect of the silicon-based material is poor, which is not conducive to subsequent two-stage deposition; when the average particle size Dv50 of the substrate material is too large, there is a risk of insufficient silicon-based material deposition, resulting in an excessively large specific surface area of the negative electrode active material, which increases interfacial side reactions, increases irreversible consumption of active ions, and reduces the initial coulombic efficiency of the negative electrode active material.
[0168] In some embodiments, the matrix material includes one or more of carbon materials, graphite materials, and transition metal oxide materials.
[0169] In some embodiments, the matrix material includes a carbon material, which includes one or more of activated carbon, biomass carbon, pyrolytic carbon, and resin carbon.
[0170] In this application, the matrix material can be obtained commercially or prepared according to methods known in the art, such as high-temperature pyrolysis of an organic carbon source or chemical activation treatment. The organic carbon source may include one or more of biomass materials and polymeric materials. The chemical activation treatment may be achieved by creating pores in the matrix material (e.g., carbon material) using a pore-forming agent (e.g., an alkaline solution).
[0171] In some embodiments, the step of dispersing silicon-based material into the porous structure of the matrix material includes the following steps: placing the matrix material comprising multiple porous structures as a substrate in a reactor, introducing a first mixed gas containing silicon source gas and depositing at a first temperature T1 for a first time t1, and stopping the introduction of the first mixed gas after the deposition is completed; after the temperature inside the reactor drops to a second temperature T2, introducing a second mixed gas containing silicon source gas and depositing at the second temperature T2 for a second time t2, and obtaining the negative electrode active material after the deposition is completed, wherein the silicon-based material includes crystalline silicon-based material and amorphous silicon-based material, and in the cross-sectional image of the negative electrode active material, the total cross-sectional area of the crystalline silicon-based material in the outer region is smaller than the total cross-sectional area of the crystalline silicon-based material in the inner region, and the total cross-sectional area of the amorphous silicon-based material in the outer region is larger than the total cross-sectional area of the amorphous silicon-based material in the inner region.
[0172] In some embodiments, the process of dispersing silicon-based materials into the porous structure of the substrate material is a vapor deposition process. The vapor deposition process includes chemical vapor deposition and physical vapor deposition, and can be selected as chemical vapor deposition, such as any one of thermochemical vapor deposition, plasma-enhanced chemical vapor deposition, and microwave plasma-assisted chemical vapor deposition.
[0173] In some embodiments, the reactor includes, but is not limited to, any one of a deposition furnace, a rotary furnace, a tubular furnace, and a fluidized bed.
[0174] This application employs a two-stage vapor deposition process to deposit crystalline and amorphous silicon-based materials in the porous structure of the substrate material in stages. Compared with conventional liquid phase deposition processes, vapor deposition facilitates better deposition and uniform dispersion of silicon-based materials in the porous structure of the substrate material, and avoids problems such as agglomeration of silicon-based materials and / or excessive deposition on the surface of the substrate material.
[0175] In some embodiments, before introducing the first mixture containing the silicon source gas, the method further includes the step of:
[0176] A matrix material with multiple porous structures is placed in a reactor and purged with a protective gas and preheated. Optionally, the preheating temperature is 200℃-300℃. This helps to remove residual moisture from the matrix material, which in turn facilitates the subsequent deposition and formation of crystalline silicon-based materials.
[0177] In some embodiments, in the step of dispersing silicon-based material into the porous structure of the matrix material, the volume percentage V1 of the silicon source gas in the first mixed gas is greater than the volume percentage V2 of the silicon source gas in the second mixed gas. This facilitates the adjustment of the distribution regions of crystalline and amorphous silicon-based materials, ensuring that the crystalline silicon-based material is mainly located in the internal region of the negative electrode active material, while the amorphous silicon-based material is mainly located in the external region of the negative electrode active material. This allows for the full utilization of both the improvement in initial coulombic efficiency by the crystalline silicon-based material and the improvement in cycle performance and reduction in volume expansion by the amorphous silicon-based material.
[0178] In some embodiments, during the step of dispersing the silicon-based material into the porous structure of the matrix material, T1 > T2.
[0179] In some embodiments, during the step of dispersing the silicon-based material into the porous structure of the matrix material, t1 <t2。
[0180] In some embodiments, during the step of dispersing the silicon-based material into the porous structure of the matrix material, T1 > T2 and t1 <t2。
[0181] In the step of dispersing silicon-based materials into the porous structure of the matrix material, by adjusting the first temperature during deposition to be greater than the second temperature, it is beneficial to adjust the distribution areas of crystalline and amorphous silicon-based materials. This ensures that the crystalline silicon-based materials are mainly located in the internal region of the negative electrode active material, while the amorphous silicon-based materials are mainly located in the external region of the negative electrode active material. This allows both the improvement of the initial coulombic efficiency by the crystalline silicon-based materials and the improvement of cycle performance and reduction of volume expansion by the amorphous silicon-based materials to be fully utilized.
[0182] By adjusting the first deposition time to be shorter than the second deposition time, it is beneficial to regulate the content and distribution area of crystalline silicon-based materials.
[0183] In some embodiments, after introducing a first mixed gas containing silicon source gas, the pressure inside the furnace can be adjusted to a slightly positive pressure, for example, 200 Pa to 600 Pa higher than atmospheric pressure, which is beneficial for the smooth progress of the deposition process.
[0184] In some embodiments, the first mixed gas includes a silicon source gas and a protective gas. Optionally, the volume percentage V1 of the silicon source gas in the first mixed gas is 10%-50%, for example, it can be any range consisting of 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50% or more.
[0185] In some embodiments, the total gas flow rate of the first mixed gas is 0.5 L / min to 20 L / min. For example, it can be 1 L / min, 2 L / min, 3 L / min, 4 L / min, 5 L / min, 6 L / min, 7 L / min, 8 L / min, 9 L / min, 10 L / min, 12 L / min, 14 L / min, 16 L / min, 18 L / min, 20 L / min, or any range of the above values.
[0186] In some embodiments, the first temperature T1 is 500°C-700°C, for example, it can be a range consisting of any value of 520°C, 540°C, 560°C, 580°C, 600°C, 620°C, 640°C, 660°C, 680°C, 700°C or above.
[0187] In some embodiments, the first time t1 is 0.5h-8h, for example, it can be a range of 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h or any of the above values. Optionally, the first time t1 is 0.5h-4h.
[0188] By adjusting at least one of the composition ratio of the first mixed gas, the total gas flow rate of the first mixed gas, the first temperature, and the first time to be within the above range, it is beneficial to form crystalline silicon-based materials, and also beneficial to adjust parameters such as the distribution area, grain size, and deposition amount of the crystalline silicon-based materials.
[0189] When the volume percentage of silicon source gas in the first mixture is too high and / or the total gas flow rate of the first mixture is too large, the content and distribution area of crystalline silicon-based materials increase, which is detrimental to the improvement of the cycle performance and storage performance of the secondary battery. When the volume percentage of silicon source gas in the first mixture is too low and / or the total gas flow rate of the first mixture is too small, the deposition amount of crystalline silicon-based materials may be insufficient, which is detrimental to the improvement of the initial coulombic efficiency of the secondary battery. When the first temperature is too low, it is not conducive to the formation of crystalline silicon-based materials. When the first temperature is too high, the grain size of silicon-based materials increases, which is detrimental to the improvement of the cycle performance and storage performance of the secondary battery. When the first time is too short, the deposition amount of crystalline silicon-based materials may be insufficient, which is detrimental to the improvement of the initial coulombic efficiency of the secondary battery. When the first time is too long, the content and distribution area of crystalline silicon-based materials increase, which is detrimental to the improvement of the cycle performance and storage performance of the secondary battery.
[0190] In some embodiments, after introducing a second mixed gas containing silicon source gas, the pressure inside the furnace can be adjusted to a slightly positive pressure, for example, 200 Pa to 600 Pa higher than atmospheric pressure, which is beneficial for the smooth progress of the deposition process.
[0191] In some embodiments, the second mixed gas may include a silicon source gas and a protective gas. Optionally, the volume percentage V2 of the silicon source gas in the second mixed gas is 5%-20%, for example, it may be a range of any value consisting of 5%, 6%, 8%, 10%, 12%, 14%, 16%, 18%, 20% or more.
[0192] In some embodiments, the second mixed gas may include a silicon source gas, a carbon source gas, and a protective gas. Optionally, the volume percentage V2 of the silicon source gas in the second mixed gas is 5%-20%, and the volume percentage of the carbon source gas is 5%-10%. This facilitates the adjustment of the distribution areas of crystalline silicon-based materials and amorphous silicon-based materials, so that the crystalline silicon-based materials are mainly located in the internal region of the negative electrode active material, while the amorphous silicon-based materials are mainly located in the external region of the negative electrode active material. This allows for the full utilization of both the improvement of the first coulombic efficiency by the crystalline silicon-based materials and the improvement of cycle performance and reduction of volume expansion by the amorphous silicon-based materials.
[0193] In some embodiments, the total gas flow rate of the second mixture is 0.5 L / min to 20 L / min. For example, it can be 1 L / min, 2 L / min, 3 L / min, 4 L / min, 5 L / min, 6 L / min, 7 L / min, 8 L / min, 9 L / min, 10 L / min, 12 L / min, 14 L / min, 16 L / min, 18 L / min, 20 L / min, or any range of the above values.
[0194] In some embodiments, the second temperature T2 is 400°C-500°C, for example, it can be a range consisting of any of the following values: 400°C, 410°C, 420°C, 430°C, 440°C, 450°C, 460°C, 470°C, 480°C, 490°C or above.
[0195] In some embodiments, the second time t2 is 2h-16h, for example, it can be a range of 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h or any of the above values. Optionally, the second time t2 is 4h-16h.
[0196] By adjusting at least one of the composition ratio of the second mixed gas, the total gas flow rate of the second mixed gas, the second temperature, and the second time to be within the above range, it is beneficial to form amorphous silicon-based materials, and also beneficial to adjust parameters such as the distribution area and deposition amount of the amorphous silicon-based materials.
[0197] When the volume percentage of silicon source gas in the second mixture is too high and / or the total gas flow rate of the second mixture is too large, amorphous silicon-based materials may deposit on the surface of the substrate material, which may increase the difficulty of preparing the negative electrode slurry, and may also increase interfacial side reactions and irreversible consumption of active ions; when the volume percentage of silicon source gas in the second mixture is too low and / or the total gas flow rate of the second mixture is too small, the deposition amount of amorphous silicon-based materials may be insufficient, resulting in a larger specific surface area of the negative electrode active material, increased interfacial side reactions, increased irreversible consumption of active ions, and reduced initial coulombic efficiency; when the second temperature is too low... First, silicon-based materials have poor deposition performance and cannot be effectively deposited. Second, if the temperature is too high, crystalline silicon-based materials are easily formed, which is detrimental to improving the cycle performance and storage performance of secondary batteries. Third, if the time is too short, the deposition amount of amorphous silicon-based materials may be insufficient, resulting in a larger specific surface area of the negative electrode active material, increased interfacial side reactions, increased irreversible consumption of active ions, and reduced initial coulombic efficiency. Fourth, if the time is too long, amorphous silicon-based materials may be deposited on the surface of the substrate material, which may increase the difficulty of preparing the negative electrode slurry, and may also increase interfacial side reactions and irreversible consumption of active ions.
[0198] In some embodiments, the total gas flow rate of the second mixture may be the same as the total gas flow rate of the first mixture.
[0199] In some embodiments, the method further includes the step of forming a coating layer on at least the surface of the obtained negative electrode active material, the coating layer comprising one or more of carbon materials, conductive polymers, metal oxides and metal sulfides.
[0200] The method of forming a coating layer on at least the surface of the obtained negative electrode active material is not specifically limited and can be selected according to the composition of the coating layer, for example, any one of solid phase coating, liquid phase coating or gas phase coating can be used.
[0201] In some embodiments, the step of forming the coating layer includes the following steps: mixing the obtained negative electrode active material with the coating material and then performing a carbonization treatment. Optionally, the coating material includes one or more of asphalt (e.g., coal tar pitch, petroleum asphalt, etc.) and polymer materials. Optionally, the carbonization treatment temperature is 500℃-1000℃.
[0202] In some embodiments, the step of forming the coating layer includes the following steps: placing the obtained negative electrode active material in a reactor, introducing a third mixed gas containing a carbon source gas, and depositing it at a third temperature T3 for a third time t3 to obtain a carbon-coated negative electrode active material. This facilitates the formation of a uniform carbon layer.
[0203] In some embodiments, the third mixture includes a carbon source gas and a protective gas. Optionally, the volume percentage V3 of the carbon source gas in the third mixture is 10%-50%, for example, it can be any range consisting of 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50% or more.
[0204] In some embodiments, the total gas flow rate of the third mixture is 0.5 L / min to 20 L / min. For example, it can be 1 L / min, 2 L / min, 3 L / min, 4 L / min, 5 L / min, 6 L / min, 7 L / min, 8 L / min, 9 L / min, 10 L / min, 12 L / min, 14 L / min, 16 L / min, 18 L / min, 20 L / min, or any range of the above values.
[0205] In some embodiments, the third temperature T3 is 600°C-700°C, for example, it can be a range consisting of any value of 600°C, 610°C, 620°C, 630°C, 640°C, 650°C, 660°C, 670°C, 680°C, 690°C, 700°C or above.
[0206] In some embodiments, the third time t3 is 0.5h-2h, for example, it can be a range consisting of 0.5h, 0.6h, 0.8h, 1h, 1.2h, 1.4h, 1.6h, 1.8h, 2h or any of the above values.
[0207] By adjusting at least one of the composition ratio of the third mixed gas, the total gas flow rate of the third mixed gas, the third temperature, and the third time to be within the above range, it is beneficial to form a coating layer of appropriate thickness and avoid the coating layer being too thick, which would reduce the initial coulombic efficiency and / or specific capacity of the negative electrode active material.
[0208] In this application, the term "protective gas" includes nitrogen and rare gases, which may include one or more of argon, helium, etc.
[0209] In this application, the term "silicon source gas" refers to a gas capable of forming the silicon-based material of this application. Optionally, the silicon source gas includes, but is not limited to, silane (H4Si), silane (H6Si2), propane (H8Si3), silicon tetrachloride (Cl4Si), trichlorosilane (Cl3HSi), dichlorosilane (Cl2H2Si), chlorosilane (ClH3Si), silicon tetrafluoride (F4Si), trifluorosilane (F3HSi), difluorosilane (F2H2Si), fluorosilane (FH3Si), hexachlorodisilane (Cl6Si2), pentachlorodisilane (Cl5HSi2), and tetrachlorodisilane (Cl4H2). Si2, including 1,1,2,2-tetrachlorodisilane, 1,1,1,2-tetrachlorodisilane, trichlorodisilane (Cl3H3Si2, including 1,1,2-trichlorodisilane, 1,1,1-trichlorodisilane), dichlorodisilane (Cl2H4Si2, including 1,1-dichlorodisilane, 1,2-dichlorodisilane), monochlorodisilane (ClH5Si2), hexafluorodisilane (F6Si2), pentafluorodisilane (F5HSi2), 1,1,2,2-tetrafluorodisilane (F4H2Si2), 1,1,1-trifluorodisilane (F3H3 One or more of the following: Si2), difluorodisilane (F2H4Si2, including 1,1-difluorodisilane, 1,2-difluorodisilane), monofluorodisilane (FH5Si2), methylsilane, ethylsilane, dimethylsilane, trimethylsilane, tetramethylsilane, methyldisilane, dimethyldisilane, trimethyldisilane, tetramethyldisilane, hexamethylsilane, methyltrichlorosilane, methylchlorosilane, chloroethylsilane, dichlorodimethylsilane, and dichlorodiethylsilane.
[0210] In this application, "carbon source gas" refers to a gas capable of forming carbon materials. Optionally, the carbon source gas includes, but is not limited to, one or more of the following: methane, ethane, propane, isopropane, butane, isobutane, ethylene, propylene, butene, acetylene, chloroethane, fluoroethane, difluoroethane, chloromethane, fluoromethane, difluoromethane, trifluoromethane, vinyl chloride, vinyl fluoride, difluoroethylene, methylamine, formaldehyde, benzene, toluene, xylene, styrene, and phenol.
[0211] Unless otherwise specified, all raw materials and instruments used in the preparation method of this application can be obtained commercially.
[0212] Secondary batteries
[0213] The third aspect of this application provides a secondary battery.
[0214] The secondary battery mentioned in the embodiments or implementations of this application refers to a single physical module comprising one or more battery cells to provide higher voltage and capacity. For example, the secondary battery mentioned in this application may include battery cells, battery modules, or battery packs. A battery cell is the smallest unit constituting a secondary battery, capable of charging and discharging independently. This application does not impose any particular limitation on the shape of the battery cell; it can be cylindrical, square, or any other arbitrary shape. Figure 2 The example shown is a square-structured battery cell 5.
[0215] In some embodiments, a single battery cell includes an electrode assembly and an electrolyte, and the single battery cell may also include an outer packaging.
[0216] The electrode assembly can be manufactured from positive electrode sheets, negative electrode sheets, and separators through winding and / or stacking processes. Outer packaging can be used to encapsulate the electrode assembly. The outer packaging can be a rigid shell, such as a hard plastic shell, aluminum shell, or steel shell. Alternatively, it can be a flexible package, such as a pouch. The flexible package can be made of plastic, such as one or more of polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).
[0217] In some embodiments, such as Figure 3 As shown, the outer packaging may include a housing 51 and a cover 53. The housing 51 may include a base plate and side plates connected to the base plate, the base plate and side plates enclosing a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the cover 53 is used to cover the opening to close the receiving cavity. Electrode assemblies 52 are encapsulated in the receiving cavity. The number of electrode assemblies 52 contained in the battery cell 5 may be one or more, and can be adjusted as needed.
[0218] In some embodiments of this application, individual battery cells can be assembled into a battery module. The number of individual battery cells contained in a battery module can be multiple, and the specific number can be adjusted according to the application and capacity of the battery module. Figure 3 This is a schematic diagram of battery module 4 as an example. Figure 4 As shown, in battery module 4, multiple battery cells 5 can be arranged sequentially along the length of battery module 4. Of course, they can also be arranged in any other manner. Furthermore, these multiple battery cells 5 can be fixed in place using fasteners.
[0219] Optionally, the battery module 4 may also include a housing with a receiving space in which multiple battery cells 5 are received.
[0220] In some embodiments, the battery modules described above can also be assembled into a battery pack, and the number of battery modules contained in the battery pack can be adjusted according to the application and capacity of the battery pack. Figure 5 and Figure 6 This is a schematic diagram of battery pack 1 as an example.
[0221] like Figure 5 and Figure 6 As shown, the battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box includes an upper body 2 and a lower body 3. The upper body 2 covers the lower body 3, forming a closed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.
[0222] This application does not impose any particular restrictions on the type of secondary battery. For example, secondary batteries may include, but are not limited to, lithium-ion batteries, sodium-ion batteries, etc.
[0223] [Negative electrode plate]
[0224] In some embodiments, the negative electrode sheet includes a negative current collector and a negative electrode film layer disposed on at least one surface of the negative current collector and comprising a negative electrode active material. For example, the negative current collector has two surfaces opposite each other in its thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative current collector.
[0225] In some embodiments, the negative electrode film layer comprises the negative electrode active material of the first aspect of the present application or the negative electrode active material prepared by the method of the second aspect of the present application. This enables the secondary battery to achieve high energy density, high initial coulombic efficiency, long cycle life, and long storage life.
[0226] In some embodiments, the negative electrode film layer may further include other negative electrode active materials besides the aforementioned negative electrode active materials. In some embodiments, the other negative electrode active materials include, but are not limited to, one or more of natural graphite, artificial graphite, soft carbon, hard carbon, elemental silicon, silicon oxide, silicon-nitrogen composites, silicon alloys, elemental tin, tin oxides, tin alloys, and lithium titanate. This application is not limited to these materials, and other conventionally known materials that can be used as negative electrode active materials for secondary batteries may also be used.
[0227] In some embodiments, the negative electrode film layer may optionally include a negative electrode conductive agent. This application does not impose any particular limitation on the type of negative electrode conductive agent. As an example, the negative electrode conductive agent may include one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0228] In some embodiments, the negative electrode film layer may optionally include a negative electrode binder. This application does not impose any particular limitation on the type of negative electrode binder. As an example, the negative electrode binder may include one or more of the following: styrene-butadiene rubber (SBR), water-soluble unsaturated resin SR-1B, waterborne acrylic resins (e.g., polyacrylic acid PAA, polymethacrylic acid PMAA, sodium polyacrylate PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), and carboxymethyl chitosan (CMCS).
[0229] In some embodiments, the negative electrode film may optionally include other additives. As an example, other additives may include thickeners, such as sodium carboxymethyl cellulose (CMC), PTC thermistor materials, etc.
[0230] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. As an example of the metal foil, copper foil may be used. The composite current collector may include a polymeric material substrate and a metal material layer formed on at least one surface of the polymeric material substrate. As an example, the metal material may include one or more of copper, copper alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys. As an example, the polymeric material substrate may include one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).
[0231] The negative electrode film layer is typically formed by coating a negative electrode slurry onto a negative electrode current collector, followed by drying and cold pressing. The negative electrode slurry is typically formed by dispersing a negative electrode active material, optional conductive agent, optional binder, and other optional additives in a solvent and stirring until homogeneous. The solvent can be N-methylpyrrolidone (NMP) or deionized water, but is not limited to these.
[0232] The negative electrode sheet does not exclude other additional functional layers besides the negative electrode film layer. For example, in some embodiments, the negative electrode sheet of this application may further include a conductive undercoat layer (e.g., composed of a conductive agent and an adhesive) sandwiched between the negative electrode current collector and the negative electrode film layer and disposed on the surface of the negative electrode current collector; in some embodiments, the negative electrode sheet of this application may further include a protective layer covering the surface of the negative electrode film layer.
[0233] [Positive electrode plate]
[0234] In some embodiments, the positive electrode includes a positive current collector and a positive electrode film layer disposed on at least one surface of the positive current collector and comprising a positive electrode active material. For example, the positive current collector has two surfaces opposite each other in its thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive current collector.
[0235] The positive electrode film layer includes a positive electrode active material, which may be a positive electrode active material known in the art for use in secondary batteries.
[0236] When the secondary battery of this application is a lithium-ion battery, the positive electrode active material may include one or more of lithium transition metal oxides, lithium-containing phosphates with an olivine structure, and their respective modified compounds. Examples of lithium transition metal oxides may include one or more of lithium cobalt oxides, lithium nickel oxides, lithium manganese oxides, lithium nickel cobalt oxides, lithium manganese cobalt oxides, lithium nickel manganese oxides, lithium nickel cobalt manganese oxides, lithium nickel cobalt aluminum oxides, and their respective modified compounds. Examples of lithium-containing phosphates with an olivine structure may include one or more of lithium iron phosphate, lithium iron phosphate and carbon composites, lithium manganese phosphate, lithium manganese phosphate and carbon composites, lithium manganese iron phosphate, lithium manganese iron phosphate and carbon composites, and their respective modified compounds. This application is not limited to these materials, and other conventionally known materials that can be used as positive electrode active materials for secondary batteries may also be used.
[0237] In some embodiments, to further improve the energy density of secondary batteries, the positive electrode active material for lithium-ion batteries may include materials with the general formula Li. a Ni b Co c M d O e A fOne or more of lithium transition metal oxides and their modified compounds. 0.8≤a≤1.2, 0.5≤b<1, 0<c<1, 0<d<1, 1≤e≤2, 0≤f≤1, M includes one or more selected from Mn, Al, Zr, Zn, Cu, Cr, Mg, Fe, V, Ti and B, and A includes one or more selected from N, F, S and Cl.
[0238] As an example, positive electrode active materials for lithium-ion batteries may include LiCoO2, LiNiO2, LiMnO2, LiMn2O4, and LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2(NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2(NCM523), LiNi 0.6 Co 0.2 Mn 0.2 O2(NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2(NCM811), LiNi 0.85 Co 0.15 Al 0.05 One or more of O2, LiFePO4 and LiMnPO4.
[0239] When the secondary battery of this application is a sodium-ion battery, the positive electrode active material may include, but is not limited to, one or more of sodium-containing transition metal oxides, polyanionic materials (such as phosphates, fluorophosphates, pyrophosphates, sulfates, etc.), and Prussian blue materials.
[0240] As an example, positive electrode active materials for sodium-ion batteries may include NaFeO2, NaCoO2, NaCrO2, NaMnO2, NaNiO2, and NaNi 1 / 2 Ti 1 / 2 O2, NaNi 1 / 2 Mn 1 / 2 O2, Na 2 / 3 Fe 1 / 3 Mn 2 / 3 O2, NaNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, NaFePO4, NaMnPO4, NaCoPO4, Prussian blue materials and materials with the general formula X p M' q (PO4) r O x Y 3-xOne or more of the materials. In general formula X p M' q (PO4) r O x Y 3-x In the given condition, 0 < p ≤ 4, 0 < q ≤ 2, 1 ≤ r ≤ 3, 0 ≤ x ≤ 2, and X includes elements selected from H. + Li + Na + K + and NH4 + One or more of the following, M' is a transition metal cation, which may be selected from one or more of V, Ti, Mn, Fe, Co, Ni, Cu and Zn, and Y is a halide anion, which may be selected from one or more of F, Cl and Br.
[0241] In this application, the modified compounds of the above-mentioned positive electrode active materials may be those that have undergone doping modification and / or surface coating modification of the positive electrode active materials.
[0242] In some embodiments, the positive electrode film may optionally include a positive electrode conductive agent. This application does not impose any particular limitation on the type of positive electrode conductive agent. As an example, the positive electrode conductive agent includes one or more of superconducting carbon, conductive graphite, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0243] In some embodiments, the positive electrode film layer may optionally include a positive electrode binder. This application does not impose any particular limitation on the type of positive electrode binder. As an example, the positive electrode binder may include one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resins.
[0244] In some embodiments, the positive current collector may be a metal foil or a composite current collector. An example of the metal foil is aluminum foil. The composite current collector may include a polymer base layer and a metal layer formed on at least one surface of the polymer base layer. An example of the metal material may be one or more of aluminum, aluminum alloys, nickel, nickel alloys, titanium, titanium alloys, silver, and silver alloys. An example of the polymer base layer may be one or more of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), and polyethylene (PE).
[0245] The positive electrode film is typically formed by coating a positive electrode slurry onto a positive electrode current collector, followed by drying and cold pressing. The positive electrode slurry is typically formed by dispersing the positive electrode active material, optional conductive agent, optional binder, and any other components in a solvent and stirring until homogeneous. The solvent may be N-methylpyrrolidone (NMP), but is not limited to this.
[0246] [Electrolytes]
[0247] The electrolyte acts as a conductor of active ions between the positive and negative electrode plates. This application does not impose specific limitations on the type of electrolyte; it can be selected according to requirements. For example, the electrolyte may include one or more selected from solid electrolytes and liquid electrolytes (i.e., electrolyte solutions).
[0248] In some embodiments, the electrolyte is an electrolyte solution comprising an electrolyte salt and a solvent.
[0249] When the secondary battery of this application is a lithium-ion battery, as an example, the electrolyte salt may include one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium perchlorate (LiClO4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalate borate (LiDFOB), lithium dioxalate borate (LiBOB), lithium difluorophosphate (LiPO2F2), lithium difluorodioxalate phosphate (LiDFOP), and lithium tetrafluorooxalate phosphate (LiTFOP).
[0250] When the secondary battery of this application is a sodium-ion battery, particularly a sodium-ion secondary battery, the electrolyte salt may include one or more of the following: sodium hexafluorophosphate (NaPF6), sodium tetrafluoroborate (NaBF4), sodium perchlorate (NaClO4), sodium hexafluoroarsenate (NaAsF6), sodium bis(fluorosulfonyl)imide (NaFSI), sodium bis(trifluoromethanesulfonyl)imide (NaTFSI), sodium trifluoromethanesulfonate (NaTFS), sodium difluorooxalate borate (NaDFOB), sodium dioxalate borate (NaBOB), sodium difluorophosphate (NaPO2F2), sodium difluorodioxalate phosphate (NaDFOP), and sodium tetrafluorooxalate phosphate (NaTFOP).
[0251] The type of solvent is not specifically limited and can be selected according to actual needs. In some embodiments, as an example, the solvent may include one or more of the following: ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butyl carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS), and diethyl sulfone (ESE).
[0252] In some embodiments, the electrolyte may optionally include additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery performance, such as additives that improve battery overcharge performance, additives that improve battery high-temperature performance, and additives that improve battery low-temperature power performance.
[0253] [Isolation membrane]
[0254] Secondary batteries using electrolytes, as well as some secondary batteries using solid electrolytes, also include a separator. The separator is disposed between the positive and negative electrodes, primarily serving to prevent short circuits between the positive and negative electrodes while allowing active ions to pass through. This application does not impose any particular limitation on the type of separator; any known porous separator with good chemical and mechanical stability can be selected.
[0255] In some embodiments, the material of the separator may include one or more of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator may be a single-layer film or a multi-layer composite film. When the separator is a multi-layer composite film, the materials of each layer may be the same or different.
[0256] [Preparation Method]
[0257] The method for preparing the secondary battery described in this application is well known. In some embodiments, a positive electrode, a separator, a negative electrode, and an electrolyte can be assembled to form a secondary battery. As an example, the positive electrode, separator, and negative electrode can be formed into an electrode assembly through a winding process and / or a stacking process. The electrode assembly is placed in an outer packaging, dried, and then injected with an electrolyte. After vacuum sealing, settling, formation, and shaping processes, a battery cell is obtained. Multiple battery cells can be further connected in series, parallel, or a combination thereof to form a battery module. Multiple battery modules can also be connected in series, parallel, or a combination thereof to form a battery pack. In some embodiments, multiple battery cells can also be directly assembled into a battery pack.
[0258] Electrical appliances
[0259] This application also provides an electrical device, which includes the secondary battery of this application.
[0260] The secondary battery can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device can be, but is not limited to, mobile devices (e.g., mobile phones, tablets, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.
[0261] The electrical device can select the specific type of secondary battery according to its usage requirements, such as a battery cell, battery module, or battery pack.
[0262] Figure 7 This is a schematic diagram illustrating an example of an electrical device. This device could be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. To meet the device's requirements for high power and high energy density, a battery pack or battery module can be used as the power source.
[0263] Another example of an electrical device could be a mobile phone, tablet, or laptop. These devices typically require a slim and lightweight design and can use a single battery cell as their power source.
[0264] Example
[0265] The following embodiments describe the disclosure of this application in more detail. These embodiments are merely illustrative, as various modifications and variations will be apparent to those skilled in the art within the scope of the disclosure of this application. Unless otherwise stated, all parts, percentages, and ratios reported in the following embodiments are based on mass, and all reagents used in the embodiments are commercially available or synthesized by conventional methods and can be used directly without further processing, and the instruments used in the embodiments are commercially available.
[0266] Example 1
[0267] (1) Preparation of negative electrode active materials
[0268] One kilogram of commercially available porous biomass carbon with a porosity of 45% was selected as the substrate and placed in a vapor deposition furnace. The furnace rotation speed was maintained at 0.5 rpm, and argon gas was used for purging. The temperature was then preheated to 200°C. The temperature was further increased to 600°C, and a first gas mixture of 30% silane and 70% argon (volume ratio) was introduced at a total gas flow rate of 2 L / min. The furnace pressure was a slightly positive pressure 400 Pa higher than atmospheric pressure, and the deposition time was 4 hours. The introduction of the first gas mixture was then stopped, and the furnace temperature was allowed to drop to 450°C. A second gas mixture of 15% silane and 85% argon (volume ratio) was then introduced at a total gas flow rate of 2 L / min, and deposition continued for 8 hours. The second mixed gas was shut off, and the temperature was raised again to 650℃. The third mixed gas was introduced with 20% acetylene and 80% argon (volume ratio), with a total gas flow rate of 2L / min and a deposition time of 0.5h. After the deposition was completed, the mixture was cooled, discharged, and passed through a 325-mesh sieve to obtain the negative electrode active material.
[0269] (2) Preparation of secondary batteries (full cells)
[0270] Preparation of negative electrode sheet: The negative electrode active material prepared above is mixed with conductive agent conductive carbon black and carbon nanotubes and binder polyacrylic acid at a mass ratio of 95:1.9:0.1:3. The mixture is then added to deionized water as a solvent and stirred under the action of a high-speed stirrer until the system is homogeneous, thereby obtaining a negative electrode slurry with a solid content of 45%. The negative electrode slurry is uniformly coated on the negative electrode current collector copper foil and dried at 85°C. After cold pressing, the negative electrode sheet is obtained.
[0271] Preparation of the positive electrode: The positive electrode active material LiNi... 0.8 Co 0.1 Mn 0.1 O2 (NCM811), conductive agent carbon black (Super P), and binder polyvinylidene fluoride (PVDF) are mixed thoroughly in an appropriate amount of solvent NMP at a mass ratio of 97:1:2 to form a uniform positive electrode slurry. The positive electrode slurry is then uniformly coated onto the surface of the positive electrode current collector aluminum foil, and after drying and cold pressing, a positive electrode sheet is obtained.
[0272] Preparation of electrolyte: Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed uniformly in a volume ratio of 20:20:60 as an organic solvent. LiPF6 was then dissolved in the organic solvent, and fluoroethylene carbonate (FEC) was added. The concentration of LiPF6 in the electrolyte was 1 mol / L, and the mass percentage of FEC was 5 wt%.
[0273] Preparation of the separator membrane: Celgard 2400 separator membrane was used.
[0274] Preparation of secondary batteries: The positive electrode, separator, and negative electrode are stacked and wound in sequence to obtain an electrode assembly; the electrode assembly is placed in an outer packaging, dried, and then injected with electrolyte. After vacuum sealing, standing, formation, and shaping, a secondary battery is obtained.
[0275] (3) Preparation of button cell (half cell)
[0276] The prepared negative electrode active material was mixed with conductive carbon black (conductive agent) and polyacrylic acid (binder) at a mass ratio of 8:1:1. The mixture was then added to deionized water and stirred under high speed until homogeneous, yielding a negative electrode slurry with a solid content of 45%. This slurry was uniformly coated onto a copper foil current collector and dried at 85°C. After cold pressing, the electrode sheet was obtained. A lithium metal sheet was used as the counter electrode, a Celgard 2400 separator was employed, and the same electrolyte as used in the secondary battery preparation was injected to assemble a coin cell.
[0277] Examples 2-19 and Comparative Example 5
[0278] The preparation methods for secondary batteries and coin cells are similar to those in Example 1, except that the preparation process parameters of the negative electrode active material are adjusted, as detailed in Table 1.
[0279] Comparative Example 1
[0280] The preparation methods for secondary batteries and coin cells are similar to those in Example 1, except that the preparation process parameters of the negative electrode active material are adjusted.
[0281] Amorphous carbon-coated crystalline silicon is used as the negative electrode active material, with a coating thickness of 300 nm.
[0282] Comparative Example 2
[0283] The preparation methods for secondary batteries and coin cells are similar to those in Example 1, except that the preparation process parameters of the negative electrode active material are adjusted.
[0284] One kilogram of commercially available porous biomass carbon with a porosity of 45% was selected as the substrate and placed in a vapor deposition furnace. The furnace rotation speed was maintained at 0.5 rpm, and argon gas was used for purging. The temperature was preheated to 200°C. The temperature was then increased to 600°C, and a first mixed gas mixture of 30% silane and 70% argon (volume ratio) was introduced at a total gas flow rate of 2 L / min. The furnace pressure was a slightly positive pressure 400 Pa higher than atmospheric pressure, and the deposition time was 12 h. The first mixed gas mixture was then turned off, and the temperature was increased again to 650°C. A second mixed gas mixture of 20% acetylene and 80% argon (volume ratio) was introduced at a total gas flow rate of 2 L / min, and the deposition time was 0.5 h. After deposition, the material was cooled, discharged, and sieved through a 325-mesh sieve to obtain the negative electrode active material.
[0285] Comparative Example 3
[0286] The preparation methods for secondary batteries and coin cells are similar to those in Example 1, except that the preparation process parameters of the negative electrode active material are adjusted.
[0287] One kilogram of commercially available porous biomass carbon with a porosity of 45% was selected as the substrate and placed in a vapor deposition furnace. The furnace rotation speed was maintained at 0.5 rpm, and argon gas was used for purging. The temperature was preheated to 200°C. The temperature was then increased to 450°C, and a first mixed gas of 15% silane and 85% argon (volume ratio) was introduced at a total gas flow rate of 2 L / min. The furnace pressure was a slightly positive pressure 400 Pa higher than atmospheric pressure, and the deposition time was 16 h. The first mixed gas was then turned off, and the temperature was increased again to 650°C. A second mixed gas of 20% acetylene and 80% argon (volume ratio) was introduced at a total gas flow rate of 2 L / min, and the deposition time was 0.5 h. After deposition, the material was cooled, discharged, and sieved through a 325-mesh sieve to obtain the negative electrode active material.
[0288] Comparative Example 4
[0289] The preparation methods for secondary batteries and coin cells are similar to those in Example 1, except that the preparation process parameters of the negative electrode active material are adjusted.
[0290] One kg of commercially available porous biomass carbon with a porosity of 45% was selected as the substrate and placed in a vapor deposition furnace. The furnace rotation speed was maintained at 0.5 rpm, and argon gas was used for purging. The temperature was preheated to 200℃. The temperature was then increased to 450℃, and a first gas mixture of 15% silane and 85% argon (volume ratio) was introduced at a total gas flow rate of 2 L / min. The furnace pressure was a slightly positive pressure 400 Pa higher than atmospheric pressure, and the deposition time was 8 h. The first gas mixture was then stopped, the furnace temperature was increased to 600℃, and a second gas mixture of 30% silane and 70% argon (volume ratio) was introduced at a total gas flow rate of 2 L / min. The deposition time was 4 h. The second gas mixture was shut off, and the temperature was raised again to 650°C. A third gas mixture of 20% acetylene and 80% argon (volume ratio) was introduced, with a total gas flow rate of 2 L / min and a deposition time of 0.5 h. After the deposition was completed, the mixture was cooled, discharged, and passed through a 325-mesh sieve to obtain the negative electrode active material.
[0291] Table 1
[0292]
[0293] Test section
[0294] (1) Grain size and area testing of crystalline silicon-based materials
[0295] A dual-beam focused ion beam microscope was used to extract cross-sectional images of the negative electrode active material particles from their cores. Then, a high-resolution transmission electron microscope was used to observe and calculate the grain size of the crystalline silicon-based material. In the acquired cross-sectional images, regions exhibiting lattice fringes were defined as a single grain, and the diameter of this region was taken as the grain size. The average of at least 50 grain sizes was used as the test result. The testing instruments included a Thermo Fisher Scientific Helios 5CX dual-beam focused ion beam / scanning electron microscope system and a Thermo Fisher Scientific Spectra S / TEM scanning transmission electron microscope.
[0296] The grain area is calculated with the grain shape being spherical, and the diameter of the sphere is calculated using the grain size.
[0297] The region defined by the outer surface of the negative electrode active material particles extending into the particle from a distance of 0.5 times the length between any point on the outer surface of the particle and the particle core is called the outer region, and the region inside the outer region is called the inner region.
[0298] In the above cross-sectional images, the ratio of the total cross-sectional area of the crystalline silicon-based material in the outer region to the total cross-sectional area of the crystalline silicon-based material in the inner region is denoted as α1. The ratio of the total cross-sectional area of the crystalline silicon-based material in the outer region to the total cross-sectional area of the amorphous silicon-based material in the above cross-sectional images is denoted as β1. The ratio of the total cross-sectional area of the crystalline silicon-based material in the inner region to the total cross-sectional area of the amorphous silicon-based material in the above cross-sectional images is denoted as β2. The ratio of the total cross-sectional area of the crystalline silicon-based material in the above cross-sectional images to the total cross-sectional area of the negative electrode active material is denoted as γ1. The ratio of the total cross-sectional area of the amorphous silicon-based material in the above cross-sectional images to the total cross-sectional area of the negative electrode active material is denoted as γ2.
[0299] (2) Element content test of negative electrode active material
[0300] The carbon content in the negative electrode active material is tested according to GB / T 20123-2006 / ISO 15350:2000. The testing instrument can be an HCS-140 infrared carbon-sulfur analyzer.
[0301] The silicon content in the negative electrode active material was tested according to GB / T 20975.5-2020.
[0302] (3) Test of average particle size Dv50 of negative electrode active material
[0303] Referring to GB / T 19077-2016, the volumetric particle size distribution curve of the negative electrode active material was obtained, and the particle size corresponding to the cumulative volume distribution percentage reaching 50% was taken as the average particle size Dv50. The testing instrument can be a Mastersizer 3000 laser particle size analyzer from Malvern Instruments Ltd., UK.
[0304] (4) Specific surface area test of negative electrode active material
[0305] Referring to GB / T 19587-2004, the nitrogen adsorption specific surface area analysis method was used for testing, and the specific surface area of the negative electrode active material was calculated using the BET (Brunauer Emmett Teller) method. The testing instrument was a TRISTAR II 3020 specific surface area and porosity analyzer from Micromeritics, USA.
[0306] (5) Pore volume test of negative electrode active material
[0307] The pore volume of the negative electrode active material was tested according to GB / T 21650.2-2008. The testing instrument can be a TRISTAR II 3020 specific surface area and porosity analyzer from Micromeritics, USA.
[0308] (6) First Coulomb efficiency test
[0309] After the prepared coin cell was left to stand for 60 minutes, it was discharged at a constant current of 0.05C to 5mV, and then discharged at 50μA to 5mV. The total discharge capacity of the coin cell was recorded as the initial lithium intercalation capacity. After standing for 10 minutes, the coin cell was charged at a constant current of 0.1C to 0.8V. The charging capacity of the coin cell was recorded as the initial lithium deintercalation capacity.
[0310] The initial coulombic efficiency of the negative electrode active material = initial delithiation capacity / initial lithium insertion capacity.
[0311] (7) Cycle performance test of secondary batteries
[0312] At 25°C, the prepared secondary battery was fully charged at 0.5C and then fully discharged at 1C. This constitutes one charge-discharge cycle. The discharge capacity at this point is recorded as the initial discharge capacity. The secondary battery was then subjected to cyclic charge-discharge tests using the above method, and the discharge capacity after each cycle was recorded until the discharge capacity of the secondary battery decreased to 80% of the initial discharge capacity. The number of cycles at this point characterizes the cycle performance of the secondary battery. The higher the number of cycles, the better the cycle performance.
[0313] (8) Volume expansion test of negative electrode sheet
[0314] At 25°C, the prepared secondary battery was fully charged at 0.33C, and then disassembled in a drying room to obtain the negative electrode sheet. The thickness H1 of the negative electrode sheet under full charge was recorded. The volume expansion rate of the negative electrode sheet = (H1-H0) / H0, where H0 represents the initial thickness of the negative electrode sheet after cold pressing.
[0315] Table 2
[0316]
[0317]
[0318] Table 3
[0319] Serial Number γ1 γ2 α1 β1 β2 Example 1 15% 48% 3.1:100 0.9:100 100:10 Example 2 20% 43% 10:100 5:100 100:2 Example 3 25% 38% 40:100 20:100 100:0 Example 4 10% 53% 0:100 0:100 100:60 Example 5 5% 58% 0:100 0:100 100:240 Comparative Example 5 40% 25% 120:100 80:100 100:0
[0320] As shown in Table 2, by ensuring that at least a portion of the silicon-based material is located within the porous structure of the matrix material, and by including both crystalline and amorphous silicon-based materials, with the crystalline silicon-based material primarily located in the internal region of the negative electrode active material and the amorphous silicon-based material primarily located in the external region, the advantages of crystalline silicon-based materials in improving initial coulombic efficiency can be fully realized, while the advantages of amorphous silicon-based materials in improving cycle performance and reducing volume expansion can also be fully realized. Therefore, the negative electrode active material provided in this application exhibits high capacity, high initial coulombic efficiency, and low volume expansion, and also enables the secondary battery to achieve high energy density, high initial coulombic efficiency, long cycle life, and long storage life.
[0321] The negative electrode active materials prepared in the above embodiments of this application all satisfy the condition that the total cross-sectional area of the crystalline silicon-based material in the outer region of the cross-sectional image is smaller than the total cross-sectional area of the crystalline silicon-based material in the inner region. Based on the test results in Tables 2 and 3, it can be seen that when the total cross-sectional area of the crystalline silicon-based material in the outer region of the cross-sectional image of the negative electrode active material is larger than the total cross-sectional area of the crystalline silicon-based material in the inner region, the secondary battery exhibits poor cycle performance and high volume expansion, failing to achieve high energy density, high initial coulombic efficiency, long cycle life, and long storage life simultaneously.
[0322] The test results from Tables 2 and 3 also show that when the negative electrode active material further satisfies the requirement that the ratio α1 of the total cross-sectional area of the crystalline silicon-based material in the outer region to the total cross-sectional area of the crystalline silicon-based material in the inner region of the cross-sectional image is (0-50):100, or can be selected as (0-10):100, the secondary battery using the negative electrode active material can better balance high energy density, high initial coulombic efficiency, long cycle life, and long storage life.
[0323] Comparative Example 1 uses carbon-coated crystalline silicon as the negative electrode active material. Crystalline silicon exhibits a significant volume effect, while the surface carbon layer offers limited protection. Furthermore, the carbon layer cracks after multiple charge-discharge cycles, leading to repeated damage and reconstruction of the SEI film, increasing the irreversible consumption of active ions. Moreover, the SEI film thickness increases with the number of charge-discharge cycles, consequently increasing the impedance of the secondary battery. Therefore, the secondary battery prepared in Comparative Example 1 exhibits very poor cycle performance.
[0324] In the negative electrode active material prepared in Comparative Example 2, the silicon-based material only includes crystalline silicon-based material and does not include amorphous silicon-based material. Because crystalline silicon-based material has large volume expansion and poor structural stability, it leads to poor cycle performance and high volume expansion of the secondary battery, and cannot enable the secondary battery to achieve high energy density, high initial coulombic efficiency, long cycle life and long storage life.
[0325] In the negative electrode active material prepared in Comparative Example 3, the silicon-based material only includes amorphous silicon-based material and does not include crystalline silicon-based material. Since the initial coulombic efficiency of amorphous silicon-based material is low, the actual capacity loss of the secondary battery is large. Therefore, the secondary battery cannot achieve high energy density, high initial coulombic efficiency, long cycle life and long storage life.
[0326] In the negative electrode active material prepared in Comparative Example 4, the crystalline silicon-based material is located in the outer region of the negative electrode active material, while the amorphous silicon-based material is located in the inner region of the negative electrode active material. This results in poor cycle performance and high volume expansion of the secondary battery, which prevents the secondary battery from simultaneously achieving high energy density, high initial coulombic efficiency, long cycle life, and long storage life.
[0327] It should be noted that this application is not limited to the above-described embodiments. The above embodiments are merely examples, and any embodiments with the same structure and effect as the technical concept within the scope of this application are included in the technical scope of this application. Furthermore, various modifications that can be conceived by those skilled in the art to the embodiments, and other ways of constructing by combining some of the constituent elements of the embodiments, without departing from the spirit of this application, are also included in the scope of this application.
Claims
1. A negative electrode active material, wherein, The negative electrode active material includes a matrix material and a silicon-based material. The matrix material includes multiple pore structures and has a porosity of 30% to 60%. The matrix material is a carbon material, which is one or more of activated carbon, biomass carbon, pyrolytic carbon, and resin carbon. At least a portion of the silicon-based material is located within the pore structures of the matrix material, and there are voids between the silicon-based material and the matrix material. The silicon-based material includes crystalline silicon-based material with a grain size greater than 0 and less than or equal to 8 nm. The region formed by extending from the outer surface of the negative electrode active material to the interior of the particle to a distance of 0.5 times the length between any point on the outer surface of the particle and the particle core is denoted as the outer region. The region inside the outer region is denoted as the inner region. In the cross-sectional image of the negative electrode active material, the total cross-sectional area of the crystalline silicon-based material in the outer region is smaller than the total cross-sectional area of the crystalline silicon-based material in the inner region. The silicon-based material also includes amorphous silicon-based material. In the cross-sectional image of the negative electrode active material, the total cross-sectional area of the amorphous silicon-based material in the outer region is greater than the total cross-sectional area of the amorphous silicon-based material in the inner region.
2. The negative electrode active material according to claim 1, wherein, The cross-sectional image of the negative electrode active material includes a cross-sectional image passing through the particle core of the negative electrode active material.
3. The negative electrode active material according to claim 1 or 2, wherein, In the cross-sectional image of the negative electrode active material, the ratio α1 of the total cross-sectional area of the crystalline silicon-based material in the outer region to the total cross-sectional area of the crystalline silicon-based material in the inner region is (0~50):
100.
4. The negative electrode active material according to claim 3, wherein, α1 is (0~10):
100.
5. The negative electrode active material according to claim 1, wherein, The ratio α2 of the total cross-sectional area of the amorphous silicon-based material in the inner region to the total cross-sectional area of the amorphous silicon-based material in the outer region is (5~30):
100.
6. The negative electrode active material according to claim 5, wherein, α2 is (5~10):
100.
7. The negative electrode active material according to claim 1, wherein, In the outer region of the cross-sectional image of the negative electrode active material, the ratio β1 of the total cross-sectional area of the crystalline silicon-based material to the total cross-sectional area of the amorphous silicon-based material is (0~25):
100. And / or, In the inner region of the cross-sectional image of the negative electrode active material, the ratio β2 of the total cross-sectional area of the crystalline silicon-based material to the total cross-sectional area of the amorphous silicon-based material is 100:(2~250).
8. The negative electrode active material according to claim 7, wherein, β1 is (0~5):100; And / or, β2 is 100:(2~100).
9. The negative electrode active material according to claim 7 or 8, wherein, In the outer region of the cross-sectional image of the negative electrode active material, the total cross-sectional area of the crystalline silicon-based material is 0.
10. The negative electrode active material according to claim 1, wherein, In the cross-sectional image of the negative electrode active material, the ratio γ1 of the total cross-sectional area of the crystalline silicon-based material to the total cross-sectional area of the negative electrode active material is greater than 0 and less than or equal to 25%; and / or, In the cross-sectional image of the negative electrode active material, the ratio γ2 of the total cross-sectional area of the amorphous silicon-based material to the total cross-sectional area of the negative electrode active material is greater than or equal to 35% and less than 100%.
11. The negative electrode active material according to claim 10, wherein, γ1 is 5%~20%; And / or, γ2 is 40%~60%.
12. The negative electrode active material according to claim 1, 2, 4, 5, 6, 7, 8, 10, or 11, wherein, The mass percentage of the crystalline silicon-based material in the silicon-based material is greater than 0 and less than or equal to 40 wt%.
13. The negative electrode active material according to claim 12, wherein, The mass percentage of the crystalline silicon-based material in the silicon-based material is 10wt% to 30wt%.
14. The negative electrode active material according to claim 1, wherein, The crystalline silicon-based material includes one or more of crystalline elemental silicon, silicon oxide, silicon-carbon materials, silicon-nitrogen composites, and silicon alloys, and / or, The amorphous silicon-based material includes one or more of amorphous elemental silicon, silicon oxide, silicon-carbon materials, silicon-nitrogen composites, and silicon alloys, and / or, The silicon-based materials include vapor-deposited silicon-based materials.
15. The negative electrode active material according to claim 14, wherein, The crystalline silicon-based material includes crystalline elemental silicon; And / or, The amorphous silicon-based material includes amorphous elemental silicon; And / or, The silicon-based material includes vapor-deposited elemental silicon.
16. The negative electrode active material according to claim 1, 2, 4, 5, 6, 7, 8, 10, 11, 13, 14, or 15, wherein, The matrix material satisfies the following condition (1): (1) The porosity of the matrix material is 40%~50%.
17. The negative electrode active material according to claim 1, 2, 4, 5, 6, 7, 8, 10, 11, 13, 14, or 15, wherein, The negative electrode active material further includes a coating layer located on at least a portion of the surface of the matrix material, and the coating layer satisfies at least one of the following conditions (1) to (2): (1) The coating layer includes one or more of carbon materials, conductive polymers, metal oxides and metal sulfides; (2) The thickness of the coating layer is 0nm~200nm.
18. The negative electrode active material according to claim 17, wherein, The coating layer includes carbon materials, which include one or more of hard carbon, soft carbon, graphene, carbon fiber, and carbon nanotubes. And / or, The thickness of the coating layer is 10nm~150nm.
19. The negative electrode active material according to claim 1, 2, 4, 5, 6, 7, 8, 10, 11, 13, 14, 15, or 18, wherein, The negative electrode active material includes carbon and silicon. The negative electrode active material contains 40wt% to 60wt% of carbon and 38wt% to 58wt% of silicon.
20. The negative electrode active material according to claim 19, wherein, The negative electrode active material contains 45wt% to 50wt% carbon by mass and 40wt% to 55wt% silicon by mass.
21. The negative electrode active material according to claim 19, wherein, The negative electrode active material also includes other elements, including one or more of oxygen, metallic elements, and nitrogen. The sum of the mass percentages of other elements in the negative electrode active material is 0 wt% to 20 wt%.
22. The negative electrode active material according to claim 21, wherein, The sum of the mass percentages of other elements in the negative electrode active material is 0 wt% to 10 wt%.
23. The negative electrode active material according to claim 1, 2, 4, 5, 6, 7, 8, 10, 11, 13, 14, 15, 18, 20, 21, or 22, wherein, The pore volume of the negative electrode active material is 0.001 cm³. 3 / g~0.02cm 3 / g, and / or, The average particle size Dv50 of the negative electrode active material is 4μm~12μm; and / or, The BET specific surface area of the negative electrode active material is 1m². 2 / g~15m 2 / g.
24. The negative electrode active material according to claim 23, wherein, The pore volume of the negative electrode active material is 0.01 cm³. 3 / g~0.02cm 3 / g.
25. A method for preparing a negative electrode active material, comprising the following steps: providing a matrix material comprising a plurality of pore structures; dispersing a silicon-based material into the pore structures of the matrix material to obtain the negative electrode active material, wherein, The negative electrode active material includes a matrix material and a silicon-based material. The matrix material has a plurality of pore structures and a porosity of 30% to 60%. The matrix material is a carbon material, specifically one or more of activated carbon, biomass carbon, pyrolytic carbon, and resin carbon. At least a portion of the silicon-based material is located within the pore structures of the matrix material, and there are voids between the silicon-based material and the matrix material. The silicon-based material includes crystalline silicon, and the grain size of the crystalline silicon is greater than 0 and less than or equal to 8 nm. The silicon-based material extends from the outer surface of the particles to the interior of the particles. The region defined by a distance of 0.5 times the length between any point on the outer surface of the particle and the particle core is denoted as the outer region, and the region inside the outer region is denoted as the inner region. In the cross-sectional image of the negative electrode active material, the total cross-sectional area of the crystalline silicon-based material in the outer region is smaller than the total cross-sectional area of the crystalline silicon-based material in the inner region. The silicon-based material also includes amorphous silicon-based material. In the cross-sectional image of the negative electrode active material, the total cross-sectional area of the amorphous silicon-based material in the outer region is larger than the total cross-sectional area of the amorphous silicon-based material in the inner region.
26. The method according to claim 25, wherein, The matrix material satisfies at least one of the following conditions (1) to (2): (1) The porosity of the matrix material is 40%~50%; (2) The average particle size Dv50 of the matrix material is 4μm~12μm.
27. The method according to claim 25, wherein, The steps of dispersing silicon-based materials into the porous structure of the matrix material include the following steps: placing the matrix material, which includes multiple porous structures, as a substrate in a reactor, introducing a first mixed gas containing silicon source gas and depositing it at a first temperature T1 for a first time t1, and stopping the introduction of the first mixed gas after the deposit is completed; after the temperature inside the furnace drops to a second temperature T2, introducing a second mixed gas containing silicon source gas and depositing it at a second temperature T2 for a second time t2, and obtaining the negative electrode active material after the deposit is completed.
28. The method according to claim 27, wherein, Before introducing the first mixed gas containing silicon source gas, the process further includes the following steps: placing a matrix material with multiple porous structures as a substrate in a reactor, and performing purging and preheating treatment using a protective gas, wherein the preheating temperature is 200°C to 300°C.
29. The method according to claim 27, wherein, The volume percentage V1 of the silicon source gas in the first mixture is greater than the volume percentage V2 of the silicon source gas in the second mixture; and / or, T1>T2; and / or, t1 <t2。 30. The method according to claim 27, wherein, The first mixed gas includes a silicon source gas and a protective gas, wherein the volume percentage V1 of the silicon source gas in the first mixed gas is 10% to 50%; and / or, The total gas flow rate of the first mixed gas is 0.5 L / min to 20 L / min; and / or, The first temperature T1 is 500℃~700℃; and / or, The first time interval t1 is 0.5h~8h.
31. The method according to claim 30, wherein, The first time interval t1 is 0.5h to 4h.
32. The method according to claim 27, wherein, The second mixture includes a silicon source gas and a protective gas, wherein the volume percentage V2 of the silicon source gas in the second mixture is 5% to 20%; and / or, The total gas flow rate of the second mixture is 0.5 L / min to 20 L / min; and / or, The second temperature T2 is 400℃~500℃; and / or, The second time t2 is 2h~16h, and / or, The total gas flow rate of the second mixture is the same as the total gas flow rate of the first mixture.
33. The method according to claim 32, wherein, The second mixed gas includes a silicon source gas, a carbon source gas, and a protective gas. The volume percentage (V2) of the silicon source gas in the second mixed gas is 5% to 20%, and the volume percentage of the carbon source gas is 5% to 10%.
34. The method according to claim 32 or 33, wherein, The second time, t2, is 4h to 16h.
35. The method according to claim 25 or 26 or 27 or 28 or 29 or 30 or 31 or 32 or 33, further comprising the step of forming a coating layer on at least the surface of the obtained negative electrode active material, said coating layer comprising one or more of carbon materials, conductive polymers, metal oxides and metal sulfides.
36. The method according to claim 35, wherein, The step of forming the coating layer includes the following steps: placing the obtained negative electrode active material in a reactor, introducing a third mixed gas containing carbon source gas, and depositing it at a third temperature T3 for a third time t3 to obtain a carbon-coated negative electrode active material.
37. The method of claim 36, wherein, The third mixture includes a carbon source gas and a protective gas, wherein the volume percentage (V3) of the carbon source gas in the third mixture is 10% to 50%; and / or, The total gas flow rate of the third mixture is 0.5 L / min to 20 L / min; and / or The third temperature T3 is 600℃~700℃; and / or, The third time, t3, is 0.5h to 2h.
38. A secondary battery, comprising a negative electrode sheet, said negative electrode sheet comprising the negative electrode active material according to any one of claims 1 to 24 or the negative electrode active material prepared by any one of claims 25 to 37.
39. An electrical device comprising the secondary battery of claim 38.
Citation Information
Patent Citations
Anode active material for lithium secondary battery and lithium secondary battery including the anode active material
CN105655568A
Silicon-carbon negative electrode material and preparation method thereof
CN114864917A