A perovskite solar cell film, its preparation method and application

By pre-forming an atmosphere rich in primary source gas on the substrate and utilizing the ALD-CVD-ALD combined reaction, the problem of nucleation delay caused by island growth in atomic layer deposition was solved, enabling the preparation of high-quality films, improving the performance of perovskite solar cells and reducing costs.

CN116782727BActive Publication Date: 2026-11-17WUXI UTMOST LIGHT TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310742361.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-21
Publication Date
2026-11-17
Estimated Expiration
2043-06-21

AI Technical Summary

Technical Problem

In the existing atomic layer deposition method for preparing perovskite solar cell films, the island-like growth pattern leads to delayed nucleation, hindering continuous film growth and affecting film quality and cost.

Method used

An atmosphere rich in primary source gas is pre-formed on the substrate, and a film is prepared by atomic layer deposition to provide more nucleation sites. An ALD-CVD-ALD combined reaction is used to shorten the preparation time.

Benefits of technology

It forms a dense, complete, high-quality film layer, improves battery performance, saves manufacturing time, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116782727B_ABST
    Figure CN116782727B_ABST
Patent Text Reader

Abstract

This invention provides a perovskite solar cell film layer, its preparation method, and its application. The preparation method includes the following steps: (1) introducing a first source gas and a protective gas into a first substrate to form an atomic layer of the first source gas on the first substrate, thereby obtaining a second substrate; (2) introducing the first source gas and the second source gas into the second substrate to perform an ALD reaction, thereby obtaining the perovskite solar cell film layer. This invention first creates an atmosphere rich in the first source gas, allowing an atomic layer of the first source gas to be pre-formed on the substrate. This enables the first source gas to be better adsorbed on the surface of the substrate and provides more nucleation sites, thus forming a denser, more complete, and higher-quality film layer in subsequent processes, effectively improving battery performance. Furthermore, this method saves processing time and reduces costs.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of photovoltaics, specifically relating to a perovskite solar cell film layer, its preparation method, and its application. Background Technology

[0002] In recent years, perovskite solar cell technology has developed rapidly. In perovskite solar cells, the perovskite layer, electron transport layer, hole transport layer, and electrodes are all important components, and their quality has a significant impact on the performance of the cell.

[0003] Among existing film fabrication processes, atomic layer deposition (ALD) has received widespread attention due to its high film quality. ALD is a self-limiting surface reaction, providing conformal growth layer by layer with thicknesses in the nanometer range, and has proven to be an excellent technique for preparing perovskite buffer layers. However, ALD relies on self-limiting surface reactions closely related to surface groups on the deposition substrate. Wilfried Vandervorst et al. proposed that when the substrate does not react with the reactants in ALD, the process becomes island-like growth, also known as substrate-inhibited growth. Recent studies have increasingly shown that island-like growth is detrimental to continuous film growth. Byung Joon Choi et al. also mentioned that in island-like growth mode, the nucleation stage of ALD is unsatisfactory, hindering layer-by-layer growth and leading to delayed nucleation. This phenomenon occurs because there are fewer reaction sites on the substrate surface, meaning that grain nucleation requires more time, leading to increased costs.

[0004] Therefore, how to provide more nucleation sites for the reactants in atomic layer deposition in order to form denser, more complete, and higher-quality thin films is a technical problem that urgently needs to be solved. Summary of the Invention

[0005] To address the shortcomings of existing technologies, the present invention aims to provide a perovskite solar cell film, its preparation method, and its applications. In preparing the film using atomic layer deposition (ALD), the present invention first creates an atmosphere rich in a primary source gas, pre-forming an atomic layer of the primary source gas on the substrate. This allows the primary source gas to be better adsorbed onto the substrate surface and provides more nucleation sites, resulting in a denser, more complete, and higher-quality film in subsequent processes. The performance of the battery prepared using this method is significantly improved. Furthermore, this preparation method saves processing time and reduces costs.

[0006] To achieve this objective, the present invention adopts the following technical solution:

[0007] In a first aspect, the present invention provides a method for preparing a film layer of a perovskite solar cell, the method comprising the following steps:

[0008] (1) A first source gas and a protective gas are introduced into a first substrate to form an atomic layer of the first source gas on the first substrate, thereby obtaining a second substrate;

[0009] (2) Introduce the first source gas and the second source gas into the second substrate to carry out the ALD reaction and obtain the perovskite solar cell film layer.

[0010] In this invention, when preparing the film layer using atomic layer deposition, an atmosphere rich in a first source gas is first created, so that an atomic layer of the first source gas is pre-formed on the substrate. This allows the first source gas to be better adsorbed on the surface of the substrate and provides more nucleation sites, thereby enabling the formation of a denser and more complete high-quality film layer in subsequent processes. The performance of the battery prepared based on this method is significantly improved.

[0011] As a preferred technical solution of the present invention, in step (1), the atomic layer of the first source gas is a single atomic layer.

[0012] Preferably, in step (1), the first source gas is carried into the reaction chamber by the first carrier gas.

[0013] In this invention, the first carrier gas can refer to a gas that does not chemically react with the substances it comes into contact with during the transport process, and is used to transport the substances to be transported. The carrier gas can be an inert gas, such as any one or a combination of at least two of nitrogen, helium, neon, argon, krypton, xenon, and radon. The term "second carrier gas" follows the same principle.

[0014] In this invention, if multiple substances transported by the first carrier gas are mixed, they will contaminate each other, leading to problems such as pipe blockage and source contamination.

[0015] Preferably, the first source gas comprises tetra(dimethylamino)tin or trimethylaluminum.

[0016] Preferably, the protective gas includes nitrogen.

[0017] Preferably, the flow rate of the first source gas is 500-2000 sccm, for example, it can be 500 sccm, 1000 sccm, 1500 sccm or 2000 sccm.

[0018] In this invention, the flow rate of the first source gas refers to the flow rate of the first source gas transported by the first carrier gas in a gaseous state, including a mist state.

[0019] Preferably, the flow rate of the first carrier gas is 5000-8000 sccm, for example, it can be 5000 sccm, 5500 sccm, 6000 sccm, 6500 sccm, 7000 sccm, 7500 sccm or 8000 sccm, etc.

[0020] Preferably, the flow rate of the protective gas in step (1) is denoted as L1, the flow rate of the first source gas in step (1) is denoted as L2, and the flow rate of the first carrier gas is denoted as L3, where L1 = L2 + L3.

[0021] Preferably, the time for forming the atomic layer of the first source gas in step (1) is 5-30s, for example, it can be 5s, 6s, 7s, 8s, 9s, 10s, 15s, 20s, 25s or 30s.

[0022] In this invention, if the time for forming the atomic layer of the first source gas in step (1) is too short, the first source gas will not completely cover the substrate surface; if the time for forming the atomic layer of the first source gas in step (1) is too long, the coverage will be too thick, resulting in incomplete subsequent reactions.

[0023] As a preferred technical solution of the present invention, in step (1), the first source gas and the protective gas are alternately introduced into the same chamber to carry out a time-type ALD reaction, so that the atomic layer of the first source gas is adsorbed on the first substrate.

[0024] It should be noted that time-type ALD refers to the process in which a first source gas and a protective gas are alternately introduced into the same chamber, so that only a monolayer of the first source gas is adsorbed and formed on the first substrate.

[0025] Preferably, the alternating insertion is performed at least once, for example, once, twice, three times, or four times.

[0026] As a preferred technical solution of the present invention, in step (2), the first source gas and the second source gas are sequentially introduced into the same chamber to carry out a time-type ALD reaction to obtain a perovskite solar cell film layer.

[0027] Preferably, in step (2), the first source gas, the first inert source gas, the second source gas, and the second inert source gas are sequentially introduced into the same chamber to carry out a time-type ALD reaction, thereby obtaining a perovskite solar cell film layer.

[0028] It should be noted that the function of the first inert source gas and the second inert source gas is to purge. The first inert source gas is used to purge the second substrate after it has adsorbed the first source gas, and the second inert source gas is used to purge the second substrate after it has adsorbed the second source gas.

[0029] Preferably, the first inert gas and the second inert gas are of the same type.

[0030] The present invention does not specifically limit the types of the first inert source gas and the second inert source gas. For example, they can be nitrogen, helium, neon, argon, krypton, xenon or radon.

[0031] As another preferred technical solution of the present invention, in step (1), the first source gas and the protective gas are simultaneously introduced into different chambers to carry out a spatial ALD reaction, so that the atomic layer of the first source gas is adsorbed on the first substrate.

[0032] It should be noted that the spatial ALD reaction refers to the adsorption and purging of the first source gas on the first substrate by using different chambers to form a monolayer of the first source gas.

[0033] Preferably, the spatial ALD reaction is repeated at least once, for example, once, twice, three times, or four times.

[0034] Preferably, step (1) further includes introducing a first inert gas and a second inert gas into the first substrate. The first gas, the first inert gas, the protective gas, and the second inert gas are introduced into the first chamber, the second chamber, the third chamber, and the fourth chamber simultaneously. The first chamber, the second chamber, the third chamber, and the fourth chamber are divided clockwise or counterclockwise.

[0035] In this invention, the flow rates of the first inert source gas and the second inert source gas are greater than or equal to the flow rate of the first source gas or the protective gas, which can achieve the separation function. Therefore, the first inert source gas and the second inert source gas are also referred to as separating gases.

[0036] Preferably, the rotational speed of the first substrate is 10-50 rpm, for example, it can be 10 rpm, 12 rpm, 14 rpm, 16 rpm, 18 rpm, 20 rpm, 22 rpm, 24 rpm, 26 rpm, 28 rpm, 30 rpm, 35 rpm, 40 rpm, 45 rpm or 50 rpm.

[0037] Preferably, in step (2), the first source gas and the second source gas are simultaneously introduced into different chambers to carry out a spatial ALD reaction, thereby obtaining a perovskite solar cell film layer.

[0038] Preferably, step (2) further includes introducing a first inert source gas and a second inert source gas into the second substrate. In step (2), the first source gas, the first inert source gas, the second source gas and the second inert source gas are simultaneously introduced into the first chamber, the second chamber, the third chamber and the fourth chamber, respectively, to carry out a spatial ALD reaction and obtain a perovskite solar cell film layer.

[0039] Preferably, in step (2), the rotational speed of the second substrate is 20-100 rpm, for example, it can be 20 rpm, 40 rpm, 60 rpm, 80 rpm or 100 rpm. Preferably, in step (2), the second source gas is carried into the reaction chamber by the second carrier gas.

[0040] The present invention does not specifically limit the type of the second carrier; for example, it may be nitrogen.

[0041] Preferably, the second source gas includes any one of O2, O3, H2O, or H2O2.

[0042] Preferably, the flow rate of the second source gas is 500-2000 sccm, for example, it can be 500 sccm, 1000 sccm, 1500 sccm or 2000 sccm.

[0043] In this invention, the flow rate of the second source gas refers to the flow rate of the second source gas transported by the second carrier gas in a gaseous state, including a mist state.

[0044] Preferably, the flow rate of the second carrier gas is 5000-8000 sccm, for example, it can be 5000 sccm, 5500 sccm, 6000 sccm, 6500 sccm, 7000 sccm, 7500 sccm or 8000 sccm, etc.

[0045] Preferably, during the ALD reaction in step (2), the temperature of the second substrate is 80-150°C, for example, it can be 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C or 150°C.

[0046] Preferably, the ALD reaction time in step (2) is 50-200s, for example, it can be 50s, 75s, 100s, 125s, 150s, 175s or 200s.

[0047] As a preferred technical solution of the present invention, the ALD reaction in step (2) includes a first-order reaction, a second-order reaction and a third-order reaction carried out in sequence.

[0048] This invention completes a combined reaction of atomic layer deposition-chemical vapor deposition-atomic layer deposition, namely a combined reaction of ALD reaction-CVD reaction-ALD reaction. Under the premise of obtaining high-quality film, it greatly shortens the preparation time and meets the requirements of industrialization.

[0049] It should be noted that in this invention, for the combined ALD reaction-CVD reaction-ALD reaction, the ALD reaction refers to the process where, after the first source gas undergoes an adsorption reaction, it is purged with an inert gas, leaving only a layer of the first source gas adsorbed on the substrate surface. This layer reacts fully with the subsequently adsorbed second source gas, and then the excess second source gas is purged with an inert gas, leaving only the reaction products. The CVD reaction refers to the process where, after the first source gas undergoes an adsorption reaction, it is purged with an inert gas, but a relatively thick layer of the first source gas adsorbed on the substrate surface remains, not having been purged into a single atomic layer. After reacting with the subsequently adsorbed second source gas, a portion of the first source gas that did not participate in the reaction, the reaction products, and the excess second source gas remain. The excess second source gas is then purged with an inert gas, but a certain thickness of the second source gas is still retained, not having been purged into a single atomic layer. The products at this point sequentially include the first source gas, the reaction products, and the second source gas.

[0050] Preferably, the rotational speed of the second substrate during the first-order reaction in step (2) is the same as that of the first substrate in step (1).

[0051] In this invention, the rotational speed of the second substrate during the first-order reaction in step (2) is the same as that of the first substrate in step (1), which is beneficial for the connection and transition with the subsequent normal process.

[0052] Preferably, in step (2), the flow rates of the first inert gas and the second inert gas during the second-order reaction are less than the flow rates during the first-order reaction and the third-order reaction.

[0053] In this invention, when the flow rates of the first and second inert source gases are high, the purging effect is strong, allowing reactants to deposit only a single atomic layer without residue, thus enabling first-order or third-order reactions. When the flow rates of the first and second inert source gases are slow, the purging effect is weak, and reactants remain, thus enabling second-order reactions. The specific gas flow rate design can be selected by those skilled in the art based on the specific type of chemical reaction, with the actual effect meeting the requirements; this application does not impose any limitations.

[0054] Preferably, the rotational speed of the substrate during the second-order reaction is greater than that during the first-order reaction, and the rotational speed of the substrate during the second-order reaction is greater than that during the third-order reaction.

[0055] In this invention, if the substrate rotation speed is equal during the first-order, second-order, and third-order reactions, only the same reaction will be carried out, making it difficult to simultaneously achieve short preparation time and high-quality film preparation. If the substrate rotation speed is greater than that during the second-order reaction in both the first-order and third-order reactions, a combined reaction of chemical vapor deposition-atomic layer deposition-chemical vapor deposition will occur, reducing the film quality.

[0056] Preferably, the rotational speed of the substrate during the first-order reaction is 20-60 rpm, for example, it can be 20 rpm, 30 rpm, 40 rpm, 50 rpm or 60 rpm.

[0057] Preferably, the substrate rotation speed during the second-order reaction is 60-100 rpm, for example, it can be 60 rpm, 70 rpm, 80 rpm, 90 rpm or 100 rpm.

[0058] Preferably, the substrate rotation speed during the third-order reaction is 20-60 rpm, for example, it can be 20 rpm, 30 rpm, 40 rpm, 50 rpm or 60 rpm, etc.

[0059] In a second aspect, the present invention provides a membrane preparation device used in the preparation method described in the first aspect. The membrane preparation device includes a reaction chamber and a vacuum device communicating with the reaction chamber. A rotating device is provided at the bottom of the inner cavity of the reaction chamber. The space above the rotating device is divided into at least two working areas in a counterclockwise or clockwise direction.

[0060] Of the at least two working areas, at least one working area is connected to the first gas source via a pipeline, and at least one working area is connected to the second gas source via a pipeline.

[0061] In this invention, the type of gas source is not limited; for example, it may be a source bottle, etc.

[0062] In this invention, the rotating device is not limited; for example, it may be a rotating tray or a guide rail.

[0063] In this invention, the rotating tray is controlled by a motor to rotate within the reaction chamber.

[0064] In this invention, the type of vacuum pump is not limited; for example, it may be a mechanical pump or a Roots pump.

[0065] As a preferred technical solution of the present invention, the space above the rotating device is divided into four working areas along the counterclockwise or clockwise direction, including a first working area, a second working area, a third working area and a fourth working area;

[0066] Of the four working areas, the first working area is connected to the first gas source through a pipeline, the second working area is connected to the third gas source through a pipeline, the third working area is connected to the second gas source through a pipeline, and the fourth working area is connected to the fourth gas source through a pipeline.

[0067] The present invention does not specifically limit the temperature of the container containing the source gas. For example, the temperature of the container containing the source gas can be 60-100℃, including 60℃, 70℃, 80℃, 90℃ or 100℃, etc.

[0068] The present invention does not specifically limit the temperature of the pipeline connecting the working area and the gas source. For example, the pipeline temperature can be 70-90℃, including 70℃, 75℃, 80℃, 85℃ or 90℃, etc.

[0069] Preferably, the first source gas and the first carrier gas in the first gas source are mixed in the pipeline and enter the reaction chamber. The protective gas is first introduced into the reaction chamber through the pipeline connecting the third working area and the second gas source, and then the second source gas and the second carrier gas in the second gas source are introduced into the pipeline and mixed in the pipeline and enter the reaction chamber.

[0070] In this invention, the purpose of first introducing a protective gas into the reaction chamber is to create an atmosphere rich in the first source gas within the reaction chamber, thereby enabling the substrate surface to adsorb and form an atomic layer of the first source gas, providing more nucleation sites for subsequent reactions and enabling better film formation. This greatly improves battery performance and saves process time.

[0071] Preferably, the gases in the third and fourth gas sources are both inert source gases.

[0072] As a preferred technical solution of the present invention, a chamber cover is provided at the top opening of the reaction chamber, and the chamber cover includes a ventilation panel corresponding to the working area arranged in a counterclockwise or clockwise direction.

[0073] Preferably, the ventilation panel has a ventilation port.

[0074] Preferably, each of the ventilation panels has at least one ventilation port.

[0075] Preferably, the vent is selected from a slit or a hole.

[0076] In this invention, using slits or holes as vents allows the introduced gas to be deposited more evenly on the substrate.

[0077] Preferably, the reaction chamber is provided with a partition, which divides the space above the rotating device into a first chamber, a second chamber, a third chamber, and a fourth chamber in a counterclockwise or clockwise direction, respectively corresponding to the first working area, the second working area, the third working area, and the fourth working area.

[0078] Thirdly, the present invention provides a perovskite solar cell film layer, wherein the perovskite solar cell film layer is prepared by the preparation method described in the first aspect.

[0079] Preferably, the thickness of the film layer is 5-30nm, for example, it can be 5nm, 10nm, 15nm, 20nm, 25nm or 30nm, etc.

[0080] Preferably, the film layer includes any one of a perovskite layer, an electron transport layer, a hole transport layer, or an encapsulation layer.

[0081] Fourthly, the present invention provides a photovoltaic device, the photovoltaic device comprising the film layer of a perovskite solar cell as described in the third aspect.

[0082] The numerical range described in this invention includes not only the point values ​​listed above, but also any point values ​​within the numerical ranges not listed above. Due to space limitations and for the sake of brevity, this invention will not exhaustively list all the specific point values ​​included in the range.

[0083] Compared with the prior art, the present invention has the following beneficial effects:

[0084] (1) In the present invention, when preparing the film layer by atomic layer deposition, an atomic layer of the first source gas is formed on the substrate in advance, which can provide more nucleation sites for the subsequent deposition of the first source gas, thereby forming a denser and more complete high-quality film in the subsequent process. The performance of the battery prepared based on this method is significantly improved.

[0085] (2) The preparation method provided by the present invention saves the preparation time of the film layer and reduces the cost. Attached Figure Description

[0086] Figure 1 This is a process flow diagram for preparing the film layer in Example 1 of the present invention.

[0087] Figure 2 This is a schematic diagram of the film preparation equipment used in Embodiment 1 of the present invention.

[0088] Figure 3 This is a schematic diagram of the chamber cover plate in the membrane preparation equipment used in Embodiment 1 of the present invention.

[0089] Figure 4 This is a schematic diagram of the rotating tray in the preparation equipment used in Embodiment 1 of the present invention.

[0090] Among them, 1-reaction chamber, 2-rotating device, 3-chamber cover, 4-ventilation panel, 5-ventilation port, 6-first base, 7-partition. Detailed Implementation

[0091] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.

[0092] In one embodiment, the present invention provides a method for preparing a film layer of a perovskite solar cell, the method comprising the following steps;

[0093] (1) A 20 nm nickel oxide layer was prepared as a hole transport layer on a cleaned 2.5 × 2.5 cm fluorine-doped tin oxide (FTO) conductive glass substrate using magnetron sputtering. A perovskite layer was then prepared on the hole transport layer using slot coating, and an electron transport layer C was prepared using thermal evaporation. 60 Thus, the first basis is obtained;

[0094] (2) Place the first substrate in the reaction chamber, alternately introduce the first source gas and the protective gas into the reaction chamber, and carry out a time-type ALD reaction for 5-30s to form a monoatom layer of the first source gas on the first substrate to obtain the second substrate. The number of times the gas is alternately introduced is at least once.

[0095] The first source gas is carried into the reaction chamber by the first carrier gas. The first source gas is tetra(dimethylamino)tin or trimethylaluminum, and the flow rate is 500-2000 sccm. The first carrier gas is nitrogen, and the flow rate is 5000-8000 sccm. The protective gas is nitrogen, and the flow rate is the total flow rate of the first source gas and the first carrier gas.

[0096] (3) The first source gas, the first inert source gas, the second source gas and the second inert source gas are sequentially introduced into the reaction chamber to carry out a time-type ALD reaction of 50-200s to obtain the perovskite solar cell film layer.

[0097] The second source gas is carried into the reaction chamber by the second carrier gas. The flow rate of the second source gas is 500-2000 sccm, and the flow rate of the second carrier gas is 5000-8000 sccm. The first inert source gas and the second inert source gas are both nitrogen, and their flow rates are greater than or equal to the flow rates of the first source gas or the protective gas.

[0098] In another embodiment, the present invention provides the following examples.

[0099] Example 1

[0100] This embodiment provides a method for preparing the film layer of a perovskite solar cell, and the process flow diagram of the preparation method is shown below. Figure 1 As shown, the preparation method employs the following... Figure 2 The membrane preparation apparatus shown includes the following steps in its preparation method:

[0101] (1) A 20 nm nickel oxide layer was prepared as a hole transport layer on a cleaned 2.5 × 2.5 cm fluorine-doped tin oxide (FTO) conductive glass substrate using magnetron sputtering. A perovskite layer was then prepared on the hole transport layer using slot coating, and an electron transport layer C was prepared using thermal evaporation. 60 Thus, the first base 6 is obtained;

[0102] (2) Place the first substrate 6 on the rotating tray 2 of the reaction chamber 1, such as Figure 4 As shown, the temperature of the first substrate 6 is controlled at 120°C, and a vacuum is drawn into the reaction chamber 1 to a vacuum level of 10Pa by a mechanical pump.

[0103] Each ventilation panel in the chamber cover has two slits.

[0104] (3) Tetra(dimethylamino)tin (TDMASn) with a flow rate of 2000 sccm and a first carrier gas (i.e., nitrogen) with a flow rate of 5000 sccm are mixed in a pipeline to form a gas with a total flow rate of 7000 sccm. This gas is introduced into the first working area. At the same time, nitrogen with a flow rate of 7000 sccm is introduced into the second working area through a pipeline. At the same time, nitrogen with a flow rate of 7000 sccm is introduced into the third working area through a pipeline. At the same time, nitrogen with a flow rate of 7000 sccm is introduced into the fourth working area through a pipeline. The introduction time is 30s. The rotating tray 2 is rotated at a speed of 20 rpm so that the first substrate 6 passes through the first working area, the second working area, the third working area and the fourth working area in sequence, so that a single atomic layer of TDMASn is adsorbed and formed on the first substrate 6 to obtain the second substrate.

[0105] The source bottle temperature of TDMASn is 80℃, and the temperature of the pipeline is 90℃.

[0106] (4) TDMASn with a flow rate of 1000 sccm and nitrogen with a flow rate of 6000 sccm are mixed in a pipeline to form a gas with a total flow rate of 7000 sccm. This gas is introduced into the first working area. At the same time, nitrogen with a flow rate of 7000 sccm is introduced into the second working area through a pipeline. At the same time, H2O with a flow rate of 2000 sccm and nitrogen with a flow rate of 5000 sccm are mixed in a pipeline and introduced into the third working area. At the same time, nitrogen with a flow rate of 7000 sccm is introduced into the fourth working area through a pipeline. The rotating tray 2 is rotated stepwise so that the second substrate passes through the first working area, the second working area, the third working area and the fourth working area in sequence. At the same time, it is rotated at 20 rpm for 40 s, at 60 rpm for 20 s and at 20 rpm for 40 s in sequence to complete the first-order reaction, the second-order reaction and the third-order reaction, and obtain the SnO2 buffer layer, that is, the film layer, with a thickness of 10 nm.

[0107] The source bottle temperature of TDMASn is 80℃, the temperature of the pipeline is 90℃, and the source bottle temperature of H2O is 80℃.

[0108] Figure 3 A schematic diagram of the chamber cover plate in the membrane preparation equipment used in this embodiment is shown.

[0109] Example 2

[0110] This embodiment provides a method for preparing a film layer of a perovskite solar cell. The preparation method uses the film preparation equipment described in Example 1, and includes the following steps:

[0111] (1) A 20 nm nickel oxide layer was prepared as a hole transport layer on a cleaned 2.5 × 2.5 cm fluorine-doped tin oxide (FTO) conductive glass substrate using magnetron sputtering. A perovskite layer was then prepared on the hole transport layer using slot coating, and an electron transport layer C was prepared using thermal evaporation. 60 Thus, the first base 6 is obtained;

[0112] (2) Place the first substrate 6 on the rotating tray 2 of the reaction chamber 1, and control the temperature of the first substrate 6 to 80°C. Use a mechanical pump to evacuate the vacuum in the reaction chamber 1 to 10Pa.

[0113] Each ventilation panel in the chamber cover has two slits.

[0114] (3) Tetra(dimethylamino)tin (TDMASn) with a flow rate of 1500 sccm and a first carrier gas (i.e., nitrogen) with a flow rate of 5500 sccm are mixed in a pipeline to form a gas with a total flow rate of 7000 sccm. This gas is introduced into the first working area. At the same time, nitrogen with a flow rate of 7000 sccm is introduced into the second working area through a pipeline. At the same time, nitrogen with a flow rate of 7000 sccm is introduced into the third working area through a pipeline. At the same time, nitrogen with a flow rate of 7000 sccm is introduced into the fourth working area through a pipeline. The introduction time is 15s. The rotating tray 2 is rotated at a speed of 40 rpm so that the first substrate 6 passes through the first working area, the second working area, the third working area and the fourth working area in sequence, so that a single atomic layer of TDMASn is adsorbed and formed on the first substrate 6 to obtain the second substrate.

[0115] The source bottle temperature of TDMASn is 60℃, and the temperature of the pipeline is 70℃.

[0116] (4) TDMASn with a flow rate of 1000 sccm and nitrogen with a flow rate of 6000 sccm are mixed in a pipeline to form a gas with a total flow rate of 7000 sccm. This gas is introduced into the first working area. At the same time, nitrogen with a flow rate of 7000 sccm is introduced into the second working area through a pipeline. At the same time, H2O with a flow rate of 1000 sccm and nitrogen with a flow rate of 6000 sccm are mixed in a pipeline and introduced into the third working area. At the same time, nitrogen with a flow rate of 7000 sccm is introduced into the fourth working area through a pipeline. The rotating tray 2 is rotated stepwise so that the second substrate passes through the first working area, the second working area, the third working area and the fourth working area in sequence. At the same time, it is rotated at 40 rpm for 80 s, at 80 rpm for 40 s and at 40 rpm for 80 s in sequence to complete the first-order reaction, the second-order reaction and the third-order reaction, to obtain the SnO2 buffer layer, that is, the film layer, with a thickness of 20 nm.

[0117] The source bottle temperature of TDMASn is 60℃, the temperature of the pipeline is 70℃, and the source bottle temperature of H2O is 60℃.

[0118] Example 3

[0119] This embodiment provides a method for preparing a film layer of a perovskite solar cell. The preparation method uses the film preparation equipment described in Example 1, and includes the following steps:

[0120] (1) A 20 nm nickel oxide layer was prepared as a hole transport layer on a cleaned 2.5 × 2.5 cm fluorine-doped tin oxide (FTO) conductive glass substrate using magnetron sputtering. A perovskite layer was then prepared on the hole transport layer using slot coating, and an electron transport layer C was prepared using thermal evaporation. 60 Thus, the first base 6 is obtained;

[0121] (2) Place the first substrate 6 on the rotating tray 2 of the reaction chamber 1, and control the temperature of the first substrate 6 to 150°C. Use a mechanical pump to evacuate the vacuum in the reaction chamber 1 to 10Pa.

[0122] Each ventilation panel in the chamber cover has two slits.

[0123] (3) Tetra(dimethylamino)tin (TDMASn) with a flow rate of 1000 sccm and a first carrier gas (i.e., nitrogen) with a flow rate of 6000 sccm are mixed in a pipeline to form a gas with a total flow rate of 7000 sccm. This gas is introduced into the first working area. At the same time, nitrogen with a flow rate of 7000 sccm is introduced into the second working area through a pipeline. At the same time, nitrogen with a flow rate of 7000 sccm is introduced into the third working area through a pipeline. At the same time, nitrogen with a flow rate of 7000 sccm is introduced into the fourth working area through a pipeline. The introduction time is 10 s. The rotating tray 2 is rotated at a speed of 60 rpm so that the first substrate 6 passes through the first working area, the second working area, the third working area and the fourth working area in sequence, so that a single atomic layer of TDMASn is adsorbed and formed on the first substrate 6 to obtain the second substrate.

[0124] The source bottle temperature of TDMASn is 100℃, and the temperature of the pipeline is 80℃.

[0125] (4) TDMASn with a flow rate of 500 sccm and nitrogen with a flow rate of 6500 sccm are mixed in a pipeline to form a gas with a total flow rate of 7000 sccm. This gas is introduced into the first working area. At the same time, nitrogen with a flow rate of 7000 sccm is introduced into the second working area through a pipeline. At the same time, H2O with a flow rate of 500 sccm and nitrogen with a flow rate of 6500 sccm are mixed in a pipeline and introduced into the third working area. At the same time, nitrogen with a flow rate of 7000 sccm is introduced into the fourth working area through a pipeline. The rotating tray 2 is rotated stepwise so that the second substrate passes through the first working area, the second working area, the third working area and the fourth working area in sequence. At the same time, it is rotated at 60 rpm for 20 s, at 100 rpm for 10 s and at 60 rpm for 20 s in sequence to complete the first-order reaction, the second-order reaction and the third-order reaction, and obtain the SnO2 buffer layer, that is, the film layer, with a thickness of 5 nm.

[0126] The source bottle temperature of TDMASn is 90℃, the temperature of the pipeline is 80℃, and the source bottle temperature of H2O is 90℃.

[0127] Example 4

[0128] The difference between this embodiment and embodiment 1 is that the time for introducing the substance in step (3) is 2 seconds.

[0129] The remaining preparation methods and parameters are consistent with those in Example 1.

[0130] Example 5

[0131] The difference between this embodiment and embodiment 1 is that the time for introducing the substance in step (3) is 35 seconds.

[0132] The remaining preparation methods and parameters are consistent with those in Example 1.

[0133] Example 6

[0134] The difference between this embodiment and embodiment 1 is that the rotational speed of the rotating tray 2 in step (3) is 5 rpm.

[0135] The remaining preparation methods and parameters are consistent with those in Example 1.

[0136] Example 7

[0137] The difference between this embodiment and embodiment 1 is that the rotational speed of the rotating tray 2 in step (3) is 60 rpm.

[0138] The remaining preparation methods and parameters are consistent with those in Example 1.

[0139] Comparative Example 1

[0140] The difference between this comparative example and Example 1 is that step (3) is omitted.

[0141] The remaining preparation methods and parameters are consistent with those in Example 1.

[0142] Performance testing

[0143] The samples prepared in Examples 1-7 and Comparative Example 1 were taken out, and then a Cu metal electrode was prepared on the surface of the sample using vacuum deposition to obtain an effective area of ​​1 cm². 2 Perovskite solar cells.

[0144] The photoelectric performance of the perovskite solar cells obtained above was tested.

[0145] Test conditions: AM1.5, 1000W / m 2 , 25±2℃.

[0146] The test results are shown in Table 1.

[0147] Table 1

[0148]

[0149] analyze:

[0150] As shown in the table above, when preparing the film layer using atomic layer deposition, the present invention first creates an atmosphere rich in the first source gas, so that the first source gas can be better adsorbed on the surface of the substrate and provide more nucleation sites, thereby forming a denser and more complete high-quality film in subsequent processes. The performance of the battery prepared based on this method is significantly improved.

[0151] A comparison of the data results from Examples 1 and 4-5 shows that if the time for introducing the precursor in step (3) is too short, the tin-rich precursor atmosphere will be insufficient, resulting in the substrate not being able to completely cover a layer of tin precursor, and insufficient nucleation sites for the SnO2 film, thus leading to a decrease in battery efficiency. If the time for introducing the precursor in step (3) is too long, the tin precursor coverage will be too thick, thus affecting the subsequent normal ALD reaction and causing a decrease in battery efficiency.

[0152] Comparison of the data results of Example 1 and Examples 6-7 shows that if the rotation speed of the rotating tray in step (3) is too low, the deposited tin precursor is too thin, the substrate cannot completely cover a layer of tin precursor, and the battery performance will decrease; if the rotation speed of the rotating tray in step (3) is too high, the tin precursor will be covered too thickly, thereby affecting the subsequent normal ALD reaction and the battery efficiency will decrease.

[0153] A comparison of the data results from Example 1 and Comparative Example 1 shows that if an atmosphere rich in the first source gas is not created before the film layer is formed, it is difficult to increase the nucleation sites on the substrate, resulting in delayed nucleation, making it difficult to obtain a dense and complete film layer, reducing the film quality, and thus making it difficult to improve the performance of the battery.

[0154] The applicant declares that the present invention is illustrated by the above embodiments, but the present invention is not limited to the above process steps, that is, it does not mean that the present invention must rely on the above process steps to be implemented. Those skilled in the art should understand that any improvements to the present invention, equivalent substitutions of the raw materials used in the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a film layer of a perovskite solar cell, characterized in that, The preparation method includes the following steps: (1) Introduce a first source gas and a protective gas into the first substrate to form an atomic layer of the first source gas on the first substrate to obtain a second substrate; in step (1), the first source gas includes tetra(dimethylamino)tin or trimethylaluminum; (2) The first source gas and the second source gas are simultaneously introduced into different chambers, and the second substrate is rotated step by step so that the second substrate passes through the first chamber, the second chamber, the third chamber and the fourth chamber in sequence to complete the first-order ALD reaction, the second-order CVD reaction and the third-order ALD reaction, and obtain the film layer of the perovskite solar cell; the rotation speed of the second substrate during the second-order CVD reaction is greater than that during the first-order ALD reaction, and the rotation speed of the second substrate during the second-order CVD reaction is greater than that during the third-order ALD reaction; Step (2) further includes introducing a first inert source gas and a second inert source gas into the second substrate. In step (2), the first source gas, the first inert source gas, the second source gas and the second inert source gas are simultaneously introduced into the first chamber, the second chamber, the third chamber and the fourth chamber, respectively. The flow rates of the first inert source gas and the second inert source gas during the second-order CVD reaction are less than the flow rates during the first-order ALD reaction and the third-order ALD reaction.

2. The production method according to claim 1, characterized by, Step (1) The first source gas has a single atomic layer.

3. The production method according to claim 1, characterized by, Step (1) The first source gas is carried into the reaction chamber by the first carrier gas.

4. The method of claim 1, wherein, The protective gas in step (1) includes nitrogen.

5. The preparation method according to claim 1, characterized in that, Step (1) The flow rate of the first source gas is 500-2000 sccm.

6. The method of claim 1, wherein, The time for forming the atomic layer of the first source gas in step (1) is 5-30s.

7. The preparation method according to claim 1, characterized in that, Step (1) The first source gas and the protective gas are alternately introduced into the same chamber to carry out a time-type ALD reaction, so that the atomic layer of the first source gas is adsorbed on the first substrate; The number of alternating insertions is at least once.

8. The method of claim 1, wherein, Step (1) The first source gas and the protective gas are simultaneously introduced into different chambers to carry out a spatial ALD reaction, so that the atomic layer of the first source gas is adsorbed on the first substrate. The spatial ALD reaction is repeated at least once.

9. The preparation method according to claim 8, characterized in that, Step (1) further includes introducing a first inert gas and a second inert gas into the first substrate. The first gas, the first inert gas, the protective gas and the second inert gas are introduced into the first chamber, the second chamber, the third chamber and the fourth chamber at the same time. The first chamber, the second chamber, the third chamber and the fourth chamber are divided in a clockwise direction or in a counterclockwise direction.

10. The preparation method according to claim 1, characterized in that, The rotational speed of the first substrate is 10-50 rpm.

11. The method of claim 1, wherein, Step (2) The rotational speed of the second substrate is 20-100 rpm.

12. The method of claim 1, wherein, Step (2) The second source gas is carried into the reaction chamber by the second carrier gas.

13. The method of claim 1, wherein, The second source gas includes any one of O2, O3, H2O, or H2O2.

14. The method of claim 1, wherein, The flow rate of the second source gas is 500-2000 sccm.

15. The method of claim 1, wherein, During the reaction described in step (2), the temperature of the second substrate is 80-150℃.

16. The preparation method according to claim 1, characterized in that, The reaction time in step (2) is 50-200 s.

17. The preparation method according to claim 1, characterized in that, In step (2), the rotational speed of the second substrate during the first-order ALD reaction is the same as that of the first substrate in step (1).

18. A film layer for a perovskite solar cell, characterized in that, The film layer of the perovskite solar cell is prepared by the preparation method according to any one of claims 1-17; The thickness of the film is 5-30 nm.

19. A photovoltaic device, characterized in that, The photovoltaic device includes the film layer of the perovskite solar cell as described in claim 18.

Citation Information

Patent Citations

  • Atomic layer deposition systems and methods

    CN101611167A

  • Mechanism, system and method for manufacturing semiconductor

    CN106887398A