A method for improving the strength of waste paper fiber by using modified xylanase and pectinase system
Through the synergistic treatment of modified xylanase and pectinase, the problems of reduced fiber quality and low paper strength of office waste paper are solved, efficient removal of ink and improvement of paper physical properties are achieved, simplifying operations and reducing chemical costs. The use of pharmaceuticals significantly improves the fiber strength and whiteness of waste paper.
Patent Information
- Application Number
- CN202310642804.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-01
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-06-01
AI Technical Summary
The existing technology has the problems of reduced fiber quality and low paper strength during the recycling process of office waste paper. In particular, it is difficult to effectively remove laser printing ink, and the deinking treatment method is complicated, which cannot effectively solve the problem of laser printing ink.
Using a synergistic system of modified xylanase and pectinase, the modified xylanase removes the hemicellulose and carbohydrate complex structures in the pulp, changes the fiber structure, and combines with pectinase to remove the extracts from the fiber surface. and ink particles to improve the physical strength and optical properties of paper.
It significantly improves the physical strength and optical properties of waste paper fibers, reduces the effective residual ink concentration, simplifies operation, reduces the use of chemicals, and is environmentally friendly.
Smart Images

Figure CN116815537B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of the interdisciplinary subject of pulping and papermaking engineering and bioengineering, and specifically relates to a method for improving the strength of waste paper fibers by utilizing a modified xylanase in coordination with a pectinase system. Background Art
[0002] Faced with the problem of fiber raw material shortage caused by the ban on foreign waste paper imports, increasing the recycling of waste paper and improving the performance of waste paper fibers are important solutions to the current resource shortage in the papermaking industry.
[0003] Waste paper in my country can be roughly divided into the following categories: old newsprint, waste corrugated cardboard, and mixed office waste (MOW). In the process of mixed office waste paper reuse, waste paper deinking is a key step in waste paper recycling and has always been a hot topic of concern to researchers. The commonly used deinking methods at home and abroad are: traditional alkaline deinking, weak alkaline deinking and neutral deinking, cavitation jet deinking, agglomeration-magnetic deinking, steam explosion and enzyme deinking process. Enzyme deinking has attracted widespread attention from scientific researchers because it is environmentally friendly and has significant effects.
[0004] Xylanase is a commonly used enzyme in the papermaking industry. In terms of fiber performance enhancement, xylanase mainly degrades part of hemicellulose, etches the fiber, increases the space between fibers, modifies the fiber surface structure, and then increases the bonding force between fibers. In terms of deinking, xylanase attacks the xylosidic bonds in the fiber, destroys the fiber LCC (lignin-carbohydrate complex) structure, removes lignin from the fiber surface, and helps to remove some ink particles. Pectinase is also widely used in pulping and papermaking. When deinking waste paper pulp, pectinase is mainly used to remove pectin in the intercellular layer of the fiber, and removes extracts attached to the fiber surface, reducing the connection between the fiber and the ink. However, the effect of single enzyme in deinking and enhancing the physical properties of paper during use is not ideal, while composite enzymes can play more advantages and achieve more ideal results. While deinking the paper, the physical strength of the paper is improved.
[0005] In view of the problems of reduced fiber quality and low paper strength in the process of recycling office waste paper, Singh A et al. used xylanase and pectinase produced by the same alkali-resistant heat strain for deinking school office waste paper. The addition of the two biological enzymes at the same time and combined with chemical deinking can reduce 50% of chemicals, reduce BOD and COD by 20.15% and 22.64% respectively, and improve various physical properties of paper (Singh A, Yadav RD, Kaur A, et al. Anecofriendly cost effective enzymatic methodology for deinking of school waste paper [J]. Bioresource Technology, 2012, 120 (none): 322-327.). The main components of the waste paper in this document are a mixture of used high-quality registration pages (33.5%), test papers (27.0%) and low-quality registration pages containing blue ballpoint pen ink (39.5%). The waste paper composition is too complex and most of it is waste paper produced by blue ballpoint pens. The quality of the waste paper is poor and it is rarely used. Compared with the ink produced by handwriting with a ballpoint pen, the laser printing ink of office waste paper produced by laser printers is more stubborn and more difficult to remove. In addition, the PFI pulping treatment is required again after the deinking treatment in the literature, and the treatment method is too complicated and not conducive to practical application. Moreover, the waste paper used is mostly waste paper with blue ballpoint pen ink, which has few market applications and cannot solve the problem of laser printing ink in waste paper deinking. Summary of the invention
[0006] In order to overcome the shortcomings of the prior art, the purpose of the present invention is to provide a method for improving the strength of waste paper fibers by using a modified xylanase in conjunction with a pectinase system.
[0007] The purpose of the present invention is achieved by at least one of the following technical solutions.
[0008] The present invention provides a method for improving the strength of waste paper fibers by using a modified xylanase in collaboration with a pectinase system, comprising the following steps:
[0009] (1) adding waste paper into water, and then performing pulping in a pulper, adjusting the pulp concentration to obtain waste paper pulp for standby use;
[0010] (2) immobilizing the xylanase using Eudragit L-100 to form a modified xylanase;
[0011] (3) adding modified xylanase and pectinase to the waste paper pulp in step (1), adjusting the pH value of the pulp with a buffer solution and then performing a biological enzyme treatment, placing the pulp sample after the biological enzyme treatment in a flotation tank for flotation deinking treatment, and washing to obtain a pulp sample after deinking treatment;
[0012] (4) Sheet metal is formed from the pulp sample treated with the biological enzyme in step (3) to obtain paper having improved fiber strength by using the modified xylanase in combination with the pectinase system.
[0013] Furthermore, the waste paper in step (1) is mixed office waste (MOW).
[0014] Furthermore, in step (1), the rotation speed during the pulping treatment is 300-350 r / min, the time of the pulping treatment is 15-25 min, and the temperature of the pulping treatment is 45-60°C.
[0015] Furthermore, the waste paper pulp in step (1) has a pulp concentration of 8wt% to 10wt%.
[0016] Furthermore, the Eudragit L-100 immobilization treatment in step (2) is:
[0017] Take an appropriate amount of Eudragit L and stir it, add the xylanase solution, make up the volume with a phosphate buffer solution of pH = 7.2, place it in a constant temperature oscillator to react for 1 hour, add an appropriate amount of 3M HCl solution after the reaction to lower the pH value until it is in a coagulated state and stand for 10 to 30 minutes, centrifuge it, pour out the supernatant, wash the precipitate with acetic acid solution, stand for 10 to 30 minutes, repeat the centrifugation steps, and finally place the precipitate in an acetic buffer solution to form a modified xylanase solution.
[0018] Furthermore, the order of adding the modified xylanase and pectinase in step (3) is: first adding the modified xylanase for pretreatment, and then adding the pectinase.
[0019] Furthermore, the temperature of the modified xylanase added in step (3) is 55-75° C., the reaction time is 20-80 min, and the reaction is heated in a constant temperature water bath at a rotation speed of 200-300 r / min.
[0020] Furthermore, the temperature of the pectinase reaction in step (3) is 55-75° C., the reaction time is 20-80 min, and the reaction is heated in a constant temperature water bath at a rotation speed of 200-300 r / min.
[0021] Furthermore, in step (3), the pH value of the waste paper pulp solution is adjusted to 6-8, which can be adjusted using disodium hydrogen phosphate / monohydrate citric acid buffer solution.
[0022] Furthermore, the dosage of the modified xylanase in step (3) is 5 to 25 U of modified xylanase per gram of absolute dry mass of waste paper pulp, that is, the dosage of the modified xylanase in step (3) is 5 to 25 U / g of absolute dry waste paper pulp; the absolute dry waste paper pulp is the mass of the waste paper weighed during the pulping in step (1).
[0023] Furthermore, the dosage of pectinase in step (3) is 5 to 20 U of pectinase per gram of absolute dry mass of waste paper pulp, that is, the dosage of pectinase in step (3) is 5 to 20 U / g of absolute dry mass of waste paper pulp; the absolute dry mass of waste paper pulp is the mass of waste paper weighed during pulping in step (1).
[0024] Furthermore, the deinking treatment described in step (3) is as follows: placing the pulp after the biological enzyme treatment in an intermittent flotation tank, adjusting the pulp concentration to 0.05% to 1%, adding 3% of Tween 80 (i.e., the amount of Tween 80 is 3% of the mass of the waste paper weighed during pulping in step (1)), the air pressure is 0.15 to 0.30 MPa, the temperature is 60°C, and the flotation time is 30 to 45 minutes.
[0025] Furthermore, the washing in step (3) is washing with water until the filtrate is colorless.
[0026] The present invention first uses modified xylanase to remove part of the hemicellulose and carbohydrate complex (LCC) structure in the pulp, changes the fiber structure, makes the fiber cell wall loose and porous, and makes the fiber soft and plastic, further promotes pectinase to remove extracts and ink particles on the fiber surface, removes pectin in the intercellular layer of the cell wall, and reduces the connection between the fiber and the ink particles. While removing the ink particles and increasing the whiteness of the paper, the physical strength performance of the paper is further improved. Compared with unmodified fibers, after being treated with modified xylanase and pectinase, the optical properties and physical properties of the paper made from the fiber are greatly improved.
[0027] After the xylanase is modified, its reaction activity and stability are enhanced. At 50-90°C, the relative enzyme activity is increased to 70%-80%; at pH=6-9, the relative enzyme activity is increased to more than 95%, indicating that after the xylanase is modified, the stability is improved under high temperature and high alkaline conditions. The modified xylanase is preferentially used to treat pulp fibers to degrade the lignin-carbohydrate complex (LCC) structure in the pulp, which can change the fiber structure and promote the dissolution of lignin. At the same time, the specific surface area of the fiber is increased, which promotes the subsequent pectinase to remove the extract from the fiber surface, reduce the connection between the fiber and the ink particles, and help remove the ink particles during the flotation process.
[0028] The present invention provides paper produced by the above method of improving the strength of waste paper fiber by using modified xylanase in coordination with pectinase system.
[0029] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0030] (1) The method provided by the present invention for improving the strength of waste paper fiber by using a modified xylanase in collaboration with a pectinase system uses a modified xylanase to remove part of the hemicellulose and carbohydrate complex (LCC) structure in the pulp, which helps dissolve lignin and improves the optical properties of paper. At the same time, the fiber voids increase and the specific surface area increases, which is conducive to promoting the subsequent pectinase to remove the extracts on the fiber surface, thereby reducing the connection between the fiber and the ink particles, which helps to remove the ink particles in the subsequent flotation process.
[0031] (2) The method provided by the present invention for improving the strength of waste paper fiber by using a modified xylanase in combination with a pectinase system is simple to operate, reduces the use of chemicals, has mild reaction conditions and is environmentally friendly, and does not cause secondary pollution to the environment.
[0032] (3) The paper obtained by the method of the present invention has excellent comprehensive mechanical properties, and its tensile index is 35.28-38.31 N·m·g -1 , burst resistance index is 1.81~1.94kPa·m 2 ·g -1 , tear index is 5.17~5.57mN·m 2 ·g -1 , ring pressure index is 7.01~7.23N·m·g -1 Moreover, the effective residual ink concentration of the paper obtained by the method of the present invention can be reduced by 63.82%, and the whiteness value of the paper can reach 101.3 ISO%. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 The effect of the reaction time of the modified xylanase in Example 3 on paper properties (effective residual ink, brightness, tensile index) is shown.
[0034] Figure 2 The effect of pectinase reaction time on paper properties (effective residual ink, whiteness, tensile index) in Example 4 is shown. DETAILED DESCRIPTION
[0035] The following examples further illustrate the specific implementation of the present invention, but the implementation and protection of the present invention are not limited thereto. It should be pointed out that if there are processes that are not specifically described below, they can be implemented or understood by those skilled in the art with reference to the prior art. The reagents or instruments used without indicating the manufacturer are deemed to be conventional products that can be purchased commercially. The mixed office waste paper is the output of an office laser printer. For process parameters that are not specifically indicated, conventional techniques can be used.
[0036] Example 1
[0037] Example 1 provides a method for improving the strength of waste paper fibers by using a modified xylanase in conjunction with a pectinase system, comprising the following steps:
[0038] (1) Immobilize xylanase with Eudragit L-100 to form modified xylanase; the immobilization method is as follows: take 2 ml of 5% (W / V) Eudragit L-100, stir and add 20 U of xylanase, dilute to 10 mL with pH=7.2 phosphate buffer solution, and react in a constant temperature oscillator at 30°C and 100 rpm for 1 hour. After the reaction, add 500 ml of 3M HCL until it solidifies, stand at room temperature for 20 minutes, centrifuge for 10 minutes (speed 4000 rpm), pour out the supernatant, and recover the precipitate; wash the precipitate with pH=4 acetic acid solution, stand at room temperature for 10 minutes, centrifuge for 10 minutes (speed 4000 rpm), pour out the supernatant, dissolve the precipitate in pH=6 acetic buffer solution, dilute to 10 mL, and form a modified xylanase solution;
[0039] (2) weighing 50 g of absolutely dry mixed office waste paper (MOW), cutting it into pieces, soaking it in water, and then pulping the waste paper in a high-consistency pulper, with the pulping speed set to 350 r / min, the pulping concentration controlled to 10 wt%, the temperature set to 50° C., and the pulping time set to 20 min; after the pulping is completed, collecting the pulp to obtain waste paper pulp;
[0040] (3) The waste paper pulp described in step (2) is adjusted to a pH value of 6.0 using a sodium hydrogen phosphate / citric acid buffer solution, and then a modified xylanase is added to the waste paper pulp (the amount of the modified xylanase added is 25 U / g, that is, 25 U is added per gram of the absolute dry mass of the waste paper pulp) and the waste paper pulp is transferred to a constant temperature water bath for heating treatment at a temperature of 60° C., a speed of 200 r / min, and a heating time of 60 min; then pectinase is added (the amount of the pectinase added is 20 U / g, that is, 20 U is added per gram of the absolute dry mass of the waste paper pulp), and the waste paper pulp is transferred to a constant temperature water bath for heating treatment at a temperature of 60° C., a speed of 200 r / min, and a heating time of 60 min; after the reaction is completed, the waste paper pulp is washed with water until the filtrate is colorless to obtain a pulp sample treated with a biological enzyme;
[0041] (4) placing the pulp sample after the enzyme treatment in an intermittent flotation tank for flotation deinking treatment, the deinking treatment conditions are as follows: adjusting the pulp concentration to 1%, adding 3% of Tween 80 (i.e., the amount of Tween 80 is 3% of the mass of the waste paper weighed during pulping in step (2), air pressure of 0.15 MPa, temperature of 60° C., and flotation time of 30 min;
[0042] (5) The pulp was collected with a 200-mesh pulp bag and placed in a constant temperature and humidity chamber to balance the moisture content. The moisture content of the pulp sample was measured and then paper was made to obtain paper (the treated sample of Example 1) in which the strength of waste paper fiber was improved by using the modified xylanase and pectinase system.
[0043] The paper obtained in Example 1 with fiber strength enhanced by modified xylanase in combination with pectinase (treated sample in Example 1) was subjected to physical property tests, wherein the tensile strength was measured according to the national standard GB / T453-2002, the bursting strength was measured according to the national standard GB / T454-2002, the tear strength was measured according to the national standard GB / T455-2002, and the ring crush strength was measured according to TAPPI T810om-98.
[0044] Control sample: The treatment method of the control sample is the same as above, except that in step (3), modified xylanase is added but pectinase is not added, and the heat treatment is performed. The amount of modified xylanase used is the same as in step (3), and other operating parameters or substance amounts not mentioned are the same as in the above method, to obtain paper as a control sample.
[0045] The control sample was tested for physical properties, including tensile strength according to national standard GB / T453-2002, bursting strength according to national standard GB / T454-2002, tear strength according to national standard GB / T455-2002, and ring crush strength according to TAPPIT810om-98.
[0046] Blank sample: The blank sample is processed in the same manner as above, except that in step (3), neither modified xylanase nor pectinase is added, and the heat treatment is performed. Other operating parameters or amounts of substances not mentioned are the same as those in the above method, to obtain a blank sample of paper.
[0047] The blank samples were tested for physical properties, including tensile strength according to GB / T453-2002, bursting strength according to GB / T454-2002, tear strength according to GB / T455-2002, and ring crush strength according to TAPPIT810om-98.
[0048] The paper made from the treated samples, control samples and blank samples was tested to obtain the data in Table 1 below, in order to explore the effect of the modified xylanase synergistic pectinase system treatment on the physical properties of MOW.
[0049] Table 1
[0050]
[0051] Analysis: The test results of MOW after being processed and made into paper are shown in Table 1. It can be seen from Table 1 that after being treated with xylanase, modified xylanase and pectinase, the tensile index increased by 14.37% and 25.23% respectively, the bursting index increased by 10.39% and 17.53% respectively, the tearing index increased by 16.12% and 20.79% respectively, and the ring pressure index increased by 12.87% and 25.74% respectively. It can be seen that the physical strength of the paper treated with modified xylanase is improved, but the strength performance of the paper treated with modified xylanase and pectinase system is significantly improved compared with the blank sample and the control sample.
[0052] Example 2 Investigating the effect of different addition orders of two enzymes on paper properties
[0053] Example 2 provides a method for improving the strength of waste paper fibers by using a modified xylanase in conjunction with a pectinase system, comprising the following steps:
[0054] (1) Immobilize xylanase with Eudragit L-100 to form modified xylanase; the immobilization conditions are as follows: take 2 ml of 5% (W / V) Eudragit L-100, stir and add 20 U of xylanase, dilute to 10 mL with pH=7.2 phosphate buffer solution, and react in a constant temperature oscillator at 30°C and 100 rpm for 1 hour. After the reaction, add 500 ml of 3M HCL until it solidifies, stand at room temperature for 20 minutes, centrifuge for 10 minutes (speed 4000 rpm), pour out the supernatant, and recover the precipitate; wash the precipitate with pH=4 acetic acid solution, stand at room temperature for 10 minutes, centrifuge for 10 minutes (speed 4000 rpm), pour out the supernatant, dissolve the precipitate in pH=6 acetic buffer solution, dilute to 10 mL, and form a modified xylanase solution;
[0055] (2) weighing 50 g of absolutely dry mixed office waste paper (MOW), cutting it into pieces, soaking it in water, and then pulping the waste paper in a high-consistency pulper, with the pulping speed set to 320 r / min, the pulping concentration controlled to 10 wt%, the temperature set to 45° C., and the pulping time set to 20 min; after the pulping is completed, collecting the pulp to obtain waste paper pulp;
[0056] (3) The waste paper pulp in step (2) is adjusted to a pH value of 6.0 using a sodium dihydrogen phosphate / citric acid buffer solution, and then a modified xylanase is added to the waste paper pulp (the amount of the modified xylanase added is 18 U / g, that is, 18 U is added per gram of the absolute dry mass of the waste paper pulp), and the waste paper pulp is transferred to a constant temperature water bath for heating treatment at a temperature of 60° C., a speed of 250 r / min, and a heating time of 80 min; then pectinase is added (the amount of the pectinase added is 12 U / g, that is, 12 U is added per gram of the absolute dry mass of the waste paper pulp), and the waste paper pulp is transferred to a constant temperature water bath for heating treatment at a temperature of 60° C., a speed of 250 r / min, and a heating time of 80 min; after the reaction is completed, the waste paper pulp is washed with water until the filtrate is colorless to obtain a pulp sample treated with a biological enzyme;
[0057] (4) placing the pulp sample after the enzyme treatment in an intermittent flotation tank for flotation deinking treatment, the deinking treatment conditions are as follows: adjusting the pulp concentration to 1%, adding 3% of Tween 80 (i.e., the amount of Tween 80 is 3% of the mass of the waste paper weighed during pulping in step (2), air pressure of 0.15 MPa, temperature of 60° C., and flotation time of 30 min;
[0058] (5) The pulp was collected with a 200-mesh pulp bag and placed in a constant temperature and humidity chamber to balance the moisture content. The moisture content of the pulp sample was measured and then paper was made to obtain paper (the treated sample of Example 2) in which the strength of waste paper fiber was improved by using the modified xylanase and pectinase system.
[0059] The paper obtained in Example 2, in which the fiber strength was improved by using the modified xylanase and pectinase system (the treated sample in Example 2), was tested for effective residual ink concentration, whiteness and physical properties. The effective residual ink concentration was measured according to the national standard GB / T 20216-2016, the whiteness was measured according to the national standard QBT 2804-2006, the tensile strength was measured according to the national standard GB / T453-2002, the bursting strength was measured according to the national standard GB / T454-2002, the tear strength was measured according to the national standard GB / T455-2002, and the ring crush strength was measured according to TAPPI T810om-98.
[0060] Control sample: The treatment method of the control sample is the same as above, except that the order of adding the biological enzymes in step (3) is different: pectinase is added first, heat treatment is performed, and then modified xylanase is added. The amounts of modified xylanase and pectinase are the same as in step (3). Other operating parameters or amounts of substances not mentioned are the same as in the above method, and paper as a control sample is obtained.
[0061] The control sample was subjected to paper performance testing, wherein the tensile strength was measured according to the national standard GB / T453-2002, the bursting strength was measured according to the national standard GB / T454-2002, the tear strength was measured according to the national standard GB / T455-2002, and the ring crush strength was measured according to TAPPIT810om-98.
[0062] Blank sample: The processing method of the blank sample is the same as above, except that in step (3), neither pectinase nor modified xylanase is added, and the heat treatment is performed. Other operating parameters or substance amounts not mentioned are the same as the above method to obtain paper as a blank sample.
[0063] The blank samples were tested for physical properties, including tensile strength according to GB / T453-2002, bursting strength according to GB / T454-2002, tear strength according to GB / T455-2002, ring crush strength according to TAPPIT810om-98, effective residual ink concentration according to GB / T 20216-2016, and whiteness according to QBT2804-2006.
[0064] The paper made from the treated samples, control samples and blank samples was tested to obtain the data in Tables 2 and 3 below to explore the effect of the modified xylanase synergistic pectinase system treatment on the physical properties of MOW.
[0065] Table 2
[0066]
[0067] Table 3
[0068]
[0069] Analysis: The performance test results of the mixed office waste paper after being processed and made into paper are shown in Tables 2 and 3. It can be seen from Tables 2 and 3 that the paper treated with modified xylanase first and then pectinase has better physical properties and deinking effect. In terms of paper physical properties, the tensile index increased by 35.99%, the burst index increased by 25.97%, the tear index increased by 30.14%, and the ring pressure index increased by 24.69%, which is much higher than the strength performance of the paper treated with modified xylanase first and then pectinase. In terms of deinking effect, the effective residual ink concentration of the paper was reduced by 54.15% after the modified xylanase was first added and then pectinase was added, and the whiteness of the paper increased by 6.52%, which is also higher than the treatment of modified xylanase first and then pectinase. It can be explained as follows: preferentially adding modified xylanase can remove part of the LCC structure in the pulp, change the fiber structure, make the fiber cell wall loose and porous, and make the fiber soft and plastic, which can further promote the removal of fiber surface substances by pectinase. When pectinase is added, the pectin, extracts and ink particles in the fiber cell wall can be better removed, reducing the connection between the fiber and the ink particles. While removing the ink particles and increasing the whiteness of the paper, the physical strength of the paper is further improved. However, preferentially adding pectinase and then adding modified xylanase will cause some of the ink particles removed by pectinase in the early stage to be re-adsorbed on the fiber, resulting in a higher effective residual ink concentration and a higher whiteness value, which affects the bonding between fibers and further affects the physical strength of the paper. It can be seen that the effective residual ink concentration, whiteness and physical strength of the paper treated with the pectinase system after preferentially adding modified xylanase are significantly improved compared with the blank sample and the control sample.
[0070] Example 3 Investigating the effect of different treatment times of modified xylanase on paper properties
[0071] Example 3 provides a method for improving the strength of waste paper fibers by using a modified xylanase in conjunction with a pectinase system, comprising the following steps:
[0072] (1) Immobilize xylanase using Eudragit L-100 to form modified xylanase; the immobilization conditions are as follows: take 2 ml of 5% (W / V) Eudragit L-100, stir and add 20 U of xylanase, dilute to 10 mL with pH = 7.2 phosphate buffer solution, and react in a constant temperature oscillator at 30°C and 100 rpm for 1 hour. After the reaction, add 500 ml of 3M HCL until it solidifies, stand at room temperature for 20 minutes, centrifuge for 10 minutes (speed 4000 rpm), pour out the supernatant, and recover the precipitate; the obtained precipitate is washed with pH = 4 acetic acid solution, stand at room temperature for 10 minutes, centrifuge for 10 minutes (speed 4000 rpm), pour out the supernatant, dissolve the precipitate in pH = 6 acetic buffer solution, dilute to 10 mL, and form a modified xylanase solution;
[0073] (2) weighing 50 g of absolutely dry mixed office waste paper (MOW), cutting it into pieces, soaking it in water, and then pulping the waste paper in a high-consistency pulper, with the pulping speed set to 350 r / min, the pulping concentration controlled to 10 wt%, the temperature set to 50° C., and the pulping time set to 15 min; after the pulping is completed, collecting the pulp to obtain waste paper pulp;
[0074] (3) The waste paper pulp in step (2) was adjusted to a pH value of 6.0 using a sodium hydrogen phosphate / citric acid buffer solution, and then (the amount of modified xylanase added was 15 U / g, that is, 15 U of modified xylanase was added per gram of the absolute dry mass of the waste paper pulp) was added to the waste paper pulp, and the waste paper pulp was transferred to a constant temperature water bath for heating treatment, the heating temperature was 60°C, the heating speed was 200 r / min, and the heating time was 0 min, 20 min, 40 min, 60 min, 80 min, and 100 min respectively; then 12 U / g of pectinase was added, that is, 12 U of pectinase was added per gram of the absolute dry mass of the waste paper pulp), and the waste paper pulp was transferred to a constant temperature water bath for heating treatment, the heating temperature was 60°C, the heating speed was 200 r / min, and the heating time was 80 min; after the reaction was completed, the waste paper pulp was washed with water until the filtrate was colorless to obtain a biologically treated pulp sample;
[0075] (4) placing the pulp sample after the enzyme treatment in an intermittent flotation tank for flotation deinking treatment, the deinking treatment conditions are as follows: adjusting the pulp concentration to 1%, adding 3% of Tween 80 (i.e., the amount of Tween 80 is 3% of the mass of the waste paper weighed during pulping in step (2), air pressure of 0.15 MPa, temperature of 60° C., and flotation time of 30 min;
[0076] (5) The pulp was collected with a 200-mesh pulp bag and placed in a constant temperature and humidity chamber to balance the moisture content. The moisture content of the pulp sample was measured and then paper was made to obtain paper (the treated sample of Example 3) in which the strength of waste paper fiber was improved by using the modified xylanase and pectinase system.
[0077] The paper obtained in Example 3 using the modified xylanase synergistic pectinase system to improve fiber strength was subjected to paper performance testing under different modified xylanase reaction times (treated samples in Example 3). The tensile strength was measured according to the national standard GB / T453-2002, the effective residual ink concentration was measured according to the national standard GB / T 20216-2016, and the whiteness was measured according to the national standard QBT 2804-2006.
[0078] Blank sample: The processing method of the blank sample is the same as above, except that in step (3), neither pectinase nor modified xylanase is added, and the heat treatment is performed. Other operating parameters or substance amounts not mentioned are the same as the above method to obtain paper as a blank sample.
[0079] The blank sample was subjected to paper performance testing, wherein the tensile strength was measured according to the national standard GB / T453-2002, the effective residual ink concentration was measured according to the national standard GB / T 20216-2016, and the whiteness was measured according to the national standard QBT 2804-2006.
[0080] The paper made from the treated sample and the blank sample was tested and the following Table 4 and Figure 1 The data were collected to explore the effect of reaction time of modified xylanase in the modified xylanase synergistic pectinase system on the physical properties of MOW.
[0081] Table 4
[0082]
[0083] Analysis: The test results of mixed office waste paper after processing and making paper are shown in Table 4 and Figure 1 As shown in Table 4 and Figure 1It can be seen that with the increase of the reaction time of the modified xylanase, the increment of the tensile index increased from 4.72% to 78.75%, the effective residual ink concentration decreased to a flat state, the reduction of the effective residual ink concentration increased from 32.36% to 63.82%, the whiteness value of the paper increased to a certain extent and tended to be flat, and the increment of the whiteness value increased from 2.25% to 8.57%. It can be seen that if the modified xylanase and pectinase are added at the same time (0min), or the modified xylanase does not have sufficient reaction time (less than 20min), the modified xylanase has little effect on the hemicellulose or fiber LCC structure, and the fiber has a low degree of water swelling, which will make the pectinase unable to act well on the extracts and ink particles on the fiber surface, and ultimately make it difficult to remove the ink particles, the whiteness value is low, and the improvement of the physical strength of the paper is affected. If the reaction time of the modified xylanase is long (more than 80min), the improvement of the physical strength of the paper will decrease slightly, and the energy consumption will increase. Therefore, appropriate and sufficient reaction time of the modified xylanase should be ensured.
[0084] Example 4: Investigating the effect of different reaction times of pectinase on paper properties
[0085] Example 4 provides a method for improving the strength of waste paper fibers by using a modified xylanase in combination with a pectinase system, comprising the following steps:
[0086] (1) Immobilize xylanase with Eudragit L-100 to form modified xylanase; the immobilization conditions are as follows: take 2 ml of 5% (W / V) Eudragit L-100, stir and add 20 U of xylanase, dilute to 10 mL with pH=7.2 phosphate buffer solution, and react in a constant temperature oscillator at 30°C and 100 rpm for 1 hour. After the reaction, add 500 ml of 3M HCL until it solidifies, stand at room temperature for 20 minutes, centrifuge for 10 minutes (speed 4000 rpm), pour out the supernatant, and recover the precipitate; wash the precipitate with pH=4 acetic acid solution, stand at room temperature for 10 minutes, centrifuge for 10 minutes (speed 4000 rpm), pour out the supernatant, dissolve the precipitate in pH=6 acetic buffer solution, dilute to 10 mL, and form a modified xylanase solution;
[0087] (2) weighing 50 g of absolutely dry mixed office waste (MOW), cutting it into pieces, soaking it in water, and then pulping the waste paper in a high-consistency pulper, with the pulping speed set to 320 r / min, the pulping concentration controlled to 10 wt%, the temperature set to 60° C., and the pulping time set to 25 min; after the pulping is completed, collecting the pulp to obtain waste paper pulp;
[0088] (3) The waste paper pulp described in step (2) is adjusted to a pH value of 6.0 with a sodium hydrogen phosphate / citric acid buffer solution, and then a modified xylanase is added to the waste paper pulp (the amount of the modified xylanase added is 18 U / g, that is, 18 U is added per gram of the absolute dry mass of the waste paper pulp), and the waste paper pulp is transferred to a constant temperature water bath for heating treatment, the heating temperature is 60°C, the heating speed is 300 r / min, and the heating time is 80 min; then pectinase is added (the amount of pectinase added is 12 U / g, that is, 12 U is added per gram of the absolute dry mass of the waste paper pulp), and the waste paper pulp is transferred to a constant temperature water bath for heating treatment, the heating temperature is 60°C, the heating speed is 300 r / min, and the heating time is 0 min, 20 min, 40 min, 60 min, 80 min, and 100 min respectively; after the reaction is completed, the waste paper pulp is washed with water until the filtrate is colorless to obtain a pulp sample treated with a biological enzyme;
[0089] (4) placing the pulp sample after the enzyme treatment in an intermittent flotation tank for flotation deinking treatment, the deinking treatment conditions are as follows: adjusting the pulp concentration to 1%, adding 3% of Tween 80 (i.e., the amount of Tween 80 is 3% of the mass of the waste paper weighed during pulping in step (2), air pressure of 0.15 MPa, temperature of 60° C., and flotation time of 30 min;
[0090] (5) The pulp was collected with a 200-mesh pulp bag and placed in a constant temperature and humidity chamber to balance the moisture content. The moisture content of the pulp sample was measured and then paper was made to obtain paper (the treated sample of Example 3) in which the strength of waste paper fiber was improved by using the modified xylanase and pectinase system.
[0091] The paper obtained in Example 4, which was prepared by using the modified xylanase to enhance the fiber strength in cooperation with the pectinase system and at different pectinase reaction times (the treated sample in Example 4), was subjected to paper performance testing. The tensile strength was measured according to the national standard GB / T453-2002, the effective residual ink concentration was measured according to the national standard GB / T 20216-2016, and the whiteness was measured according to the national standard QBT2804-2006.
[0092] Blank sample: The processing method of the blank sample is the same as above, except that in step (3), neither pectinase nor modified xylanase is added, and the heat treatment is performed. Other operating parameters or substance amounts not mentioned are the same as the above method to obtain paper as a blank sample.
[0093] The blank samples were tested for physical properties, including tensile strength measured according to national standard GB / T453-2002, effective residual ink concentration measured according to national standard GB / T 20216-2016, and whiteness measured according to national standard QBT 2804-2006.
[0094] The paper made from the treated sample and the blank sample was tested and the following results were obtained: Figure 2 The data were collected to explore the effect of modified xylanase synergistic pectinase system treatment on the physical properties of MOW.
[0095] Table 5
[0096]
[0097] Analysis: The test results of mixed office waste paper after being treated with modified xylanase and pectinase are shown in Table 5 and Figure 2 As shown in Table 5 and Figure 2 It can be seen that with the extension of pectinase reaction time, the tensile index of the paper first increases to the maximum value and then decreases slightly. The increment of the tensile index increases from 8.66% to 46.79%, the effective residual ink concentration decreases to a gentle state, the reduction of the effective residual ink concentration increases from 23.44% to 58.72%, the whiteness value of the paper increases to a certain extent and tends to be gentle, and the increment of the whiteness value increases from 4.47% to 10.11%. It can be seen that if the pectinase does not have sufficient reaction time (less than 20 minutes), the pectinase will not be able to fully act on the fiber surface extract and ink particles, resulting in a low ink particle removal rate and a low whiteness value, which in turn affects the improvement of the physical strength of the paper. If the pectinase reaction time is long (more than 80 minutes), the ink particles will be re-adsorbed on the fiber with the help of the mechanical force of the stirring rod, and the removal effect of the ink particles will be weakened and the energy consumption will increase. Therefore, an appropriate and sufficient pectinase reaction time (20 to 80 minutes) should be guaranteed.
[0098] Example 5
[0099] Example 5 provides a method for improving the strength of waste paper fibers by using a modified xylanase in conjunction with a pectinase system, comprising the following steps:
[0100] (1) Immobilize xylanase with Eudragit L-100 to form modified xylanase; the immobilization method is as follows: take 2 ml of 5% (W / V) Eudragit L-100, stir and add 20 U of xylanase, dilute to 10 mL with pH=7.2 phosphate buffer solution, and react in a constant temperature oscillator at 30°C and 100 rpm for 1 hour. After the reaction, add 500 ml of 3M HCL until it solidifies, stand at room temperature for 20 minutes, centrifuge for 10 minutes (speed 4000 rpm), pour out the supernatant, and recover the precipitate; wash the precipitate with pH=4 acetic acid solution, stand at room temperature for 10 minutes, centrifuge for 10 minutes (speed 4000 rpm), pour out the supernatant, dissolve the precipitate in pH=6 acetic buffer solution, dilute to 10 mL, and form a modified xylanase solution;
[0101] (2) weighing 50 g of absolutely dry mixed office waste (MOW), cutting it into pieces, soaking it in water, and then pulping the waste paper in a high-consistency pulper, with the pulping speed set to 350 r / min, the pulping concentration controlled to 10 wt%, the temperature set to 45° C., and the pulping time set to 20 min; after the pulping is completed, collecting the pulp to obtain waste paper pulp;
[0102] (3) The waste paper pulp described in step (2) is adjusted to a pH value of 6.0 with a sodium hydrogen phosphate / citric acid buffer solution, and then a modified xylanase is added to the waste paper pulp (the amount of the modified xylanase added is 5 U / g, that is, 5 U is added per gram of the absolute dry mass of the waste paper pulp) and transferred to a constant temperature water bath for heating treatment at a temperature of 55° C., a speed of 200 r / min, and a heating time of 70 min; then pectinase is added (the amount of the pectinase added is 8 U / g, that is, 8 U is added per gram of the absolute dry mass of the waste paper pulp), and the waste paper pulp is transferred to a constant temperature water bath for heating treatment at a temperature of 55° C., a speed of 200 r / min, and a heating time of 70 min; after the reaction is completed, the waste paper pulp is washed with water until the filtrate is colorless to obtain a pulp sample treated with a biological enzyme;
[0103] (4) placing the pulp sample after the enzyme treatment in an intermittent flotation tank for flotation deinking treatment, the deinking treatment conditions are as follows: adjusting the pulp concentration to 1%, adding 3% of Tween 80 (i.e., the amount of Tween 80 is 3% of the mass of the waste paper weighed during pulping in step (2), air pressure of 0.15 MPa, temperature of 60° C., and flotation time of 30 min;
[0104] (5) The pulp was collected with a 200-mesh pulp bag and placed in a constant temperature and humidity chamber to balance the moisture content. The moisture content of the pulp sample was measured and then paper was made to obtain paper (the treated sample of Example 1) in which the strength of waste paper fiber was improved by using the modified xylanase and pectinase system.
[0105] The paper obtained in Example 1 with fiber strength enhanced by modified xylanase in combination with pectinase (treated sample in Example 1) was subjected to physical property tests, wherein the tensile strength was measured according to the national standard GB / T453-2002, the bursting strength was measured according to the national standard GB / T454-2002, the tear strength was measured according to the national standard GB / T455-2002, and the ring crush strength was measured according to TAPPI T810om-98.
[0106] Control sample: The treatment method of the control sample is the same as above, except that in step (3), modified xylanase is added but pectinase is not added, and the heat treatment is performed. The amount of modified xylanase used is the same as in step (3), and other operating parameters or substance amounts not mentioned are the same as in the above method, to obtain paper as a control sample.
[0107] The control sample was tested for physical properties, including tensile strength according to national standard GB / T453-2002, bursting strength according to national standard GB / T454-2002, tear strength according to national standard GB / T455-2002, and ring crush strength according to TAPPIT810om-98.
[0108] Blank sample: The blank sample is processed in the same manner as above, except that in step (3), neither modified xylanase nor pectinase is added, and the heat treatment is performed. Other operating parameters or amounts of substances not mentioned are the same as those in the above method, to obtain a blank sample of paper.
[0109] The blank samples were tested for physical properties, including tensile strength according to GB / T453-2002, bursting strength according to GB / T454-2002, tear strength according to GB / T455-2002, and ring crush strength according to TAPPIT810om-98.
[0110] The paper made from the treated samples, control samples and blank samples was tested to obtain the data in Table 6 below to explore the effect of the modified xylanase synergistic pectinase system treatment on the physical properties of MOW.
[0111] Table 6
[0112]
[0113] Analysis: The test results of MOW after being processed and made into paper are shown in Table 6. It can be seen from Table 6 that after being treated with xylanase, modified xylanase and pectinase, the tensile index increased by 14.37% and 23.10%, the burst index increased by 10.39% and 18.18%, the tear index increased by 16.12% and 22.42%, and the ring pressure index increased by 12.87% and 27.51%. It can be seen that the physical strength of the paper treated with modified xylanase is improved, but the strength performance of the paper treated with modified xylanase and pectinase system is significantly improved compared with the blank sample and the control sample.
Claims
1. A method for improving the strength of waste paper fiber by using modified xylanase in collaboration with pectinase system, characterized in that: The following steps are involved: (1) Pulping the waste paper, adjusting the pulp concentration to obtain waste paper pulp, and balancing the moisture content for later use; (2) Immobilizing xylanase using Eudragit L-100 to form modified xylanase; (3) adjusting the pH value of the waste paper pulp in step (1) with a buffer solution and then performing a bio-enzyme treatment, wherein the bio-enzyme treatment is firstly performed by adding a modified xylanase for pretreatment, and then adding a pectinase for treatment, placing the pulp sample treated with the bio-enzyme in a flotation tank for flotation deinking treatment, and washing to obtain a pulp sample after deinking treatment; (4) Sheeting the pulp sample after the deinking treatment in step (3) to obtain paper having improved fiber strength by using the modified xylanase and pectinase system; The waste paper in step (1) is mixed office waste paper; Step (2) Eudragit L-100 immobilization treatment is as follows: take Eudragit L and add xylanase solution while stirring, make up the volume with phosphate buffer solution, place in a constant temperature oscillator for reaction, add HCl solution to lower the pH value after the reaction is completed until it is in a coagulated state and stand, then centrifuge, pour out the supernatant, wash the precipitate with acetic acid solution, stand for 10 to 30 minutes, repeat the centrifugation step, and finally place the precipitate in acetic buffer solution to form a modified xylanase solution; The temperature of adding modified xylanase in step (3) is 55-75°C, the reaction time is 20-80 min, and the reaction is heated in a constant temperature water bath at a speed of 200-300 r / min; The reaction temperature of adding pectinase in step (3) is 55-75°C, the reaction time is 20-80 min, and the reaction is heated in a constant temperature water bath at a speed of 200-300 r / min; In step (3), the amount of the modified xylanase is 5-25 U of modified xylanase per gram of the absolute dry mass of the waste paper pulp; the amount of the pectinase is 5-20 U of pectinase per gram of the absolute dry mass of the waste paper pulp.
2. The method for improving the strength of waste paper fiber by using modified xylanase in collaboration with pectinase system according to claim 1, characterized in that: The rotation speed during the pulping treatment in step (1) is 300-350 r / min, the pulping treatment time is 15-25 min, and the pulping treatment temperature is 45-60°C.
3. The method for improving the strength of waste paper fiber by using modified xylanase in collaboration with pectinase system according to claim 1, characterized in that: The waste paper pulp in step (1) has a pulp concentration of 8 wt% to 10 wt%.
4. The method for improving the strength of waste paper fiber by using modified xylanase in collaboration with pectinase system according to claim 1, characterized in that: The buffer used for adjusting the pH value in step (3) is disodium hydrogen phosphate dodecahydrate / citric acid monohydrate, and the pH value is adjusted to 6-8.
5. The method for improving the strength of waste paper fiber by using modified xylanase in collaboration with pectinase system according to claim 1, characterized in that: The deinking treatment in step (3) is as follows: placing the pulp after the bio-enzyme treatment in an intermittent flotation tank, adjusting the pulp concentration to 0.05%-1%, adding 3% Tween 80, the air pressure to 0.15-0.30 MPa, the temperature to 60°C, and the flotation time to 30-45 min.
6. A paper produced by the method for improving the strength of waste paper fiber by using modified xylanase in collaboration with pectinase system as described in any one of claims 1 to 5.