Core and its preparation method and cylindrical battery

By designing multiple core units arranged from the inside to the outside in a cylindrical cell, and utilizing electrode formulation formulas and density design, the problems of inner electrode breakage and material loss were solved, thereby improving battery energy density and lifespan.

CN116826142BActive Publication Date: 2026-11-17JIANGSU PYLON BATTERY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310980328.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-08-04
Publication Date
2026-11-17
Estimated Expiration
2043-08-04

AI Technical Summary

Technical Problem

In existing technologies, the inner electrode sheets of cylindrical cells experience high mechanical stress due to curvature changes during the winding process, leading to electrode breakage and material loss, which affects battery performance.

Method used

Multiple core units are nested sequentially from the inside out. Each unit consists of an electrode and a separator. The electrode formulation and density design meet specific relationships. The stress in the inner ring is reduced by a discontinuous winding method. Combined with the electrode design of different core units, the proportion of active material and the energy density of the battery are improved.

Benefits of technology

It effectively avoids the breakage and material loss of the inner electrode sheet, improves the energy density and lifespan of the battery, alleviates electrode stress problems, and increases the design space for battery thickness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116826142B_ABST
    Figure CN116826142B_ABST
Patent Text Reader

Abstract

This invention relates to the field of battery technology, disclosing a wound core, its preparation method, and a cylindrical battery. The wound core comprises n (n≥2) wound core units arranged sequentially from the inside out. Each wound core unit consists of a first separator, a negative electrode, a second separator, and a positive electrode wound sequentially. The electrode formulation formula is: 100% = α n %+β n %+γ n %, α n % represents the percentage of active material in the electrode, β n % represents the percentage of conductive agent in the electrode, γ n % represents the percentage of binder in the electrode, β n =a×n b The value of a ranges from 1 to 5, and the value of b is -0.393; γ n =c×n d d is -0.409, and a and c satisfy c = 2.99 × a 0.4313 The preparation method includes winding the first core unit once to form a second core unit, then finishing the winding, and repeating this process. A cylindrical battery is produced, comprising the aforementioned core. The core provided by this invention improves electrode breakage and material loss, and exhibits good electrochemical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of battery technology, and more specifically, to a winding core, a method for its preparation, and a cylindrical battery. Background Technology

[0002] As is well known, during the winding process of cylindrical battery cells, the curvature of the electrodes decreases as the number of winding turns increases. In existing technologies, positive and negative electrode sheets with the same design are usually wound around a winding needle to form a core according to the designed thickness. Therefore, the inner electrode sheets have a larger curvature, resulting in greater mechanical stress. During charging and discharging, as the electrode sheets expand and contract, this stress on the inner electrode sheets changes continuously. Furthermore, during the cycling process, the expansion of the electrode sheets increases continuously, which also increases the stress on the electrode sheets, especially the inner electrode sheets. This can lead to electrode sheet breakage or material loss due to increased stress on the inner electrode sheets, resulting in a significant degradation in battery performance.

[0003] In view of this, the present invention is proposed. Summary of the Invention

[0004] The purpose of this invention is to provide a winding core, a method for preparing the same, and a cylindrical battery, aiming to improve at least one of the problems mentioned in the background art.

[0005] This invention is implemented as follows: In a first aspect, the present invention provides a core comprising n (n≥2) core units arranged sequentially from the inside out, each core unit comprising an electrode sheet and a separator, the electrode sheet comprising a positive electrode sheet and a negative electrode sheet, the separator comprising a first separator and a second separator, and each core unit comprising a first separator, a negative electrode sheet, a second separator and a positive electrode sheet wound sequentially. The formulation formula for the electrode is as follows: Σ n =α n %+β n %+γ n %, α n % represents the percentage of active material in the electrode, β n % represents the percentage of conductive agent in the electrode, γ n % represents the percentage of binder in the electrode, Σn=100%, and satisfies the following relationship: β n =a×n b , where a and b are constants, with a taking values ​​from 1 to 5 and b being -0.393; γ n =c×n d Where c and d are constants, d is -0.409, and a and c satisfy c = 2.99 × a 0.4313 ; The surface density σ of the positive electrode satisfies the formula: σn =11.3×ln(n)+k, where k ranges from 15 to 25, and σ is in mg / cm³. 2 ; The surface density ω of the negative electrode satisfies the formula: C 负 ×ω n ×α n正 %=λ×C 正 ×σ n ×α n负 %, ω is in mg / cm³ 2 Where λ is a constant of 1.05~1.25, C 正 C represents the specific capacity of the positive electrode, expressed in mAh / g. 负 The specific capacity of the negative electrode is expressed in mAh / g; α n正 % represents the percentage of active material in the positive electrode; α n负 % represents the percentage of active material in the negative electrode.

[0006] In an optional embodiment, the active material in the positive electrode is a nickel-cobalt-manganese ternary material, lithium iron phosphate, or lithium cobalt oxide.

[0007] In an optional embodiment, the active material in the negative electrode sheet is graphite, hard carbon, soft carbon, silicon negative electrode material, or lithium titanate.

[0008] In an optional embodiment, the diaphragm is a PP, PE, or PP and PE composite membrane, or a PP, PE, or PP and PE composite membrane coated with ceramic or PVDF composite membrane.

[0009] In an optional implementation, the thickness D of each of the core units n =δ×n+μ, where δ and μ are constants, δ=2~6, μ=10~20, D n The unit is mm; Secondly, the present invention provides a method for preparing a winding core, for preparing a winding core as described in any of the foregoing embodiments, comprising: The first diaphragm, negative electrode, second diaphragm and positive electrode are sequentially placed on the winding needle and wound. After winding, the end is finished to obtain the first core unit. The first core unit is sequentially arranged with a first diaphragm, a negative electrode sheet, a second diaphragm, and a positive electrode sheet, and then wound. After the winding is completed, the second core unit is obtained by finishing the winding. When n=2, the core is obtained after obtaining the second core unit; when n>2, at least one core unit is wound on the basis of the second core unit, following the method for obtaining the second core unit.

[0010] Thirdly, the present invention provides a cylindrical battery comprising a winding core as described in any of the foregoing embodiments.

[0011] The present invention has the following beneficial effects: 1. It can greatly improve the phenomenon of electrode breakage and material loss caused by high stress in the inner ring of the core; 2. Using electrode designs with different core units can improve the energy density of the battery while ensuring battery performance; 3. The problem of electrode stress has been improved, and the design can further increase the battery thickness in the direction of the existing cylindrical battery thickness, thereby increasing the battery's energy density. Attached Figure Description

[0012] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the embodiments will be briefly introduced below. It should be understood that the following drawings only show some embodiments of the present invention and should not be regarded as a limitation on the scope. For those skilled in the art, other related drawings can be obtained based on these drawings without creative effort.

[0013] Figure 1 This is a schematic diagram of the core structure provided in an embodiment of the present invention. Detailed Implementation

[0014] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.

[0015] The features and performance of the present invention will be further described in detail below with reference to embodiments.

[0016] like Figure 1 As shown, an embodiment of the present invention provides a wound core comprising n (n≥2) wound core units sequentially nested from the inside out. Each wound core unit includes an electrode sheet and a separator. The electrode sheet includes a positive electrode sheet and a negative electrode sheet, and the separator includes a first separator and a second separator. Each wound core unit is composed of a first separator, a negative electrode sheet, a second separator, and a positive electrode sheet wound sequentially. The formulation formula of the electrode sheet is as follows: Σ n =α n %+β n %+γ n %, α n % represents the percentage of active material in the electrode, β n % represents the percentage of conductive agent in the electrode, γ n % represents the percentage of binder in the electrode, Σn=100%, and satisfies the following relationship: βn =a×n b , where a and b are constants, with a taking values ​​from 1 to 5 and b being -0.393; γ n =c×n d Where c and d are constants, d is -0.409, and a and c satisfy c = 2.99 × a 0.4313 ; The surface density σ of the positive electrode satisfies the formula: σ n =11.3×ln(n)+k, where k ranges from 15 to 25, and σ is in mg / cm³. 2 ; The surface density ω of the negative electrode satisfies the formula: C 负 ×ω n ×α n正 %=λ×C 正 ×σ n ×α n负 %, ω is in mg / cm³ 2 Where λ is a constant of 1.05~1.25, C 正 C represents the specific capacity of the positive electrode, expressed in mAh / g. 负 The specific capacity of the negative electrode is expressed in mAh / g; α n正 % represents the percentage of active material in the positive electrode; α n负 % represents the percentage of active material in the negative electrode.

[0017] The core provided in this invention is composed of multiple core units nested sequentially. Through extensive creative work by the inventors, it was discovered that when the design of the electrode sheet of this non-continuous core meets the requirements defined by the above formulas, the phenomenon of inner ring electrode sheet breakage and material loss during the use of the core can be effectively avoided, thereby improving the battery's service life. Moreover, as the number of winding turns increases, the proportion of active material in the electrode sheet is increased, and the energy density of the battery can be improved without reducing performance such as rate capability and service life.

[0018] Furthermore, to ensure the overall performance of the battery, the thickness D of each core unit is... n =δ×n+μ, where δ and μ are constants, δ=2~6, μ=10~20, D n The unit is mm; Furthermore, the first diaphragm and the second diaphragm are diaphragms of the same specification, and the diaphragms used in different core units are of the same specification.

[0019] Optionally, the active material in the positive electrode sheet can be any active material that can be used in the positive electrode of a battery, such as nickel-cobalt-manganese ternary materials, lithium iron phosphate, or lithium cobalt oxide.

[0020] Optionally, the active material in the negative electrode sheet can be any active material that can be used in the battery negative electrode, such as graphite, hard carbon, soft carbon, silicon negative electrode material, or lithium titanate.

[0021] Optionally, the diaphragm is a PP, PE, or PP and PE composite membrane, or a PP, PE, or PP and PE composite membrane coated with ceramic or PVDF composite membrane.

[0022] The first and second diaphragms within each core unit are made of the same material and have the same specifications; the diaphragm materials and thicknesses between different core units may differ, but the width must be consistent.

[0023] This invention provides a method for preparing a winding core, which includes: The first separator, negative electrode, second separator and positive electrode are sequentially placed on the winding needle and wound. After winding, the finishing adhesive is applied to finish the winding, and the first core unit is obtained. The first core unit is sequentially set with a first diaphragm, a negative electrode sheet, a second diaphragm, and a positive electrode sheet, and then wound. After winding, a finishing adhesive is applied to finish the winding, thus obtaining the second core unit. When n=2, the core is obtained after obtaining the second core unit; when n>2, at least one core unit is wound on the basis of the second core unit, following the method for obtaining the second core unit.

[0024] During fabrication, the number of turns of the core unit is determined by its thickness, i.e., the thickness D of each core unit is calculated using the formula. n =δ×n+μ, where δ and μ are constants, δ=2~6, μ=10~20, D n The unit is mm.

[0025] An embodiment of the present invention provides a cylindrical battery, which includes a wound core provided in this embodiment. Specifically, the wound core is disposed within the space enclosed by the casing and the cover plate.

[0026] The following provides several embodiments and comparative examples to illustrate the technical solutions provided in this application.

[0027] In the following embodiments and comparative examples.

[0028] The positive electrode active material is lithium iron phosphate, the positive electrode conductive agent is carbon black, and the positive electrode binder is PVDF.

[0029] The negative electrode active material is graphite, and the negative electrode binder is CMC and SBR, with a ratio of 2:3.

[0030] The specific capacity of the positive electrode active material is known to be 142 mAh / g, and the specific capacity of the negative electrode active material is known to be 335 mAh / g.

[0031] The parameter settings for each embodiment are shown in Tables 1-4: Table 1 Parameter settings for Example 1

[0032] Table 2 Parameter settings for Example 2

[0033] Table 3 Parameter settings for Example 3

[0034] Table 4 Parameter settings for Example 4

[0035] Comparative Example 1 The positive electrode, negative electrode, and separator of this comparative example are exactly the same as those of the first core unit in Example 3. The core is made with the existing continuous winding method and has a thickness that is basically the same as that of Example 3 (rounded to the nearest integer of 60 mm; note: due to the different winding methods, it is impossible to make them exactly the same).

[0036] Comparative Example 2 The positive electrode, negative electrode, and separator of this comparative example are exactly the same as those of the second core unit in Example 3. The core is made with the existing continuous winding method and has a thickness that is basically the same as that of Example 3 (rounded to the nearest integer of 60 mm; note: due to the different winding methods, it is impossible to make them exactly the same).

[0037] Comparative Example 3 The positive electrode, negative electrode, and separator of this comparative example are exactly the same as those of the third core unit in Example 3. The core is made with the existing continuous winding method and has a thickness that is basically the same as that of Example 3 (rounded to the nearest integer of 60 mm; note: due to the different winding methods, it is impossible to make them exactly the same).

[0038] Experimental Example The winding cores provided in the various embodiments and comparative examples were used to fabricate cylindrical batteries, and their electrochemical performance was tested.

[0039] Record the test results in Table 5.

[0040] Table 5. Electrochemical performance of the battery cells in each embodiment and comparative example.

[0041] As can be seen from the table above, the cells provided in each embodiment all exhibit good electrochemical performance after being manufactured into batteries. Comparing Example 3 with the comparative examples, the capacity retention rate of Example 3 is almost no worse than that of the comparative examples, and the energy density is significantly higher. Therefore, it is evident that the cell provided by the present invention has better electrochemical performance than existing cells.

[0042] In summary, the winding core provided by the present invention has the following advantages: 1. It can greatly improve the phenomenon of electrode breakage and material loss caused by high stress in the inner ring of the core; 2. Using electrode designs with different core units can improve the energy density of the battery while ensuring battery performance; 3. The problem of electrode stress has been improved, and the design can further increase the battery thickness in the direction of the existing cylindrical battery thickness, thereby increasing the battery's energy density.

[0043] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A type of winding core, characterized in that, It includes n (n is 2 to 4) core units arranged sequentially from the inside to the outside. Each core unit includes an electrode and a separator. The electrode includes a positive electrode and a negative electrode. The separator includes a first separator and a second separator. Each core unit is composed of a first separator, a negative electrode, a second separator and a positive electrode wound sequentially. The formulation formula for the electrode is as follows: Σ n =α n %+β n %+γ n %, α n % represents the percentage of active material in the electrode, β n % represents the percentage of conductive agent in the electrode, γ n % represents the percentage of binder in the electrode, Σn=100%, and satisfies the following relationship: β n =a×n b , where a and b are constants, with a taking values ​​from 1 to 5 and b being -0.393; γ n =c×n d Where c and d are constants, d is -0.409, and a and c satisfy c = 2.99 × a 0.4313 ; The surface density σ of the positive electrode satisfies the formula: σ n =11.3×ln(n)+k, where k ranges from 15 to 25, and σ is in mg / cm³. 2 ; The surface density ω of the negative electrode satisfies the formula: C 负 ×ω n ×α n正 %=λ×C 正 ×σ n ×α n负 %, ω is in mg / cm³ 2 Where λ is a constant of 1.05~1.25, C 正 The specific capacity of the positive electrode active material is expressed in mAh / g; C 负 The specific capacity of the negative electrode active material is expressed in mAh / g; α n正 % represents the percentage of active material in the positive electrode; α n负 % represents the percentage of active material in the negative electrode.

2. The winding core according to claim 1, characterized in that, The active material in the positive electrode is a nickel-cobalt-manganese ternary material, lithium iron phosphate, or lithium cobalt oxide.

3. The winding core according to claim 1, characterized in that, The active material in the negative electrode sheet is graphite, hard carbon, soft carbon, silicon negative electrode material, or lithium titanate.

4. The winding core according to claim 1, characterized in that, The diaphragm is a PP, PE, or PP and PE composite membrane, or a PP, PE, PP and PE composite membrane coated with ceramic or PVDF composite membrane.

5. The winding core according to any one of claims 1 to 4, characterized in that, The thickness D of each of the core units n =δ×n+μ, where δ and μ are constants, δ=2~6, μ=10~20, D n The unit is mm.

6. A method for preparing a winding core, characterized in that, For preparing the core as described in any one of claims 1 to 5, comprising: The first diaphragm, negative electrode, second diaphragm and positive electrode are sequentially placed on the winding needle and wound. After winding, the end is finished to obtain the first core unit. A first diaphragm, a negative electrode sheet, a second diaphragm, and a positive electrode sheet are sequentially arranged and wound on the first core unit. After the winding is completed, the second core unit is obtained by finishing the winding. When n=2, the core is obtained after obtaining the second core unit; when n>2, at least one core unit is wound on the basis of the second core unit, following the method for obtaining the second core unit.

7. A cylindrical battery, characterized in that, Includes the core as described in any one of claims 1 to 5.

Citation Information

Patent Citations

  • A multi-layer coiling column battery and its making technology

    CN101188308A

  • Cylindrical battery

    CN217182241U