A kind of all-sulfur liquid flow battery and preparation method thereof
By using (NH4)2Sm and (NH4)2Sn as electrolytes in alkali metal/sulfur batteries, combined with catalyst-loaded porous carbon material electrodes, the problems of low electronic conductivity and short cycle life of sulfur batteries are solved and achieved Efficient energy storage and long life of all-sulfur flow batteries.
Patent Information
- Application Number
- CN202310974241.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-03
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-08-03
AI Technical Summary
The commercial application of alkali metal/sulfur batteries has been hindered by the low electronic conductivity of sulfur, the shuttle effect, and short cycle life.
Using (NH4)2Sm (6≤m≤8) and (NH4)2Sn (4≤n≤6) as the positive and negative active materials of the flow battery, combined with the porous carbon material electrode loaded with catalyst, through selective ammonium ions Exchange membrane separation is used to construct an all-sulfur flow battery, and the electrochemical reaction efficiency is improved through an electrolyte circulation system.
It achieves long-term use, flexibility, scalability and rechargeability, improves the Coulomb efficiency and voltage efficiency of the battery, and extends the cycle life of the battery.
Smart Images

Figure CN116845311B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of energy storage, and mainly relates to an all-sulfur liquid flow battery and a preparation method thereof. Background Art
[0002] Alkali metal / sulfur batteries with high energy density are 5 to 6 times that of commercialized graphite / lanthanum ammonium phosphate batteries, and elemental sulfur is abundant and environmentally friendly, so they have attracted much attention in recent years. However, sulfur as an electrode active material also has shortcomings. 1) Elemental sulfur and discharge product sulfides have low electronic conductivity. 2) The discharge intermediate product polysulfide is easily dissolved in the electrolyte, and the shuttle effect causes low coulombic efficiency. 3) The volume effect of the sulfur electrode before and after charging and discharging leads to a short cycle life. These problems hinder the commercialization of alkali metal / sulfur batteries. Summary of the invention
[0003] In order to overcome the deficiencies of the prior art, an object of the present invention is to provide an all-sulfur liquid flow battery and a preparation method thereof.
[0004] The purpose of the present invention is achieved by at least one of the following technical solutions.
[0005] The present invention proposes a full-sulfur liquid flow battery that can be used for large-scale energy storage, using (NH4)2S m (6≤m≤8), (NH4)2S n (4≤n≤6) is used as the positive and negative active materials of the liquid flow battery, and the porous carbon material electrode loaded with catalyst is used as the electrochemical reaction matrix.
[0006] The all-sulfur liquid flow battery provided by the present invention comprises: electrodes, a battery stack body and an electrolyte storage tank; the battery stack body is hollow, and the interior is divided into a positive electrode chamber and a negative electrode chamber by a diaphragm; the electrolyte storage tank comprises a positive electrode electrolyte tank and a negative electrode electrolyte tank; the positive electrode electrolyte tank is provided with a positive electrode electrolyte; the negative electrode electrolyte tank is provided with a negative electrode electrolyte; the positive electrode electrolyte tank and the positive electrode chamber form a circulation path through pipes and pumps; the negative electrode electrolyte tank and the negative electrode chamber form a circulation path through pipes and pumps; the electrodes comprise a positive electrode and a negative electrode; the positive electrode is placed in the positive electrode chamber and contacts with the positive electrode electrolyte; the negative electrode is placed in the negative electrode chamber and contacts with the negative electrode electrolyte; the positive electrode electrolyte is (NH4)2S m A solution, wherein 6≤m≤8; the negative electrode electrolyte is (NH4)2S n of solutions, 4≤n≤6.
[0007] Furthermore, the separator is a selective ammonium ion exchange membrane. The separator can separate the positive electrode and the negative electrode.
[0008] Furthermore, the electrode is a porous carbon material.
[0009] Preferably, the porous carbon material is carbon felt.
[0010] Preferably, the electrode is a porous carbon material loaded with a catalyst; the catalyst is one or more of cerium hydroxide, praseodymium hydroxide, and lanthanum hydroxide.
[0011] Further preferably, the catalyst is one of cerium hydroxide, praseodymium hydroxide, lanthanum hydroxide, a mixture of cerium hydroxide and praseodymium hydroxide, a mixture of cerium hydroxide and lanthanum hydroxide, a mixture of praseodymium hydroxide and lanthanum hydroxide, and a mixture of cerium hydroxide, praseodymium hydroxide and lanthanum hydroxide.
[0012] Furthermore, the catalyst loading is 0.1 to 10 g / cm 2 .
[0013] The present invention provides a method for preparing an all-sulfur liquid flow battery, comprising the following steps:
[0014] (1) Preparation of (NH4)2S m Solution and (NH4)2S n of solution;
[0015] (2) (NH4)2S m The solution is placed in the positive electrode electrolyte tank, (NH4)2S n The solution is placed in the negative electrode electrolyte tank, the electrodes and the diaphragm are assembled in the battery stack body, and then the battery stack body, the positive electrode electrolyte tank, and the negative electrode electrolyte tank are connected to assemble the all-sulfur liquid flow battery.
[0016] Furthermore, the (NH4)2S m Solution or (NH4)2S n The preparation of the solution comprises:
[0017] Dissolve (NH4)2S and ammonium salt in a solvent (preferably anhydrous ethanol), stir evenly at a temperature of 20 to 80°C to obtain a mixed solution, then add sulfur and mix evenly to obtain the (NH4)2S m Solution or (NH4)2S n of solution.
[0018] Furthermore, the ammonium salt is one or more of ammonium perchlorate, ammonium hexafluorophosphate, ammonium hexafluoroarsenate, ammonium hexafluoroantimonate, ammonium tetrafluoroborate, ammonium trifluoromethylsulfonate, ammonium di(trifluoromethylsulfonyl)imide, ammonium bis(trifluoromethanesulfonyl)imide, and ammonium nitrate; in the mixed solution, the concentration of the ammonium salt is 0.01 to 5 mol / L; and the solvent is anhydrous ethanol.
[0019] Further, when preparing (NH4)2S mWhen the solution is prepared, the molar ratio of (NH4)2S to sulfur is 1:5-7; the molar volume ratio of (NH4)2S to the solvent is 0.1-5:1 mol / L.
[0020] Preferably, when preparing (NH4)2S m When the solution is prepared, the molar ratio of (NH4)2S to sulfur is 1:7.
[0021] Further, when preparing (NH4)2S n When the solution is prepared, the molar ratio of (NH4)2S to sulfur is 1:3-5; the molar volume ratio of (NH4)2S to the solvent is 0.1-5:1 mol / L.
[0022] Preferably, when preparing the (NH4)2S4 electrolyte, the molar ratio of (NH4)2S to sulfur is 1:3.
[0023] The present invention uses highly soluble polysulfides to prepare an all-sulfur liquid flow battery. Preferably, the all-sulfur liquid flow battery includes a battery stack unit, an electrolyte circulation system, a battery management system and an auxiliary system, and the battery stack unit is composed of an electrolyte, a positive electrode, a negative electrode, an exchange membrane, a bipolar plate and a current collector. (NH4)2S m (6≤m≤8), (NH4)2S n (4≤n≤6) are dissolved in anhydrous ethanol and used as the electrolyte of the all-sulfur flow battery and as the positive and negative active materials, respectively stored in two liquid storage tanks. The porous carbon material loaded with catalyst is used as the positive and negative electrodes, respectively, and the selective ammonium ion exchange membrane is used as the diaphragm.
[0024] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0025] The all-sulfur liquid flow battery provided by the present invention adopts (NH4)2S m (6≤m≤8) solution as positive electrode electrolyte and (NH4)2S n The solution of (4≤n≤6) as the negative electrode electrolyte not only solves the three problems of sulfur as a battery material, namely low electronic conductivity, low coulombic efficiency caused by shuttle effect and short cycle life, but also takes advantage of the high capacity density of sulfur and the high solubility of polysulfide, so that the prepared all-sulfur liquid flow battery has the function of large-scale energy storage. The all-sulfur liquid flow battery has the characteristics of long-term use, flexibility, scalability, rechargeability and environmental friendliness. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a graph showing the electrical performance test results of the all-sulfur liquid flow battery prepared in Example 1 of the present invention;
[0027] Figure 2This is a graph showing the electrical performance test results of the all-sulfur liquid flow battery prepared in Example 2 of the present invention;
[0028] Figure 3 This is a graph showing the electrical performance test results of the all-sulfur liquid flow battery prepared in Example 3 of the present invention;
[0029] Figure 4 This is a graph showing the electrical performance test results of the all-sulfur liquid flow battery prepared in Example 4 of the present invention;
[0030] Figure 5 This is a graph showing the electrical performance test results of the all-sulfur liquid flow battery prepared in Example 5 of the present invention;
[0031] Figure 6 This is a graph showing the electrical performance test results of the all-sulfur liquid flow battery prepared in Example 6 of the present invention;
[0032] Figure 7 This is a graph showing the electrical performance test results of the all-sulfur liquid flow battery prepared in Example 7 of the present invention;
[0033] Figure 8 This is a graph showing the electrical performance test results of the all-sulfur liquid flow battery prepared in Example 8 of the present invention;
[0034] Fig. 9 This is a graph showing the electrical performance test results of the all-sulfur liquid flow battery prepared in Example 9 of the present invention;
[0035] Fig.10 This is a graph showing the electrical performance test results of the all-sulfur liquid flow battery prepared in Example 10 of the present invention. DETAILED DESCRIPTION
[0036] The specific implementation of the present invention is further described below in conjunction with examples, but the implementation and protection of the present invention are not limited thereto. It should be noted that if there are processes that are not particularly described in detail below, they can be implemented or understood by those skilled in the art with reference to the prior art. If the manufacturer of the reagents or instruments used is not indicated, they are deemed to be conventional products that can be purchased commercially.
[0037] Example 1
[0038] The all-sulfur liquid flow battery provided in Example 1 of the present invention comprises: an electrode, a battery stack body and an electrolyte storage tank; the battery stack body is hollow, and the interior is divided into a positive electrode chamber and a negative electrode chamber by a diaphragm; the electrolyte storage tank comprises a positive electrode electrolyte tank and a negative electrode electrolyte tank; the positive electrode electrolyte tank is provided with a positive electrode electrolyte; the negative electrode electrolyte tank is provided with a negative electrode electrolyte; the positive electrode electrolyte tank and the positive electrode chamber form a circulation path through a pipeline and a pump; the negative electrode electrolyte tank and the negative electrode chamber form a circulation path through a pipeline and a pump; the electrode comprises a positive electrode and a negative electrode; the positive electrode is a porous carbon material (carbon felt) loaded with a catalyst, which is placed in the positive electrode chamber and in contact with the positive electrode electrolyte; the negative electrode is a porous carbon material (carbon felt) loaded with a catalyst, which is placed in the negative electrode chamber and in contact with the negative electrode electrolyte; the selective ammonium ion exchange membrane is a diaphragm; the positive electrode electrolyte is (NH4)2S m and an ethanol solution of an ammonium salt, wherein m is 7, and the negative electrode electrolyte is (NH4)2S n and ethanol solution of ammonium salt, the value of n is 4.
[0039] The (NH4)2S m The preparation of a solution (i.e., (NH4)2S8 positive electrode electrolyte) includes: dissolving (NH4)2S and ammonium perchlorate in anhydrous ethanol to obtain a mixed solution, in which the concentration of ammonium perchlorate is 0.01 mol / L; then adding elemental sulfur at 40°C and stirring evenly to obtain the (NH4)2S8 positive electrode electrolyte. m A solution ((NH4)2S8 positive electrode electrolyte), wherein the molar ratio of (NH4)2S to elemental sulfur is 1:7, and the (NH4)2S m The molar volume ratio to the solvent is 4:1 mol / L.
[0040] The (NH4)2S n The preparation of a solution (i.e., (NH4)2S4 negative electrode electrolyte) includes: dissolving (NH4)2S and ammonium perchlorate in anhydrous ethanol to obtain a mixed solution, in which the concentration of ammonium perchlorate is 0.01 mol / L; then adding elemental sulfur at 50°C and stirring evenly to obtain the (NH4)2S n A solution ((NH4)2S4 negative electrode electrolyte), wherein the molar ratio of (NH4)2S to elemental sulfur is 1:3, and the (NH4)2S n The molar volume ratio to the solvent is 4:1 mol / L.
[0041] The positive electrode and the negative electrode are both made of porous carbon materials loaded with catalysts; the catalyst loaded on the positive electrode is cerium hydroxide with a loading of 3 g / cm 2 The catalyst loaded on the negative electrode is cerium hydroxide, with a loading of 3 g / cm 2 .
[0042] Effect verification
[0043] The electrical performance of the all-sulfur liquid flow battery provided in Example 1 of the present invention was tested with reference to the standard (GB / T 33339-2016, all-vanadium liquid flow battery system test method).
[0044] When the test operating temperature is 30°C, the (NH4)2S8 positive electrode electrolyte circulates between the positive electrode of the battery stack and the positive electrode electrolyte storage tank at a flow rate of 400L / h, and the (NH4)2S4 negative electrode electrolyte circulates between the negative electrode of the battery stack and the negative electrode electrolyte storage tank at a flow rate of 400L / h. 2 Electrochemical reduction and oxidation reactions occur at voltages of 0.3 to 0.9 V, respectively, completing the charge and discharge cycle of the all-sulfur liquid flow battery. Figure 1 The electrical performance test result diagram of the all-sulfur liquid flow battery prepared in Example 1 of the present invention is shown in FIG. Figure 1 As shown, the all-sulfur liquid flow battery prepared in Example 1 has no obvious attenuation in battery energy efficiency after 500 charge and discharge cycles. The coulomb efficiency of the all-sulfur liquid flow battery prepared in Example 1 is 86.92% to 91.63% within 500 charge and discharge cycles, and the first coulomb efficiency is 90.02%; its voltage efficiency within 500 charge and discharge cycles is 82.06% to 85.00%, and the first voltage efficiency is 85.06%; its energy efficiency within 500 charge and discharge cycles is 71.44% to 80.10%, and the first energy efficiency is 80.11%.
[0045] Example 2
[0046] The specific assembly and testing techniques of the all-sulfur liquid flow battery of this embodiment are basically the same as those of Embodiment 1.
[0047] The all-sulfur liquid flow battery of this embodiment is different from the all-sulfur liquid flow battery provided in Example 1 in that:
[0048] The (NH4)2S m The preparation of a solution (i.e., (NH4)2S6 positive electrode electrolyte) includes: dissolving (NH4)2S and ammonium hexafluorophosphate in anhydrous ethanol to obtain a mixed solution, in which the concentration of ammonium hexafluorophosphate is 1 mol / L; then adding elemental sulfur at 50°C and stirring evenly to obtain the (NH4)2S6 positive electrode electrolyte. m A solution ((NH4)2S6 positive electrode electrolyte), wherein the molar ratio of (NH4)2S to elemental sulfur is 1:5, and the (NH4)2S m The molar volume ratio to the solvent is 0.1:1 mol / L.
[0049] The (NH4)2Sn The preparation of a solution (i.e., (NH4)2S6 negative electrode electrolyte) includes: dissolving (NH4)2S and ammonium hexafluorophosphate in anhydrous ethanol to obtain a mixed solution, in which the concentration of ammonium hexafluorophosphate is 0.01 mol / L; then adding elemental sulfur at 50°C and stirring evenly to obtain the (NH4)2S6 negative electrode electrolyte. n A solution ((NH4)2S6 negative electrode electrolyte), wherein the molar ratio of (NH4)2S to elemental sulfur is 1:5, and the (NH4)2S n The molar volume ratio to the solvent is 0.1:1 mol / L.
[0050] The positive electrode and the negative electrode are both made of porous carbon materials loaded with catalysts; the catalyst loaded on the positive electrode is praseodymium hydroxide, with a loading amount of 10 g / cm 2 The catalyst loaded on the negative electrode is praseodymium hydroxide, with a loading of 10 g / cm 2 .
[0051] Figure 2 The electrical performance test result diagram of the all-sulfur liquid flow battery prepared in Example 2 of the present invention; after testing, the all-sulfur liquid flow battery prepared in Example 2 has no obvious attenuation in battery energy efficiency after 500 charge and discharge cycles. The coulomb efficiency of the all-sulfur liquid flow battery prepared in Example 2 within 500 charge and discharge cycles is 83.29% to 88.15%, and the first coulomb efficiency is 88.03%; its voltage efficiency within 500 charge and discharge cycles is 82.10% to 87.85%, and the first voltage efficiency is 87.05%; its energy efficiency within 500 charge and discharge cycles is 76.16% to 82.00%, and the first energy efficiency is 82.02%.
[0052] Example 3
[0053] The specific assembly and testing techniques of the all-sulfur liquid flow battery of this embodiment are basically the same as those of Embodiment 1.
[0054] The all-sulfur liquid flow battery of this embodiment is different from the all-sulfur liquid flow battery provided in Example 1 in that:
[0055] The (NH4)2S m The preparation of a solution (i.e., (NH4)2S7 positive electrode electrolyte) includes: dissolving (NH4)2S and ammonium trifluoromethylsulfonate in anhydrous ethanol to obtain a mixed solution, in which the concentration of ammonium trifluoromethylsulfonate is 1.8 mol / L; then adding elemental sulfur at 20°C and stirring evenly to obtain the (NH4)2S m solution ((NH4)2S7 positive electrolyte), in which (NH4)2S mThe molar ratio of elemental sulfur to elemental sulfur is 1:6, and the molar volume ratio of elemental sulfur to solvent is 5:1 mol / L.
[0056] The (NH4)2S n The preparation of a solution (i.e., (NH4)2S5 negative electrode electrolyte) includes: dissolving (NH4)2S and ammonium trifluoromethylsulfonate in anhydrous ethanol to obtain a mixed solution, in which the concentration of ammonium trifluoromethylsulfonate is 1.8 mol / L; then adding elemental sulfur at 20°C and stirring evenly to obtain the (NH4)2S n A solution ((NH4)2S5 negative electrode electrolyte), wherein the molar ratio of (NH4)2S to elemental sulfur is 1:4, and the (NH4)2S n The molar volume ratio to the solvent is 5:1 mol / L.
[0057] The positive electrode and the negative electrode are both made of porous carbon materials loaded with catalysts; the catalyst loaded on the positive electrode is a mixture of cerium hydroxide / praseodymium hydroxide / lanthanum hydroxide, with a loading of 0.5 g / cm 2 The mass ratio of cerium hydroxide, praseodymium hydroxide and lanthanum hydroxide is 1:1:1; the catalyst loaded on the negative electrode is a mixture of cerium hydroxide / praseodymium hydroxide / lanthanum hydroxide, with a loading of 0.5 g / cm 2 , wherein the mass ratio of cerium hydroxide, praseodymium hydroxide and lanthanum hydroxide is 1:1:1.
[0058] Figure 3 The electrical performance test result diagram of the all-sulfur liquid flow battery prepared in Example 3 of the present invention; after testing, the all-sulfur liquid flow battery prepared in Example 3 has no obvious attenuation in battery energy efficiency after 500 charge and discharge cycles. The coulomb efficiency of the all-sulfur liquid flow battery prepared in Example 3 within 500 charge and discharge cycles is 79.11% to 83.69%, and the first coulomb efficiency is 83.07%; its voltage efficiency within 500 charge and discharge cycles is 82.96% to 89.00%, and the first voltage efficiency is 89.01%; its energy efficiency within 500 charge and discharge cycles is 78.74% to 85.00%, and the first energy efficiency is 85.02%.
[0059] Example 4
[0060] The specific assembly and testing techniques of the all-sulfur liquid flow battery of this embodiment are basically the same as those of Embodiment 1.
[0061] The all-sulfur liquid flow battery of this embodiment is different from the all-sulfur liquid flow battery provided in Example 1 in that:
[0062] The (NH4)2S mThe preparation of a solution (i.e., (NH4)2S8 positive electrode electrolyte) comprises: dissolving (NH4)2S and ammonium bis(trifluoromethanesulfonyl)imide in anhydrous ethanol to obtain a mixed solution, wherein the concentration of ammonium bis(trifluoromethanesulfonyl)imide in the mixed solution is 4.9 mol / L; then adding elemental sulfur at 60°C and stirring evenly to obtain the (NH4)2S8 positive electrode electrolyte. m A solution ((NH4)2S8 positive electrode electrolyte), wherein the molar ratio of (NH4)2S to elemental sulfur is 1:7, and the (NH4)2S m The molar volume ratio to the solvent is 3:1 mol / L.
[0063] (NH4)2S n The preparation of a solution (i.e., (NH4)2S4 negative electrode electrolyte) includes: dissolving (NH4)2S and ammonium bis(trifluoromethanesulfonyl)imide in anhydrous ethanol to obtain a mixed solution, in which the concentration of ammonium bis(trifluoromethanesulfonyl)imide is 4.9 mol / L; then adding elemental sulfur at 60°C and stirring evenly to obtain the (NH4)2S n A solution ((NH4)2S4 negative electrode electrolyte), wherein the molar ratio of (NH4)2S to elemental sulfur is 1:3, and the (NH4)2S n The molar volume ratio to the solvent is 3:1 mol / L.
[0064] The positive electrode and the negative electrode are both made of porous carbon materials loaded with catalysts; the catalyst loaded on the positive electrode is a mixture of cerium hydroxide / praseodymium hydroxide, with a loading of 0.5 g / cm 2 , wherein the mass ratio of cerium hydroxide to praseodymium hydroxide is 2:1; the catalyst loaded on the negative electrode is cerium hydroxide, with a loading amount of 0.5 g / cm 2 .
[0065] Figure 4 The electrical performance test result diagram of the all-sulfur liquid flow battery prepared in Example 4 of the present invention; after testing, the all-sulfur liquid flow battery prepared in Example 4 has no obvious attenuation in battery energy efficiency after 500 charge and discharge cycles. The coulomb efficiency of the all-sulfur liquid flow battery prepared in Example 4 within 500 charge and discharge cycles is 80.75% to 87.21%, and the first coulomb efficiency is 87.04%; its voltage efficiency within 500 charge and discharge cycles is 83.99% to 90.86%, and the first voltage efficiency is 90.05%; its energy efficiency within 500 charge and discharge cycles is 77.41% to 83.29%, and the first energy efficiency is 82.09%.
[0066] Example 5
[0067] The specific assembly and testing techniques of the all-sulfur liquid flow battery of this embodiment are basically the same as those of Embodiment 1.
[0068] The all-sulfur liquid flow battery of this embodiment is different from the all-sulfur liquid flow battery provided in Example 1 in that:
[0069] (NH4)2S m The preparation of a solution (i.e., (NH4)2S7 positive electrode electrolyte) includes: dissolving (NH4)2S and ammonium di(trifluoromethylsulfonyl)imide in anhydrous ethanol to obtain a mixed solution, in which the concentration of ammonium di(trifluoromethylsulfonyl)imide is 3 mol / L; then adding elemental sulfur at 70°C and stirring evenly to obtain the (NH4)2S7 positive electrode electrolyte. m A solution ((NH4)2S7 positive electrode electrolyte), wherein the molar ratio of (NH4)2S to elemental sulfur is 1:6, and the (NH4)2S m The molar volume ratio to the solvent is 2:1 mol / L.
[0070] (NH4)2S n The preparation of a solution (i.e., (NH4)2S4 negative electrode electrolyte) includes: dissolving (NH4)2S and ammonium di(trifluoromethylsulfonyl)imide in anhydrous ethanol to obtain a mixed solution, in which the concentration of ammonium di(trifluoromethylsulfonyl)imide is 3 mol / L; then adding elemental sulfur at 70°C and stirring evenly to obtain the (NH4)2S n A solution ((NH4)2S4 negative electrode electrolyte), wherein the molar ratio of (NH4)2S to elemental sulfur is 1:3, and the (NH4)2S n The molar volume ratio to the solvent is 2:1 mol / L.
[0071] The positive electrode and the negative electrode are both made of porous carbon materials loaded with catalysts; the catalyst loaded on the positive electrode is praseodymium hydroxide, with a loading amount of 0.3 g / cm 2 The catalyst loaded on the negative electrode is praseodymium hydroxide, with a loading of 0.3 g / cm 2 .
[0072] Figure 5 The electrical performance test result diagram of the all-sulfur liquid flow battery prepared in Example 5 of the present invention; after testing, the all-sulfur liquid flow battery prepared in Example 5 has no obvious attenuation in battery energy efficiency after 500 charge and discharge cycles. The coulomb efficiency of the all-sulfur liquid flow battery prepared in Example 5 is 79.16% to 84.00% within 500 charge and discharge cycles, and the first coulomb efficiency is 82.05%; its voltage efficiency within 500 charge and discharge cycles is 76.32% to 81.35%, and the first voltage efficiency is 84.04%; its energy efficiency within 500 charge and discharge cycles is 70.80% to 81.00%, and the first energy efficiency is 81.07%.
[0073] Example 6
[0074] The specific assembly and testing techniques of the all-sulfur liquid flow battery of this embodiment are basically the same as those of Embodiment 1.
[0075] The all-sulfur liquid flow battery of this embodiment is different from the all-sulfur liquid flow battery provided in Example 1 in that:
[0076] The (NH4)2S m The preparation of a solution (i.e., (NH4)2S8 positive electrode electrolyte) includes: dissolving (NH4)2S and ammonium hexafluoroarsenate in anhydrous ethanol to obtain a mixed solution, in which the concentration of ammonium hexafluoroarsenate is 0.3 mol / L; then adding elemental sulfur at 20°C and stirring evenly to obtain the (NH4)2S8 positive electrode electrolyte. m A solution ((NH4)2S8 positive electrode electrolyte), wherein the molar ratio of (NH4)2S to elemental sulfur is 1:7, and the (NH4)2S m The molar volume ratio to the solvent is 0.2:1 mol / L.
[0077] The (NH4)2S n The preparation of a solution (i.e., (NH4)2S5 negative electrode electrolyte) includes: dissolving (NH4)2S and ammonium hexafluoroarsenate in anhydrous ethanol to obtain a mixed solution, in which the concentration of ammonium hexafluoroarsenate is 0.3 mol / L; then adding elemental sulfur at 20°C and stirring evenly to obtain the (NH4)2S5 negative electrode electrolyte. n A solution ((NH4)2S5 negative electrode electrolyte), wherein the molar ratio of (NH4)2S to elemental sulfur is 1:4, and the (NH4)2S n The molar volume ratio to the solvent is 0.2:1 mol / L.
[0078] The positive electrode and the negative electrode are both made of porous carbon materials loaded with catalysts; the catalyst loaded on the positive electrode is a mixture of lanthanum hydroxide and praseodymium hydroxide, with a loading of 10 g / cm 2 , wherein the mass ratio of praseodymium hydroxide to lanthanum hydroxide is 5:3; the catalyst loaded on the negative electrode is a mixture of lanthanum hydroxide and praseodymium hydroxide, with a loading of 10 g / cm 2 , wherein the mass ratio of praseodymium hydroxide to lanthanum hydroxide is 5:3.
[0079] Figure 6The electrical performance test result diagram of the all-sulfur liquid flow battery prepared in Example 6 of the present invention; after testing, the all-sulfur liquid flow battery prepared in Example 6 has no obvious attenuation in battery energy efficiency after 500 charge and discharge cycles. The coulomb efficiency of the all-sulfur liquid flow battery prepared in Example 6 within 500 charge and discharge cycles is 78.16% to 82.91%, and the first coulomb efficiency is 82.01%; its voltage efficiency within 500 charge and discharge cycles is 78.42% to 84.90%, and the first voltage efficiency is 84.04%; its energy efficiency within 500 charge and discharge cycles is 75.02% to 81.00%, and the first energy efficiency is 81.08%.
[0080] Example 7
[0081] The specific assembly and testing techniques of the all-sulfur liquid flow battery of this embodiment are basically the same as those of Embodiment 1.
[0082] The all-sulfur liquid flow battery of this embodiment is different from the all-sulfur liquid flow battery provided in Example 1 in that:
[0083] The (NH4)2S m The preparation of a solution (i.e., (NH4)2S7 positive electrode electrolyte) includes: dissolving (NH4)2S and ammonium hexafluoroantimonate in anhydrous ethanol to obtain a mixed solution, in which the concentration of ammonium tetrafluoroborate is 2.5 mol / L; then adding elemental sulfur at 30°C and stirring evenly to obtain the (NH4)2S7 positive electrode electrolyte. m A solution ((NH4)2S7 positive electrode electrolyte), wherein the molar ratio of (NH4)2S to elemental sulfur is 1:6, and the (NH4)2S m The molar volume ratio to the solvent is 2.5:1 mol / L.
[0084] The (NH4)2S n The preparation of a solution (i.e., (NH4)2S6 negative electrode electrolyte) includes: dissolving (NH4)2S and ammonium tetrafluoroborate in anhydrous ethanol to obtain a mixed solution, in which the concentration of ammonium tetrafluoroborate is 2.5 mol / L; then adding elemental sulfur at 30°C and stirring evenly to obtain the (NH4)2S6 negative electrode electrolyte. n A solution ((NH4)2S6 negative electrode electrolyte), wherein the molar ratio of (NH4)2S to elemental sulfur is 1:5, and the (NH4)2S n The molar volume ratio to the solvent is 2.5:1 mol / L.
[0085] The positive electrode and the negative electrode are both made of porous carbon materials loaded with catalysts; the catalyst loaded on the positive electrode is praseodymium hydroxide, with a loading of 7 g / cm 2 The catalyst loaded on the negative electrode is praseodymium hydroxide, with a loading of 7 g / cm 2.
[0086] Figure 7 The figure is a result of the electrical performance test of the all-sulfur liquid flow battery prepared in Example 7 of the present invention; after testing, the all-sulfur liquid flow battery prepared in Example 7 has no obvious attenuation in battery energy efficiency after 500 charge and discharge cycles. The coulomb efficiency of the all-sulfur liquid flow battery prepared in Example 7 within 500 charge and discharge cycles is 72.30% to 81.00%, and the first coulomb efficiency is 81.06%; its voltage efficiency within 500 charge and discharge cycles is 78.34% to 83.42%, and the first voltage efficiency is 83.03%; its energy efficiency within 500 charge and discharge cycles is 81.03% to 86.00%, and the first energy efficiency is 86.02%.
[0087] Example 8
[0088] The specific assembly and testing techniques of the all-sulfur liquid flow battery of this embodiment are basically the same as those of Embodiment 1.
[0089] The all-sulfur liquid flow battery of this embodiment is different from the all-sulfur liquid flow battery provided in Example 1 in that:
[0090] (NH4)2S m The preparation of a solution (i.e., (NH4)2S6 positive electrode electrolyte) includes: dissolving (NH4)2S and ammonium tetrafluoroborate in anhydrous ethanol to obtain a mixed solution, in which the concentration of ammonium tetrafluoroborate is 3.5 mol / L; then adding elemental sulfur at 55°C and stirring evenly to obtain the (NH4)2S6 positive electrode electrolyte. m A solution ((NH4)2S6 positive electrode electrolyte), wherein the molar ratio of (NH4)2S to elemental sulfur is 1:5, and the (NH4)2S m The molar volume ratio to the solvent is 3.5:1 mol / L.
[0091] (NH4)2S n The preparation of a solution (i.e., (NH4)2S4 negative electrode electrolyte) includes: dissolving (NH4)2S and ammonium tetrafluoroborate in anhydrous ethanol to obtain a mixed solution, in which the concentration of ammonium tetrafluoroborate is 3.5 mol / L; then adding elemental sulfur at 55°C and stirring evenly to obtain the (NH4)2S n A solution ((NH4)2S4 negative electrode electrolyte), wherein the molar ratio of (NH4)2S to elemental sulfur is 1:3, and the (NH4)2S n The molar volume ratio to the solvent is 3.5:1 mol / L.
[0092] The positive electrode and the negative electrode are both made of porous carbon materials loaded with catalysts; the catalyst loaded on the positive electrode is lanthanum hydroxide, with a loading of 3 g / cm2 The catalyst loaded on the negative electrode is lanthanum hydroxide, with a loading of 3 g / cm 2 .
[0093] Figure 8 The electrical performance test result diagram of the all-sulfur liquid flow battery prepared in Example 8 of the present invention; after testing, the all-sulfur liquid flow battery prepared in Example 8 has no obvious attenuation in battery energy efficiency after 500 charge and discharge cycles. The coulomb efficiency of the all-sulfur liquid flow battery prepared in Example 8 within 500 charge and discharge cycles is 79.70% to 84.01%, and the first coulomb efficiency is 84.03%; its voltage efficiency within 500 charge and discharge cycles is 73.17% to 82.62%, and the first voltage efficiency is 82.04%; its energy efficiency within 500 charge and discharge cycles is 79.04% to 84.24%, and the first energy efficiency is 84.05%.
[0094] Example 9
[0095] The specific assembly and testing techniques of the all-sulfur liquid flow battery of this embodiment are basically the same as those of Embodiment 1.
[0096] The all-sulfur liquid flow battery of this embodiment is different from the all-sulfur liquid flow battery provided in Example 1 in that:
[0097] (NH4)2S m The preparation of a solution (i.e., (NH4)2S8 positive electrode electrolyte) includes: dissolving (NH4)2S and ammonium nitrate in anhydrous ethanol to obtain a mixed solution, in which the concentration of ammonium nitrate is 3.5 mol / L; then adding elemental sulfur at 45°C and stirring evenly to obtain the (NH4)2S8 positive electrode electrolyte. m A solution ((NH4)2S8 positive electrode electrolyte), wherein the molar ratio of (NH4)2S to elemental sulfur is 1:7, and the (NH4)2S m The molar volume ratio to the solvent is 0.2:1 mol / L.
[0098] (NH4)2S n The preparation of a solution (i.e., (NH4)2S6 negative electrode electrolyte) includes: dissolving (NH4)2S and ammonium nitrate in anhydrous ethanol to obtain a mixed solution, in which the concentration of ammonium nitrate is 3.5 mol / L; then adding elemental sulfur at 45°C and stirring evenly to obtain the (NH4)2S6 negative electrode electrolyte. n A solution ((NH4)2S6 negative electrode electrolyte), wherein the molar ratio of (NH4)2S to elemental sulfur is 1:5, and the (NH4)2S n The molar volume ratio to the solvent is 0.2:1 mol / L.
[0099] The positive electrode and the negative electrode are both made of porous carbon materials loaded with catalysts; the catalyst loaded on the positive electrode is praseodymium hydroxide, with a loading of 6 g / cm 2 The catalyst loaded on the negative electrode is praseodymium hydroxide, with a loading of 6 g / cm 2 .
[0100] Fig. 9 The electrical performance test result diagram of the all-sulfur liquid flow battery prepared in Example 9 of the present invention; after testing, the all-sulfur liquid flow battery prepared in Example 9 has no obvious attenuation in battery energy efficiency after 500 charge and discharge cycles. The coulomb efficiency of the all-sulfur liquid flow battery prepared in Example 9 within 500 charge and discharge cycles is 78.58% to 83.29%, and the first coulomb efficiency is 83.08%; its voltage efficiency within 500 charge and discharge cycles is 75.03% to 81.26%, and the first voltage efficiency is 81.01%; its energy efficiency within 500 charge and discharge cycles is 81.42% to 88.38%, and the first energy efficiency is 88.03%.
[0101] Example 10
[0102] The specific assembly and testing techniques of the all-sulfur liquid flow battery of this embodiment are the same as those of Embodiment 1.
[0103] The all-sulfur liquid flow battery of this embodiment is different from the all-sulfur liquid flow battery provided in Example 1 in that:
[0104] (NH4)2S m The preparation of a solution (i.e., (NH4)2S8 positive electrode electrolyte) includes: dissolving (NH4)2S and ammonium trifluoromethylsulfonate in anhydrous ethanol to obtain a mixed solution, in which the concentration of ammonium trifluoromethylsulfonate is 4.5 mol / L; then adding elemental sulfur at 75°C and stirring evenly to obtain the (NH4)2S8 positive electrode electrolyte. m A solution ((NH4)2S8 positive electrode electrolyte), wherein the molar ratio of (NH4)2S to elemental sulfur is 1:7, and the (NH4)2S m The molar volume ratio to the solvent is 4.5:1 mol / L.
[0105] (NH4)2S n The preparation of a solution (i.e., (NH4)2S5 negative electrode electrolyte) includes: dissolving (NH4)2S and ammonium trifluoromethylsulfonate in anhydrous ethanol to obtain a mixed solution, in which the concentration of ammonium trifluoromethylsulfonate is 4.5 mol / L; then adding elemental sulfur at 75°C and stirring evenly to obtain the (NH4)2S5 negative electrode electrolyte. n A solution ((NH4)2S5 negative electrode electrolyte), wherein the molar ratio of (NH4)2S to elemental sulfur is 1:4, and the (NH4)2S nThe molar volume ratio to the solvent is 4.5:1 mol / L.
[0106] The positive electrode and the negative electrode are both made of porous carbon materials loaded with catalysts; the catalyst loaded on the positive electrode is lanthanum hydroxide with a loading of 4 g / cm 2 The catalyst loaded on the negative electrode is a mixture of cerium hydroxide and praseodymium hydroxide, with a loading of 4 g / cm 2 , wherein the mass ratio of cerium hydroxide to praseodymium hydroxide is 5:3.
[0107] Fig.10 The electrical performance test result diagram of the all-sulfur liquid flow battery prepared in Example 10 of the present invention; after testing, the all-sulfur liquid flow battery prepared in Example 10 has no obvious attenuation in battery energy efficiency after 500 charge and discharge cycles. The coulomb efficiency of the all-sulfur liquid flow battery prepared in Example 10 within 500 charge and discharge cycles is 76.83% to 83.00%, and the first coulomb efficiency is 83.04%; its voltage efficiency within 500 charge and discharge cycles is 74.20% to 81.00%, and the first voltage efficiency is 81.02%; its energy efficiency within 500 charge and discharge cycles is 81.33% to 88.64%, and the first energy efficiency is 88.06%.
[0108] The above embodiments are only preferred implementation modes of the present invention and are only used to explain the present invention rather than to limit the present invention. Any changes, substitutions, modifications, etc. made by those skilled in the art without departing from the spirit of the present invention should fall within the scope of protection of the present invention.
Claims
1. An all-sulfur liquid flow battery, characterized in that: include: Electrode, battery stack body and electrolyte storage tank; the battery stack body is hollow, and the interior is divided into a positive electrode chamber and a negative electrode chamber by a diaphragm; the electrolyte storage tank includes a positive electrode electrolyte tank and a negative electrode electrolyte tank; the positive electrode electrolyte tank is provided with a positive electrode electrolyte; the negative electrode electrolyte tank is provided with a negative electrode electrolyte; the positive electrode electrolyte tank and the positive electrode chamber form a circulation path; the negative electrode electrolyte tank and the negative electrode chamber form a circulation path; the electrodes include a positive electrode and a negative electrode; the positive electrode is placed in the positive electrode chamber and contacts with the positive electrode electrolyte; the negative electrode is placed in the negative electrode chamber and contacts with the negative electrode electrolyte; the positive electrode electrolyte is (NH4)2S m A solution, wherein 6≤m≤8; the negative electrode electrolyte is (NH4)2S n A solution, wherein 4≤n≤6; the preparation method of the all-sulfur liquid flow battery comprises the following steps: (1) preparing (NH4)2S m Solution and (NH4)2S n solution; (2) (NH4)2S m The solution is placed in the positive electrode electrolyte tank, (NH4)2S n The solution is placed in the negative electrode electrolyte tank, the electrodes and the diaphragm are assembled in the battery stack body, and then the battery stack body, the positive electrode electrolyte tank, and the negative electrode electrolyte tank are connected to assemble the all-sulfur liquid flow battery; the (NH4)2S m Solution or (NH4)2S n The preparation of the solution includes: dissolving (NH4)2S and ammonium salt in a solvent, stirring evenly at a temperature of 20-80°C to obtain a mixed solution, then adding sulfur, mixing evenly, and obtaining the (NH4)2S m Solution or (NH4)2S n The ammonium salt is one or more of ammonium perchlorate, ammonium hexafluorophosphate, ammonium hexafluoroarsenate, ammonium hexafluoroantimonate, ammonium tetrafluoroborate, ammonium trifluoromethylsulfonate, ammonium di(trifluoromethylsulfonyl)imide, ammonium bis(trifluoromethanesulfonyl)imide and ammonium nitrate; in the mixed solution, the concentration of the ammonium salt is 0.01-5 mol / L; and the solvent is anhydrous ethanol.
2. The all-sulfur liquid flow battery according to claim 1, characterized in that: The diaphragm is a selective ammonium ion exchange membrane.
3. The all-sulfur liquid flow battery according to claim 1, characterized in that: The electrode is made of porous carbon material.
4. The all-sulfur liquid flow battery according to claim 3, characterized in that: The electrode is a porous carbon material loaded with a catalyst; the catalyst is one or more of cerium hydroxide, praseodymium hydroxide and lanthanum hydroxide.
5. The all-sulfur liquid flow battery according to claim 4, characterized in that: The catalyst loading is 0.1-10 g / cm 2 .
6. The method for preparing an all-sulfur liquid flow battery according to claim 1, characterized in that: When preparing (NH4)2S m When the solution is prepared, the molar ratio of (NH4)2S to sulfur is 1:5-7; the molar volume ratio of (NH4)2S to the solvent is 0.1-5:1 mol / L.
7. The method for preparing an all-sulfur liquid flow battery according to claim 1, characterized in that: When preparing (NH4)2S n When the solution is prepared, the molar ratio of (NH4)2S to sulfur is 1:3-5; the molar volume ratio of (NH4)2S to the solvent is 0.1-5:1 mol / L.
Citation Information
Patent Citations
Electrolyte for lithium sulfur battery, and preparation method thereof
CN104810546A
Preparation method of high-concentration polysulfide solution and application of high-concentration polysulfide solution in flow battery
CN116207317A
Alkali PolySulphide Flow Battery
US20210242519A1