A self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst, its synthesis method and application

By using a self-supporting nitrogen-doped carbon-coated Fe-Ni2P/Ni5P4 electrocatalyst, the problems of high cost of precious metal catalysts and insufficient activity of transition metal phosphides were solved, achieving high-efficiency electrocatalytic performance for hydrogen production from water electrolysis, especially exhibiting excellent electrocatalytic activity and stability under alkaline conditions.

CN116855979BActive Publication Date: 2026-11-17XUZHOU NORMAL UNIVERSITY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310352810.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-04
Publication Date
2026-11-17
Estimated Expiration
2043-04-04

AI Technical Summary

Technical Problem

Existing precious metal catalysts are expensive and rare, and transition metal phosphides have insufficient electrocatalytic activity, which limits the efficient application of hydrogen production through water electrolysis, especially under alkaline conditions where the reaction kinetics are slow and the overpotential is high.

Method used

A self-supporting nitrogen-doped carbon-coated Fe-Ni2P/Ni5P4 electrocatalyst was developed by synthesizing a nanosheet array structure on a nickel foam substrate and combining it with the Fe-Ni2P/Ni5P4 heterostructure to improve electrocatalytic activity and stability.

Benefits of technology

Under alkaline conditions, highly efficient electrocatalytic hydrogen evolution, oxygen evolution, and complete water splitting performance were achieved, improving reaction kinetics and enhancing catalyst stability and the number of active sites.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116855979B_ABST
    Figure CN116855979B_ABST
Patent Text Reader

Abstract

This invention discloses a self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst, its synthesis method, and its application. Ferric nitrate nonahydrate, nickel acetate, 2,6-naphthalenedicarboxylic acid, and 1,2-benzisothiazol-3-one are uniformly dissolved in a reactor containing nickel foam and heated for a period of time. After the reaction, the nickel foam is removed, washed, and dried to obtain a NiFe-MOF precursor with a nanosheet array structure. The synthesized NiFe-MOF precursor is then calcined and phosphated under vacuum. By selecting appropriate heating rates, calcination temperatures, and calcination times, the self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4@N-C electrocatalyst is obtained. The prepared Fe-Ni2P / Ni5P4@N-C electrocatalyst exhibits higher electrocatalytic performance than Ni2P / Ni5P4@N-C and pure nickel foam.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst, its synthesis method, and its application, belonging to the field of nanomaterials. Background Technology

[0002] Energy crisis and environmental pollution are among the most serious problems facing humanity. Hydrogen energy, with its advantages of being clean, environmentally friendly, having high conversion efficiency, and high energy density, is hailed as the "ultimate energy source" in the field of clean energy. Water electrolysis is a green and sustainable energy conversion technology and a major pathway to obtaining hydrogen energy.

[0003] Electrolysis of water mainly involves two half-reactions: the hydrogen evolution reaction (HER) at the cathode and the oxygen evolution reaction (OER) at the anode. Under alkaline conditions, the reaction kinetics of these two half-reactions are slow, resulting in high overpotentials. Therefore, a very high external voltage is required to drive the electrolysis reaction, increasing energy consumption.

[0004] Therefore, finding efficient electrocatalysts to reduce overpotential and improve the reaction kinetics of both half-reactions is a key research focus for realizing the large-scale application of hydrogen production through water electrolysis. Although noble metal catalysts such as Pt and IrO2 have high electrocatalytic activity, their high price and scarce reserves have hindered their large-scale application.

[0005] Nickel, a transition metal, is abundant in the Earth's crust. Its phosphides offer advantages such as low cost, abundant reserves, and good electrocatalytic activity, making them a promising alternative to noble metal-based electrocatalysts for large-scale water electrolysis to produce hydrogen. However, factors such as the limited number of active sites, poor conductivity, and poor stability still affect the electrocatalytic activity of nickel-based phosphides, thus limiting their practical application. Summary of the Invention

[0006] The technical problem to be solved by this invention is to provide a self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst, its synthesis method, and its application, which can obtain a nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 self-supporting electrode with highly efficient electrocatalytic water splitting performance. This invention uses nickel foam as a substrate to synthesize a self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 catalyst with a nanosheet array structure to improve electrocatalytic activity and stability.

[0007] To solve the above-mentioned technical problems, the technical solution of the present invention is as follows: a method for synthesizing a self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst, the innovation of which is that the method for synthesizing the self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst includes the following steps:

[0008] Step S1: Synthesis of self-supporting NiFe-MOF precursors

[0009] Ferric nitrate nonahydrate and nickel nitrate in a weight ratio of 7-9:1-3 were dissolved in deionized water to obtain a clear solution. The solution was then transferred to a reaction vessel containing nickel foam. Next, 2,6-naphthalenedicarboxylic acid and 1,2-benzisothiazol-3-one in a weight ratio of 3-4:1-2 were dissolved in anhydrous ethanol. After standing, the mixture was transferred to the reaction vessel to form a reaction mixture. The nickel foam in the reaction mixture was then heated. After heating, the nickel foam was removed, washed, and dried to obtain a self-supporting NiFe-MOF precursor with a nanosheet array structure.

[0010] Step S2: Preparation of Fe-Ni2P / Ni5P4@NC self-supporting electrocatalyst

[0011] The self-supporting NiFe-MOF precursor obtained in step S1 was calcined and phosphated under vacuum to obtain Fe-Ni2P / Ni5P4@NC electrocatalyst.

[0012] Preferably, in step S1, the volume ratio of deionized water to anhydrous ethanol in the reaction mixture is 1:2.

[0013] Preferably, in step S1, ferric nitrate nonahydrate and nickel nitrate are dissolved in deionized water and subjected to ultrasonic treatment to obtain a clear solution; in step S1, 2,6-naphthalenedicarboxylic acid and 1,2-benzisothiazol-3-one are dissolved in anhydrous ethanol, subjected to ultrasonic treatment, and then allowed to stand.

[0014] Preferably, the weight ratio of the nonahydrated ferric nitrate, nickel nitrate, and deionized water is 7-9:1-3:1400-1600.

[0015] Preferably, the weight ratio of 2,6-naphthalenedicarboxylic acid, 1,2-benzisothiazol-3-one, and anhydrous ethanol is 3-4:1-2:700-800.

[0016] Preferably, the nickel foam is a blocky solid.

[0017] Preferably, the heating treatment in step S1 is to heat the nickel foam to 80°C in a high-temperature and high-pressure reactor for 20 hours.

[0018] Preferably, the calcination phosphating in step S2 is performed by calcining at 400°C for 2 hours under vacuum conditions at a heating rate of 5°C / min, followed by cooling to room temperature.

[0019] Sodium hypophosphite is added during the calcination phosphating process, and the weight of sodium hypophosphite is 1g per batch.

[0020] A self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst is prepared by a synthesis method for a self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst.

[0021] An application of a self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst, wherein the self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst is used in electrocatalytic water splitting.

[0022] The advantages of this invention are:

[0023] This invention discloses a simple method for preparing self-supporting nitrogen-doped carbon-encapsulated Fe-Ni2P / Ni5P4@NC electrocatalysts. The method synthesizes a self-supporting nanoarray Fe-Ni2P / Ni5P4 heterostructure coated with a nitrogen-doped carbon layer. The Fe-Ni2P / Ni5P4@NC catalyst exhibits excellent electrocatalytic hydrogen evolution, oxygen evolution, and total water splitting performance under alkaline conditions. The synergistic effect of Fe doping and the Ni2P / Ni5P4 heterostructure alters the electronic configuration environment, reduces the binding energy of reaction intermediates, and ultimately enhances the intrinsic activity of the Fe-Ni2P / Ni5P4@NC catalyst. The high specific surface area of ​​the self-supporting nanosheet array structure accelerates mass transfer while providing abundant active sites. Furthermore, the highly conductive nitrogen-doped carbon layer simultaneously accelerates reaction kinetics and improves the stability of the reaction structure. Attached Figure Description

[0024] The present invention will now be described in further detail with reference to the accompanying drawings and specific embodiments.

[0025] Figure 1 These are scanning electron microscope (SEM) images of the self-supporting NiFe-MOF precursor synthesized in the embodiments of the present invention, wherein (a) is a low-magnification SEM image of the self-supporting NiFe-MOF precursor; and (b) is a high-magnification SEM image of the self-supporting NiFe-MOF precursor.

[0026] Figure 2 These are scanning electron microscope (SEM) images of the self-supporting Fe-Ni2P / Ni5P4@NC synthesized in the embodiments of the present invention, wherein (a) is a low-magnification SEM image of the self-supporting Fe-Ni2P / Ni5P4@NC; and (b) is a high-magnification SEM image of the self-supporting Fe-Ni2P / Ni5P4@NC.

[0027] Figure 3 This is the X-ray powder diffraction pattern of the self-supporting Fe-Ni2P / Ni5P4@NC synthesized in the embodiments of the present invention;

[0028] Figure 4 These are (a) a high-resolution transmission electron microscope image and (b) a lattice fringe pattern of the self-supporting Fe-Ni2P / Ni5P4@NC synthesized in the embodiments of the present invention;

[0029] Figure 5 The following are the hydrogen evolution performance graphs of Fe-Ni2P / Ni5P4@NC, Ni2P / Ni5P4@NC and nickel foam (NF) under 1 mol / L KOH conditions: (a) overpotential comparison graph; (b) Tafel slope comparison graph; (c) LSV curve comparison graph of Fe-Ni2P / Ni5P4@NC before and after 1000 cycles of CV and its (d) chronopotential curve graph;

[0030] Figure 6 The following are the oxygen evolution performance graphs of Fe-Ni2P / Ni5P4@NC, Ni2P / Ni5P4@NC and NF under 1mol / L KOH conditions: (a) overpotential comparison graph; (b) Tafel slope comparison graph; (c) LSV curve comparison graph of Fe-Ni2P / Ni5P4@NC before and after 1000 cycles of CV and (d) chronopotential curve graph;

[0031] Figure 7 The following are the water-splitting performance diagrams of Fe-Ni2P / Ni5P4@NC, Ni2P / Ni5P4@NC and NF under 1mol / L KOH conditions: (a) Comparison of water-splitting performance; (b) Chronopotential diagram of Fe-Ni2P / Ni5P4@NC. Detailed Implementation

[0032] The synthesis method of the self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst of the present invention includes the following steps:

[0033] Step S1: Synthesis of self-supporting NiFe-MOF precursors

[0034] Ferric nitrate nonahydrate and nickel nitrate in a weight ratio of 7-9:1-3 were dissolved in deionized water to obtain a clear solution. The solution was then transferred to a reaction vessel containing nickel foam. Next, 2,6-naphthalenedicarboxylic acid and 1,2-benzisothiazol-3-one in a weight ratio of 3-4:1-2 were dissolved in anhydrous ethanol. After standing, the mixture was transferred to the reaction vessel to form a reaction mixture. The nickel foam in the reaction mixture was then heated. After heating, the nickel foam was removed, washed, and dried to obtain a self-supporting NiFe-MOF precursor with a nanosheet array structure.

[0035] Step S2: Preparation of Fe-Ni2P / Ni5P4@NC self-supporting electrocatalyst

[0036] The self-supporting NiFe-MOF precursor obtained in step S1 was calcined and phosphated under vacuum to obtain Fe-Ni2P / Ni5P4@NC electrocatalyst.

[0037] In step S1, the nickel foam is a blocky solid. The volume ratio of deionized water to anhydrous ethanol in the reaction mixture is 1:2. In step S1, ferric nitrate nonahydrate and nickel nitrate are dissolved in deionized water and ultrasonically treated to obtain a clear solution. In step S1, 2,6-naphthalenedicarboxylic acid and 1,2-benzisothiazol-3-one are dissolved in anhydrous ethanol, ultrasonically treated, and then allowed to stand.

[0038] To control the appropriate proportions, the weight ratio of ferric nitrate nonahydrate, nickel nitrate, and deionized water is 7-9:1-3:1400-1600. The weight ratio of 2,6-naphthalenedicarboxylic acid, 1,2-benzisothiazol-3-one, and anhydrous ethanol is 3-4:1-2:700-800.

[0039] The heating treatment in step S1 involves heating the nickel foam to 80°C in a high-temperature, high-pressure reactor for 20 hours. The calcination phosphating in step S2 involves calcining the nickel foam at 400°C for 2 hours under vacuum conditions with a heating rate of 5°C / min, followed by cooling to room temperature.

[0040] Sodium hypophosphite is added during the calcination phosphating process, and the weight of sodium hypophosphite is 1g per batch.

[0041] A self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst is prepared by a synthesis method for a self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst.

[0042] An application of a self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst: The self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst is used in the electrocatalytic total water splitting process.

[0043] Example 1

[0044] A method for preparing a self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst includes the following steps:

[0045] S1: Synthesis of self-supporting NiFe-MOF precursors;

[0046] 0.009 g of ferric nitrate nonahydrate and 0.002 g of nickel nitrate were dissolved in 1.5 mL of deionized water, and the solution was sonicated to obtain a clear solution. This solution was then transferred to a reaction vessel. Next, 0.015 g of 2,6-naphthalenedicarboxylic acid and 0.006 g of 1,2-benzisothiazol-3-one were uniformly dissolved in 3 mL of anhydrous ethanol. After sonication for 10-15 min, the solution was transferred to a reaction vessel containing 2.5 cm × 1 cm × 0.5 mm nickel foam and heated to 80 °C for 20 h. After the reaction, the nickel foam was removed, washed three times with deionized water, and dried to obtain the self-supporting NiFe-MOF precursor with a nanosheet array structure.

[0047] Low-magnification and high-magnification scanning electron microscope images of the self-supporting NiFe-MOF precursor synthesized in this embodiment are shown below. Figure 1 As shown. From Figure 1 As can be seen from the above, the NiFe-MOF nanosheet array structure synthesized in this embodiment is uniformly grown on nickel foam.

[0048] S2: Synthesis of Fe-Ni2P / Ni5P4@NC self-supporting electrocatalyst with nanosheet array structure;

[0049] A piece of nickel foam with dimensions of 2.5cm×1cm×0.5mm and loaded with NiFe-MOF precursor was placed in a tube furnace, 1g of sodium hypophosphite was added, and the furnace was calcined at 400℃ for 2h under vacuum conditions with a heating rate of 5℃ / min. After cooling to room temperature, Fe-Ni2P / Ni5P4@NC electrocatalyst was obtained.

[0050] The scanning electron microscope image of the Fe-Ni2P / Ni5P4@NC synthesized in this embodiment is shown below. Figure 2 As shown, from Figure 2 As can be seen in (b), the surface of the Fe-Ni2P / Ni5P4@NC nanosheets is wrinkled, but the nanosheet array structure is still well maintained.

[0051] The X-ray powder diffraction pattern of the Fe-Ni2P / Ni5P4@NC synthesized in this embodiment is shown below. Figure 3 As shown, the diffraction peak positions of the synthesized Fe-Ni2P / Ni5P4@NC perfectly match the standard cards for Ni, Ni2P, and Ni5P4, proving that the Fe-Ni2P / Ni5P4@NC material was successfully synthesized in this embodiment.

[0052] The transmission electron microscope (TEM) image of the Fe-Ni2P / Ni5P4@NC synthesized in this embodiment is shown below. Figure 4 As shown.

[0053] The testing methods for electrocatalytic hydrogen evolution and oxygen evolution performance are as follows:

[0054] An electrochemical workstation was used with a three-electrode system to test the electrocatalytic hydrogen evolution and oxygen evolution performance of the electrodes in an alkaline electrolyte. The test electrolyte was 1M potassium hydroxide; the prepared electrode was the working electrode; the carbon rod was the counter electrode; and the mercuric oxide electrode was the reference electrode. The test conditions were 2 mV / s. -1 Linear voltammetric scans were performed. Before electrochemical testing, all scans were performed at 50 mV / s. -1 Perform more than 10 CV or LSV scans until the curve stabilizes to ensure that the electrode and electrolyte are in full contact.

[0055] Figure 5 and Figure 6 The figures show a comparison of the HER and OER performance of Fe-Ni2P / Ni5P4@NC, Ni2P / Ni5P4@NC, and NF in a 1 mol / L KOH electrolyte. The stability test results for Fe-Ni2P / Ni5P4@NC synthesized in this embodiment are shown below. Figure 5 (c,d) and Figure 6 As shown in (c,d), by Figure 5 (c) and Figure 6 (c) shows that its hydrogen evolution and oxygen evolution performance decreases very little before and after the stability test; Figure 5 (d) and Figure 6 As shown in (d), it can achieve a current of 100 mA cm over 60 hours. -2 It operates with a stable current density.

[0056] The test method for electrocatalytic water splitting performance is as follows:

[0057] An electrochemical workstation was used, employing a two-electrode system. The working electrodes for both the anode and cathode were prepared in this embodiment. The electrolyte was a 1M potassium hydroxide solution, and the mercury oxide electrode served as the reference electrode.

[0058] Figure 7 This is a comparison of the total water splitting performance of Fe-Ni2P / Ni5P4@NC, Ni2P / Ni5P4@NC, and NF in a 1 mol / L KOH electrolyte. The figure shows that the Fe-Ni2P / Ni5P4@NC electrode synthesized in this embodiment simultaneously serves as both cathode and anode in the total water splitting reaction at a current density of 10 mA cm⁻¹. -2 At that time, the voltage was 1.56V, and at 100mA cm -2 It can operate stably for 100 hours at current density.

[0059] Example 2:

[0060] 0.002 g of nickel nitrate was dissolved in 1.5 mL of deionized water and sonicated to obtain a clear solution. This solution was then transferred to a reaction vessel. Next, 0.015 g of 2,6-naphthalenedicarboxylic acid and 0.006 g of 1,2-benzisothiazol-3-one were uniformly dissolved in 3 mL of anhydrous ethanol. After sonication for 10-15 min, the solution was transferred to a reaction vessel containing 2.5 cm × 1 cm × 0.5 mm nickel foam and heated to 80 °C for 20 h. After the reaction, the nickel foam was removed, washed three times with deionized water, and dried to obtain the self-supporting Ni-MOF precursor with a nanosheet array structure.

[0061] A piece of nickel foam with dimensions of 2.5cm×1cm×0.5mm and loaded with Ni-MOF precursor was placed in a tube furnace, 1g of sodium hypophosphite was added, and the furnace was calcined at 400℃ for 2h under vacuum conditions with a heating rate of 5℃ / min. After cooling to room temperature, Ni2P / Ni5P4@NC electrocatalyst was obtained.

[0062] The electrocatalytic hydrogen evolution, oxygen evolution, and total water splitting performance of the Ni2P / Ni5P4@NC electrocatalyst prepared in this example under alkaline conditions were tested using the test methods described in Examples 1 and 2.

[0063] As can be seen, the Fe-Ni2P / Ni5P4@NC electrode of this invention can serve as a highly efficient self-supported electrode for electrocatalytic water splitting, exhibiting excellent water splitting activity and stability under alkaline conditions. This patent provides a new approach for preparing self-supported nanosheet array electrodes for electrocatalytic water splitting, while also promoting the application of nickel-based catalysts in the field of energy conversion. The preparation process of this invention is simple, with low reaction temperature, mild reaction conditions, convenient operation, and low cost, making it suitable for industrial production.

[0064] Any numerical values ​​cited herein include all values ​​ranging from a lower limit to an upper limit, increasing by one unit, with at least two units between any lower and any higher value. For example, if the quantity of a component or the value of a process variable (e.g., temperature, pressure, time, etc.) is described as being from 1 to 90, preferably from 20 to 80, more preferably from 30 to 70, the purpose is to illustrate that values ​​such as 15 to 85, 22 to 68, 43 to 51, 30 to 32 are also explicitly listed in this specification. For values ​​less than 1, a unit is appropriately considered to be 0.0001, 0.001, 0.01, 0.1, etc. These are merely examples intended for explicit expression, and it can be assumed that all possible combinations of values ​​listed between the minimum and maximum values ​​are similarly explicitly stated in this specification.

[0065] Unless otherwise stated, all ranges include the endpoints and all numbers between them. The terms "approximately" or "about" used with ranges apply to both endpoints of the range. Thus, "approximately 20 to 30" is intended to cover "approximately 20 to approximately 30," including at least the specified endpoints.

[0066] All articles and references disclosed herein, including patent applications and publications, are incorporated herein by reference for various purposes. The term “substantially constitutes…” used to describe a combination should include the identified elements, components, parts, or steps, as well as other elements, components, parts, or steps that do not substantially affect the essential novelty of the combination. The use of the terms “comprising” or “including” to describe combinations of elements, components, parts, or steps herein also contemplates embodiments substantially constituted by such elements, components, parts, or steps. The use of the term “may” herein is intended to indicate that any described attribute included by “may” is optional.

[0067] Multiple elements, components, parts, or steps can be provided by a single integrated element, component, part, or step. Alternatively, a single integrated element, component, part, or step can be divided into multiple separate elements, components, parts, or steps. The use of "a" or "an" to describe an element, component, part, or step does not imply the exclusion of other elements, components, parts, or steps.

[0068] It should be understood that the above description is for illustrative purposes and not for limitation. Many embodiments and applications beyond the provided examples will be apparent to those skilled in the art upon reading the above description. Therefore, the scope of this teaching should not be determined by reference to the above description, but rather by reference to the appended claims and the full scope of their equivalents. For purposes of completeness, all articles and references, including patent applications and publications, are incorporated herein by reference. The omission of any aspect of the subject matter disclosed herein in the preceding claims is not intended as a waiver of that subject matter, nor should it be construed as an indication that the inventors have not considered that subject matter as part of the disclosed inventive subject matter.

Claims

1. A method for synthesizing a self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst, characterized in that: The synthesis method of the self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst includes the following steps: Step S1: Synthesis of self-supporting NiFe-MOF precursors Ferric nitrate nonahydrate and nickel nitrate in a weight ratio of 7-9:1-3 were dissolved in deionized water to obtain a clear solution. The solution was then transferred to a reaction vessel containing nickel foam. Next, 2,6-naphthalenedicarboxylic acid and 1,2-benzisothiazol-3-one in a weight ratio of 3-4:1-2 were dissolved in anhydrous ethanol. After standing, the mixture was transferred to the reaction vessel to form a reaction mixture. The nickel foam in the reaction mixture was then heated. After heating, the nickel foam was removed, washed, and dried to obtain a self-supporting NiFe-MOF precursor with a nanosheet array structure. Step S2: Preparation of Fe-Ni2P / Ni5P4@NC self-supporting electrocatalyst The self-supporting NiFe-MOF precursor obtained in step S1 was calcined and phosphated under vacuum to obtain Fe-Ni2P / Ni5P4@NC electrocatalyst.

2. The method for synthesizing a self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst as described in claim 1, characterized in that: In step S1, the volume ratio of deionized water to anhydrous ethanol in the reaction mixture is 1:

2.

3. The method for synthesizing a self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst as described in claim 1, characterized in that: In step S1, ferric nitrate nonahydrate and nickel nitrate are dissolved in deionized water and ultrasonically treated to obtain a clear solution; in step S1, 2,6-naphthiazol-3-one are dissolved in anhydrous ethanol and ultrasonically treated before being allowed to stand.

4. The method for synthesizing a self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst as described in claim 1, characterized in that: The weight ratio of the nonahydrated ferric nitrate, nickel nitrate, and deionized water is 7-9:1-3:1400-1600.

5. The method for synthesizing a self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst as described in claim 1, characterized in that: The weight ratio of 2,6-naphthalenedicarboxylic acid, 1,2-benzisothiazol-3-one, and anhydrous ethanol is 3-4:1-2:700-800.

6. The method for synthesizing a self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst as described in claim 1, characterized in that: The nickel foam is a blocky solid.

7. The method for synthesizing a self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst as described in claim 1, characterized in that: The heating treatment in step S1 involves heating the nickel foam to 80°C in a high-temperature and high-pressure reactor for 20 hours.

8. The method for synthesizing a self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst as described in claim 1, characterized in that: In step S2, the calcination phosphating is carried out by calcining at a temperature of 400°C for 2 hours under vacuum conditions with a heating rate of 5°C / min, followed by cooling to room temperature. Sodium hypophosphite is added during the calcination phosphating process, and the weight of sodium hypophosphite is 1g per batch.

9. A self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst, characterized in that: A self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst was prepared by using the synthesis method of any one of claims 1 to 8.

10. The application of a self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst, characterized in that: The self-supporting nitrogen-doped carbon-coated Fe-Ni2P / Ni5P4 electrocatalyst as described in claim 9 is applied in the electrocatalytic total water splitting.

Citation Information

Patent Citations

  • Micron nickel phosphide electro-catalytic material used for hydrogen evolution / oxygen evolution double functions

    CN105854911A

  • Iron-doped bimetal phosphide electrocatalyst and preparation method and application thereof

    CN109174162A