positive electrode
By using active materials containing Li, Ni, Mn, Co, and A in the positive electrode in combination with polyether polymers and polysiloxane compounds, the capacity leakage problem of PEO-based electrolytes was solved, thus improving the performance of lithium-ion batteries.
Patent Information
- Application Number
- CN202180086812.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-12-24
- Filing Date
- 2021-12-23
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2041-12-23
AI Technical Summary
Existing PEO-based solid electrolyte positive electrodes suffer from capacity leakage, causing electron current to leak from the anode to the cathode, affecting battery performance.
The positive electrode active material contains Li, Ni, Mn, Co and A, where A is Al or other elements. It is combined with polyether polymer and polysiloxane compound to form polymer electrolyte through a specific reaction, thereby reducing capacity leakage.
It significantly reduces capacity leakage and improves the performance of lithium-ion batteries, especially showing improved battery performance in solid-state lithium-ion batteries.
Smart Images

Figure CN116868397B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a positive electrode for a lithium-ion secondary battery, the positive electrode comprising a positive electrode active material and at least one polymer electrolyte. Background Technology
[0002] Polymer electrolytes are an interesting alternative to liquid electrolytes in batteries. In this context, polyethylene oxide (PEO)-based electrolytes have been extensively studied in the literature.
[0003] For example, Ruoyuan Tao et al. disclosed a positive electrode in J. Appl. Electrochem. 35, 163-168 (2005) comprising poly(ethylene oxide) and lithium bis(trifluoromethanesulfonyl)imide (Li(N(SO2CF3)2), also known as LiTFSI). PEO and LiTFSI were dissolved in acetonitrile to prepare an electrolyte solution. The positive electrode active material was then added to the electrolyte solution.
[0004] US 7,585,934 B2 discloses the use of EO / PO / AGE and lithium bis(trifluoromethanesulfonyl)imide (LiTFSI, Li(N(SO2CF3)2)) as solid polymer electrolyte membranes. The document discloses a copolymerization procedure for EO, PO, and AGE in working examples. Specifically, LiTFSI is added in the form of a Li salt to a polyether polymer composition comprising the EO / PO / AGE copolymer in an amount such that the ratio of (moles of lithium atoms in the electrolyte salt) to (moles of oxygen atoms in the polyether polymer) is 0.05.
[0005] Despite recent progress in this field, capacity leakage remains a problem for positive electrodes containing PEO-based solid electrolytes. Capacity leakage is a phenomenon in which the electrolyte acquires electronic conductivity, causing an electronic current to leak from the anode to the cathode.
[0006] Therefore, there is a need for improved positive electrodes, especially positive electrodes with reduced capacity leakage when used in batteries. Summary of the Invention
[0007] The inventors have surprisingly discovered that an improved positive electrode can be provided to meet the above-mentioned needs.
[0008] Therefore, the main objective of this invention is a positive electrode for a lithium-ion secondary battery, comprising a positive electrode active material and at least one polymer electrolyte, wherein the positive electrode active material comprises at least Li, M' and oxygen, wherein M' is composed of Ni, Mn, Co and A, and the positive electrode material has a Ni:(Mn+Co+A) molar ratio (or atomic ratio) of (1-xyz):(x+y+z) as measured by ICP, wherein 0.00≤x≤0.70, 0.00≤y≤0.40 and 0.00≤z≤0.10, wherein when A is present, A is different from Ni, Mn, Co and Li, and is preferably Al or at least one of the following: B, Mg, Al, Nb, Ti, Y, W, S, Ba, Sr and Zr, and the polymer electrolyte is obtained by a reaction between the following substances: i. At least one polyether polymer [polymer (P) hereinafter], said polymer (P) comprising: a) At least 70.0 mol% of oxyethylidene units (EO); b) 0.0 mol% to 10.0 mol% of oxypropylene units (PO); and c) 1.00 mol% to 4.0 mol% of repeating units derived from at least one monomer of formula (I) or formula (II) [monomer (M) hereinafter]:
[0009] Formula (I)
[0010] or
[0011] Equation (II)
[0012] in
[0013] - Each of R1 and R2 may be the same as or different from each other and is a C1-6 alkyldiyl in each occurrence, wherein the C1-6 alkyldiyl is optionally substituted by one or more substituents selected from halide ions, C1-4 alkyl, C3-6 cycloalkyl, CF3, OR8, and wherein each R8 is the same as or different from each other and is independently selected from hydrogen and C1-4 alkyl in each occurrence; n is an integer of 0, 1, or 2; - Each X is a leaving group selected from halide ions, trifluoromethanesulfonate, nonafluorobutanesulfonate, p-toluenesulfonate and methanesulfonate; and ii. At least one polysiloxane compound having formula (III):
[0014] Equation (III)
[0015] in
[0016] - Each of R3, R4, R5, R6, and R7 may be the same as or different from each other and, each time it appears, is independently selected from C1-6 alkyl, C3-6 cycloalkyl, aryl, C1-6 alkoxy, and heterocyclic groups, wherein the C1-6 alkyl, C3-6 cycloalkyl, aryl, C1-6 alkoxy, and heterocyclic groups are optionally substituted by one or more substituents selected from halide ions, C1-4 alkyl, C3-6 cycloalkyl, CF3, and OR9, and wherein each R9 may be the same as or different from each other and, each time it appears, is independently selected from hydrogen, C1-4 alkyl, and a hydroxyl protecting group. - m is an integer of at least 3; and The at least one polysiloxane compound having formula (III) is grafted onto the at least one polymer (P) by reacting at least a portion of the -CH=CH2 portion of the monomer (M) with the H-Si portion of the polysiloxane compound having formula (III).
[0017] A second object of the present invention relates to a positive electrode for a lithium-ion secondary battery, the positive electrode comprising a positive electrode active material and at least one polymer electrolyte, said positive electrode active material comprising at least an element selected from Li, M' and oxygen, wherein the metal M' has the following formula: Ni 1-x-y-z Mn x Co y A z Where 0.00≤x≤0.70, 0.00≤y≤0.40 and 0.00≤z≤0.10, as measured by ICP, wherein when A is present, A is different from Ni, Mn, Co and Li, and preferably at least one of the following: B, Mg, Al, Nb, Ti, Y, W, S, Ba, Sr and Zr, and the polymer electrolyte is obtained by a reaction between the following substances: i. At least one polyether polymer [polymer (P) hereinafter], said polymer (P) comprising: a) At least 70.0 mol% of oxyethylidene units (EO); b) 0.0 mol% to 10.0 mol% of oxypropylene units (PO); and c) 1.00 mol% to 4.0 mol% of repeating units derived from at least one monomer of formula (I) or formula (II) [monomer (M) hereinafter]: Formula (I) or Equation (II) in - Each of R1 and R2 is either the same as or different from each other and is C each time it appears. 1-6 Alkyl, wherein the C 1-6 Alkyl groups are optionally selected from halide ions, C 1-4 Alkyl, C 3-6 One or more substituents of cycloalkyl, CF3, and OR8 are used, wherein each R8 is the same as or different from each other and is independently selected from hydrogen and C each time it appears. 1-4 Alkyl; n is an integer, either 0, 1, or 2; - Each X is a leaving group selected from halide ions, trifluoromethanesulfonate, nonafluorobutanesulfonate, p-toluenesulfonate and methanesulfonate; as well as ii. At least one polysiloxane compound having formula (III): Equation (III) in - Each of R3, R4, R5, R6, and R7 is either the same as or different from each other, and is independently selected from C each time it appears. 1-6 Alkyl, C 3-6 cycloalkyl, aryl, C 1-6 alkoxy, heterocyclic group, wherein the C 1-6 Alkyl, C 3-6 cycloalkyl, aryl, C 1-6 The alkoxy group and heterocyclic group are optionally selected from halide ions, C 1-4 Alkyl, C 3-6 One or more substituents of cycloalkyl, CF3, and OR9 are used, wherein each R9 is the same as or different from each other and is independently selected from hydrogen, C, and D in each occurrence. 1-4 Alkyl and hydroxyl protecting groups, - m is an integer of at least 3; and The at least one polysiloxane compound having formula (III) is grafted onto the at least one polymer (P) by reacting at least a portion of the -CH=CH2 portion of the monomer (M) with the H-Si portion of the polysiloxane compound having formula (III).
[0018] Another object of the present invention is to provide a polymer battery including the positive electrode.
[0019] Another object of the present invention is to provide an electrochemical single cell including the positive electrode.
[0020] Another object of the present invention is to provide the use of the positive electrode in a battery. Attached Figure Description
[0021] Figure 1GPC elution profiles of a polymer electrolyte, polymer (P), and polysiloxane prepared according to one embodiment are shown. Figure 2 The polymer electrolyte according to the embodiment is shown to be a Q 总 The impact of the value. Detailed Implementation
[0022] positive electrode
[0023] As used herein and in the claims, the term "comprising" should not be construed as limited to the manner listed thereafter; it does not exclude other elements or steps. It should be interpreted as specifying the presence of the mentioned feature, integer, step, or component, but does not exclude the presence or addition of one or more other features, integers, steps, or components or groups thereof. Therefore, the scope of the expression "a composition comprising component A and component B" should not be limited to compositions consisting solely of components A and B. This means that, with respect to the present invention, the only relevant components of the composition are A and B. Therefore, the terms "comprising" and "including" encompass the more restrictive terms "consistently composed of" and "composed of".
[0024] As used herein, the terms “optional” or “optionally” mean that an event or situation described below may or may not occur, and the description includes instances where said event or situation occurs and instances where said event or situation does not occur.
[0025] The term "positive electrode active material" is intended to refer to a material that is electrochemically active in a positive electrode. This active material is capable of capturing and releasing Li ions when subjected to voltage changes over a predetermined time period.
[0026] The inventors have surprisingly discovered that when the positive electrode according to the invention is used in a battery, particularly in a solid-state lithium-ion battery, capacity leakage is reduced, resulting in improved battery performance, as demonstrated in the working examples.
[0027] In the context of this invention, the term "positive electrode active material" is defined as a material that is electrochemically active in a positive electrode. This active material is capable of capturing and releasing Li ions when subjected to voltage changes over a predetermined time period.
[0028] In the context of this invention, the expression "at least one polyether polymer [polymer (P) hereinafter]" is intended to represent one or more polymers (P). Similarly, the expressions "at least one polysiloxane compound having formula (III)" and "at least one polymer electrolyte" are intended to represent one or more polysiloxane compounds having formula (III) and correspondingly one or more polymer electrolytes.
[0029] In the remainder of this document, for the purposes of this invention, the expressions “polymer (P)”, “polymer electrolyte” and “polysiloxane compound having formula (III)” should be understood as both plural and singular.
[0030] As used herein, the term "alkyl" has the broadest meaning as commonly understood in the art and may include portions that are straight-chain or branched or combinations thereof.
[0031] The term "alkyl," alone or in combination, refers to a group derived from straight-chain or branched alkane, such as C1. F-G Alkyl groups are defined as straight-chain or branched alkyl groups having F to G carbon atoms, such as C 1-4 Alkyl is defined as a straight-chain or branched alkyl group having 1 to 4 carbon atoms, such as methyl, ethyl, 1-propyl, 2-propyl (isopropyl), 1-butyl, 2-butyl, 2-methyl-2-propyl (tert-butyl), and 2-methyl-1-propyl (isobutyl).
[0032] The term "cycloalkyl," alone or in combination, refers to a group derived from cyclic alkane, such as C L-M Cycloalkyl is defined as a cyclic alkyl group having L to M carbon atoms, such as C 3-6 Cycloalkyl is defined as a cyclic alkyl group having 3 to 6 carbon atoms, such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, etc.
[0033] The term "aryl," alone or in combination, refers to a phenyl, naphthyl, or anthracene group, optionally fused with a cycloalkyl or heterocyclic carbocyclic ring having preferably 5-7, more preferably 5-6 ring members, and / or optionally substituted with 1 to 5 groups or substituents. The aryl group may be optionally substituted, whereby the substituent is connected to the aryl group at one point, or whereby the substituent is connected to the aryl group at two points to form a bicyclic system, such as benzodioxane, benzodioxane, or benzimidazole.
[0034] The term "heterocyclic group," alone or in combination, refers to a cyclic alkane-derived group in which at least one carbon atom is independently substituted by a heteroatom selected from oxygen, nitrogen, and sulfur, such as pyrrolidine, piperidine, or morpholine.
[0035] The term "alkoxy group," alone or in combination, refers to a group derived from straight-chain or branched alkane compounds, wherein the carbon atom carrying the group is replaced by an oxygen atom. The alkoxy moiety has a -0-R... x Structure, where R x It is an alkyl group.
[0036] The term "alkyldiyl" refers, alone or in combination, to a divalent group derived from a straight-chain or branched alkyl group.
[0037] A first aspect of the present invention provides a positive electrode for a lithium-ion secondary battery, the positive electrode comprising a positive electrode active material and at least one polymer electrolyte, said positive electrode active material comprising Ni, Mn, Co and A, said positive electrode material having a Ni:(Mn+Co+A) molar ratio of (1-xyz):(x+y+z) as measured by ICP, wherein 0.00≤x≤0.70, 0.00≤y≤0.40 and 0.00≤z≤0.10, wherein when A is present, A is different from Ni, Mn, Co and Li, and preferably is Al or at least one of the following: B, Mg, Al, Nb, Ti, Y, W, S, Ba, Sr and Zr, and said polymer electrolyte is obtained by a reaction between the following substances: i. At least one polyether polymer [polymer (P) hereinafter], said polymer (P) comprising: - At least 70.0 mol% of oxyethylidene units (EO); - 0.0 mol% to 10.0 mol% of oxypropylene units (PO); and - 1.00 mol% to 4.0 mol% of repeating units derived from at least one monomer of general formula (I) or general formula (II) [monomer (M) hereinafter]: Formula (I) or Equation (II) in - Each of R1 and R2 is either the same as or different from each other and is C each time it appears. 1-6 Alkyl, wherein the C 1-6 Alkyl groups are optionally selected from halide ions, C 1-4 Alkyl, C 3-6 One or more substituents of cycloalkyl, CF3, and OR8 are used, wherein each R8 is the same as or different from each other and is independently selected from hydrogen and C each time it appears. 1-4 Alkyl; n is an integer, either 0, 1, or 2; - Each X is a leaving group selected from halide ions, trifluoromethanesulfonate, nonafluorobutanesulfonate, p-toluenesulfonate and methanesulfonate; as well as ii. At least one polysiloxane compound having formula (III):
[0038] Equation (III)
[0039] in
[0040] - Each of R3, R4, R5, R6, and R7 is either the same as or different from each other, and is independently selected from C each time it appears. 1-6 Alkyl, C 3-6 cycloalkyl, aryl, C 1-6 alkoxy, heterocyclic group, wherein the C 1-6 Alkyl, C 3-6 cycloalkyl, aryl, C 1-6 The alkoxy group and heterocyclic group are optionally selected from halide ions, C 1-4 Alkyl, C 3-6 One or more substituents of cycloalkyl, CF3, and OR9 are used, wherein each R9 is the same as or different from each other and is independently selected from hydrogen, C, and D in each occurrence. 1-4 Alkyl and hydroxyl protecting groups, - m is an integer of at least 3; and The at least one polysiloxane compound having formula (III) is grafted onto the at least one polymer (P) by reacting at least a portion of the -CH=CH2 portion of the monomer (M) with the H-Si portion of the polysiloxane compound having formula (III).
[0041] Alternatively, one embodiment of the present invention provides a positive electrode for a lithium-ion secondary battery, the positive electrode comprising a positive electrode active material and at least one polymer electrolyte, said positive electrode active material comprising at least Li, M' and oxygen, wherein M' is composed of Ni, Mn, Co and A, said positive electrode material having a Ni:(Mn+Co+A) molar ratio as measured by ICP (1-xyz):(x+y+z), wherein 0.00≤x≤0.70, 0.00≤y≤0.40 and 0.00≤z≤0.10, wherein when A is present, A is different from Ni, Mn, Co and Li, and preferably is Al or at least one of the following: B, Mg, Al, Nb, Ti, Y, W, S, Ba, Sr and Zr, and said polymer electrolyte is obtained by a reaction between the following substances: i. At least one polyether polymer [polymer (P) hereinafter], said polymer (P) comprising: - At least 70.0 mol% of oxyethylidene units (EO); - 0.0 mol% to 10.0 mol% of oxypropylene units (PO); and - 1.00 mol% to 4.0 mol% of repeating units derived from at least one monomer of general formula (I) or general formula (II) [monomer (M) hereinafter]: Formula (I) or Equation (II) in - Each of R1 and R2 is either the same as or different from each other and is C each time it appears. 1-6 Alkyl, wherein the C 1-6 Alkyl groups are optionally selected from halide ions, C 1-4 Alkyl, C 3-6 One or more substituents of cycloalkyl, CF3, and OR8 are used, wherein each R8 is the same as or different from each other and is independently selected from hydrogen and C each time it appears. 1-4 Alkyl; n is an integer, either 0, 1, or 2; - Each X is a leaving group selected from halide ions, trifluoromethanesulfonate, nonafluorobutanesulfonate, p-toluenesulfonate and methanesulfonate; and ii. At least one polysiloxane compound having formula (III):
[0042] Equation (III)
[0043] in
[0044] - Each of R3, R4, R5, R6, and R7 is either the same as or different from each other, and is independently selected from C each time it appears. 1-6 Alkyl, C 3-6 cycloalkyl, aryl, C 1-6 alkoxy, heterocyclic group, wherein the C 1-6 Alkyl, C 3-6 cycloalkyl, aryl, C 1-6 The alkoxy group and heterocyclic group are optionally selected from halide ions, C 1-4 Alkyl, C 3-6 One or more substituents of cycloalkyl, CF3, and OR9 are used, wherein each R9 is the same as or different from each other and is independently selected from hydrogen, C, and D in each occurrence. 1-4 Alkyl and hydroxyl protecting groups, - m is an integer of at least 3; and The at least one polysiloxane compound having formula (III) is grafted onto the at least one polymer (P) by reacting at least a portion of the -CH=CH2 portion of the monomer (M) with the H-Si portion of the polysiloxane compound having formula (III).
[0045] As described above, the polymer (P) contains
[0046] a) At least 70.0 mol% of repeating units of oxyethylidene (EO); b) 0.0 mol% to 10.0 mol% of oxypropylene units (PO); and c) 1.00 mol% to 4.0 mol% of repeating units derived from at least one monomer of formula (I) or formula (II) [monomer (M) hereinafter]: Formula (I) or Equation (II) in - Each of R1 and R2 is either the same as or different from each other and is C each time it appears. 1-6 Alkyl, wherein the C 1-6 Alkyl groups are optionally selected from halide ions, C 1-4 Alkyl, C 3-6 One or more substituents of cycloalkyl, CF3, and OR8 are used, wherein each R8 is the same as or different from each other and is independently selected from hydrogen and C each time it appears. 1-4 Alkyl; n is an integer, either 0, 1, or 2; - Each of X is a leaving group selected from halide ions, trifluoromethanesulfonate, nonafluorobutanesulfonate, p-toluenesulfonate, and methanesulfonate.
[0047] Therefore, at least 70.0 mol%, preferably at least 80.0 mol%, preferably at least 85.0 mol%, preferably at least 90.0 mol%, more preferably at least 92.0 mol%, and more preferably at least 94.0 mol% of the repeating unit of the polymer (P) is an oxyethylene repeating unit (EO).
[0048] It should also be understood that at most 99.0 mol%, more preferably at most 98.5 mol%, and even more preferably at most 98.0 mol% of the repeating units of the polymer (P) are EO units.
[0049] In a preferred embodiment, the polymer (P) comprises at least 80.0 mol% and at most 99.0 mol%, preferably at least 90.0 mol% and at most 98.5 mol%, preferably at least 92.0 mol% and at most 98.5 mol% of EO units, and preferably at least 94.0 mol% and at most 98.5 mol% of EO units.
[0050] When an oxypropylene repeating unit (PO) is present in a polymer (P), at most 10.0 mol%, more preferably at most 6.0 mol%, even more preferably at most 5.0 mol%, even more preferably at most 4.0 mol%, even more preferably at most 3.0 mol% of the repeating unit of the polymer (P) is a PO unit.
[0051] Advantageously, the polymer (P) comprises at least 0.1 mol%, or at least 0.5 mol%, or at least 1.0 mol% of PO units.
[0052] In a preferred embodiment, the polymer (P) comprises at least 0.5 mol% and at most 6.0 mol%, or at least 0.5 mol% and at most 5.0 mol%, or at least 0.5 mol% and at most 4.0 mol%, or at least 1.0 mol% and at most 4.0 mol%, or at least 1.0 mol% and at most 3.0 mol% of PO units.
[0053] The presence of PO units reduces the crystallinity of the polymer (P), which improves its ionic conductivity.
[0054] For the purposes of this invention, the term "oxypropylidene (PO)" is intended to refer to the formula -O-CH2-CH2-CH2- or -O-CH2-CH(CH3)-, preferably –O-CH2-CH(CH3)-.
[0055] Preferably, at least 1.2 mol%, or at least 1.5 mol%, or at least 1.8 mol%, or at least 2.2 mol% of the repeating units of the polymer (P) are repeating units derived from monomers (M) of general formula (I) or general formula (II) as detailed above.
[0056] It should also be understood that at most 4.0 mol%, more preferably at most 3.5 mol%, and even more preferably at most 3.0 mol% of the repeating units of the polymer (P) are derived from repeating units of monomers (M) of general formula (I) or general formula (II) as detailed above.
[0057] In a preferred embodiment, the polymer (P) comprises at least 1.2 mol% and at most 4.0 mol%, preferably at least 1.5 mol% and at most 3.5 mol%, preferably at least 1.5 mol% and at most 3.0 mol% of repeating units derived from at least one monomer (M) of formula (I) or formula (II) as detailed above.
[0058] When the repeating unit in the polymer (P) is derived from the monomer (M) of general formula (II), it should be understood that the repeating unit is the result of the ring-opening polymerization of the epoxide moiety.
[0059] When the repeating unit in the polymer (P) originates from a monomer (M) of general formula (I) (where X is an acyl chloride or acyl bromide), it should be understood that the repeating unit can be the result of a process in which the monomer (M) reacts with, for example, the terminal OH group of the EO unit or PO unit of a dihydroxy-terminated polyethylene oxide (or a PEO-co-PPO copolymer) to form an ester moiety.
[0060] When the repeating unit in the polymer (P) originates from a monomer (M) of general formula (I) (where X is trifluoromethanesulfonate, nonafluorobutanesulfonate, p-toluenesulfonate, or methanesulfonate), the repeating unit can be the result of a process in which, in the presence of a strong base (such as NaH), the monomer (M) undergoes a Williamson-type reaction with, for example, the terminal OH group of the EO or PO unit of a dihydroxy-terminated polyethylene oxide (or PEO-co-PPO copolymer), thereby forming an ether moiety. This is followed by alkoxide formation and subsequent substitution of the X moiety of the monomer (M).
[0061] These polymerization reactions are known in the art and were developed by H.-Q. Xie, J.-S. Guo, G.-Q. Yu and J. Zu. Journal of Applied Polymer Science 2001, 80 , 2446 is described in detail.
[0062] Preferably, each of the X in the monomer (M) of general formula (I) is a halide ion, more preferably a halide ion selected from chloride ions, bromide ions and iodide ions.
[0063] According to a preferred embodiment, the monomer (M) has formula (II). Equation (II) in - Each of R1 and R2 is either the same as or different from each other and is C each time it appears. 1-2 Alkyl, and n is an integer 0 or 1, preferably n is 1.
[0064] In another preferred embodiment of the positive electrode for a lithium-ion secondary battery, the monomer (M) according to the invention is selected from those of formulas (Ia) to (If) and (IIa) to (IIe):
[0065] Formula (IIa)
[0066] Equation (IIb)
[0067] Formula (IIc)
[0068] Formula (IId)
[0069] Formula (IIe)
[0070] Formula (Ia)
[0071] Formula (Ib)
[0072] Formula (Ic)
[0073] Formula(Id)
[0074] Formula (Ie)
[0075] Formula (If)
[0076] Wherein X is selected from halide ions, trifluoromethanesulfonate, nonafluorobutanesulfonate, p-toluenesulfonate and methanesulfonate, acyl chloride, and acyl bromide. Preferably, X is a halide ion, more preferably a halide ion selected from chloride ions, bromide ions, and iodide ions. Even more preferably, X is a bromide ion.
[0077] More preferably, the monomer (M) according to the invention is a compound selected from those monomers of formula (Ia) to (If).
[0078] Most preferably, the monomer (M) is a compound of formula (Ia).
[0079] According to a preferred embodiment of the positive electrode suitable for lithium-ion secondary batteries, the polymer (P) is essentially composed of the following substances: a) 94.0 mol% to 98.5 mol% of repeating EO units; b) 0.5 mol% to 3.0 mol% of repeating PO units; and c) 1.0 mol% to 3.0 mol% of repeating units derived from monomer (M) of general formula (II): Equation (II) Each of R1 and R2 is either the same as or different from each other, and is C each time it appears. 1-2 Alkyl, and n is an integer 0 or 1, preferably n is 1. It should be understood that chain defects or very small amounts of other units may be present, and it should be understood that these latter do not substantially modify the properties of the polymer (P).
[0080] Preferably, the polymer (P) as detailed above has a weight-average molecular weight (Mw) of at least 10,000 g / mol, more preferably at least 20,000 g / mol, even more preferably at least 40,000 g / mol, and even more preferably at least 50,000 g / mol.
[0081] It should be understood that the polymer (P) as detailed above preferably has a Mw of up to 150,000 g / mol, more preferably up to 100,000 g / mol.
[0082] In a preferred embodiment, the polymer (P) as detailed above has a Mw of at least 10,000 g / mol and at most 150,000 g / mol, preferably at least 20,000 g / mol and at most 150,000 g / mol, more preferably at least 40,000 g / mol and at most 100,000 g / mol, and even more preferably at least 50,000 g / mol and at most 100,000 g / mol.
[0083] According to the present invention, Mw is measured by GPC with PEO standard calibration. Therefore, the Mw mentioned is the PEO equivalent.
[0084] Alternatively and even more preferably, the polymer (P) as detailed above has a number-average molecular weight of at least 10,000 g / mol, more preferably at least 20,000 g / mol, even more preferably at least 40,000 g / mol, even more preferably at least 50,000 g / mol.
[0085] It should be understood that the polymer (P) as detailed above preferably has a Mn content of up to 150,000 g / mol, more preferably up to 100,000 g / mol.
[0086] In a preferred embodiment, the polymer (P) as detailed above has at least 10,000 g / mol and at most 150,000 g / mol, preferably at least 20,000 g / mol and at most 150,000 g / mol, more preferably at least 40,000 g / mol and at most 100,000 g / mol, and even more preferably at least 50,000 g / mol and at most 100,000 g / mol of Mn.
[0087] According to the present invention, Mn is measured by GPC with PEO standard calibration. Therefore, the Mn mentioned is the PEO equivalent.
[0088] Preferably, the polymer (P) according to the invention is a random or block copolymer, more preferably a random copolymer.
[0089] Preferably, the polymer (P) according to the invention is linear or branched, more preferably linear.
[0090] The particularly preferred polymer (P) is a linear random copolymer, wherein it is noteworthy that the main chain can be described according to formula (IV): (IV) In the polymer (P) of formula (IV), the ratio of o to q (o / q) is between 25 and 100, or between 35 and 75, or between 40 and 60. In the polymer (P) of formula (IV), the ratio of p to q (p / q) is advantageously between 0.05 and 1.50, preferably between 0.10 and 1.00, and more preferably between 0.20 and 0.60.
[0091] It is worth noting that this type of polymer (P) can be marketed under the trade name Alkox. ® The CP-A series was purchased from Meisei Chemicalworks Ltd.
[0092] As described, a polysiloxane compound having formula (III) will be used. Equation (III) in - Each of R3, R4, R5, R6, and R7 is either the same as or different from each other, and is independently selected from C each time it appears. 1-6 Alkyl, C 3-6 cycloalkyl, aryl, C 1-6 alkoxy, heterocyclic group, wherein the C 1-6 Alkyl, C 3-6 cycloalkyl, aryl, C 1-6 The alkoxy group and heterocyclic group are optionally selected from halide ions, C 1-4 Alkyl, C 3-6 One or more substituents of cycloalkyl, CF3, and OR9 are used, wherein each R9 is the same as or different from each other and is independently selected from hydrogen, C, and D in each occurrence. 1-4 Alkyl and hydroxyl protecting groups, and - m is an integer of at least 3; The monomer (M) is grafted onto the polymer (P) as detailed above by reacting at least a portion of the -CH=CH2 portion of the monomer (M) with the H-Si portion of a polysiloxane compound having formula (III).
[0093] Preferably, each of R3 and R4 is the same as or different from each other and independently represents C each time it occurs. 1-6Alkyl, more preferably, each of R3 and R4 is the same as or different from each other and is methyl, ethyl, propyl or isopropyl each time it appears, even more preferably, each of R3 and R4 is the same as or different from each other and is methyl each time it appears.
[0094] Preferably, each of R5 and R6 is the same as or different from each other and is independently selected from C each time it appears. 1-4 alkyl or phenyl, wherein the C 1-4 Alkyl groups are optionally selected from halide ions, C 1-4 One or more substituents of alkyl or CF3 are used for substitution. More preferably, each of R5 and R6 is the same as or different from each other and is methyl, ethyl, propyl or isopropyl each time it appears. Even more preferably, each of R5 and R6 is the same as or different from each other and is methyl each time it appears.
[0095] Preferably, each R7 is C 1-6 Alkyl, more preferably, each R7 is C 1-4 Alkyl groups, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, or tert-butyl.
[0096] Preferably, m is an integer of at least 5, more preferably at least 7, or even more preferably at least 8.
[0097] It should also be understood that m is preferably an integer of at most 1000, more preferably at most 500, even more preferably at most 100, even more preferably at most 20, even more preferably at most 15.
[0098] In a preferred embodiment of the invention, m is an integer of at least 5 and at most 1000, preferably at least 5 and at most 500, more preferably at least 5 and at most 100, even more preferably at least 5 and at most 20, even more preferably at least 7 and at most 20, even more preferably at least 8 and at most 15.
[0099] In the context of this invention, it should be understood that the -CH=CH2 moiety of monomer (M) can react with the H-Si moiety of a polysiloxane compound having formula (III) as detailed above, in order to obtain a covalent bond between the two moieties. Such reactions are commonly referred to as hydrosilylation reactions. It should also be understood that the reactions may involve the formation of one or more intermediates, including metal complexes and σ complexes.
[0100] For the reaction of at least a portion of the -CH=CH2 portion of the monomer (M) as detailed above with the H-Si portion of the polysiloxane compound having formula (III) as detailed above, several techniques known in the art can be successfully used.
[0101] It is worth noting that the polymer (P) as detailed above and the polysiloxane having formula (III) as detailed above can react significantly in the molten state; melt compounding machines such as extruders, melt kneaders or other devices can be advantageously used for this purpose.
[0102] It is worth noting that the polymer (P) as detailed above and the polysiloxane having formula (III) as detailed above can react in solution; according to this embodiment, the polymer (P) and the polysiloxane having formula (III) as detailed above are at least partially dissolved in a solvent. Dissolution can be achieved at room temperature or preferably by heating to at least 70°C, more preferably at least 80°C, and even more preferably at the reflux temperature of the solvent. The choice of solvent is not critical, provided that it effectively solvates both the polymer (P) as detailed above and the polysiloxane having formula (III) without interfering with the hydrosilylation reaction. Generally, organic solvents are preferred. Among these organic solvents, benzene, toluene, xylene, methyl isopropylbenzene, etc. are worth mentioning.
[0103] Furthermore, it is worth noting that the polymer (P) as detailed above and the polysiloxane having formula (III) as detailed above can react in the presence of a catalyst, especially a hydrosilylation catalyst.
[0104] Such hydrogenation silylation catalysts are known in the art. Of particular note are ruthenium, platinum, or rhodium-based catalysts, such as, in particular, Karstedt, Wilkinson, Speier, and mixtures thereof.
[0105] In the context of this invention, the expression "by reacting at least a portion of the -CH=CH2 of monomer (M) with the H-Si portion of a polysiloxane compound having formula (III)" means that only a portion or all of the CH=CH2 of monomer (M) can react with the H-Si portion of a polysiloxane compound having formula (III).
[0106] Preferably, the polysiloxane compound having formula (III) is grafted onto the polymer (P) as detailed above by reacting the -CH=CH2 portion of a monomer (M) of at least 10 mol%, more preferably at least 15 mol%, even more preferably at least 20 mol%, even more preferably at least 25 mol%, even more preferably at least 30 mol%, even more preferably at least 35 mol%, even more preferably at least 40 mol%, even more preferably at least 45 mol% of the monomer (M) with the H-Si portion of the polysiloxane compound having formula (III).
[0107] It should also be understood that the -CH=CH2 portion of a monomer (M) having formula (III) can be reacted with the H-Si portion of a polysiloxane compound having formula (III) as detailed above, by reacting 100 mol%, more preferably up to 95 mol%, even more preferably up to 90 mol%, even more preferably up to 85 mol%, even more preferably up to 80 mol%, even more preferably up to 75 mol%, even more preferably up to 70 mol%, even more preferably up to 65 mol%, even more preferably up to 60 mol% of the monomer (M) with the polysiloxane compound having formula (III), as detailed above, onto the polymer (P) as detailed above.
[0108] In a preferred embodiment, the polysiloxane compound having formula (III) is grafted onto the polymer (P) as detailed above by reacting the -CH=CH2 portion of a monomer (M) of at least 10 mol% and at most 90 mol%, more preferably at least 30 mol% and at most 70 mol%, even more preferably at least 40 mol% and at most 60 mol% with the H-Si portion of the polysiloxane compound having formula (III).
[0109] This reaction can be monitored using known analytical methods, such as, in particular, by using GPC or 1 The H-NMR method is described in the experimental section.
[0110] Preferably, the polymer electrolyte is obtained by a reaction between the at least one polymer (P) and at least 6% by weight, at least 7% by weight, or at least 8% by weight of the at least one polysiloxane compound relative to the total amount of the at least one polymer (P) and the at least one polysiloxane compound.
[0111] Preferably, the polymer electrolyte is obtained by a reaction between the at least one polymer (P) and at most 27% by weight, 25% by weight, or 22% by weight of the at least one polysiloxane compound relative to the total amount of the at least one polymer (P) and the at least one polysiloxane compound.
[0112] In a preferred embodiment, the polymer electrolyte is obtained by a reaction between the at least one polymer (P) and at least 6% by weight and at most 27% by weight, or at least 7% by weight and at most 25% by weight, or at least 8% by weight and at most 22% by weight of the at least one polysiloxane compound relative to the total amount of the at least one polymer (P) and the at least one polysiloxane compound.
[0113] As described above, the positive electrode for a lithium-ion secondary battery comprises a positive electrode active material and at least one polymer electrolyte, wherein the positive electrode active material comprises at least an element selected from Li, M', and oxygen, wherein the metal M' has the following formula: Ni 1-x-y-z Mn x Co y A z Wherein 0.00≤x≤0.70, 0.00≤y≤0.40, and 0.00≤z≤0.10, as measured by ICP, wherein when A is present, A is different from Ni, Mn, Co, and Li, and preferably is at least one of the following: B, Mg, Al, Nb, Ti, Y, W, S, Ba, Sr, and Zr, and the polymer electrolyte is obtained by a reaction between the following substances: preferably, A is Al, wherein the atomic ratio of A to the total amount of Ni, Mn, and / or Co is greater than 0, preferably greater than 0.001, more preferably greater than 0.003, and most preferably greater than 0.006. Preferably, A is Al, wherein the atomic ratio of A to the total amount of Ni, Mn, and / or Co is less than 0.1, preferably less than 0.05, more preferably less than 0.01, and most preferably less than 0.008. Preferably, A is Al, and the atomic ratio of A to the total amount of Ni, Mn and / or Co is in the range of 0.001-0.1, more preferably in the range of 0.002-0.05, more preferably in the range of 0.003-0.01, and most preferably in the range of 0.006-0.008.
[0114] According to certain embodiments of the positive electrode of the present invention, the weight ratio of the polymer electrolyte to the positive electrode active material is at least 5%, more preferably at least 10%, and even more preferably at least 15%.
[0115] Preferably, the weight ratio of the polymer electrolyte to the positive electrode active material in the positive electrode according to the present invention is at most 50%, more preferably at most 30%, and even more preferably at most 25%.
[0116] In a preferred embodiment, the weight ratio of the polymer electrolyte to the positive electrode active material in the positive electrode according to the invention is 5% to 50%, preferably 10% to 30%, and more preferably 15% to 25%. Alternatively, the weight ratio of the polymer electrolyte to the positive electrode active material in the positive electrode according to the invention is 5% to 50%, preferably 20% to 45%, and more preferably 30% to 40%.
[0117] In a preferred embodiment of the positive electrode of the present invention, the positive electrode comprises the polymer electrolyte as described above, the positive electrode active material as detailed above, and further comprises at least one lithium salt (Li salt), said at least one lithium salt (Li salt) selected from: LiTFSI, LiFSI, LiPF6, LiBF4, and LiClO4. Such a positive electrode is defined as a cathode electrolyte. Optionally, the Li salt is present in the positive electrode in a polymer electrolyte:Li salt ratio of 60:40 to 80:20 by weight, more preferably 70:30 to 75:25 by weight.
[0118] In a preferred embodiment of the positive electrode of the present invention, the [weight ratio × 100] of the Li salt to the polymer electrolyte in the positive electrode of the present invention is 5% to 50%, preferably 20% to 45%, and more preferably 30% to 40%.
[0119] In another preferred embodiment, the Li salt is LiTFSI.
[0120] Preferably, the positive electrode active material, as detailed above, is a particulate material, particularly a powder.
[0121] Batteries and electrochemical single cells
[0122] In another aspect, the present invention provides a polymer battery comprising a positive electrode according to a first aspect of the invention.
[0123] In another aspect, the present invention provides an electrochemical single cell comprising a positive electrode according to a first aspect of the present invention.
[0124] In another aspect, the present invention provides the use of the positive electrode according to the invention in a battery.
[0125] In a final aspect, the present invention provides a battery or electrochemical single cell comprising a positive electrode active material and a polymer electrolyte, wherein the positive electrode active material comprises at least Li, M' and oxygen, wherein M' is composed of Ni, Mn, Co and A, the positive electrode material having a Ni:(Mn+Co+A) molar ratio of (1-xyz):(x+y+z) as measured by ICP, wherein 0.00≤x≤0.70, 0.00≤y≤0.40 and 0.00≤z≤0.10, wherein when A is present, A is different from Ni, Mn, Co and Li, and is preferably Al or at least one of the following: B, Mg, Al, Nb, Ti, Y, W, S, Ba, Sr and Zr, and the polymer electrolyte is obtained by a reaction between the following substances: i. At least one polyether polymer [polymer (P) hereinafter], said polymer (P) comprising: a) At least 70.0 mol% of oxyethylidene units (EO); b) 0.0 mol% to 10.0 mol% of oxypropylene units (PO); and c) 1.00 mol% to 4.0 mol% of repeating units derived from at least one monomer of formula (I) or formula (II) [monomer (M) hereinafter]: Formula (I) or Equation (II) in - Each of R1 and R2 is either the same as or different from each other and is C each time it appears. 1-6 Alkyl, wherein the C 1-6 Alkyl groups are optionally selected from halide ions, C 1-4 Alkyl, C 3-6 One or more substituents of cycloalkyl, CF3, and OR8 are used, wherein each R8 is the same as or different from each other and is independently selected from hydrogen and C each time it appears. 1-4 Alkyl; n is an integer, either 0, 1, or 2; - Each X is a leaving group selected from halide ions, trifluoromethanesulfonate, nonafluorobutanesulfonate, p-toluenesulfonate and methanesulfonate; and ii. At least one polysiloxane compound having formula (III):
[0126] Equation (III)
[0127] in
[0128] - Each of R3, R4, R5, R6, and R7 is either the same as or different from each other, and is independently selected from C each time it appears. 1-6 Alkyl, C 3-6 cycloalkyl, aryl, C 1-6 alkoxy, heterocyclic group, wherein the C 1-6 Alkyl, C 3-6 cycloalkyl, aryl, C 1-6 The alkoxy group and heterocyclic group are optionally selected from halide ions, C 1-4 Alkyl, C 3-6 One or more substituents of cycloalkyl, CF3, and OR9 are used, wherein each R9 is the same as or different from each other and is independently selected from hydrogen, C, and D in each occurrence. 1-4 Alkyl and hydroxyl protecting groups, - m is an integer of at least 3; and The at least one polysiloxane compound having formula (III) is grafted onto the at least one polymer (P) by reacting at least a portion of the -CH=CH2 portion of the monomer (M) with the H-Si portion of the polysiloxane compound having formula (III).
[0129] One embodiment of the present invention is a battery pack or electrochemical single cell comprising a positive electrode active material and a polymer electrolyte, wherein the positive electrode active material comprises Ni, Mn, Co and A, and the positive electrode material has a Ni:(Mn+Co+A) molar ratio of (1-xyz):(x+y+z) as measured by ICP, wherein 0.00≤x≤0.70, 0.00≤y≤0.40 and 0.00≤z≤0.10, wherein when A is present, A is different from Ni, Mn, Co and Li, and is preferably Al or at least one of the following: B, Mg, Al, Nb, Ti, Y, W, S, Ba, Sr and Zr, and the polymer electrolyte is obtained by a reaction between the following substances: i. At least one polyether polymer [polymer (P) hereinafter], said polymer (P) comprising: a) At least 70.0 mol% of oxyethylidene units (EO); b) 0.0 mol% to 10.0 mol% of oxypropylene units (PO); and c) 1.00 mol% to 4.0 mol% of repeating units derived from at least one monomer of formula (I) or formula (II) [monomer (M) hereinafter]: Formula (I) or Equation (II) in - Each of R1 and R2 is either the same as or different from each other and is C each time it appears. 1-6 Alkyl, wherein the C 1-6 Alkyl groups are optionally selected from halide ions, C 1-4 Alkyl, C 3-6 One or more substituents of cycloalkyl, CF3, and OR8 are used, wherein each R8 is the same as or different from each other and is independently selected from hydrogen and C each time it appears. 1-4 Alkyl; n is an integer, either 0, 1, or 2; - Each X is a leaving group selected from halide ions, trifluoromethanesulfonate, nonafluorobutanesulfonate, p-toluenesulfonate and methanesulfonate; and ii. At least one polysiloxane compound having formula (III):
[0130] Equation (III)
[0131] in
[0132] - Each of R3, R4, R5, R6, and R7 is either the same as or different from each other, and is independently selected from C each time it appears. 1-6 Alkyl, C 3-6 cycloalkyl, aryl, C 1-6 alkoxy, heterocyclic group, wherein the C 1-6 Alkyl, C 3-6 cycloalkyl, aryl, C 1-6 The alkoxy group and heterocyclic group are optionally selected from halide ions, C 1-4 Alkyl, C 3-6 One or more substituents of cycloalkyl, CF3, and OR9 are used, wherein each R9 is the same as or different from each other and is independently selected from hydrogen, C, and D in each occurrence. 1-4 Alkyl and hydroxyl protecting groups, - m is an integer of at least 3; and The at least one polysiloxane compound having formula (III) is grafted onto the at least one polymer (P) by reacting at least a portion of the -CH=CH2 portion of the monomer (M) with the H-Si portion of the polysiloxane compound having formula (III).
[0133] In a preferred embodiment, the battery is a lithium-ion battery.
[0134] In a preferred embodiment, the battery or electrochemical single cell of the present invention comprises a polymer electrolyte, as described in the positive electrode section provided above.
[0135] Examples and Comparative Examples
[0136] The following examples are intended to further illustrate the invention, but not to limit the scope of the invention.
[0137] 1.1. Materials and Methods
[0138] Unless otherwise stated, use the following materials as described below.
[0139] Random polymer (P) was purchased from Meisei Chemical Works Ltd under the trade name CP series CP-A. Alternatively, polymer (P) can be manufactured by following the instructions of H.-Q. Xie, J.-S. Guo, G.-Q. Yu and J. Zu. Journal of Applied Polymer Science 2001, 80 Prepared using the procedure disclosed in , 2446.
[0140] Monohydride-terminated polydimethylsiloxane (SiH-terminated PDMS, M w =850g / mol) purchased from Gelest, Inc.
[0141] The silica-supported Karsted catalyst was prepared according to QJ Miao, Z.-P. Fang and GP Cai, Catalysis Communications 2003, 4, 637-639.
[0142] LiTFSI (lithium bis(trifluoromethanesulfonyl)imide, based on 99.95% trace metal) was purchased from Sigma-Aldrich .
[0143] Anhydrous acetonitrile 99.8% by weight purchased from Sigma-Aldrich .
[0144] Timcal Super P is made by Imerys Graphite & Carbon The manufactured conductive carbon black powder (CAS No. 1333-86-4).
[0145] Polyethylene oxide (with M of 1,000,000) w The PEO was purchased from Alfa Aesar.
[0146] Recorded at room temperature on a JEOL JNM ECZ 500MHz NMR spectrometer 1 H-spectroscopy. The polymer sample was dissolved in CDCl3 and the internal standard was optimized using tetramethylsilane (TMS).
[0147] Using Agilent 720 ICP-OES ( Agilent Technologies , https: / / www.agilent.com / cs / library / brochures / 5990-6497EN%20720-725_ICP-OES_LR.pdf Inductively coupled plasma (ICP) measurements were performed. One gram of powder sample was dissolved in 50 mL of high-purity hydrochloric acid (at least 37% wt% HCl relative to the total weight of the solution) in an Erlenmeyer flask. The flask was covered with a watch glass and heated on a hot plate at 380°C until the powder was completely dissolved. After cooling to room temperature, the solution in the Erlenmeyer flask was poured into a first 250 mL volumetric flask. The first volumetric flask was then filled with deionized water to the 250 mL mark, followed by complete homogenization (first dilution). A suitable amount of solution was pipetted from the first volumetric flask and transferred to a second 250 mL volumetric flask for a second dilution, in which case the second volumetric flask was filled with an internal standard and 10% hydrochloric acid to the 250 mL mark, and then homogenized. Finally, this solution was used for ICP measurements.
[0148] 1.2. Preparation of Polymer Electrolytes
[0149] The following procedure is followed to react polymer (P), a random linear copolymer characterized as shown in Table 2, with monohydride-terminated polydimethylsiloxane (SiH-terminated PDMS) via hydrosilylation: Table 2
[0150] A mixture containing 2.0 g of polymer (P) and 0.36 g of SiH-terminated PDMS was added to 50 mL of benzene containing 20 mg of silica-supported Karsted catalyst, and heated at 90 °C for 48 h under a nitrogen atmosphere. The heated mixture was filtered through diatomaceous earth to remove the solid catalyst, and then placed under reduced pressure to remove the solvent. PDMS was grafted onto polymer (P) by reacting 50 mol% of the -CH=CH2 group of the AGE unit with the H-Si moiety of PDMS.
[0151] Successful grafting 1 H-NMR and GPC were used for confirmation.
[0152] Polymer (P): 1 H-NMR (TMS, CDCl3, 500MHz): δ (ppm) 1.2 (d, CH3 in PO unit), 4 (m, -OC in AGE unit) H2 -CH=CH2), 5.2 (m, C of AGE unit) H2 =CH-), 5.8 (m, AGE unit -C) H =CH2).
[0153] Monohydride PDMS: 1 H-NMR (TMS, CDCl3, 500MHz): δ (ppm) 0.5 (m, -Si-C H 2-CH2-), 0.9 (t, C H 3-CH2-), 1.3 (br, -Si-CH2-C H 2-C H2 -CH3), 4.8 (m, H -Si-).
[0154] Polymer electrolyte: 1 H-NMR (TMS, CDCl3, 500MHz): δ (ppm): 0.5 (br, PDMS-Si-C H 2-CH2-), 0.9 (br, C of PDMS) H 3-CH2-), 1.1 (d, CH3 of PO unit), 1.2 (br, -Si-CH2-C of PDMS) H 2-CH2 -CH3), 1,4(br, -OCH2-C H2 -CH2-Si-).
[0155] In polyelectrolytes 1 The presence of a broad peak at 1.4 ppm and the absence of peaks attributable to H-Si in the H-NMR spectrum confirms successful hydrosilylation.
[0156] Figure 1 The GPC elution curves of the polymer electrolyte, polymer (P), and polysiloxane prepared as described above are shown.
[0157] Compared to polymer (P), the polymer electrolyte has a shorter elution time, which indicates that the polymer electrolyte has a higher molecular weight than polymer (P), thus PDMS was successfully grafted onto polymer (P).
[0158] The resulting polymer electrolyte was labeled PE1.
[0159] 1.3. Preparation of Positive Electrode Active Material 1 (AM1)
[0160] Lithium transition metal composite oxides were prepared as positive electrode active materials according to the following method. These lithium transition metal composite oxides have the general formula Li 1.010 (Ni 0.621 Mn 0.224 Co 0.155 ) 0.990 O 2.00 For example, measurements obtained via ICP: Step 1) Preparation of transition metal oxide hydroxide precursor: Nickel-based transition metal oxide hydroxide powder (TMH2) with a metal composition of Ni was prepared by co-precipitation in a large continuous stirred tank reactor (CSTR) containing a mixture of nickel manganese cobalt sulfate, sodium hydroxide, and ammonia. 0.621 Mn 0.224 Co 0.155 Such as measurements obtained via ICP.
[0161] Step 2) First Mixing: The TMH1 prepared in Step 1) is mixed with Li2CO3 in an industrial blender to obtain a first mixture with a lithium to metal ratio of 0.85.
[0162] Step 3) First calcination: The first mixture obtained from Step 2) is calcined at 900°C for 10 hours in a dry air atmosphere to obtain a first calcined cake. The first calcined cake is crushed to obtain a first calcined powder.
[0163] Step 4) Second Mixing: The first calcined powder obtained from Step 3) is mixed with LiOH in an industrial blender to obtain a second mixture with a lithium to metal ratio of 1.01.
[0164] Step 5) Second calcination: The second mixture from step 4) is calcined in dry air at 930°C for 10 hours, and then pulverized (bead milled) and sieved to obtain the second calcined powder.
[0165] Step 6) Third Mixing: The second calcined powder obtained from Step 5) is mixed with LiOH in an industrial blender at a total molar content of 1.5 mol% relative to Ni, Mn and Co to obtain a third mixture.
[0166] Step 7) Third calcination: The third mixture obtained from step 6) is calcined in dry air at 750°C for 10 hours to obtain AM1.
[0167] 1.4. Preparation of positive electrode EX1
[0168] A positive electrode containing PE1 and AM1 is prepared according to the following procedure: Step 1) Prepare a polymer electrolyte solution comprising a 99.8 wt% anhydrous acetonitrile solution of polymer electrolyte PE1 and LiTFSI. This polymer electrolyte solution has a polymer electrolyte to LiTFSI ratio of 74:26 by weight. This weight ratio corresponds to 35% LiTFSI:polymer electrolyte [weight ratio × 100].
[0169] Step 2) The polymer electrolyte solution prepared in Step 1), the positive electrode active material AM1 prepared according to Part 1.2, and the carbon black powder (Timcal Super carbon black) are mixed in an acetonitrile solution at a weight ratio of 21:75:4 to prepare a slurry mixture. The mixture is homogenized at 5000 rpm for 45 minutes.
[0170] Step 3) The slurry mixture obtained from Step 2) is cast onto one side of a 20µm thick aluminum foil, wherein the coating machine slit is 100µm.
[0171] Step 4) Dry the foil cast from the slurry at 30°C for 12 hours, and then press it to obtain a positive electrode with a diameter of 14 mm.
[0172] The positive electrode is labeled EX1.
[0173] 1.5. Preparation of Positive Electrode Active Material 2 (AM2)
[0174] The positive electrode active material AM2 is prepared according to the following process: Step 1) Preparation of transition metal oxide hydroxide precursor: Nickel-based transition metal oxide hydroxide powder (TMH1) with a metal composition of Ni was prepared by co-precipitation in a large continuous stirred tank reactor (CSTR) containing a mixture of nickel manganese cobalt sulfate, sodium hydroxide, and ammonia. 0.63 Mn 0.22 Co 0.15 Such as measurements obtained via ICP.
[0175] Step 2) First Mixing: The TMH1 prepared in Step 1) is mixed with Li2CO3 in an industrial blender to obtain a first mixture with a lithium to metal ratio of 0.85.
[0176] Step 3) First calcination: The first mixture obtained from Step 2) is calcined at 900°C for 10 hours in a dry air atmosphere to obtain a first calcined cake. The first calcined cake is crushed to obtain a first calcined powder.
[0177] Step 4) Second Mixing: The first calcined powder obtained from Step 3) is mixed with LiOH in an industrial blender to obtain a second mixture with a lithium to metal ratio of 1.05.
[0178] Step 5) Second calcination: The second mixture from step 4) is calcined in dry air at 930°C for 10 hours, and then pulverized (bead milled) and sieved to obtain the second calcined powder.
[0179] Step 6) Third Mixing: The second calcined powder obtained from Step 5) is mixed in an industrial blender with 2 mol% Co (e.g., obtained from Co3O4 powder) and 5 mol% LiOH relative to the total molar content of Ni, Mn and / or Co to obtain a third mixture.
[0180] Step 7) Third calcination: The third mixture obtained from step 6) is calcined in dry air at 775°C for 12 hours to produce a third calcined powder.
[0181] Step 8) Fourth mixing: The third calcined powder obtained from step 7) is mixed with 0.2% by weight of nano Al2O3 powder.
[0182] Step 9) Fourth calcination: The fourth mixture obtained from step 8) is calcined in dry air at 750°C for 10 hours to produce a fourth calcined powder.
[0183] Step 10) Fifth Mixing: The fourth calcined powder obtained from step 9) is mixed with 0.3% by weight of polyvinylidene fluoride (PVDF).
[0184] Step 11) Fifth calcination: The fifth mixture obtained from step 10) is calcined in dry air at 375°C for 5 hours to produce AM2.
[0185] 1.6. Preparation of positive electrode EX2
[0186] A positive electrode containing AM2 and PE1 is prepared according to the following procedure: Step 1) Prepare a polymer electrolyte solution comprising a 99.8% by weight anhydrous acetonitrile solution of polymer electrolyte PE1 and LiTFSI. This polymer electrolyte solution has a polymer electrolyte to LiTFSI ratio of 74:26 by weight.
[0187] Step 2) The polymer electrolyte solution prepared in Step 1), the positive electrode active material AM2, and the carbon black powder (Timcal Super carbon black) are mixed in an acetonitrile solution at a weight ratio of 21:75:4 to prepare a slurry mixture. The mixture is homogenized at 5000 rpm for 45 minutes.
[0188] Step 3) The slurry mixture obtained from Step 2) is cast onto one side of a 20µm thick aluminum foil, wherein the coating machine slit is 100µm.
[0189] Step 4) Dry the foil cast from the slurry at 30°C for 12 hours, and then press it to obtain a positive electrode with a diameter of 14 mm.
[0190] The positive electrode is labeled EX2.
[0191] 1.7. Preparation of positive electrode CEX1
[0192] A positive electrode comprising PE2 (poly(ethylene oxide) (PEO) powder purchased from Alfa Aesar (Mw = 1,000,000 g / mol)) and AM1 was prepared according to the following procedure: Step 1) Prepare a polymer electrolyte solution comprising a 99.8% by weight anhydrous acetonitrile solution of polymer electrolyte (PE2) and LiTFSI. The polymer electrolyte solution has a polymer electrolyte to LiTFSI ratio of 74:26 by weight.
[0193] Step 2) The polymer electrolyte mixture prepared in Step 1), the positive electrode active material AM1, and the conductor powder (Super P) are combined. Timcal (Imerys Graphite & Carbon) were mixed in an acetonitrile solution at a ratio of 21:75:4 by weight to prepare a slurry mixture. The mixture was homogenized at 5000 rpm for 45 minutes.
[0194] Step 3) The slurry mixture obtained from Step 2) is cast onto one side of a 20µm thick aluminum foil, wherein the coating machine slit is 100µm.
[0195] Step 4) Dry the foil cast from the slurry at 30°C for 12 hours, and then press it to obtain a positive electrode with a diameter of 14 mm.
[0196] The positive electrode is labeled CEX1.
[0197] 1.8. Preparation of Solid Polymer Electrolytes (SPEs)
[0198] The PEO-based solid polymer electrolyte (SPE) is prepared according to the following process: Step 1) Using a mixer at 2,000 rpm, mix polyethylene oxide (PEO, molecular weight 1,000,000) with LiTFSI (purchased from Soulbrain Co., Ltd. instead of Sigma Aldrich) in 99.8% wt% anhydrous acetonitrile for 30 minutes. The molar ratio of ethylene oxide to lithium is 20.
[0199] Step 2) Pour the mixture obtained from Step 1) into a Teflon dish and dry at 25°C for 12 hours.
[0200] Step 3) Separate the dried SPE from the dish and stamp the dried SPE to obtain an SPE disk with a thickness of 300µm and a diameter of 19mm.
[0201] 1.9. Polymer Battery Assembly
[0202] Assemble the button cell polymer battery in an argon-filled glove box in the following order from bottom to top: 2032 button cell casing, positive electrode (EX1, EX2, or CEX1), SPE prepared according to Section 1.8, gasket, Li anode, spacer, wave spring, and battery cap. Then, completely seal the button cell to prevent electrolyte leakage.
[0203] 2. Comparison and Testing Methods (Q) 总 )
[0204] Measure the leakage capacity (Q) of EX1, EX2 and CEX1. 总 ).
[0205] A constant current circulating station controlled by a Toscat-3100 computer (from...) Toyo, http: / / www.toyosystem.com / image / menu3 / toscat / TOSCAT-3100.pdf Each coin cell polymer battery was cycled at 80°C. The coin cell test procedure was performed according to the following schedule, which used a 1C current definition of 160 mA / g within a metallographic window of 4.4 V / Li–3.0 V / Li: Step 1) Charge in constant current mode with a C rate of 0.05 and a termination condition of 4.4 V, then let stand for 10 minutes.
[0206] Step 2) Discharge in constant current mode with a C rate of 0.05 and a termination condition of 3.0 V, then let stand for 10 minutes.
[0207] Step 3) Charge in constant current mode with a C rate of 0.05 and a termination condition of 4.4 V.
[0208] Step 4) Switch to constant voltage mode and maintain 4.4 V for 60 hours.
[0209] Step 5) Discharge in constant current mode with a C rate of 0.05 and a termination condition of 3.0 V.
[0210] Q 总 It is defined as the total leakage capacity under high voltage and high temperature in step 4) according to the test method described above. Q 总 A low value indicates high stability of the positive electrode active material powder during high-temperature operation.
[0211] Table 3. Summary of positive electrode information for the Examples and Comparative Examples
[0212] Table 4. ICP results of the positive electrode active material
[0213] a As determined by ICP measurement, Me is the total atomic fraction of Ni + Mn + Co + Al.
[0214] Table 5. Q of Examples and Comparative Examples 总 Summary .
[0215]
[0216] Figure 2 The polymer electrolyte according to the present invention is shown to react with Q. 总 The influence of the value. The X-axis represents the polymer electrolyte used in the positive electrode. The legend indicates the active material used in the positive electrode.
[0217] According to Table 5 and Figure 2 It was observed that EX1 has a lower Q than CEX1. 总 This observation indicates that the positive electrode comprising the combination of the positive electrode active material according to the invention and the polymer electrolyte provides better electrochemical performance than the combination with PEO as a conventional electrolyte. Furthermore, when using PE1 as the polymer electrolyte, the surface-modified positive electrode active material powder (EX2) according to the invention exhibits better electrochemical performance than EX1.总 A low value indicates high stability of the lithium-ion secondary battery in applications where high voltage is applied at high temperatures.
[0218] 3. Characterization of the polymer electrolyte contained in the positive electrode and the positive electrode material
[0219] The solid polymer electrolyte and the positive electrode material can be separated from each other by selectively dissolving the solid polymer electrolyte in a solvent such as DMSO, DMF, or acetonitrile, followed by separation of the liquid phase containing the solid polymer electrolyte and the solid component containing the positive electrode material by filtration or centrifugation. Drying the liquid phase yields the solid polymer electrolyte, which can be characterized by NMR spectroscopy as described in Example 1.2. Optionally, the solid polymer electrolyte needs to be purified by precipitation in a non-solvent such as hexane or cyclohexane, followed by filtration and drying. ICP analysis of the solid component will reveal that the solid component contains the metallic composition determined for AM1 or AM2 as shown in Table 4, respectively.
Claims
1. A positive electrode for a lithium-ion secondary battery, the positive electrode comprising a positive electrode active material and at least one polymer electrolyte, the positive electrode active material comprising Ni, Mn, Co, and A, the positive electrode material having a Ni:(Mn+Co+A) molar ratio of (1-xyz):(x+y+z) as measured by ICP, wherein 0.00≤x≤0.70, 0.00≤y≤0.40, and 0.00≤z≤0.10, wherein when A is present, A is different from Ni, Mn, Co, and Li, and the polymer electrolyte is obtained by a reaction between the following substances: i. At least one polymer P, said polymer P being a polyether polymer, said polymer P comprising: - At least 70.0 mol% of oxyethylidene units (EO); - 0.0 mol% to 10.0 mol% of oxypropylene units PO; and - 1.00 mol% to 4.0 mol% of repeating units derived from at least one monomer M of general formula (I) or general formula (II): Equation (I) or Equation (II) in - Each of R1 and R2 is either the same as or different from each other and is C each time it appears. 1-6 Alkyl, wherein the C 1-6 Alkyl groups are optionally selected from halide ions, C 1-4 Alkyl, C 3-6 One or more substituents of cycloalkyl, CF3, and OR8 are used, wherein each R8 is the same as or different from each other and is independently selected from hydrogen and C each time it appears. 1-4 Alkyl; n is an integer, either 0, 1, or 2; - Each X is a leaving group selected from halide ions, trifluoromethanesulfonate, nonafluorobutanesulfonate, p-toluenesulfonate and methanesulfonate; and ii. At least one polysiloxane compound having formula (III): Equation (III) in - Each of R3, R4, R5, R6, and R7 is either the same as or different from each other, and is independently selected from C each time it appears. 1-6 Alkyl, C 3-6 cycloalkyl, aryl, C 1-6 alkoxy, heterocyclic group, wherein the C 1-6 Alkyl, C 3-6 cycloalkyl, aryl, C 1-6 The alkoxy group and heterocyclic group are optionally selected from halide ions, C 1-4 Alkyl, C 3-6 One or more substituents of cycloalkyl, CF3, and OR9 are used, wherein each R9 is the same as or different from each other and is independently selected from hydrogen, C, and D in each occurrence. 1-4 Alkyl and hydroxyl protecting groups, - m is an integer of at least 3; and The at least one polysiloxane compound having formula (III) is grafted onto the at least one polymer P by reacting at least a portion of the -CH=CH2 portion of monomer M with the H-Si portion of a polysiloxane compound having formula (III).
2. The positive electrode according to claim 1, wherein A is Al or at least one of the following: B, Mg, Al, Nb, Ti, Y, W, S, Ba, Sr and Zr.
3. The positive electrode according to claim 1, wherein 80.0 mol% to 99.0 mol% of the repeating units of the polymer P are EO units.
4. The positive electrode according to claim 3, wherein 90.0 mol% to 98.5 mol% of the repeating units of the polymer P are EO units.
5. The positive electrode according to claim 3, wherein 92.0 mol% to 98.5 mol% of the repeating units of the polymer P are EO units.
6. The positive electrode according to claim 3, wherein 94.0 mol% to 98.5 mol% of the repeating units of the polymer P are EO units.
7. The positive electrode according to any one of claims 1 to 6, wherein 0.5 mol% to 6.0 mol% of the repeating units of the polymer P are PO units.
8. The positive electrode according to claim 7, wherein 0.5 mol% to 5.0 mol% of the repeating units of the polymer P are PO units.
9. The positive electrode according to claim 7, wherein 0.5 mol% to 4.0 mol% of the repeating units of the polymer P are PO units.
10. The positive electrode according to claim 7, wherein 1.0 mol% to 4.0 mol% of the repeating units of the polymer P are PO units.
11. The positive electrode according to claim 7, wherein 1.0 mol% to 3.0 mol% of the repeating units of the polymer P are PO units.
12. The positive electrode according to any one of claims 1 to 6, wherein 1.2 mol% to 4.0 mol% of the repeating units of the polymer P are repeating units derived from monomer M of general formula (I) or general formula (II), wherein R1, R2, n and X are the same as defined in claim 1.
13. The positive electrode according to claim 12, wherein 1.5 mol% to 3.5 mol% of the repeating units of the polymer P are repeating units derived from monomer M of general formula (I) or general formula (II).
14. The positive electrode according to claim 12, wherein 1.5 mol% to 3.0 mol% of the repeating units of the polymer P are repeating units derived from monomer M of general formula (I) or general formula (II).
15. The positive electrode according to any one of claims 1 to 6, wherein the monomer M has formula (II) Equation (II) in - Each of R1 and R2 is either the same as or different from each other and is C each time it appears. 1-2 Alkyl, and n is an integer 0 or 1.
16. The positive electrode according to claim 15, wherein n is 1.
17. The positive electrode according to any one of claims 1 to 6, wherein each of R3, R4, and R7 is the same as or different from each other and independently constitutes C each time it appears. 1-6 Alkyl; each of R5 and R6 may be the same as or different from each other and is independently selected from C1 each time it appears. 1-4 alkyl or phenyl, wherein the C 1-4 Alkyl groups are optionally selected from halide ions, C 1-4 One or more substituents of alkyl or CF3 are used; m is an integer of at least 5 and at most 1000.
18. The positive electrode of claim 17, wherein m is an integer of at least 5 and at most 500.
19. The positive electrode of claim 17, wherein m is an integer of at least 5 and at most 100.
20. The positive electrode of claim 17, wherein m is an integer of at least 5 and at most 20.
21. The positive electrode of claim 17, wherein m is an integer of at least 7 and at most 20.
22. The positive electrode of claim 17, wherein m is an integer of at least 8 and at most 15.
23. The positive electrode according to any one of claims 1 to 6, wherein the polysiloxane compound having formula (III) is grafted onto polymer P by reacting at least 10 mol% and at most 90 mol% of the -CH=CH2 portion of the monomer M with the H-Si portion of the polysiloxane compound having formula (III).
24. The positive electrode according to claim 23, wherein at least 30 mol% and at most 70 mol% of the -CH=CH2 portion of the monomer M reacts with the H-Si portion of the polysiloxane compound having formula (III).
25. The positive electrode according to claim 23, wherein at least 40 mol% and at most 60 mol% of the -CH=CH2 portion of the monomer M reacts with the H-Si portion of the polysiloxane compound having formula (III).
26. The positive electrode according to any one of claims 1 to 6, wherein the weight ratio of the polymer electrolyte to the positive electrode active material is 5% to 50%.
27. The positive electrode according to claim 26, wherein the weight ratio of the polymer electrolyte to the positive electrode active material is 20% to 45%.
28. The positive electrode according to claim 26, wherein the weight ratio of the polymer electrolyte to the positive electrode active material is 30% to 40%.
29. The positive electrode according to any one of claims 1 to 6, wherein the positive electrode further comprises at least one lithium salt selected from: LiTFSI, LiFSI, LiPF6, LiBF4 and LiClO4.
30. The positive electrode according to any one of claims 1 to 6, wherein A is Al, and the atomic ratio of A to the total amount of Ni, Mn and / or Co is greater than 0.
31. A polymer battery comprising a positive electrode according to any one of the preceding claims.
32. An electrochemical single cell, the electrochemical single cell comprising a positive electrode according to any one of claims 1 to 30.
33. Use of the positive electrode according to any one of claims 1 to 30 in a battery.
34. A battery comprising a positive electrode active material and a polymer electrolyte, the positive electrode active material comprising Ni, Mn, Co and A, the positive electrode material having a Ni:(Mn+Co+A) molar ratio of (1-xyz):(x+y+z) measured by ICP, wherein 0.00≤x≤0.70, 0.00≤y≤0.40 and 0.00≤z≤0.10, wherein when A is present, A is different from Ni, Mn, Co and Li, and the polymer electrolyte is obtained by a reaction between the following substances: i. At least one polymer P, said polymer P being a polyether polymer, said polymer P comprising: - At least 70.0 mol% of oxyethylidene units (EO); - 0.0 mol% to 10.0 mol% of oxypropylene units PO; and - 1.00 mol% to 4.0 mol% of repeating units derived from at least one monomer M of general formula (I) or general formula (II): Equation (I) or Equation (II) in - Each of R1 and R2 is either the same as or different from each other and is C each time it appears. 1-6 Alkyl, wherein the C 1-6 Alkyl groups are optionally selected from halide ions, C 1-4 Alkyl, C 3-6 One or more substituents of cycloalkyl, CF3, and OR8 are used, wherein each R8 is the same as or different from each other and is independently selected from hydrogen and C each time it appears. 1-4 Alkyl; n is an integer, either 0, 1, or 2; - Each X is a leaving group selected from halide ions, trifluoromethanesulfonate, nonafluorobutanesulfonate, p-toluenesulfonate and methanesulfonate; and ii. At least one polysiloxane compound having formula (III): Equation (III) in - Each of R3, R4, R5, R6, and R7 is either the same as or different from each other, and is independently selected from C each time it appears. 1-6 Alkyl, C 3-6 cycloalkyl, aryl, C 1-6 alkoxy, heterocyclic group, wherein the C 1-6 Alkyl, C 3-6 cycloalkyl, aryl, C 1-6 The alkoxy group and heterocyclic group are optionally selected from halide ions, C 1-4 Alkyl, C 3-6 One or more substituents of cycloalkyl, CF3, and OR9 are used, wherein each R9 is the same as or different from each other and is independently selected from hydrogen, C, and D in each occurrence. 1-4 Alkyl and hydroxyl protecting groups, - m is an integer of at least 3; and The at least one polysiloxane compound having formula (III) is grafted onto the at least one polymer P by reacting at least a portion of the -CH=CH2 portion of monomer M with the H-Si portion of a polysiloxane compound having formula (III).
35. The battery according to claim 34, wherein A is at least one selected from Al or B, Mg, Al, Nb, Ti, Y, W, S, Ba, Sr and Zr.
36. The battery according to claim 34 or 35, wherein the battery comprises at least one lithium salt selected from: LiTFSI, LiFSI, LiPF6, LiBF4 and LiClO4.
37. An electrochemical single cell comprising a positive electrode active material and a polymer electrolyte, the positive electrode active material comprising Ni, Mn, Co and A, the positive electrode material having a Ni:(Mn+Co+A) molar ratio of (1-xyz):(x+y+z) as measured by ICP, wherein 0.00≤x≤0.70, 0.00≤y≤0.40 and 0.00≤z≤0.10, wherein when A is present, A is different from Ni, Mn, Co and Li, and the polymer electrolyte is obtained by a reaction between the following substances: i. At least one polymer P, said polymer P being a polyether polymer, said polymer P comprising: - At least 70.0 mol% of oxyethylidene units (EO); - 0.0 mol% to 10.0 mol% of oxypropylene units PO; and - 1.00 mol% to 4.0 mol% of repeating units derived from at least one monomer M of general formula (I) or general formula (II): Equation (I) or Equation (II) in - Each of R1 and R2 is either the same as or different from each other and is C each time it appears. 1-6 Alkyl, wherein the C 1-6 Alkyl groups are optionally selected from halide ions, C 1-4 Alkyl, C 3-6 One or more substituents of cycloalkyl, CF3, and OR8 are used, wherein each R8 is the same as or different from each other and is independently selected from hydrogen and C each time it appears. 1-4 Alkyl; n is an integer, either 0, 1, or 2; - Each X is a leaving group selected from halide ions, trifluoromethanesulfonate, nonafluorobutanesulfonate, p-toluenesulfonate and methanesulfonate; and ii. At least one polysiloxane compound having formula (III): Equation (III) in - Each of R3, R4, R5, R6, and R7 is either the same as or different from each other, and is independently selected from C each time it appears. 1-6 Alkyl, C 3-6 cycloalkyl, aryl, C 1-6 alkoxy, heterocyclic group, wherein the C 1-6 Alkyl, C 3-6 cycloalkyl, aryl, C 1-6 The alkoxy group and heterocyclic group are optionally selected from halide ions, C 1-4 Alkyl, C 3-6 One or more substituents of cycloalkyl, CF3, and OR9 are used, wherein each R9 is the same as or different from each other and is independently selected from hydrogen, C, and D in each occurrence. 1-4 Alkyl and hydroxyl protecting groups, - m is an integer of at least 3; and The at least one polysiloxane compound having formula (III) is grafted onto the at least one polymer P by reacting at least a portion of the -CH=CH2 portion of monomer M with the H-Si portion of a polysiloxane compound having formula (III).
38. The electrochemical single cell according to claim 37, wherein A is at least one selected from Al or B, Mg, Al, Nb, Ti, Y, W, S, Ba, Sr and Zr.
39. The electrochemical single cell according to claim 37 or 38, wherein the electrochemical single cell comprises at least one lithium salt selected from: LiTFSI, LiFSI, LiPF6, LiBF4 and LiClO4.
Citation Information
Patent Citations
Process for producing polyether polymer composition, polyether polymer composition, and solid electrolyte film
US7585934B2
Hydrophilic macromers and hydrogels comprising the same
CN104272142A
Polar polysiloxane electrolytes for lithium batteries
CN110997684A