High-elasticity sulfur-containing polymer electrolyte as well as preparation method and application thereof
By using high elastic sulfur-containing polymer electrolytes in lithium batteries, the problems of low ionic conductivity and insufficient mechanical strength of polymer electrolytes are solved, and the high energy density and stable circulation of lithium batteries at room temperature are achieved, which improves the battery's Safety performance and application prospects.
Patent Information
- Application Number
- CN202411331747.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-12-03
AI Technical Summary
The low room temperature ionic conductivity and low mechanical strength of existing polymer electrolytes limit the energy density and safety performance of lithium batteries, especially the problem of decreasing battery life under high temperature cycles.
Highly elastic sulfur-containing polymer electrolyte is used, which is formed by condensation reaction of thiol compounds, lithium salts, sulfur and fillers in organic solvents to form a solid electrolyte membrane with high ionic conductivity and toughness, which is suitable for all-solid lithium batteries.
It realizes high ionic conductivity, wide electrochemical stability window and good toughness of lithium-ion batteries at room temperature, enhances the charging and discharging capabilities and self-repair characteristics of lithium-ion batteries, reduces the solid-solid interface impedance of solid-state batteries, and improves the Cycle stability of the battery.
Smart Images

Figure CN119069788A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a highly elastic sulfur-containing polymer electrolyte and a preparation method and application technology thereof, belonging to the field of energy storage technology. Background Art
[0002] Battery energy storage is an important part of the development of new energy, especially in the context of a high proportion of renewable energy generation. It can solve problems such as the intermittent nature of new energy sources such as solar energy and wind energy, and reduce the impact of new energy on the power grid. In addition, power batteries are also the core components of pure electric vehicles, which have an important impact on the development of electric vehicles in my country. Therefore, the battery system occupies a core position in the development of new energy throughout the entire process from power generation to power consumption. Lithium batteries occupy a very high proportion in energy storage systems due to their good cycle performance and high specific capacity. At present, automotive power batteries are basically power lithium batteries, but commercial lithium batteries based on liquid organic electrolytes still have major safety risks, which is also a major reason for limiting the commercialization of lithium batteries with higher energy density.
[0003] In order to avoid the use of flammable liquid electrolytes to further improve the energy density and safety performance of lithium batteries, the development of solid electrolyte lithium battery technology is one of the most effective measures to solve the safety problems of lithium batteries and further improve their energy density. The current mainstream polymer solid electrolytes are mainly polyether and polyester. They have good toughness, good contact with the electrode interface, easy large-scale preparation, and good development prospects. However, their room temperature chain segment mobility is poor, there are major deficiencies in lithium ion conduction, and the mechanical strength is low. For example, the most commonly used polyethylene oxide (PEO) polymer electrolyte, the room temperature ionic conductivity is usually less than 10 -5 S / cm, it needs to be heated to 60°C to make it molten in order to operate. The requirement of high temperature cycle not only requires the battery to be equipped with an additional heating device, which greatly reduces the battery energy density, but also aggravates the interfacial side reactions, resulting in a decrease in the cycle life of the solid-state battery, which limits the further application of PEO polymer electrolytes. At present, a lot of work has been done to modify PEO due to its low ionic conductivity, such as introducing nanofillers and plasticizers, but these strategies are still not separated from the PEO polymer body, so it is difficult to significantly improve the ionic conductivity. Therefore, it is urgent to start from the polymer electrolyte segment structure and design and develop lithium-conducting polymer electrolytes with high segment mobility. Summary of the invention
[0004] Technical issues:
[0005] In view of the problems of low room temperature ionic conductivity and low mechanical strength of current polymer electrolytes, the present invention aims to provide a highly elastic sulfur-containing polymer electrolyte and its preparation method and application. The polymer electrolyte has high ionic conductivity, a wide electrochemical stability window and good toughness at room temperature, and has certain self-repairing properties, which can realize stable circulation of all-solid-state polymer lithium batteries at room temperature. The preparation method of the electrolyte is simple, low-cost, and conducive to large-scale production.
[0006] Technical solution: A highly elastic sulfur-containing polymer electrolyte, the raw materials of which are: thiol compounds, lithium salts, sulfur, organic solvents and fillers, wherein the amount of fillers added accounts for 0-20wt% of the total mass of the system, the molar ratio of thiol to sulfur is 1:1-1:10, and the concentration of lithium salt is 0.1mol / L-5.0mol / L; the raw materials are condensed with sulfur element in an organic solvent at a certain temperature to generate a highly elastic sulfur-containing polymer electrolyte solution, and a solid polymer electrolyte membrane is obtained after drying.
[0007] The thiol compound is a mixture of one or more of benzyl mercaptan, benzenethiol, isobutyl mercaptan, ethanethiol, 1,2-benzenedithiol, 1,2-ethanedithiol, 1,3-propanedithiol, 1,4-butanedithiol, 1,5-pentanedithiol, 1,6-hexanedithiol, 1,8-octanedithiol, 1,9-nonanedithiol, 1,10-decanedithiol, tetrakis(ethylene glycol)dithiol, 1,11-undecanedithiol, 2,2'-thiodiethanethiol, 2,2'-(ethylenedioxy)diethanethiol, and 4,4'-thiodibenzenethiol.
[0008] The lithium salt is a mixture of one or more of lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium nitrate, lithium tetrafluoroborate and lithium perchlorate.
[0009] The filler is alumina, silicon, silicon dioxide, zirconium dioxide, titanium dioxide, barium titanate, lithium nitride, garnet-type Li3La3Zr2O 12 (LLZO), LISICON type Li 14 ZnGe4O 16 , antiperovskite Li 2.88 PO 3.73 N 0.14 ; Perovskite-type Li 3x La 2 / 3-x□1 / 3-2x TiO3(LLTO), where 0﹤x﹤0.16, □ represents a vacancy, i.e. a missing position in the lattice; NASICON type Li 1.3 Al 0.3 Ti 1.7 (PO4)3(LATP); NASICON type Li 1+x Al x Ge2-x (PO4)3, where 0﹤x﹤0.5; sulfur-containing LISICON type Li 4-x Ge 1-x P x S4, wherein 0.08﹤x﹤0.42; antiperovskite Li3OX, wherein X=a mixture of one or more of F, Cl or Br.
[0010] The organic solvent is one or more of toluene, carbon disulfide, 1,3-dioxolane, tetrahydrofuran, ethylene glycol dimethyl ether, or a mixture thereof.
[0011] The method for preparing the highly elastic sulfur-containing polymer electrolyte comprises the following steps:
[0012] Step 1. Disperse the raw materials in an organic solvent and mix well to form a uniform liquid;
[0013] Step 2. adding sulfur, stirring and mixing at a certain temperature, and obtaining a clear liquid through a condensation reaction, which is the highly elastic sulfur-containing polymer electrolyte solution;
[0014] Step 3: Dry and solidify the sulfur-containing polymer electrolyte solution to obtain a sulfur-containing polymer solid electrolyte membrane.
[0015] The certain temperature is 0-120°C.
[0016] The electrolyte membrane preparation method is one of the following: casting method, blade coating method, electrostatic spinning and microfluidic spinning; the electrolyte membrane thickness is 5-200 μm.
[0017] An application of the highly elastic sulfur-containing polymer electrolyte in a lithium ion battery or a lithium metal battery.
[0018] A battery based on the highly elastic sulfur-containing polymer electrolyte, in which the positive electrode material is one of lithium iron phosphate, ternary material, lithium cobalt oxide, lithium manganese oxide, high-nickel cobalt-free material, lithium titanate, sulfur, oxygen, and air.
[0019] Beneficial effects:
[0020] The sulfur-containing polymer electrolyte provided by the present invention has a polysulfide skeleton with functional groups that can provide a fast channel for lithium ion transmission and has high ionic conductivity, which can reach 2.06×10 -4S / cm, and can be used in high-energy-density all-solid-state lithium batteries to enhance their charge and discharge capabilities. The rich polysulfide bonds give the electrolyte extremely high elasticity, effectively solving the problem of poor dynamic contact between the electrode / electrolyte interface in solid-state lithium batteries, reducing the solid-solid interface impedance, and the self-healing properties effectively ensure the long-term stability of the electrolyte structure. It can be used in lithium-ion batteries and lithium metal batteries with common positive electrode materials, with a wide range of applications, excellent application effects, and good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a physical picture of the sulfur-containing polymer electrolyte prepared in Example 17.
[0022] Figure 2 (a), (b), and (c) are the AC impedance spectra of the sulfur-containing polymer electrolytes prepared in Example 17, Example 11, and Comparative Example, respectively.
[0023] Figure 3 This is the linear sweep voltammogram of the sulfur-containing polymer electrolyte prepared in Example 17. DETAILED DESCRIPTION
[0024] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.
[0025] A highly elastic sulfur-containing polymer electrolyte uses a thiol compound as a raw material, and undergoes a condensation reaction with sulfur at a certain temperature in an organic solvent containing a lithium salt raw material composition that contains at least a thiol compound, a lithium salt, and an organic solvent to generate a highly elastic sulfur-containing polymer electrolyte solution, and then obtains a solid polymer electrolyte membrane after drying.
[0026] The thiol compound is a mixture of one or more of benzyl mercaptan, benzenethiol, isobutyl mercaptan, ethanethiol, 1,2-benzenedithiol, 1,2-ethanedithiol, 1,3-propanedithiol, 1,4-butanedithiol, 1,5-pentanedithiol, 1,6-hexanedithiol, 1,8-octanedithiol, 1,9-nonanedithiol, 1,10-decanedithiol, tetrakis(ethylene glycol)dithiol, 1,11-undecanedithiol, 2,2'-thiodiethanethiol, 2,2'-(ethylenedioxy)diethanethiol, 4,4'-thiodibenzenethiol, and the like.
[0027] The lithium salt is a mixture of one or more of lithium hexafluorophosphate (LiPF6), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium bisfluorosulfonyl imide (LiFSI), lithium nitrate (LiNO3), lithium tetrafluoroborate (LiBF4), and lithium perchlorate (LiClO4).
[0028] The raw material also contains fillers; the amount of the fillers added is 0-20wt% of the total mass ratio; the fillers are alumina, silicon, silicon dioxide, zirconium dioxide, titanium dioxide, barium titanate, lithium nitride, garnet-type Li3La3Zr2O 12 (LLZO), LISICON type Li 14 ZnGe4O 16 , antiperovskite Li 2.88 PO 3.73 N 0.14 , Perovskite-type Li 3x La 2 / 3-x□1 / 3-2x TiO3(LLTO), where 0﹤x﹤0.16, □ represents a vacancy, i.e. a missing position in the lattice, NASICON-type Li 1.3 Al 0.3 Ti 1.7 (PO4)3(LATP), NASICON type Li 1+x Al x Ge 2-x (PO4)3, where 0﹤x﹤0.5, sulfur-containing LISICON type Li 4-x Ge 1-x P x S4, wherein 0.08﹤x﹤0.42, antiperovskite-type Li3OX, wherein X=a mixture of one or more of F, Cl or Br.
[0029] The organic solvent is one or more of toluene, carbon disulfide, 1,3-dioxolane (DOL), tetrahydrofuran (THF), ethylene glycol dimethyl ether (DME), or a mixture thereof.
[0030] A method for synthesizing the above-mentioned sulfur-containing polymer electrolyte is provided, comprising the following steps:
[0031] 1. Evenly mix the mercaptan and the solvent, add sulfur powder, lithium salt and filler, mix and react thoroughly to obtain a polymer solution;
[0032] 2. Pour a certain amount of the polymer solution obtained in step 1 into a container, heat and dry it until it becomes solid to obtain the sulfur-containing polymer electrolyte.
[0033] According to the above scheme, the molar ratio of mercaptan to sulfur is 1:1-10.
[0034] According to the above scheme, the concentration of lithium salt is 0.1 mol / L-5.0 mol / L, preferably 0.5 mol / L-2.0 mol / L, and more preferably 0.8 mol / L-1.5 mol / L.
[0035] According to the above scheme, the amount of filler added accounts for 0.5-20wt% of the total mass ratio, preferably 0.5-10wt%, more preferably 0.5-3wt%.
[0036] According to the above scheme, the reaction temperature is 0-120°C, preferably 10-80°C, more preferably 20-60°C.
[0037] According to the above scheme, the electrolyte membrane preparation method is one of the following: casting, blade coating, electrospinning, and microfluidic spinning.
[0038] According to the above scheme, the thickness of the prepared electrolyte membrane is 5-200 μm, preferably 10-100 μm.
[0039] Provided is an application of the sulfur-containing polymer electrolyte in a lithium ion battery or a lithium metal battery.
[0040] A battery is provided, comprising the above-mentioned sulfur-containing polymer electrolyte.
[0041] According to the above scheme, the battery is a lithium ion battery or a lithium metal battery.
[0042] According to the above scheme, in the battery, the positive electrode material is one of lithium iron phosphate, ternary material, lithium cobalt oxide, lithium manganese oxide, high nickel cobalt-free material, lithium titanate, sulfur, oxygen, and air.
[0043] Comparative Example
[0044] Step 1: The sulfur-containing polymer electrolyte pEDDT was synthesized by the condensation reaction of 2,2'-(ethylenedioxy)diethanethiol (EDDT) and sulfur. 5mmol of 2,2'-(ethylenedioxy)diethanethiol (EDDT) and 200mg of LiTFSI were added to a vial containing 10mL of 1,3-dioxolane, sealed with a PE film, and magnetically stirred at 400rpm / min for 1h until the solution was clear and transparent. 5mmol of sublimated sulfur powder was slowly added at 60℃, and vigorously stirred at 800rpm / min for 2h to obtain a transparent yellow solution, which is the sulfur-containing polymer electrolyte solution.
[0045] Step 2: The solution was injected into a polytetrafluoroethylene culture dish and dried at 105° C. for 12 h to obtain an elastic solid polymer electrolyte membrane. The electrolyte membrane was cut into discs with a diameter of 15 mm.
[0046] Step 3: Weigh 3g S sublimated sulfur and 1g acetylene black, pour into an agate mortar and grind for 30 minutes until the two are fully mixed. The evenly mixed powder is introduced into a polytetrafluoroethylene liner, filled with Ar gas, placed in a reactor, sealed, and heat treated at 155°C for 12 hours to obtain a S / C composite positive electrode. Weigh 400mg S / C, 50mg PVDF, 50mg Super P, add 1.5mL N-methylpyrrolidone (NMP), and stir magnetically at 1000rpm / min for 3 hours to obtain a uniform slurry. Pour the slurry on a carbon-coated aluminum foil, spread it with a scraper, place it in a 60°C forced air oven and dry it for 3 hours, cut it into 12mm discs, and place it in a 60°C vacuum drying oven and dry it for 12 hours to obtain a sulfur positive electrode. The surface loading of the electrode is 2mg / cm 2 .
[0047] Step 4: In a glove box filled with argon, assemble a CR2025 button cell with a sulfur electrode as the positive electrode, a sulfur-containing polymer electrolyte membrane as the electrolyte membrane, and a lithium metal sheet as the negative electrode.
[0048] Step 5: The electrolyte membrane obtained in this example was used to form a symmetrical battery CR2032 in a stainless steel / electrolyte membrane / stainless steel blocking cell configuration, and an AC impedance test was performed at a frequency range of 0.01-100000 Hz and a sinusoidal amplitude of 5 mV. The ionic conductivity was calculated using the following formula.
[0049] σ=L / (A·R b )
[0050] Where: σ—ion conductivity (S / cm); L—diaphragm test thickness (cm); A—contact area between diaphragm and stainless steel sheet (cm 2 );R b —Body resistance (Ω) that can be read at the intersection of the X-axis.
[0051] The calculated ionic conductivity of the comparative electrolyte membrane at 30°C is 6.79×10 -5 S / cm.
[0052] The preparation steps of each embodiment are consistent with those of the comparative example, and only the corresponding materials need to be replaced. The comparison of the embodiment formula and the corresponding ion conductivity is shown in Table 1.
[0053] Table 1 Formulas of each case and corresponding ionic conductivity
[0054]
[0055]
[0056] From the comparison between Examples 1-3 and the comparative example, we can see that the lithium salt LiTFSI performs better than LiFSI, LiPF6 and LiClO4.
[0057] From the comparison between Examples 4-6 and the comparative example, we can see that the thiol compound 2,2'-(ethylenedioxy)diethylthiol (EDDT) performs better than 2-benzenedithiol (BDT), 4,4'-thiodibenzenethiol (TBBT) and 1,2-ethanedithiol (EDT).
[0058] From the comparison between Examples 7-9 and the comparative example, we can see that the organic solvent 1,3-dioxolane performs better than toluene / carbon disulfide mixed solution (volume ratio 1:1), tetrahydrofuran (THF) and ethylene glycol dimethyl ether (DME).
[0059] From the comparison between Examples 10-13 and the comparative example, we can see that after adding fillers, the ionic conductivity of the polymer electrolyte membrane is further improved, and the effect of Al2O3 fillers is relatively good.
[0060] Examples 14 and 15 further explored the effect of the amount of filler added on the experimental results. The results showed that under the experimental conditions, the effect of adding 10 mg of filler was relatively good.
[0061] Examples 16-18 tested the effects of different ratios of thiol to sulfur on ionic conductivity. From the test results, it can be seen that a molar ratio of thiol to sulfur of 1:3 exhibited the best ionic conductivity among all the test results.
[0062] Figure 1 This is a physical picture of the polymer electrolyte prepared in Example 17, which shows that the sulfur-containing polymer electrolyte has a uniform and dense morphology and a thickness of 80 μm.
[0063] Figure 2 (a) is the AC impedance spectrum of the polymer electrolyte prepared in Example 17. The figure shows that the bulk resistance of the sulfur-containing polymer electrolyte at 30°C is only 22Ω, and the calculated ionic conductivity is 2.06×10 -4 S / cm.
[0064] Figure 3 This is the linear sweep voltammetry spectrum of the polymer electrolyte prepared in Example 17. The figure shows that the electrochemical stability window of the sulfur-containing polymer electrolyte at 30°C is 4.3V.
[0065] The above descriptions are only some embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A highly elastic sulfur-containing polymer electrolyte, characterized in that: The raw materials are composed of thiol compounds, lithium salts, sulfur, organic solvents and fillers, wherein the amount of fillers added accounts for 0-20wt% of the total mass of the system, the molar ratio of thiol to sulfur is 1:1-10, and the concentration of lithium salt is 0.1mol / L-5.0mol / L; the raw materials are condensed with sulfur element in an organic solvent at a certain temperature to generate a high-elastic sulfur-containing polymer electrolyte solution, and a solid polymer electrolyte membrane is obtained after drying.
2. The highly elastic sulfur-containing polymer electrolyte according to claim 1, characterized in that: The thiol compound is a mixture of one or more of benzyl mercaptan, benzenethiol, isobutyl mercaptan, ethanethiol, 1,2-benzenedithiol, 1,2-ethanedithiol, 1,3-propanedithiol, 1,4-butanedithiol, 1,5-pentanedithiol, 1,6-hexanedithiol, 1,8-octanedithiol, 1,9-nonanedithiol, 1,10-decanedithiol, tetrakis(ethylene glycol)dithiol, 1,11-undecanedithiol, 2,2'-thiodiethanethiol, 2,2'-(ethylenedioxy)diethanethiol, and 4,4'-thiodibenzenethiol.
3. The highly elastic sulfur-containing polymer electrolyte according to claim 1, characterized in that: The lithium salt is a mixture of one or more of lithium hexafluorophosphate, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium nitrate, lithium tetrafluoroborate and lithium perchlorate.
4. The highly elastic sulfur-containing polymer electrolyte according to claim 1, characterized in that: The filler is alumina, silicon, silicon dioxide, zirconium dioxide, titanium dioxide, barium titanate, lithium nitride, garnet-type Li3La3Zr2O 12 (LLZO), LISICON type Li 14 ZnGe4O 16 , antiperovskite Li 2.88 PO 3.73 N 0.14 ; Perovskite-type Li 3x La 2 / 3-x□1 / 3-2x TiO3(LLTO), where 0﹤x﹤0.16, □ represents a vacancy, i.e. a missing position in the lattice; NASICON type Li 1.3 Al 0.3 Ti 1.7 (PO4)3(LATP); NASICON type Li 1+x Al x Ge 2-x (PO4)3, where 0﹤x﹤0.5; sulfur-containing LISICON type Li 4-x Ge 1-x P x S4, wherein 0.08﹤x﹤0.42; antiperovskite Li3OX, wherein X=a mixture of one or more of F, Cl or Br.
5. The highly elastic sulfur-containing polymer electrolyte according to claim 1, characterized in that: The organic solvent is one or more of toluene, carbon disulfide, 1,3-dioxolane, tetrahydrofuran, ethylene glycol dimethyl ether, or a mixture thereof.
6. A method for preparing the highly elastic sulfur-containing polymer electrolyte according to any one of claims 1 to 5, characterized in that: The following steps are involved: Step 1. Disperse the raw materials in an organic solvent and mix well to form a uniform liquid; Step 2. adding sulfur, stirring and mixing at a certain temperature, and obtaining a clear liquid through a condensation reaction, which is the highly elastic sulfur-containing polymer electrolyte solution; Step 3: Dry and solidify the sulfur-containing polymer electrolyte solution to obtain a sulfur-containing polymer solid electrolyte membrane.
7. The method for preparing a highly elastic sulfur-containing polymer electrolyte according to claim 6, characterized in that: The certain temperature is 0-120°C.
8. The method for preparing a highly elastic sulfur-containing polymer electrolyte according to claim 6, characterized in that: The electrolyte membrane preparation method is one of the following: casting method, blade coating method, electrostatic spinning and microfluidic spinning; the thickness of the electrolyte membrane is 5-200 μm.
9. Use of the highly elastic sulfur-containing polymer electrolyte according to any one of claims 1 to 5 in a lithium ion battery or a lithium metal battery.
10. A battery based on the highly elastic sulfur-containing polymer electrolyte according to any one of claims 1 to 7, characterized in that: In the battery, the positive electrode material is one of lithium iron phosphate, ternary material, lithium cobalt oxide, lithium manganese oxide, high nickel cobalt-free material, lithium titanate, sulfur, oxygen and air.
Citation Information
Cited By
Sulfur-containing all-solid-state polymer electrolyte membrane, preparation method and lithium metal battery
CN120999103A
Self-repairing sulfur-containing polymer electrolyte membrane for lithium battery as well as preparation method and application of self-repairing sulfur-containing polymer electrolyte membrane
CN121035329A
Self-repairing sulfur-containing polymer electrolyte membrane for lithium battery and preparation method and application thereof
CN121035329B