An easy-to-clean photocurable resin, its preparation method and application

By combining silicone resin prepolymer and modified composite fiber, an easy-to-clean photocurable resin is prepared, which solves the problems of insufficient mechanical properties and poor cleanability of photocurable resins in the prior art. It achieves rapid curing and high stability, and is suitable for 3D printing and other applications.

CN117024698BActive Publication Date: 2026-11-10SHENZHEN ELEGOO TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202310821573.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-06
Publication Date
2026-11-10
Estimated Expiration
2043-07-06

AI Technical Summary

Technical Problem

Existing photocurable resins have problems in 3D printing, such as insufficient mechanical properties after curing, high internal stress, high brittleness, poor impact resistance and poor heat resistance, and are difficult to clean, which affects their application in different fields.

Method used

An easy-to-clean photocurable resin is prepared by using silicone resin prepolymer and modified composite fiber in a specific ratio and process. The resin formulation is optimized by combining hydrophilic chain extenders, catalysts and other components to improve mechanical properties and cleanability.

Benefits of technology

It achieves rapid curing, low shrinkage, good stability and easy cleaning of photocurable resins, making it suitable for multiple applications and improving the accuracy and efficiency of 3D printed products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention relates to an easy-to-clean photocurable resin, its preparation method, and its applications. The raw materials for the photocurable resin of this invention include: an organosilicon resin prepolymer, a polyol, isocyanate, a catalyst, a hydrophilic chain extender, a small molecule chain extender, modified composite fibers, a polymerization inhibitor, a photoinitiator, 1,3-propanediol dimethacrylate, neopentyl glycol diacrylate, and polydipentaerythritol hexaacrylate. The organosilicon resin prepolymer is prepared from vinyltrimethoxysilane, styrene ethyltrimethoxysilane, and phenylethynyltrimethylsilane. The modified composite fibers are prepared from glass fibers with a length of 0.6 mm, short-cut carbon fibers with a length of 0.1 mm, and short-cut carbon fibers with a length of 2 mm. The photocurable resin of this invention exhibits good dispersion performance, excellent mechanical properties, short curing time, high temperature resistance and stability, is environmentally friendly, and easy to clean. It can be used in medical, aerospace, artificial intelligence, and building materials fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of 3D printing technology, specifically relating to an easy-to-clean photocurable resin, its preparation method, and its application. Background Technology

[0002] 3D printing, a rapidly developing rapid prototyping technology, is increasingly being applied in aerospace, mechanical electronics, transportation, and biomedicine due to its high performance, complexity, precision, and high degree of personalization. In recent years, my country has made significant progress in the research of photopolymer 3D printing equipment. However, with advancements in equipment and the maturation of processes, increasingly stringent requirements have been placed on photopolymer resins, such as faster curing rates, lower shrinkage rates, and more diverse functions to suit different scenarios. By optimizing resin formulations, modifying molecular structures, and adding modified fillers, the performance of photopolymer resins can be significantly improved, enhancing the diversity of applications for photopolymer 3D printing technology and greatly promoting its application.

[0003] Currently, photocurable resins suffer from insufficient or excessive crosslinking density, leading to inadequate mechanical properties after curing, or defects such as high internal stress, brittleness, poor impact resistance, and poor heat resistance due to crosslinking. Therefore, they are difficult to meet the application requirements of 3D printing curing technology. For example, Chinese patent CN110156937A discloses a method for preparing a photosensitive resin reinforced with short-cut carbon fibers. This method involves preparing an acrylate oligomer from short-cut carbon fibers, a small amount of nano-silica, a coupling agent, and acrylate oligomers. The acrylate oligomer is then further mixed with active monomers, anti-settling agents, and defoamers to obtain the photosensitive resin. The resin product obtained by this patent has high toughness, but it requires the addition of certain additives to ensure uniform dispersion of the mixture, increasing cost and industrialization difficulty. Another example is Chinese patent CN111040388A, which discloses a composite photosensitive resin material for 3D printing and its preparation method. CN114874435A discloses a washable photocurable 3D printing resin and its preparation method. This patent technology improves 3D printing efficiency to a certain extent. The mechanical properties of the printing resin have been improved, enhancing its strength and toughness. However, the resin has a long curing time and low curing efficiency, resulting in low precision. Furthermore, the resin remains difficult to clean. Chinese patent CN113045715A discloses a washable, high-temperature resistant, and conductive 3D printing photocurable material and its printing process. This 3D printing photocurable material incorporates metallic fillers and biomimetic nano-silica. While this cured material exhibits excellent conductivity and improves mechanical properties and impact resistance to some extent, its curing rate is low. The addition of metallic fillers and biomimetic nano-silica makes it difficult to disperse the mixture evenly, leading to precipitation after prolonged use. Therefore, dispersants and anti-settling agents are needed, increasing costs and industrialization difficulties.

[0004] In conclusion, there is still a long way to go in the application of current 3D printing photopolymer materials. Developing a 3D printing curing material with good mechanical properties, high impact resistance, high stability, short curing time, good water washability, and easy cleaning will enable 3D printed products to achieve high precision and efficiency, and can be widely used in various fields. Summary of the Invention

[0005] To address the problems existing in the prior art, this invention provides an easy-to-clean photocurable resin, its preparation method, and its application. The easy-to-clean photocurable resin of this invention has a short curing time, good mechanical properties and stability, good water washability, is easy to clean, has a wide range of applications, and has good application prospects.

[0006] In a first aspect, the present invention provides an easy-to-clean photocurable resin, wherein the raw materials of the photocurable resin include: organosilicon resin prepolymer, polyol, isocyanate, catalyst, hydrophilic chain extender, small molecule chain extender, modified composite fiber, polymerization inhibitor, photoinitiator, 1,3-propanediol dimethacrylate, neopentyl glycol diacrylate, and polydipentaerythritol hexaacrylate.

[0007] Furthermore, the organosilicon resin prepolymer is prepared from vinyltrimethoxysilane, styreneethyltrimethoxysilane, and phenylethynyltrimethylsilane;

[0008] Furthermore, the modified composite fiber is prepared from glass fiber with a length of 0.6 mm, chopped carbon fiber with a length of 0.1 mm, and chopped carbon fiber with a length of 2 mm.

[0009] Further, the photocurable resin comprises the following raw materials in parts by weight: 0.01-4 parts of silicone resin prepolymer, 1-40 parts of polyol, 5-10 parts of isocyanate, 0.01-2 parts of catalyst, 1-5 parts of hydrophilic chain extender, 1-10 parts of small molecule chain extender, 1-10 parts of modified composite fiber, 0.01-0.5 parts of polymerization inhibitor, 1-10 parts of photoinitiator, 5-15 parts of 1,3-propanediol dimethacrylate, 5-15 parts of neopentyl glycol diacrylate, and 5-20 parts of polydipentaerythritol hexaacrylate.

[0010] Furthermore, the polypolyol is composed of polyoxypropylene ether diol and polyether polyol MN-3050D in a mass ratio of 1:(1-3).

[0011] Furthermore, the molecular weight of the polyoxypropylene ether diol is 400-4000D.

[0012] Furthermore, the mass ratio of the glass fiber with a length of 0.6 mm, the short carbon fiber with a length of 0.1 mm, and the short carbon fiber with a length of 2 mm is (0.01~0.1):1:(0.05~0.5).

[0013] Further, the hydrophilic chain extender is one or a combination of N,N-di(2-hydroxyethyl)-2-aminoethanesulfonate sodium salt, aminoethylaminoethanesulfonate sodium salt, 2,2-dimethylolpropionic acid, dimethylolbutyric acid, dimethylolpropionic acid, and trimethylolpropane; the small molecule chain extender is selected from one or a combination of neopentyl glycol, 1,4-butanediol, and glycerol.

[0014] Further, the coupling agent is selected from A-151, A-171, A-172, KH-570γ, or KH-550R; the isocyanate is selected from one of dicyclohexane diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, isophorone diisocyanate, diphenylmethane 4,4'-diisocyanate, hexamethylene diisocyanate, methylcyclohexyl diisocyanate, 2,2,4-trimethylhexane diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, and toluene diisocyanate; the catalyst is selected from... The self-use dibutyltin dilaurate and stannous octoate are selected from one of the following: the polymerization inhibitor is selected from one or a combination of p-methoxyphenol, hydroquinone, p-hydroxyanisole, p-benzoquinone, methyl hydroquinone, 2,6-di-tert-butyl-p-cresol, and resorcinol; the photoinitiator is selected from one of 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholino)-1-propanone, 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone, and 2-hydroxy-2-methyl-1-phenylpropanone.

[0015] Further, the preparation method of the organosilicon resin prepolymer is as follows: vinyltrimethoxysilane, styreneethyltrimethoxysilane and phenylethynyltrimethylsilane are dissolved in an acidic catalyst solution, heated to carry out the reaction, cooled after the reaction is completed, separated into liquids, and the organic phase is washed to neutral. Then the water in the organic phase is dried, filtered, and the filtrate is concentrated to obtain the organosilicon resin prepolymer.

[0016] Secondly, the present invention also provides a method for preparing an easy-to-clean photocurable resin, comprising the following steps:

[0017] S1. Mix the composite fiber with a coupling agent and heat-treat to obtain the modified composite fiber;

[0018] S2. Add the polyol, isocyanate and catalyst to a reactor equipped with a condenser, and heat to 60-90°C for 1-3 hours.

[0019] S3. Continue to add hydrophilic chain extender, small molecule chain extender and polymerization inhibitor to the reactor, and carry out the reaction at 60-80℃.

[0020] S4. Add organosilicon resin prepolymer, modified composite fiber, 1,3-propanediol dimethacrylate, neopentyl glycol diacrylate, pentaerythritol hexaacrylate, and photoinitiator to step S2 and react at 60-90°C to obtain an easy-to-clean photocurable resin.

[0021] Fourthly, the present invention also provides an application of an easy-to-clean photocurable resin, the application of which includes, but is not limited to, 3D printing, medical, aerospace, artificial intelligence, building materials and other fields.

[0022] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0023] (1) The easy-to-clean photocurable resin of the present invention uses a newly synthesized organosilicon resin prepolymer. The addition of the prepolymer significantly increases the mechanical properties of the 3D printing resin, reduces the curing time of the 3D printing resin, and improves the cleanability and stability of the 3D printed surface.

[0024] (2) By adding a newly synthesized organosilicon resin prepolymer and modified composite fiber, the present invention balances the hydrophilicity and hydrophobicity of the photocurable resin, so that the resin has good washability and cleanability at the same time, with a water contact angle of 87° to 104°, which significantly improves the washability of the resin and reduces the accumulation of pollutants such as dust and oil during use, thus significantly reducing the degree of surface contamination.

[0025] (3) The easy-to-clean photocurable resin of the present invention has a heat distortion temperature of 261 to 291°C and can be used at 200°C for 9.5 to 15 hours, maintaining good heat resistance and stability.

[0026] (4) The easy-to-clean photocurable resin of the present invention has good dispersibility and compatibility, and can maintain good molding performance without adding additives. The obtained resin has excellent mechanical properties, fast curing speed, low curing shrinkage rate during printing process of 2.4 to 3.2%, and high stability. Detailed Implementation

[0027] Unless otherwise specified, the experimental methods described in the following embodiments of the present invention are generally performed under conventional conditions or as recommended by the manufacturer. All commonly used chemical reagents used in the embodiments are commercially available products.

[0028] Unless otherwise defined, all technical and scientific terms used in this invention have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used in this specification is for the purpose of describing particular embodiments only and is not intended to limit the invention.

[0029] The terms "comprising" and "having," and any variations thereof, are intended to cover non-exclusive inclusion. For example, a process, method, apparatus, product, or device that includes a series of steps is not limited to the steps or modules listed, but may optionally include steps not listed, or may optionally include other steps inherent to such process, method, product, or device.

[0030] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to specific embodiments. It should be understood that these descriptions are merely exemplary and not intended to limit the scope of the invention. Furthermore, descriptions of well-known structures and technologies are omitted in the following description to avoid unnecessarily obscuring the concepts of the invention.

[0031] The following embodiments further describe the present invention, but these embodiments are not intended to limit the scope of protection of the present invention.

[0032] Example 1: Preparation of Organosilicon Resin Prepolymer

[0033] The specific preparation steps of the organosilicon resin prepolymer in this embodiment are as follows:

[0034] At room temperature, 45g of vinyltrimethoxysilane, 12g of styreneethyltrimethoxysilane, and 15g of phenylethynyltrimethylsilane were slowly added dropwise to 95mL of sulfuric acid solution (1wt%). After the addition was complete, the temperature was raised to 55℃ and reacted for 1h, then raised to 80℃ and reacted for 4h. After the reaction was completed, the temperature was lowered to room temperature, allowed to stand, and separated. The organic phase was washed with water until neutral, and then anhydrous magnesium sulfate was added to the organic phase to dry the water. The mixture was filtered, and the filtrate was concentrated to obtain the organosilicon resin prepolymer.

[0035] In subsequent embodiments of the present invention, the silicone resin prepolymers in the easy-to-clean photocurable resins prepared are all the silicone resin prepolymers prepared in this embodiment.

[0036] Example 2: Preparation of an easy-to-clean photocurable resin

[0037] The specific preparation steps for the easy-to-clean photocurable resin prepared in this embodiment are as follows:

[0038] S1. 0.1g of glass fiber (0.6mm in length), 7.5g of chopped carbon fiber (0.1mm in length) and 0.4g of chopped carbon fiber (2mm in length) were dried at 105℃, and then placed in a mixer and mixed at 1000r / min for 15min. Then 0.15g of A-172 (vinyltris(β-methoxyethoxy)silane, purchased from Nanjing Xiangqian Chemical Co., Ltd.) was added, heated to 120℃, and mixed at 2500r / min for 15min to obtain modified composite fiber.

[0039] S2. Add 20g of polyoxypropylene ether glycol 400D, 20g of MN-3050D, 10g of hexamethylene diisocyanate and 0.3g of dibutyltin dilaurate to a reactor equipped with a condenser, and heat to 80℃ for 3h.

[0040] S3. Continue to add 2g of sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, 7g of neopentyl glycol, and 0.2g of p-methoxyphenol to the reaction vessel, and control the temperature at 65℃ for 4h.

[0041] S4. Add 0.1g of silicone resin prepolymer, 6g of modified composite fiber, 5g of 1,3-propanediol dimethacrylate, 15g of neopentyl glycol diacrylate, 12g of pentaerythritol hexaacrylate, and 6g of 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholino)-1-propanone to step S2 and react at 80°C for 2 hours to obtain an easy-to-clean photocurable resin.

[0042] Example 3: Preparation of an easy-to-clean photocurable resin

[0043] The specific preparation steps for the easy-to-clean photocurable resin prepared in this embodiment are as follows:

[0044] S1. Dry 0.5g of glass fiber (0.6mm in length), 6g of chopped carbon fiber (0.1mm in length) and 1.5g of chopped carbon fiber (2mm in length) at 105℃, then place them in a mixer and mix at 1000r / min for 15min. Then add 0.15g of A-172 (vinyltris(β-methoxyethoxy)silane, purchased from Nanjing Xiangqian Chemical Co., Ltd.), heat to 120℃, and mix at 2500r / min for 15min to obtain modified composite fiber.

[0045] S2. Add 10g of polyoxypropylene ether glycol 1000D, 30g of MN-3050D, 5g of hexamethylene diisocyanate and 0.05g of dibutyltin dilaurate to a reactor equipped with a condenser, and heat to 80℃ for 3 hours.

[0046] S3. Continue to add 5g of sodium N,N-di(2-hydroxyethyl)-2-aminoethanesulfonate, 4g of neopentyl glycol, and 0.1g of p-methoxyphenol to the reaction vessel, and control the temperature at 65℃ for 4h.

[0047] S4. Add 1.2g of silicone resin prepolymer, 6g of modified composite fiber, 12g of 1,3-propanediol dimethacrylate, 15g of neopentyl glycol diacrylate, 10g of pentaerythritol hexaacrylate, and 5g of 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholino)-1-propanone to step S2 and react at 80°C for 2 hours to obtain an easy-to-clean photocurable resin.

[0048] Example 4: Preparation of an easy-to-clean photocurable resin

[0049] The specific preparation steps for the easy-to-clean photocurable resin prepared in this embodiment are as follows:

[0050] S1. Dry 0.5g of glass fiber (0.6mm in length), 5g of chopped carbon fiber (0.1mm in length) and 2.5g of chopped carbon fiber (2mm in length) at 105℃, then place them in a mixer and mix at 1000r / min for 15min. Then add 0.15g of A-172 (vinyltris(β-methoxyethoxy)silane, purchased from Nanjing Xiangqian Chemical Co., Ltd.), heat to 120℃, and mix at 2500r / min for 15min to obtain modified composite fiber.

[0051] S2. Add 18g of polyoxypropylene ether diol 2000D, 22g of MN-3050D, 5g of hexamethylene diisocyanate and 0.1g of dibutyltin dilaurate to a reactor equipped with a condenser, and heat to 80℃ for 3 hours.

[0052] S3. Continue to add 3.5g of sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, 5.5g of neopentyl glycol, and 0.1g of p-methoxyphenol to the reaction vessel, and control the temperature at 70℃ for 4 hours.

[0053] S4. Add 1.8g of silicone resin prepolymer, 6g of modified composite fiber, 8g of 1,3-propanediol dimethacrylate, 10g of neopentyl glycol diacrylate, 18g of pentaerythritol hexaacrylate, and 5.5g of 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholino)-1-propanone to step S2 and react at 80°C for 2 hours to obtain an easy-to-clean photocurable resin.

[0054] Example 5: Preparation of an easy-to-clean photocurable resin

[0055] The specific preparation steps for the easy-to-clean photocurable resin prepared in this embodiment are as follows:

[0056] S1. Dry 2g of glass fiber (0.6mm in length), 4g of chopped carbon fiber (0.1mm in length) and 2g of chopped carbon fiber (2mm in length) at 105℃, then place them in a mixer and mix at 1000r / min for 15min. Then add 0.15g of A-172 (vinyltris(β-methoxyethoxy)silane, purchased from Nanjing Xiangqian Chemical Co., Ltd.), heat to 120℃, and mix at 2500r / min for 15min to obtain modified composite fiber.

[0057] S2. Add 15g of polyoxypropylene ether glycol, 25g of MN-3050D, 5g of hexamethylene diisocyanate and 0.1g of dibutyltin dilaurate to a reactor equipped with a condenser, and heat to 80°C for 3 hours.

[0058] S3. Continue to add 4g of sodium N,N-di(2-hydroxyethyl)-2-aminoethanesulfonate, 5g of neopentyl glycol, and 0.2g of p-methoxyphenol to the reaction vessel, and control the temperature at 70℃ for 4h.

[0059] S4. Add 3.7g of silicone resin prepolymer, 6g of modified composite fiber, 14g of 1,3-propanediol dimethacrylate, 10g of neopentyl glycol diacrylate, 12g of pentaerythritol hexaacrylate, and 3.5g of 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholino)-1-propanone to step S2 and react at 80°C for 2 hours to obtain an easy-to-clean photocurable resin.

[0060] Experimental Example 1: Performance Testing of Easy-to-Clean UV-Cure Resins

[0061] The four groups of easy-to-clean photocurable resins prepared in Examples 2-5 were added to a DLP printer and cured at 405nm to obtain four groups of standard test samples. The performance of the four groups of samples was tested, and the test indicators are as follows:

[0062] (1) Curing time: The time required for curing was recorded when the resin began to cure by using a printer to expose the resin. The curing time of the light-cured resin was measured 5 times and the average value was taken.

[0063] (2) Mechanical properties: The test was conducted in accordance with GB / T 1040.3-2006 (dumbbell sample: L=115mm, r=20mm, b2=20, h=mm; tensile speed was 50mm / min). The test temperature was room temperature. The same sample was tested 5 times in different batches and the average value was taken.

[0064] (3) Impact strength: The test was conducted in accordance with GB / T 1043.1-2008 (sample size is 80mm×10mm×4mm). The test temperature was room temperature. The same sample was tested 5 times in different batches and the average value was taken.

[0065] (4) Contact angle: The water contact angle was measured using an OCA20 contact angle meter;

[0066] (5) Hardness: The hardness of the cured sample was tested using a Shore D hardness tester in accordance with GB / T531-1999. The test temperature was room temperature. The same sample was tested 5 times in different batches and the average value was taken.

[0067] (6) Curing shrinkage rate: The density ρ1 before printing and curing was determined at room temperature using the specific gravity bottle method. Specifically, a 25mL specific gravity bottle was cleaned and dried, weighed three times on a balance and the average value was taken. Then, distilled water was added to the specific gravity bottle, and the bottle was weighed three times again and the average value was taken. The distilled water was poured off and the bottle was dried. The prepared resin was added, and the bottle was weighed three times and the average value was taken. The formula for calculating ρ1 is shown in (1):

[0068]

[0069] In the formula, ρ0 is the density of distilled water (g / cm³). 3 m0 is the mass of the specific gravity bottle (g), m1 is the mass of the specific gravity bottle and distilled water (g), and m2 is the total mass of the specific gravity bottle and resin (g).

[0070] The resin system was then placed in a printer to print a 50mm×50mm×4mm model. The density ρ2 of the cured resin system was tested, and the curing shrinkage rate S was calculated using equation (2). v :

[0071]

[0072] In the formula, ρ1 is the density before curing (g / cm³). 3 ), ρ2 is the density after curing (g / cm³) 3 ).

[0073] (7) Heat distortion temperature: The heat distortion temperature was determined using a heat distortion Vicat temperature tester. The test load was 1.8 MPa. Five parallel tests were performed, and the average value was taken.

[0074] (8) Thermal stability: The time it takes for the resin to remain stable without deformation when used at 200℃ is measured.

[0075] According to the above test methods, the performance test results of the easy-to-clean photocurable resins in Examples 2-5 are shown in Table 1.

[0076] Table 1:

[0077]

[0078]

[0079] As shown in Table 1, the four groups of easy-to-clean photocurable resins prepared in this invention exhibit excellent mechanical properties, with tensile strength, elongation at break, and impact strength ranging from 30.45 to 37.06 MPa, 3.14 to 4.21%, and 12.36 to 15.71 KJ / m, respectively. 2The curing time is only 3-6 seconds, with a fast curing speed and a hardness of 92-102 HD. The curing shrinkage rate during printing is as low as 2.4-3.2%, indicating that the easily cleanable resin of this invention has high stability. In addition, the water contact angle is 87°-104°, which significantly improves the water washing performance and reduces the accumulation of contaminants such as dust and oil during use, significantly reducing the degree of surface contamination. The easily cleanable photocurable resin of this invention has a heat distortion temperature of 261-291°C and can be used at 200°C for 9.5-15 hours, demonstrating excellent stability. In summary, the overall performance of Example 4 of this invention is the best.

[0080] Comparative Example 1

[0081] The specific preparation steps of the resin prepared in this comparative example are as follows:

[0082] S1. Dry 0.5g of glass fiber (0.6mm in length), 5g of chopped carbon fiber (0.1mm in length) and 2.5g of chopped carbon fiber (2mm in length) at 105℃, then place them in a mixer and mix at 1000r / min for 15min. Then add 0.15g of A-172, heat to 120℃, and mix at 2500r / min for 15min to obtain modified composite fiber.

[0083] S2. Add 18g of polyoxypropylene ether glycol 1000D, 22g of MN-3050D, 5g of hexamethylene diisocyanate and 0.1g of dibutyltin dilaurate to a reactor equipped with a condenser, and heat to 80℃ for 3h.

[0084] S3. Continue to add 3.5g of sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, 5.5g of neopentyl glycol, and 0.1g of p-methoxyphenol to the reaction vessel, and control the temperature at 70℃ for 4 hours.

[0085] S4. Add 6g of modified composite fiber, 8g of 1,3-propanediol dimethacrylate, 10g of neopentyl glycol diacrylate, 18g of pentaerythritol hexaacrylate, and 5.5g of 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholino)-1-propanone to step S2 and react at 80℃ for 2h to obtain resin.

[0086] Comparative Example 2

[0087] The specific preparation steps of the resin prepared in this comparative example are as follows:

[0088] S1. Dry 0.5g of glass fiber (0.6mm in length), 5g of chopped carbon fiber (0.1mm in length) and 2.5g of chopped carbon fiber (2mm in length) at 105℃, then place them in a mixer and mix at 1000r / min for 15min. Then add 0.15g of A-172, heat to 120℃, and mix at 2500r / min for 15min to obtain modified composite fiber.

[0089] S2. Add 18g of polyoxypropylene ether glycol 1000D, 22g of MN-3050D, 5g of hexamethylene diisocyanate and 0.1g of dibutyltin dilaurate to a reactor equipped with a condenser, and heat to 80℃ for 3h.

[0090] S3. Continue to add 3.5g of sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, 5.5g of neopentyl glycol, and 0.1g of p-methoxyphenol to the reaction vessel, and control the temperature at 70℃ for 4 hours.

[0091] S4. Add 6g of silicone resin prepolymer, 6g of modified composite fiber, 8g of 1,3-propanediol dimethacrylate, 10g of neopentyl glycol diacrylate, 18g of pentaerythritol hexaacrylate, and 5.5g of 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholino)-1-propanone to step S2 and react at 80℃ for 2h to obtain the resin.

[0092] Comparative Example 3

[0093] The specific preparation steps of the resin prepared in this comparative example are as follows:

[0094] S1. Dry 0.5g of glass fiber (0.6mm in length), 5g of chopped carbon fiber (0.1mm in length) and 2.5g of chopped carbon fiber (2mm in length) at 105℃, then place them in a mixer and mix at 1000r / min for 15min. Then add 0.15g of A-172, heat to 120℃, and mix at 2500r / min for 15min to obtain modified composite fiber.

[0095] S2. Add 40g of polyoxypropylene ether glycol 1000D, 5g of hexamethylene diisocyanate and 0.1g of dibutyltin dilaurate to a reactor equipped with a condenser, and heat to 80℃ for 3h.

[0096] S3. Continue to add 3.5g of sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, 5.5g of neopentyl glycol, and 0.1g of p-methoxyphenol to the reaction vessel, and control the temperature at 70℃ for 4 hours.

[0097] S4. Add 1.8g of silicone resin prepolymer, 6g of modified composite fiber, 8g of 1,3-propanediol dimethacrylate, 10g of neopentyl glycol diacrylate, 18g of pentaerythritol hexaacrylate, and 5.5g of 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholino)-1-propanone to step S2 and react at 80℃ for 2h to obtain the resin.

[0098] Comparative Example 4

[0099] The specific preparation steps of the resin prepared in this comparative example are as follows:

[0100] S1. Dry 0.5g of glass fiber (0.6mm in length), 5g of chopped carbon fiber (0.1mm in length) and 2.5g of chopped carbon fiber (2mm in length) at 105℃, then place them in a mixer and mix at 1000r / min for 15min. Then add 0.15g of A-172, heat to 120℃, and mix at 2500r / min for 15min to obtain modified composite fiber.

[0101] S2. Add 18g of polyoxypropylene ether glycol 1000D, 22g of polyoxypropylene glycol (molecular weight 1000), 5g of hexamethylene diisocyanate and 0.1g of dibutyltin dilaurate to a reaction vessel equipped with a condenser, and heat to 80°C for 3 hours.

[0102] S3. Continue to add 3.5g of sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, 5.5g of neopentyl glycol, and 0.1g of p-methoxyphenol to the reaction vessel, and control the temperature at 70℃ for 4 hours.

[0103] S4. Add 1.8g of silicone resin prepolymer, 6g of modified composite fiber, 8g of 1,3-propanediol dimethacrylate, 10g of neopentyl glycol diacrylate, 18g of pentaerythritol hexaacrylate, and 5.5g of 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholino)-1-propanone to step S2 and react at 80℃ for 2h to obtain the resin.

[0104] Comparative Example 5

[0105] The specific preparation steps of the resin prepared in this comparative example are as follows:

[0106] S1. Dry 0.5g of glass fiber (0.6mm in length), 5g of chopped carbon fiber (0.1mm in length) and 2.5g of chopped carbon fiber (2mm in length) at 105℃, then place them in a mixer and mix at 1000r / min for 15min. Then add 0.15g of A-172, heat to 120℃, and mix at 2500r / min for 15min to obtain modified composite fiber.

[0107] S2. Add 8g of polyoxypropylene ether glycol 1000D, 32g of MN-3050D, 5g of hexamethylene diisocyanate and 0.1g of dibutyltin dilaurate to a reactor equipped with a condenser, and heat to 80℃ for 3h.

[0108] S3. Continue to add 3.5g of sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, 5.5g of neopentyl glycol, and 0.1g of p-methoxyphenol to the reaction vessel, and control the temperature at 70℃ for 4 hours.

[0109] S4. Add 1.8g of silicone resin prepolymer, 6g of modified composite fiber, 8g of 1,3-propanediol dimethacrylate, 10g of neopentyl glycol diacrylate, 18g of pentaerythritol hexaacrylate, and 5.5g of 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholino)-1-propanone to step S2 and react at 80℃ for 2h to obtain the resin.

[0110] Comparative Example 6

[0111] The specific preparation steps of the resin prepared in this comparative example are as follows:

[0112] S1. Dry 8g of glass fiber (0.6mm in length) at 105℃, then place it in a mixer and mix at 1000r / min for 15min. Then add 0.15g of A-172, heat to 120℃, and mix at 2500r / min for 15min to obtain modified composite fiber.

[0113] S2. Add 18g of polyoxypropylene ether glycol 1000D, 22g of MN-3050D, 5g of hexamethylene diisocyanate and 0.1g of dibutyltin dilaurate to a reactor equipped with a condenser, and heat to 80℃ for 3h.

[0114] S3. Continue to add 3.5g of sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, 5.5g of neopentyl glycol, and 0.1g of p-methoxyphenol to the reaction vessel, and control the temperature at 70℃ for 4 hours.

[0115] S4. Add 1.8g of silicone resin prepolymer, 6g of modified composite fiber, 8g of 1,3-propanediol dimethacrylate, 10g of neopentyl glycol diacrylate, 18g of pentaerythritol hexaacrylate, and 5.5g of 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholino)-1-propanone to step S2 and react at 80℃ for 2h to obtain the resin.

[0116] Comparative Example 7

[0117] The specific preparation steps of the resin prepared in this comparative example are as follows:

[0118] S1. Dry 0.5g of glass fiber (0.6mm in length) and 7.5g of chopped carbon fiber (0.1mm in length) at 105℃, then place them in a mixer and mix at 1000r / min for 15min. Then add 0.15g of A-172, heat to 120℃, and mix at 2500r / min for 15min to obtain modified composite fiber.

[0119] S2. Add 18g of polyoxypropylene ether glycol 1000D, 22g of MN-3050D, 5g of hexamethylene diisocyanate and 0.1g of dibutyltin dilaurate to a reactor equipped with a condenser, and heat to 80℃ for 3h.

[0120] S3. Continue to add 3.5g of sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, 5.5g of neopentyl glycol, and 0.1g of p-methoxyphenol to the reaction vessel, and control the temperature at 70℃ for 4 hours.

[0121] S4. Add 1.8g of silicone resin prepolymer, 6g of modified composite fiber, 8g of 1,3-propanediol dimethacrylate, 10g of neopentyl glycol diacrylate, 18g of pentaerythritol hexaacrylate, and 5.5g of 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholino)-1-propanone to step S2 and react at 80℃ for 2h to obtain the resin.

[0122] Comparative Example 8

[0123] The specific preparation steps of the resin prepared in this comparative example are as follows:

[0124] S1. Dry 3g of glass fiber (0.6mm in length) and 5g of chopped carbon fiber (2mm in length) at 105℃, then place them in a mixer and mix at 1000r / min for 15min. Then add 0.15g of A-172, heat to 120℃, and mix at 2500r / min for 15min to obtain modified composite fiber.

[0125] S2. Add 18g of polyoxypropylene ether glycol 1000D, 22g of MN-3050D, 5g of hexamethylene diisocyanate and 0.1g of dibutyltin dilaurate to a reactor equipped with a condenser, and heat to 80℃ for 3h.

[0126] S3. Continue to add 3.5g of sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, 5.5g of neopentyl glycol, and 0.1g of p-methoxyphenol to the reaction vessel, and control the temperature at 70℃ for 4 hours.

[0127] S4. Add 1.8g of silicone resin prepolymer, 6g of modified composite fiber, 8g of 1,3-propanediol dimethacrylate, 10g of neopentyl glycol diacrylate, 18g of pentaerythritol hexaacrylate, and 5.5g of 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholino)-1-propanone to step S2 and react at 80℃ for 2h to obtain the resin.

[0128] Comparative Example 9

[0129] The specific preparation steps of the resin prepared in this comparative example are as follows:

[0130] S1. Dry 0.5g of glass fiber (0.6mm in length), 5g of chopped carbon fiber (0.1mm in length) and 2.5g of chopped carbon fiber (2mm in length) at 105℃, then place them in a mixer and mix at 1000r / min for 15min. Then add 0.15g of A-172, heat to 120℃, and mix at 2500r / min for 15min to obtain modified composite fiber.

[0131] S2. Add 18g of polyoxypropylene ether glycol 1000D, 22g of MN-3050D, 5g of hexamethylene diisocyanate and 0.1g of dibutyltin dilaurate to a reactor equipped with a condenser, and heat to 80℃ for 3h.

[0132] S3. Continue to add 3.5g of sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, 5.5g of neopentyl glycol, and 0.1g of p-methoxyphenol to the reaction vessel, and control the temperature at 70℃ for 4 hours.

[0133] S4. Add 1.8g of silicone resin prepolymer, 6g of modified composite fiber, 8g of 1,3-propanediol dimethacrylate, 10g of neopentyl glycol diacrylate, 18g of polydipentaerythritol pentaacrylate, and 5.5g of 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholino)-1-propanone to step S2 and react at 80℃ for 2h to obtain the resin.

[0134] Comparative Example 10

[0135] The specific preparation steps of the resin prepared in this comparative example are as follows:

[0136] S1. Dry 0.5g of glass fiber (0.6mm in length), 5g of chopped carbon fiber (0.1mm in length) and 2.5g of chopped carbon fiber (2mm in length) at 105℃, then place them in a mixer and mix at 1000r / min for 15min. Then add 0.15g of A-172, heat to 120℃, and mix at 2500r / min for 15min to obtain modified composite fiber.

[0137] S2. Add 18g of polyoxypropylene ether glycol 1000D, 22g of MN-3050D, 5g of hexamethylene diisocyanate and 0.1g of dibutyltin dilaurate to a reactor equipped with a condenser, and heat to 80℃ for 3h.

[0138] S3. Continue to add 3.5g of sodium N,N-bis(2-hydroxyethyl)-2-aminoethanesulfonate, 5.5g of neopentyl glycol, and 0.1g of p-methoxyphenol to the reaction vessel, and control the temperature at 70℃ for 4 hours.

[0139] S4. Add 1.8g of silicone resin prepolymer, 6g of modified composite fiber, 5g of 1,3-propanediol dimethacrylate, 5g of neopentyl glycol diacrylate, 26g of pentaerythritol hexaacrylate, and 5.5g of 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholino)-1-propanone to step S2 and react at 80℃ for 2h to obtain the resin.

[0140] Experimental Example 2: Resin Performance Testing

[0141] Ten sets of 3D printing resins prepared in Comparative Examples 1 to 10 were printed in a DLP printer to form prefabricated materials. The prefabricated materials were cured at 405nm to obtain ten sets of test samples. The performance of the ten sets of samples was tested. The test methods and indicators were the same as those in Experiment Example 1. The test results are shown in Table 2.

[0142] Table 2:

[0143]

[0144]

[0145] Combining the results in Tables 1 and 2, it can be seen that each raw material component in the easy-to-clean photocurable resin of the present invention has a certain influence on the resin properties. Among them, the silicone resin prepolymer has a significant impact on the mechanical properties, contact angle, and heat resistance of the resin. This is mainly because the addition of the silicone resin prepolymer increases the rigidity of the resin, improves its mechanical strength, and also increases its hydrophobicity, thus achieving an easy-to-clean effect. At the same time, the addition of silicone resin significantly improves the heat resistance and stability of the resin. Secondly, there are many types of polyols, and their types and contents have a certain influence on the mechanical properties, hydrophilic and hydrophobic properties of the resin, as well as its heat resistance. The present invention uses polyoxypropylene ether glycol and MN-3050D in a mass ratio of 1:1 to 3. The invention achieves good resin performance under certain conditions and exhibits high compatibility with silicone resin prepolymers and modified composite fibers. Thirdly, the invention significantly enhances the mechanical properties of the resin by adding modified composite fibers, while simultaneously achieving a good balance between washability and easy cleaning performance at specific ratios. Therefore, the modified composite fibers used in this invention are glass fibers with a length of 0.6 mm, short-cut carbon fibers with a length of 0.1 mm, and short-cut carbon fibers with a length of 2 mm, which are used to modify and improve the resin's performance. Fourthly, the invention uses 1,3-propanediol dimethacrylate, neopentyl glycol diacrylate, and pentaerythritol hexaacrylate as reactive diluents in the printing process. By introducing functional bonds into the added reactive diluents, the resin curing speed and performance are improved.

[0146] It should be noted that the specific features, structures, materials or characteristics described in this specification can be combined in any way. For the sake of brevity, not all possible combinations of the various technical features in the above embodiments have been described. Without contradiction, those skilled in the art can combine and integrate the different embodiments and features described in this specification.

[0147] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.

Claims

1. An easy-to-clean light-curing resin, characterized in that, The raw materials of the photocurable resin include: silicone resin prepolymer, polyol, isocyanate, catalyst, hydrophilic chain extender, small molecule chain extender, modified composite fiber, polymerization inhibitor, photoinitiator, 1,3-propanediol dimethacrylate, neopentyl glycol diacrylate, and pentaerythritol hexaacrylate. The photocurable resin comprises the following raw materials in parts by weight: 0.1-4 parts of silicone resin prepolymer, 1-40 parts of polyol, 5-10 parts of isocyanate, 0.01-2 parts of catalyst, 1-5 parts of hydrophilic chain extender, 1-10 parts of small molecule chain extender, 1-10 parts of modified composite fiber, 0.01-0.5 parts of polymerization inhibitor, 1-10 parts of photoinitiator, 5-15 parts of 1,3-propanediol dimethacrylate, 5-15 parts of neopentyl glycol diacrylate, and 5-20 parts of pentaerythritol hexaacrylate. The organosilicon resin prepolymer is prepared from vinyltrimethoxysilane, styrene ethyltrimethoxysilane and phenylethynyltrimethylsilane; The polyol is composed of polyoxypropylene ether diol and MN-3050D in a mass ratio of 1:(1~3), and the molecular weight of the polyoxypropylene ether diol is 400~2000D; The composite fiber is made of glass fiber with a length of 0.6 mm, chopped carbon fiber with a length of 0.1 mm, and chopped carbon fiber with a length of 2 mm. The mass ratio of the glass fiber with a length of 0.6 mm, the short carbon fiber with a length of 0.1 mm, and the short carbon fiber with a length of 2 mm is (0.01~0.5):1:(0.05~0.5); The composite fiber is mixed with a coupling agent and then heated to obtain the modified composite fiber.

2. The easy-to-clean photocurable resin according to claim 1, characterized in that, The hydrophilic chain extender is one or a combination of N,N-di(2-hydroxyethyl)-2-aminoethanesulfonate sodium salt, aminoethylaminoethanesulfonate sodium salt, 2,2-dimethylolpropionic acid, dimethylolbutyric acid, and dimethylolpropionic acid; the small molecule chain extender is selected from one or a combination of neopentyl glycol, 1,4-butanediol, and glycerol.

3. The easy-to-clean photocurable resin according to claim 1, characterized in that, The coupling agent is selected from A-151, A-171, A-172, KH-570, or KH-550; the isocyanate is selected from dicyclohexane diisocyanate, isophorone diisocyanate, methylcyclohexyl diisocyanate, 2,2,4-trimethylhexane diisocyanate, diphenylmethane diisocyanate, hexamethylene diisocyanate, and toluene diisocyanate; the catalyst is selected from dibutyltin dilaurate and stannous octoate; the polymerization inhibitor is selected from p-methoxyphenol, hydroquinone, p-benzoquinone, methyl hydroquinone, 2,6-di-tert-butyl-p-cresol, and resorcinol, or a combination thereof; the photoinitiator is selected from 2-methyl-1-[4-(methylthio)phenyl]-2-(4-morpholinyl)-1-propanone, 2,4-... One of 6-trimethylbenzoyl-diphenylphosphine oxide, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butanone, and 2-hydroxy-2-methyl-1-phenylpropanone.

4. The easy-to-clean photocurable resin according to claim 1, characterized in that, The preparation method of the organosilicon resin prepolymer is as follows: vinyltrimethoxysilane, styreneethyltrimethoxysilane and phenylethynyltrimethylsilane are dissolved in an acidic catalyst solution, heated to react, cooled after the reaction is completed, separated into liquids, the organic phase is washed to neutral, the water in the organic phase is dried, filtered, and the filtrate is concentrated to obtain the organosilicon resin prepolymer.

5. A method for preparing the easy-to-clean photocurable resin according to any one of claims 1 to 4, characterized in that, Includes the following steps: S1. Mix the composite fiber with a coupling agent and heat-treat to obtain the modified composite fiber; S2. Add the polyol, isocyanate and catalyst to a reactor equipped with a condenser, and heat to 60~90℃ for 1~3 hours. S3. Continue to add hydrophilic chain extender, small molecule chain extender, and polymerization inhibitor to the reactor, and carry out the reaction at 60~80℃. S4. Add organosilicon resin prepolymer, modified composite fiber, 1,3-propanediol dimethacrylate, neopentyl glycol diacrylate, pentaerythritol hexaacrylate, and photoinitiator to step S2 and react at 60~90℃ to obtain an easy-to-clean photocurable resin.

6. The application of the easy-to-clean photocurable resin as described in any one of claims 1 to 4 in the fields of 3D printing, medical, aerospace, artificial intelligence, and building materials.

Citation Information

Patent Citations

  • Preparation method of chopped carbon fiber reinforced photosensitive resin

    CN110156937A

  • Composite photosensitive resin material for 3D printing and preparation method thereof

    CN111040388A

  • Washable high-temperature-resistant conductive photocuring material for 3D printing and printing process thereof

    CN113045715A

  • Washable light-cured 3D printing resin and preparation method thereof

    CN114874435A

  • Washable 3D printing resin as well as preparation method and application thereof

    CN116731282A