Monomer compositions, methacrylic resins, and methods for manufacturing methacrylic resins
By using a monomer composition of methyl methacrylate and α-olefin in methacrylic resins, combined with a specific catalyst, the problem of yellowing of the resin under UV conditions was solved, achieving a balance between high heat resistance and weather resistance.
Patent Information
- Application Number
- CN202280017543.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-03-15
- Filing Date
- 2022-03-10
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-03-10
AI Technical Summary
Existing methacrylic resins are prone to yellowing when exposed to UV conditions for extended periods, and the polymerization efficiency decreases with increasing HALS addition, leading to a decline in weather resistance.
Methacrylic resins are prepared by free radical polymerization using a monomer composition containing methyl methacrylate and α-olefins. The content of α-olefins is controlled within a specific range, and transition metals or Group 13 element compounds are used as catalysts to avoid their catalytic effect during polymerization.
It effectively inhibits the yellowing of the resin, maintains excellent heat resistance and weather resistance, and avoids a decrease in polymerization efficiency.
Smart Images

Figure BDA0004416879610000161
Abstract
Description
Technical Field
[0001] This invention relates to monomer compositions, methacrylic resins, and methods for manufacturing methacrylic resins. This application claims priority based on Japan Patent Application No. 2021-041292 filed on March 15, 2021, the contents of which are incorporated herein by reference. Background Technology
[0002] Methacrylic resins exhibit excellent transparency, heat resistance, and weather resistance, and possess a balanced performance in terms of mechanical strength, thermal properties, and molding processability. In particular, methacrylic resin sheets are used in applications such as sunbeds, lighting equipment, skin treatment devices, medical devices, equipment for curing or reacting via ultraviolet light (UV), plant and animal cultivation equipment, skylights, and transparent components used in HID lamps.
[0003] In the above applications, when methacrylic resin boards are installed in environments exposed to UV, such as direct sunlight or UV lamps, there is a problem that the methacrylic resin boards turn yellow. Therefore, it is required that methacrylic resins do not turn yellow even when exposed to UV for a long time, that is, methacrylic resins with excellent weather resistance.
[0004] As a technology to improve the weather resistance of methacrylic resins, Patent Document 1 discloses a methacrylic resin formed by polymerizing monomers such as methyl methacrylate in the presence of a hindered amine compound (HALS) with a specific structure, which is one of the light stabilizers. Existing technical documents Patent documents
[0005] Patent Document 1: Japanese Patent Application Publication No. 55-139404 Summary of the Invention The problem that the invention aims to solve
[0006] However, the methacrylic resin described in Patent Document 1 has improved weather resistance as the amount of HALS added during polymerization increases, but on the other hand, there is a problem that the methacrylic resin obtained is colored because HALS itself is colored. In addition, if the amount of HALS added increases, the polymerization efficiency decreases, the residual monomer in the methacrylic resin increases, and there is a problem that the weather resistance of the obtained methacrylic resin decreases.
[0007] In view of the above circumstances, the technical problem of the present invention is to provide a methacrylic resin that ensures excellent heat resistance, excellent weather resistance and suppressed yellowing, a monomer composition for obtaining the methacrylic resin, and a method for manufacturing the methacrylic resin using the monomer composition. Technical solutions to the problem
[0008] To solve the above-mentioned technical problems, the present invention adopts the following structure. [1] A monomer composition comprising methyl methacrylate and α-olefin. [2] According to the monomer composition of [1], wherein, relative to the total mass of the α-olefin, the content of at least one compound selected from transition metal compounds and group 13 element compounds is 0 ppm by mass or more and 7 × 10⁻⁶. 4 Mass below ppm. [3] The monomer composition according to [1] or [2], wherein the α-olefin is contained in more than 0.1 ppm by mass relative to the total mass of the monomer composition. [4] The monomer composition according to any one of [1] to [3], wherein the α-olefin is a liquid or a solid at room temperature and pressure. [5] The monomer composition according to any one of [1] to [4], wherein the α-olefin contains an α-olefin having 6 or more and 12 or fewer carbon atoms. [6] The monomer composition according to any one of [1] to [5], wherein the α-olefin contains 1-octene or 1-dodecene. [7] A methacrylic resin is obtained by free radical polymerization of a monomer mixture containing any one of the monomer compositions described in [1] to [6]. [8] A methacrylic resin containing an α-olefin monomer. [9] The methacrylic resin according to [8] contains more than 0.1 ppm by mass of the α-olefin monomer.
[10] The methacrylic resin according to [8] or [9], wherein the α-olefin monomer is a liquid or a solid at room temperature and pressure.
[11] The methacrylic resin according to any one of [8] to
[10] , wherein the α-olefin monomer contains an α-olefin having 6 or more and 12 or fewer carbon atoms.
[12] The methacrylic resin according to any one of [8] to
[11] , wherein the α-olefin monomer contains 1-octene or 1-dodecene.
[13] A resin molded body obtained by molding the methacrylic resin described in any one of [8] to
[12] .
[14] A method for manufacturing a methacrylic resin, comprising free radical polymerization of a monomer mixture containing a monomer composition, wherein the monomer composition contains methyl methacrylate and an α-olefin, and the content of at least one compound selected from transition metal compounds and group 13 element compounds is 7 × 10⁻⁶ relative to the total mass of the α-olefin. 4 Mass below ppm. Invention Effects
[0009] According to the present invention, these problems can be solved. That is, the present invention provides a methacrylic resin that ensures excellent heat resistance, excellent weather resistance and suppressed yellowing, a monomer composition for obtaining the methacrylic resin, and a method for manufacturing the methacrylic resin using the monomer composition. Detailed Implementation
[0010] The following terms are defined in this specification and claims. "Monomer" refers to a compound that has polymerizable carbon-carbon double bonds. "Monomer-based units" are a general term for atomic groups directly formed by the polymerization of a single monomer and atomic groups obtained by chemically transforming a portion of the atomic group. “(Meth)acrylate” is selected from “acrylate” and “methacrylate”. “(Meth)acrylic acid” is selected from “acrylic acid” and “methacrylic acid”. "α-olefin" refers to an olefin that has a carbon-carbon double bond at the α position. "α-olefin monomer" refers to an olefin with a carbon-carbon double bond at the α position, but is used to explicitly indicate that it is a monomer that has not undergone polymerization. "Conjugation" refers to the overlap of p orbitals that cross the σ bonds that exist between them. "Non-conjugation" means that conjugation does not occur. "The obtained methacrylic resin" refers to a resin obtained by free radical polymerization of a monomer mixture containing the monomer composition of the present invention. "The obtained resin molded body" refers to the molded body formed by molding the methacrylic resin of the present invention. "mass%" indicates the percentage of a specified component contained in 100% of the total mass. "Weight-average molecular weight" is a value determined by gel permeation chromatography using standard polystyrene as a standard sample. "Room temperature" refers to 5-35℃. "Atmospheric pressure" refers to 900-1100 hPa. Transition metals refer to metallic elements located in groups 3 through 11 of the periodic table. Typical examples include: scandium (Sc), titanium (Ti), vanadium (V), chromium (Cr), manganese (Mn), iron (Fe), cobalt (Co), nickel (Ni), copper (Cu), zinc (Zn), yttrium (Y), zirconium (Zr), niobium (Nb), molybdenum (Mo), technetium (Tc), ruthenium (Ru), rhodium (Rh), palladium (Pd), silver (Ag), cadmium (Cd), lanthanum (La), and cerium (Ce). Prismium (Pr), neodymium (Nd), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), lutetium (Lu), hafnium (Hf), tantalum (Ta), tungsten (W), rhenium (Re), osmium (Os), iridium (Ir), platinum (Pt), gold (Au), and mercury (Hg), etc. "Group 13 elements" refers to elements located in Group 13 of the periodic table. Typical examples include boron (B), aluminum (Al), gallium (Ga), indium (In), and thallium (Tl). The "periodic table" refers to the "Periodic Table of Elements" (URL https: / / pubchem.ncbi.nlm.nih.gov / periodic-table / ).
[0011] <Monomer Composition> The monomer composition of the present invention contains methyl methacrylate and α-olefin. Furthermore, other components may be included without impairing the effects of the present invention.
[0012] The monomer composition of the present invention contains methyl methacrylate, resulting in a methacrylic resin with good weather resistance and suppressed yellowing.
[0013] In addition, the monomer composition of the present invention contains α-olefins, resulting in methacrylic resins with good weather resistance and suppressed yellowing.
[0014] The content of methyl methacrylate in the monomer composition of the present invention is not particularly limited, but it is preferably 85% by mass or more, more preferably 90% by mass or more, further preferably 95% by mass or more, and particularly preferably 98% by mass, relative to the total mass of the monomer composition.
[0015] However, the content of methyl methacrylate relative to 100% of the total mass of the monomer composition of the present invention is less than 100% by mass. In addition, the total content of methyl methacrylate and α-olefin is no more than 100% by mass relative to the total mass of the monomer composition of the present invention.
[0016] There is no particular limitation on the lower limit of the content of α-olefins in the monomer composition of the present invention, but from the perspective of obtaining a methacrylic resin with better weather resistance, it is preferably 0.1 ppm or more by mass relative to the total mass of the monomer composition, more preferably 10 ppm or more by mass, further preferably 60 ppm or more by mass, and particularly preferably 80 ppm or more by mass.
[0017] There is no particular limitation on the upper limit of the content of α-olefins in the monomer composition of the present invention, but from the perspective of being able to maintain the heat resistance of the obtained methacrylic resin better, it is preferably 10,000 ppm by mass or less, more preferably 5,000 ppm by mass or less, further preferably 4,000 ppm by mass or less, and particularly preferably 3,000 ppm by mass or less.
[0018] The above-mentioned preferred upper and lower limits can be combined arbitrarily. Specifically, the content of α-olefin contained in the monomer composition of the present invention is preferably 0.1 ppm by mass or more and 10,000 ppm by mass or less, more preferably 10 ppm by mass or more and 5,000 ppm by mass or less, further preferably 60 ppm by mass or more and 4,000 ppm by mass or less, and particularly preferably 80 ppm by mass or more and 3,000 ppm by mass or less.
[0019] It is speculated that the addition of α-olefins involves coupling products between olefins with free radicals generated by ultraviolet light, which are stable and exhibit excellent free radical scavenging effects. As the α-olefin, a chain-like α-olefin is preferred.
[0020] The α-olefin preferably contains α-olefins with 6 or more but less than 12 carbon atoms. There is no particular limitation on the proportion of the α-olefins with 6 or more but less than 12 carbon atoms in the α-olefin composition, but it is preferably 80% by mass or more, more preferably 90% by mass or more, and particularly preferably 99% by mass or more. The α-olefin is particularly preferably composed of α-olefins with 6 or more but less than 12 carbon atoms.
[0021] The α-olefin with 6 or more and 12 or less carbon atoms is not particularly limited as long as it has 6 or more and 12 or less carbon atoms, but is preferably 8 or more and 10 or less. The α-olefin has a carbon number above the lower limit of the range, so it is unlikely to remain in the resulting methacrylic resin due to volatilization during polymerization. Therefore, it can significantly contribute to improved weather resistance.
[0022] Examples of α-olefins having 6 or more but less than 12 carbon atoms include 2-ethyl-1-hexene, 2-methyl-1-heptene, 4-methyl-1-heptene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, and 1-dodecene. Among these, at least one selected from 2-ethyl-1-hexene, 1-octene, and 1-dodecene is preferred; 1-octene or 1-dodecene is more preferred; and from the viewpoint that they are prone to remaining in methacrylic resins, 1-octene is even more preferred. There is no particular limitation on the proportion of 1-octene in the α-olefin, but it is preferably 50% by mass or more, more preferably 80% by mass or more, relative to the total mass of the α-olefin.
[0023] In the monomer composition of the present invention, the content of at least one compound selected from transition metal compounds and group 13 element compounds is preferably 0 ppm or more and 7 × 10⁻⁶ ppm relative to the total mass of α-olefins. 4 Mass below ppm. The α-olefins used in this invention, compared to methyl methacrylate as a conjugated monomer, do not exhibit resonance stabilization and have significantly lower reactivity. Therefore, using a specific polymerization catalyst such as at least one compound selected from transition metal compounds and Group 13 element compounds, unreacted α-olefins (hereinafter also referred to as "α-olefin monomers") will remain in the resulting methacrylate resin, unless under specific conditions where they act as catalysts. It is believed that the presence of these α-olefin monomers in the methacrylate resin contributes to its good weather resistance and inhibits yellowing. That is, to prevent the at least one compound from acting as a catalyst, the content of the at least one compound relative to the total mass of the α-olefins is preferably 7 × 10⁻⁶. 4 Below ppm, more preferably 1×10 4 The content is below ppm by mass, more preferably below 1000 ppm by mass, and particularly preferably not contained. Here, "not contained" means below the detection limit.
[0024] Examples of such compounds include transition metal compounds of groups 5 to 11 having chelating ligands or Lewis acid catalysts. Specific examples of the transition metals include vanadium, niobium, tantalum, chromium, molybdenum, tungsten, manganese, iron, platinum, ruthenium, cobalt, rhodium, nickel, palladium, and copper. Among these transition metals, transition metals from Groups 8 to 11 are preferred, transition metals from Group 10 are more preferred, and nickel (Ni) or palladium (Pd) are even more preferred. These transition metals may be used alone or in combination of two or more.
[0025] The chelating ligand has at least two atoms selected from P, N, O, and S, including bidentate or multidentate ligands, and is electronically neutral or anionic. The structure of chelating ligands is illustrated in the general overview by Ittel et al. (Ittel et al., “Late-Metal Catalysts for Ethylene Homo-and Copolymerization”, Chemical Reviews, March 25, 2000, Vol. 100, No. 4, pp. 1169-1204). Examples of chelating ligands include, for example, bidentate anionic P and O ligands. Examples of bidentate anionic P and O ligands include, for example, phosphonic acid, phosphonic carboxylic acid, phosphonophenol, and phosphoenolides. Examples of chelating ligands other than bidentate anionic P and O ligands include, for example, bidentate anionic N and O ligands. Examples of bidentate anionic N and O ligands include, for example, salicylaldehyde imine and pyridine carboxylic acid. Examples of chelating ligands other than bidentate anionic P and O ligands and bidentate anionic N and O ligands include, for example, diimine ligands, diphenoxide ligands, and diamide ligands.
[0026] Here, transition metal compounds from Groups 5 to 11 with chelating ligands, i.e., catalysts, are typically known as so-called SHOP-based catalysts and Drent-based catalysts. The SHOP-based catalyst is a catalyst formed by coordinating a phosphorus-based ligand having an optionally substituent aryl group with nickel metal. Similarly, the Drent-based catalyst is a catalyst formed by coordinating a phosphorus-based ligand having an optionally substituent aryl group with palladium metal.
[0027] Furthermore, representative Lewis acid catalysts include cationic complexes of divalent palladium or platinum. These cationic complexes of divalent palladium or platinum exhibit Lewis acidity and are useful as Lewis acid catalysts for reactions such as the Diels-Alder reaction. In addition, compounds of Group 13 elements boron and aluminum, period 4 transition metals titanium, and period 5 transition metals zirconium also exhibit Lewis acidity and are therefore preferred.
[0028] Other components mentioned above include, for example, the following monomers and additives.
[0029] (monomer) 1) Methacrylates: For example, ethyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, tert-butyl methacrylate, 2-ethylhexyl methacrylate, phenyl methacrylate, or benzyl methacrylate. 2) Acrylates: For example, methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, tert-butyl acrylate, or 2-ethylhexyl acrylate. 3) Unsaturated carboxylic acids: For example, acrylic acid, methacrylic acid, maleic acid, or itaconic acid. 4) Unsaturated carboxylic anhydrides: For example, maleic anhydride or itaconic anhydride. 5) Maleimide: For example, N-phenylmaleimide or N-cyclohexylmaleimide. 6) Hydroxyl-containing vinyl monomers: For example, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, or 2-hydroxypropyl methacrylate. 7) Ethylene ester: For example, vinyl acetate or vinyl benzoate. 8) Vinyl chloride, vinylidene chloride and their derivatives. 9) Nitrogen-containing vinyl monomers: For example, methacrylamide or acrylonitrile. 10) Monomers containing epoxy groups: For example, glycidyl acrylate or glycidyl methacrylate. 11) Aromatic vinyl monomers: For example, styrene or α-methylstyrene.
[0030] 12) Alkanediol di(meth)acrylate: For example, ethylene glycol di(meth)acrylate, 1,2-propanediol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, or 1,6-hexanediol di(meth)acrylate. 13) Polyoxyalkylene glycol di(meth)acrylate: For example, diethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, triethylene glycol (meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, or neopentyl glycol di(meth)acrylate. 14) Vinyl monomers with two or more olefinic unsaturated bonds in their molecules: For example, divinylbenzene. 15) An unsaturated polyester prepolymer obtained from at least one polycarboxylic acid containing an olefinic unsaturated polycarboxylic acid and at least one diol. 16) Vinyl ester prepolymer obtained by modifying the epoxy group end with acrylic acid.
[0031] (additive) Examples of such additives include: mold release agents, lubricants, plasticizers, antioxidants, antistatic agents, light stabilizers, ultraviolet absorbers, flame retardants, flame retardant additives, polymerization inhibitors, fillers, pigments, dyes, silane coupling agents, leveling agents, defoamers, and fluorescent agents, among other known additives.
[0032] As other components, the monomer and the additive may be used alone or in combination of two or more. From the viewpoint that the obtained methacrylic resin has an excellent balance of transparency, heat resistance and moldability, the other components are preferably selected from at least one monomer selected from methyl acrylate, ethyl acrylate and n-butyl acrylate. In addition to the monomers mentioned above, the following monomers may also be cited as other components.
[0033] Examples of such additives include: mold release agents, lubricants, plasticizers, antioxidants, antistatic agents, light stabilizers, ultraviolet absorbers, flame retardants, flame retardant additives, polymerization inhibitors, fillers, pigments, dyes, silane coupling agents, leveling agents, defoamers, fluorescent agents, and other known additives. In addition, the monomer composition of the present invention may contain compounds such as isobutylene aldehyde or methanol, which are inevitably mixed into methyl methacrylate.
[0034] <Monomer Mixture> The monomer mixture of the present invention is a raw material for the methacrylic resin of the present invention, which will be described later. The monomer mixture contains 60% by mass or more of the monomer composition of the present invention described above. Here, "containing 60% by mass or more of the monomer composition of the present invention" means that, relative to 100% by mass of the total mass of the monomer mixture, it contains 100% by mass of the monomer composition of the present invention described above, or it contains 60% by mass or more but less than 100% by mass of the monomer composition of the present invention and more than 0% by mass and less than 40% by mass of "other monomers capable of copolymerizing with the monomer composition of the present invention" (also referred to as "other monomers"), and the total of the monomer composition and the other monomers does not exceed 100% by mass.
[0035] Other monomers mentioned above include monomers 1) to 16) which can be included in other compounds as described in the above description of the monomeric compositions of the present invention. As other monomers, the monomers described in 1) to 16) above can be used alone or in combination of two or more.
[0036] Of the monomers 1) to 16) above, from the viewpoint of achieving an excellent balance between heat resistance and transparency of the resulting methacrylate resin, ethylene glycol dimethacrylate or neopentyl glycol dimethacrylate is preferred.
[0037] A polymerization initiator may be added to the monomer mixture. Examples of such polymerization initiators include compounds similar to organic peroxides and azo compounds. There is no particular limitation on the amount of polymerization initiator added to the monomer mixture, but it is preferably 0.005 to 5% by mass relative to 100% by mass of the free radical polymerizable monomer in the monomer mixture.
[0038] The monomer mixture may contain various additives as needed, such as mold release agents, lubricants, plasticizers, antioxidants, antistatic agents, light stabilizers, ultraviolet absorbers, flame retardants, flame retardant additives, polymerization inhibitors, fillers, pigments, dyes, silane coupling agents, leveling agents, defoamers, fluorescent agents, or chain transfer agents.
[0039] <Methacrylic resins> The methacrylic resin of the present invention is obtained by free radical polymerization of a monomer mixture containing 60% by mass or more of the monomer composition of the present invention described above. There is no particular limitation on the mass-average molecular weight (Mw) of the methacrylic resin, but it can be appropriately set in the range of 100,000 to 1,000,000 depending on the intended use of the methacrylic resin. By appropriately increasing the mass-average molecular weight, solvent resistance and chemical resistance can be improved.
[0040] <Manufacturing Method of Methacrylic Resins> The methacrylic resin of the present invention is obtained, for example, by polymerizing a monomer mixture, wherein the monomer mixture is a monomer mixture containing 100% by mass of the monomer composition of the present invention described above, or a monomer mixture containing 60% by mass or more and less than 100% by mass of the monomer composition of the present invention and more than 0% by mass and less than 40% by mass of "other monomers capable of copolymerizing with the monomer composition of the present invention" (also referred to as "other monomers"), and the total of the monomer composition and the other monomers (including polymerization initiators and various additives) does not exceed 100% by mass.
[0041] The polymerization method for the monomer composition is not particularly limited, and examples include bulk polymerization, solution polymerization, emulsion polymerization, and suspension polymerization. From the viewpoints of the transparency of methacrylic resins, the environmental impact caused by the use of solvents, and the excellent productivity and manufacturing cost of resin laminates, bulk polymerization is preferred as the polymerization method for the monomer mixture. There are no particular restrictions on the specific means of bulk polymerization; known casting polymerization methods such as monomer casting or continuous casting can be used to manufacture it. The mass-average molecular weight (Mw) of the methacrylic resin can be controlled by adjusting the polymerization temperature, polymerization time, amount of polymerization initiator, and type and amount of chain transfer agent.
[0042] The casting polymerization method is as follows: a mixture of monomers for obtaining methacrylic resin or a slurry described later is injected into a mold consisting of two inorganic glass plates or metal plates (e.g., SUS plates) that are sealed around the perimeter with gaskets such as soft resin tubes and placed at a specified interval, and polymerized thereunder to obtain methacrylic resin. The obtained methacrylic resin is then demolded from the mold to obtain a resin molded body.
[0043] As the slurry, a slurry containing polymer (partial polymer) and unreacted monomer mixture that has been polymerized in part of the monomer mixture can be used. Alternatively, such slurries containing the methacrylic resin of the present invention can also be used in the monomer mixture.
[0044] There is no particular limitation on the molecular weight of the polymer or the dissolved methacrylic resin in the slurry; the mass-average molecular weight can be set to 50,000 or more and 300,000 or less. Furthermore, there is no particular limitation on the mixing ratio of the polymer or the dissolved methacrylic resin in the slurry to the monomer mixture; by mass ratio, it can be set to a ratio of polymer or methacrylic resin: monomer mixture = 2:98 to 50:50.
[0045] There are no particular limitations on the mold used for casting polymerization; known molds can be used. Examples of molds for obtaining sheet-like resin molded articles include molds for monomer casting and molds for continuous casting. For example, a mold used for casting individual pieces can be made by placing two plate-shaped bodies, such as inorganic glass plates, chrome-plated metal plates, or stainless steel plates, at a specified interval, and placing gaskets at their edges to form a sealed space between the plate-shaped bodies and the gaskets.
[0046] Examples of molds used for continuous casting include: a mold in which a sealed space is formed by the opposing surfaces of a pair of endless belts traveling in the same direction at the same speed and by gaskets on both sides of the endless belts traveling at the same speed as the endless belts. The gaps in the mold are adjusted appropriately to obtain a resin plate of the desired thickness, but typically 1–30 mm.
[0047] <Effects> The monomer composition of the present invention contains α-olefins. The methacrylic resin obtained by free radical polymerization of a monomer mixture containing the monomer composition of the present invention ensures excellent heat resistance, good weather resistance, and suppressed yellowing. The reason why the monomer composition of the present invention contains α-olefins to obtain methacrylic resins that ensure excellent heat resistance, good weather resistance and suppressed yellowing is not clear, but it is speculated as follows.
[0048] When exposed to light or heat, the main chain or side chains of polymers containing methyl methacrylate-based units (methacrylic resins) crack, generating free radicals. Typically, these generated free radicals lead to yellowing of methacrylic resins and a decrease in mechanical strength due to a reduction in molecular weight.
[0049] However, as described above, the α-olefin in this invention does not achieve a resonance stabilization effect compared to methyl methacrylate as a conjugated monomer, and its reactivity is significantly lower. Therefore, when using specific polymerization catalysts such as transition metal compounds or Group 13 compounds, unreacted α-olefins (also specifically referred to as "α-olefin monomers") remain in the resulting methacrylate resin, unless under specific conditions where they act as catalysts. These α-olefin monomers remain in the methacrylate resin. Furthermore, it is believed that these α-olefin monomers function as free radical scavengers.
[0050] Specifically, the hydrogen atom bonded to the carbon atom adjacent to the double bond site of the α-olefin monomer is abstracted by the aforementioned free radical species. Furthermore, the olefin after the hydrogen atom (hydrogen free radical) is abstracted captures the other aforementioned free radical species. As a result, it is believed that excellent heat resistance and weather resistance are ensured in the methacrylic resin, and yellowing is suppressed. [Example]
[0051] The present invention will now be described in more detail through embodiments, but the present invention is not limited to the embodiments described below. In the following explanation, “parts” means “parts by weight”. Additionally, in Table 1, "Amount Added (parts by mass)" is expressed as parts by mass and ppm, with the total amount of MMA and BA added set to 100 parts by mass. "Amount Added (%)" is expressed as % by mass and ppm, with the total mass of the monomer composition set to 100% by mass. Furthermore, "-" indicates that the compound was not added.
[0052] The abbreviations and names of the compounds used in the examples and comparative examples are as follows. • MMA: Methyl methacrylate (manufactured by Mitsubishi Chemical Corporation). ·BA: n-Butyl acrylate (manufactured by Mitsubishi Chemical Corporation). • OCT: 1-Octenene (manufactured by Tokyo Chemical Industry Co., Ltd.) HEX: 1-Hexene (manufactured by Tokyo Chemical Industry Co., Ltd.) ·2E1H: 2-Ethyl-1-hexene (manufactured by Tokyo Chemical Industry Co., Ltd.) ·HALS: Tetramethyl-4-piperidinyl 1,2,3,4-butanetetracarboxylate (2,2,6,6-tetramethyl-4-piperidinyl ester) (trade name: LA-57, manufactured by ADEKA).
[0053] [Determination and Evaluation Methods] <Method for Determination of Residual α-olefin Monomer in Methacrylic Resins> (1) Sample and detection solution preparation steps The resin molded body was finely crushed. 0.2 g of the crushed resin was dissolved in 10 mL of acetone (hereinafter referred to as "acetone") for pesticide residue testing. After dissolving the resin, 1 mL of internal standard solution was added using a single-standard pipette. The internal standard solution used was 0.1% (v / v) methyl salicylate / acetone solution. Three test solutions of different concentrations were prepared by diluting the standard reagent of the target substance with acetone. These solutions were then analyzed by gas chromatography-mass spectrometry (GC / MS) as described later to construct a three-point standard curve and quantify the concentration of each target substance in the sample. The internal standard solution used was 0.1% (v / v) methyl salicylate / acetone solution. (GC / MS determination conditions) Device: GC HP6890 / MS HP5973 (manufactured by Agilent Technologies) Ionization method: EI (Electron Ionization) method Chromatographic column: DB-WAX 60m × 250μm × 0.5μm (manufactured by Agilent Technologies) Heating conditions: 70℃ (5 min) → 200℃ (5 min) rate = 10℃ / min Inlet temperature: 220℃ AUX temperature: 230℃ Ion source temperature: 230℃ Flow split ratio: 10:1 Flow rate: 2.0 mL / min Average linear velocity: 37 cm / sec Injection volume: 1μL Measurement mode: SIM
[0054] <Evaluation Methods for Heat Resistance> As an indicator of the heat resistance of the methacrylic resins obtained in the examples and comparative examples, the load flexural temperature (hereinafter referred to as "HDT") (°C) of the resin molded specimens (127 mm long × 12.7 mm wide × 3 mm thick) obtained in the examples and comparative examples was measured according to JIS K 7191.
[0055] <Methods for evaluating weather resistance> The weather resistance of the methacrylic resins obtained in the examples and comparative examples was evaluated by the following method. A metal weather accelerated weathering tester (DAIPLA WINTES model KU-R5CI-A) equipped with a metal halide lamp (DAIPLA WINTES model: MW-60W) and a light cutoff filter (DAIPLA WINTES model: KF-1) was used to conduct UV exposure tests. The yellowness (YI) and its change (ΔYI) were measured from before the start of the UV exposure test to 200 hours after the start of the test, according to the method described below.
[0056] Specifically, in the evaluation chamber of the metal weather accelerated weathering tester, a test piece (a square shape with a length of 50 mm × width of 50 mm and a thickness of 5 mm) obtained by cutting the resin molded body obtained in the Example and Comparative Example into a square is set up. The intensity of ultraviolet (UV) irradiation of the test piece from the metal halide lamp was corrected to 80 mW / cm² in the wavelength range of 330–390 nm, as measured by a UV illuminometer (manufactured by Ushio Electric Co., Ltd., model name: UIT-101). 2 The evaluation chamber of the accelerated weathering test chamber for metals was set at a temperature of 63°C and a humidity of 50% RH. The test specimens were irradiated with ultraviolet light from a metal halide lamp (irradiation intensity 80 mW / cm²). 2 ).
[0057] As an indicator of weather resistance, the yellowness (yellowness index: YI) of the test pieces was measured using a spectrophotometer (manufactured by Nippon Denshoku Kogyo Co., Ltd., model name: SE-7700) according to ASTM D1925. One test piece was used before the start of the UV exposure test, and another test piece was used 200 hours after the start of the test. The change in the measured value was taken as the change in yellowness (ΔYI).
[0058] [Example 1] (1) Preparation of monomer compositions A monomer composition containing 500 ppm of 1-octene in 98.0 parts by weight of MMA and 2.0 parts by weight of BA was prepared in a reactor (polymerization vessel) equipped with a condenser, thermometer and stirrer.
[0059] (2) Preparation of slurry The prepared monomer composition was fed into a reactor, and heating was initiated while stirring and bubbling with nitrogen. When the reactor internal temperature reached 80°C, 0.12 parts by mass of 2,2'-azobis-(2,4-dimethylpentanonitrile) as a free radical polymerization initiator and 0.075 parts by mass of 1-dodecyl mercaptan as a chain transfer agent were added to prepare a monomer mixture. Further heating was carried out until the reactor internal temperature reached 100°C, and maintained for 9 minutes. Then, the reactor internal temperature was cooled to room temperature to obtain a slurry. The slurry contained 25% by mass of polymer and 75% by mass of unreacted monomer composition relative to 100% of the total mass of the slurry.
[0060] (3) Casting and polymerization To obtain a polymerizable composition, 0.15 parts by weight of tert-hexyl peroxypentanoate, acting as a free radical polymerization initiator, were added to 100 parts by weight of the aforementioned slurry. Next, the polymerizable composition was poured into a 6.5 mm gap space between two opposing SUS plates, formed by placing soft resin gaskets at the ends of the SUS plates. The mixture was heated at 80°C for 30 minutes, followed by heating at 130°C for 30 minutes to cure the polymerizable composition, yielding a methacrylic resin. The methacrylic resin was then cooled along with the SUS plates, and the SUS plates were removed, resulting in a 5 mm thick sheet-like resin molded body. The evaluation results of the obtained resin molded body are shown in Table 1.
[0061] [Examples 2-6] Except for changes to the formulation of the monomer composition as described in Table 1, the methacrylic resin and the resin molded article were manufactured using the same method as in Example 1. The evaluation results of the obtained resin molded articles are shown in Table 1.
[0062] [Example 7] Except for altering the formulation of the monomer composition as described in Table 1 and replacing 1-octene with 1-hexene, the methacrylic resin and the resin molded article were manufactured in the same manner as in Example 1. The evaluation results of the obtained resin molded articles are shown in Table 1.
[0063] [Example 8] Except for changing the formulation of the monomer composition as described in Table 1 and replacing 1-octene with 2-ethyl-1-hexene, the methacrylic resin and the resin molded article were manufactured in the same manner as in Example 1. The evaluation results of the obtained resin molded articles are shown in Table 1.
[0064] [Comparative Examples 1-3] Except that the monomer composition ratios were set as described in Table 1, the methacrylic resin and the resin molded articles were manufactured using the same method as in Example 1. The evaluation results of the obtained resin molded articles are shown in Table 1.
[0065] [Table 1] *1 Content relative to the total mass of methyl methacrylate (MMA) *2 Content ratio relative to the total mass of methacrylic resin (resin molded body)
[0066] The resin molded articles obtained in Examples 1-8 maintained excellent heat resistance, good weather resistance, and suppressed yellowing. This is believed to be due to the presence of methyl methacrylate and α-olefin in the monomer composition, and the residual α-olefin monomer in the methacrylic resin.
[0067] The resin molded articles obtained in Comparative Examples 1 and 3 did not contain α-olefins in the monomer composition and there were no residual α-olefin monomers in the methacrylic resin, so yellowing and insufficient weather resistance were observed.
[0068] The resin molded articles obtained in Comparative Example 2 exhibited yellowing and slightly insufficient weather resistance due to the presence of hindered amine compounds replacing α-olefins in the monomer composition.
Claims
1. A monomer composition comprising methyl methacrylate and an α-olefin, wherein the α-olefin content in the monomer composition is 0.1 ppm by mass or more and 3000 ppm by mass or less relative to the total mass of the monomer composition. The α-olefin contains at least one selected from 2-ethyl-1-hexene, 1-octene, and 1-dodecene. The content of methyl methacrylate is 85% by mass or more relative to the total mass of the monomer composition.
2. The monomer composition according to claim 1, wherein, The content of at least one compound selected from the group consisting of a transition metal compound and a Group 13 element compound is 0 mass ppm or more and 7 x 10 4 mass ppm or less, relative to the total mass of the α-olefin.
3. The monomer composition according to claim 1 or 2, wherein, The α-olefin contains more than 10 ppm by mass relative to the total mass of the monomer composition.
4. The monomer composition according to claim 1 or 2, wherein, The α-olefin contains more than 60 ppm by mass relative to the total mass of the monomer composition.
5. The monomer composition according to claim 1 or 2, wherein, The α-olefin contains more than 80 ppm by mass relative to the total mass of the monomer composition.
6. A methacrylic resin, which is obtained by free radical polymerization of a monomer mixture containing the monomer composition of any one of claims 1 to 5.
7. The methacrylic resin according to claim 6, wherein it contains 0.1 ppm by mass and 1300 ppm by mass of α-olefin monomer, wherein the α-olefin monomer contains at least one selected from 2-ethyl-1-hexene, 1-octene and 1-dodecene.
8. The methacrylic resin according to claim 7, wherein it contains more than 10 ppm by mass of the α-olefin monomer.
9. The methacrylic resin according to claim 7, wherein it contains 60 ppm or more of the α-olefin monomer.
10. The methacrylic resin according to claim 7, wherein it contains 80 ppm or more of the α-olefin monomer.
11. A resin molded article obtained by molding the methacrylic resin according to any one of claims 7 to 10.
12. A method for manufacturing a methacrylic resin, comprising free radical polymerization of a monomer mixture containing a monomer composition, wherein, The monomer composition contains methyl methacrylate and an α-olefin, wherein the α-olefin contains at least one selected from 2-ethyl-1-hexene, 1-octene, and 1-dodecene, and the content of the α-olefin is 0.1 ppm by mass or more and 3000 ppm by mass or less relative to the total mass of the monomer composition, and the content of at least one compound selected from transition metal compounds and Group 13 element compounds is 7 × 10⁻⁶ relative to the total mass of the α-olefin. 4 Mass below ppm.
Citation Information
Patent Citations
Methylmethacrylate polymer having high stability against ultraviolet and heat
JP1980139404A
Game machine
JP2021041292A