Anode materials and their preparation methods, batteries

By doping non-metallic conductive agents and adding metal peroxides during the graphitization process, porous amorphous carbon and conductive agent-coated graphite composite materials were prepared, solving the problems of insufficient fast-charging performance and energy density of graphite anode materials, and achieving high-efficiency electronic conductivity and ion transport rate.

CN117096310BActive Publication Date: 2026-11-17SHENZHEN GOLD MEDAL NEW ENERGY TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311135689.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-01
Publication Date
2026-11-17
Estimated Expiration
2043-09-01

AI Technical Summary

Technical Problem

Existing graphite anode materials cannot simultaneously meet the requirements of fast charging performance and high energy density.

Method used

By doping non-metallic conductive agents into coke raw materials and adding metal peroxides and metallic conductive agents during graphitization, porous amorphous carbon and conductive agent-coated graphite composite materials are formed, thereby improving the electronic conductivity and ion transport rate of the materials.

Benefits of technology

It significantly improves the material's fast-charging performance and electronic conductivity, and enhances the material's energy density and cycle performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117096310B_ABST
    Figure CN117096310B_ABST
Patent Text Reader

Abstract

This invention relates to the field of lithium-ion battery materials technology, and discloses a negative electrode material, its preparation method, and a battery. The preparation process of the negative electrode material is as follows: a coke-based raw material is uniformly mixed with a non-metallic conductive agent, pulverized, and then graphitized to obtain a precursor material; a binder is uniformly mixed with a metal peroxide, and then treated with carbon dioxide to obtain a coating material; the precursor material, coating material, and metallic conductive agent are uniformly mixed and carbonized at high temperature to obtain the negative electrode material. This invention reduces the impedance of the material by adding a non-metallic conductive agent to the coke-based raw material; it improves the liquid retention performance and ion transport rate of the material by reducing the metal peroxide with carbon dioxide, creating nano- and micro-pores; and it enhances the electronic conductivity of the material by adding a metallic conductive agent to the outer shell of the negative electrode material, through which the electron and ion transport rates of the material are improved, thus enhancing the fast-charging performance of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion battery materials technology, and in particular to a negative electrode material, its preparation method, and a battery. Background Technology

[0002] Currently, commercially available lithium-ion battery anode materials are mainly graphite, which is used in energy storage, power batteries, and digital fields due to its low cost, stable material structure, and good cycle performance. However, with the increasing market demand for fast charging performance, graphite anode materials are required to have both fast charging performance and good energy density, but existing graphite anode materials cannot meet these requirements. Summary of the Invention

[0003] The purpose of this invention is to provide a negative electrode material and its preparation method, as well as a battery, in order to solve the technical problems of low electronic conductivity and low energy density of existing graphite composite materials.

[0004] To achieve the above technical objectives, the technical solution adopted by the present invention is as follows:

[0005] In a first aspect, the present invention provides a method for preparing a negative electrode material, comprising the following steps:

[0006] Step S01: Mix coke raw materials with non-metallic conductive agents evenly, pulverize and graphitize them to obtain precursor materials;

[0007] Step S02: After the adhesive and metal peroxide are mixed evenly, carbon dioxide is introduced for treatment to obtain the coating material;

[0008] Step S03: Mix the precursor material, the coating material and the metal conductive agent evenly, and perform high-temperature carbonization treatment to obtain the negative electrode material.

[0009] Further, in step S01, the coke raw material is mixed evenly with a non-metallic conductive agent and then pulverized to 50μm~200μm for graphitization treatment.

[0010] Furthermore, the graphitization treatment is carried out at a temperature of 2800℃~3200℃ for a time of 24h~72h.

[0011] Furthermore, in step S03, the carbonization temperature is 1000℃~1300℃.

[0012] In one embodiment, the non-metallic conductive agent is at least one selected from carbon nanotubes, graphene, carbon fibers, and carbon black; and / or,

[0013] The coke raw material is at least one of petroleum coke, needle coke, and coal-associated coke.

[0014] In one embodiment, the mass ratio of the coke raw material to the non-metallic conductive agent is 100:(10-30).

[0015] This invention reduces the impedance of a graphite material by doping a non-metallic conductive agent into a coke-based raw material and then graphitizing it. Furthermore, the non-metallic conductive agent facilitates heat distribution in the coke-based raw material during graphitization, thereby increasing the catalytic temperature and accelerating the reaction process. In particular, a mass ratio of coke-based raw material to non-metallic conductive agent of 100:(10-30) results in better specific capacity and power performance. Excessive content of the non-metallic conductive agent reduces the initial efficiency and tap density, while insufficient content reduces the power performance.

[0016] In one embodiment, during the carbon dioxide treatment, the flow rate of the carbon dioxide is 100 SCCM to 500 SCCM, the introduction time is 1 h to 6 h, and the temperature is 1000 °C to 1400 °C.

[0017] In one embodiment, the metal peroxide is at least one of sodium peroxide and potassium peroxide; and / or,

[0018] The adhesive is asphalt.

[0019] In one embodiment, the mass ratio of the adhesive to the metal peroxide is 100:(1-5).

[0020] This invention, by adding metal peroxide to the binder and then reducing the metal peroxide with carbon dioxide, generates nano- and micro-sized pores, thereby improving the material's liquid retention capacity and ion transport rate. When the mass ratio of binder to metal peroxide is 100:(1-5), it has the advantages of granulation effect, reducing expansion, and increasing specific capacity. If the ratio is too high, it will reduce cycle performance, while if it is too low, fewer pore structures will be formed, thus reducing specific capacity. Simultaneously, the metal peroxide of this invention forms larger pores and larger interlayer spacing during carbonization, improving the material's fast-charging performance.

[0021] In one embodiment, the metal conductive agent is at least one of silver nanowires, copper nanowires, and nickel nanowires.

[0022] Furthermore, the diameters of the silver nanowires, copper nanowires, and nickel nanowires range from 10 nm to 200 nm.

[0023] In one embodiment, the mass ratio of the precursor material, the coating material, and the metal conductive agent is 100:(3-10):(0.5-2).

[0024] This invention introduces a metallic conductive agent during the mixing of precursor and coating materials. After carbonization, the resulting negative electrode material has a conductive outer shell, enhancing its electronic conductivity. Furthermore, the metallic conductive agent in the outer shell exerts a synergistic effect between the core and shell, improving the electron and ion transport rates and thus enhancing the material's fast-charging performance. In particular, a mass ratio of precursor material, coating material, and metallic conductive agent of 100:(3-10):(0.5-2) results in better power performance, lower expansion, and better cycle performance. Excessive metallic conductive agent content can cause material agglomeration and reduce cycle performance, while insufficient content has limited effect on improving power performance and reducing expansion.

[0025] Secondly, the present invention provides a negative electrode material, which is prepared by the above-described method for preparing negative electrode materials.

[0026] Thirdly, the present invention provides a battery including a negative electrode sheet, the negative electrode sheet comprising the aforementioned negative electrode material.

[0027] Compared with existing technologies, the beneficial effects of the negative electrode material, its preparation method, and the battery provided by this invention are as follows:

[0028] (1) By doping non-metallic conductive agents into coke raw materials, the graphite material obtained after graphitization treatment is doped with conductive agents, thereby reducing the impedance of the material. In addition, the non-metallic conductive agents are beneficial to the heat distribution of coke raw materials during the graphitization process, thereby increasing the catalytic temperature of the material and accelerating the reaction process.

[0029] (2) By adding metal peroxide to the binder and then introducing carbon dioxide to reduce the metal peroxide, nano-micro pores can be generated, which improves the liquid retention performance and ion transport rate of the material.

[0030] (3) By adding a metal conductive agent when mixing the precursor material and the coating material, the shell of the resulting negative electrode material has a conductive agent after carbonization, which improves the electronic conductivity of the material. Furthermore, the metal conductive agent in the shell plays a synergistic effect between the core and the shell, which can improve the electron and ion transport rate of the material, thereby improving the fast charging performance of the material. Attached Figure Description

[0031] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0032] in:

[0033] Figure 1 This is a SEM image of the negative electrode material prepared in Example 1 of the present invention. Detailed Implementation

[0034] The present invention will now be further described in conjunction with the accompanying drawings and specific embodiments. It should be noted that, without conflict, the various embodiments or technical features described below can be arbitrarily combined to form new embodiments.

[0035] The first aspect of this application provides a method for preparing a negative electrode material, including the following steps:

[0036] Step S01: Mix coke raw materials with non-metallic conductive agents evenly, pulverize and graphitize them to obtain precursor materials;

[0037] Step S02: After the adhesive and metal peroxide are mixed evenly, carbon dioxide is introduced for treatment to obtain the coating material;

[0038] Step S03: Mix the precursor material, the coating material and the metal conductive agent evenly, and perform high-temperature carbonization treatment to obtain the negative electrode material.

[0039] It should be noted that the steps S01 and S02 are not sequential; either the precursor material or the coating material can be prepared first.

[0040] In the method for preparing the negative electrode material provided in the first aspect of this application, a non-metallic conductive agent is doped into the coke raw material, and after graphitization, the resulting graphite material is doped with the conductive agent, thereby reducing the impedance of the material. Furthermore, the non-metallic conductive agent, during graphitization, facilitates the heat distribution of the coke raw material, increases the catalytic temperature of the material, and thus accelerates the reaction process. By introducing carbon dioxide to reduce metal peroxides, nano- and micro-pores are generated, improving the liquid retention performance and ion transport rate of the material. By adding a metallic conductive agent when mixing the precursor material and the coating material, and after carbonization, the outer shell of the resulting negative electrode material has a conductive agent, improving the electronic conductivity of the material. Moreover, the metallic conductive agent in the outer shell exerts a synergistic effect between the core and the outer shell, improving the electronic and ion transport rates of the material, thereby enhancing the fast-charging performance of the material. The negative electrode material prepared by the method provided in this embodiment is a porous amorphous carbon and conductive agent-coated graphite composite material.

[0041] A second aspect of this application provides a negative electrode material, which is prepared using the aforementioned method for preparing negative electrode materials. The negative electrode material provided by this application significantly improves fast charging performance and electronic conductivity.

[0042] A third aspect of this application provides a battery including a negative electrode sheet, the negative electrode sheet comprising the aforementioned negative electrode material. By employing the aforementioned negative electrode material, it exhibits better fast-charging performance.

[0043] The following provides specific examples for illustration.

[0044] Example 1

[0045] This embodiment provides a negative electrode material, the preparation method of which includes the following steps:

[0046] Step S1:

[0047] 100g of petroleum coke was mixed with 20g of carbon nanotubes, pulverized to 100μm, and graphitized at 3000℃ for 24h to obtain precursor material A.

[0048] Step S2:

[0049] Mix 100g of asphalt with 3g of sodium peroxide evenly, heat to 1200℃, and introduce carbon dioxide at a flow rate of 300SCCM for 3h to obtain coating material B.

[0050] Step S3:

[0051] 100g of precursor material A, 5g of coating material B and 1g of silver nanowires with a diameter of 100nm were ball-milled and mixed evenly, and then carbonized at 1200℃ for 3h to obtain the anode material, which is a porous amorphous carbon and conductive agent coated graphite composite material.

[0052] Example 2

[0053] This embodiment provides a negative electrode material, the preparation method of which includes the following steps:

[0054] Step S1:

[0055] 100g of needle-like coke raw material was mixed evenly with 10g of graphite, pulverized to 50μm, and graphitized at 2800℃ for 72h to obtain precursor material A.

[0056] Step S2:

[0057] Mix 100g of petroleum asphalt with 1g of potassium peroxide evenly, transfer to a tube furnace and heat to 1000℃, introduce carbon dioxide at a flow rate of 100SCCM for 6h to obtain coating material B.

[0058] Step S3:

[0059] 100g of precursor material A, 3g of coating material B and 0.5g of copper nanowires with a diameter of 10nm were ball-milled and mixed evenly, and then carbonized at 1000℃ for 6h to obtain the anode material, which is a porous amorphous carbon and conductive agent coated graphite composite material.

[0060] Example 3

[0061] This embodiment provides a negative electrode material, the preparation method of which includes the following steps:

[0062] Step S1:

[0063] 100g of coal-based coke was mixed evenly with 30g of carbon fiber, pulverized to 200μm, and graphitized at 3200℃ for 24h to obtain precursor material A.

[0064] Step S2:

[0065] Mix 100g of coal tar pitch with 5g of sodium peroxide evenly, heat to 1400℃, and introduce carbon dioxide at a flow rate of 500 SCCM for 1 hour to obtain coating material B.

[0066] Step S3:

[0067] 100g of precursor material A, 10g of coating material B and 2g of nickel nanowires with a diameter of 200nm were ball-milled and mixed evenly. Then the mixture was heated to 1300℃ and carbonized for 1h to obtain the anode material, which is a porous amorphous carbon and conductive agent coated graphite composite material.

[0068] Comparative Example 1:

[0069] This comparative example provides a negative electrode material. The specific implementation method differs from Example 1 in that carbon nanotubes are not added in step S1 and metal conductivity is not added in step S3. Otherwise, it is the same as Example 1.

[0070] Comparative Example 2:

[0071] This comparative example provides a negative electrode material. The specific implementation method differs from Example 1 in that sodium peroxide material is not added and carbon dioxide gas is not introduced in step S2.

[0072] The detailed preparation process is as follows: 100g of precursor material A obtained in step S1 of Example 1, 10g of asphalt and 2g of nickel nanowires are ball-milled and mixed evenly, and then heated to 1300℃ for carbonization for 1h to obtain the negative electrode material. The negative electrode material is an amorphous carbon and conductive agent coated graphite composite material.

[0073] Comparative Example 3

[0074] This comparative example provides a negative electrode material. The specific implementation method differs from Example 1 in that 50g of carbon nanotubes are doped into 100g of petroleum coke in step S1, and 100g of precursor material A, 5g of coating material B and 6g of silver nanowires are ball-milled and mixed evenly in step S3. The rest is the same as in Example 1.

[0075] Comparative Example 4

[0076] This comparative example provides a negative electrode material. The specific implementation method differs from Example 1 in that 100g of asphalt and 9g of sodium peroxide are mixed evenly in step S2, while the rest is the same as in Example 1.

[0077] Performance testing of the materials prepared in the above embodiments and comparative examples:

[0078] (1) SEM testing

[0079] The negative electrode material prepared in Example 1 was subjected to SEM testing, and the results are as follows: Figure 1 As shown. By Figure 1 It can be seen that the particle size is between 10μm and 15μm, the particle size distribution is reasonable, and there is a granulation and bonding structure.

[0080] (2) Physicochemical performance testing

[0081] The powder conductivity, tap density, specific surface area, powder OI value, and degree of graphitization of the anode materials in Examples 1 to 3 and Comparative Examples 1 to 4 were tested according to the test methods in standard GB / T-24533-2019 "Graphite Anode Materials for Lithium-ion Batteries". The OI value of the materials was tested by XRD. The test results are shown in Table 1.

[0082] Table 1

[0083]

[0084] As shown in Table 1, the conductivity, tap density, specific surface area, and graphitization degree of the anode materials prepared in Examples 1 to 3 are significantly higher than those in the comparative examples, and the powder OI value is lower than that in the comparative examples. The anode materials prepared in Examples 1 to 3 of this invention generate nano- and micro-pores by reducing metal peroxides with carbon dioxide to improve the liquid retention performance and ion transport rate of the material. Furthermore, the electronic conductivity of the material is improved by the metallic conductive agent in the outer shell, thereby increasing the conductivity and reducing the powder OI value. Simultaneously, by adding a non-metallic conductive agent to the coke-based raw materials, the conductive agent facilitates the heat distribution of the coke-based raw materials during graphitization, increasing the catalytic temperature of the material and accelerating the reaction process.

[0085] (3) Button cell battery test

[0086] The negative electrode materials prepared in Examples 1 to 3 and the negative electrode materials prepared in Comparative Examples 1 to 4 were assembled into coin cells according to the following method:

[0087] The negative electrode materials prepared in Examples 1 to 3 and each comparative example were used as negative electrodes and assembled into coin cells with lithium sheets, electrolytes, and separators in a glove box with argon and water contents both below 0.1 ppm. The separator was Celegard 2400; the electrolyte was a LiPF6 solution with a LiPF6 concentration of 1.1 mol / L, and the solvent was a mixed solution obtained by mixing ethylene carbonate (EC) and diethyl carbonate (DMC) in a 1:1 weight ratio.

[0088] The prepared coin cells were labeled A-1, B-1, C-1, D-1, E-1, F-1, and G-1, respectively. The performance of the coin cells was then tested using a blue electrode tester. The test conditions were: 0.1C charge-discharge rate, voltage range of 0.005-2V. The initial discharge specific capacity and initial efficiency were tested. After 3 cycles, the test was stopped, and the coin cell DCR (50% SOC, 25℃) was tested. The test results are shown in Table 2.

[0089] Table 2

[0090]

[0091] As can be seen from Table 2, the coin cells made using the negative electrode materials of Examples 1 to 3 exhibit significantly higher initial discharge capacity and efficiency than the comparative examples. By adding a non-metallic conductive agent to the coke-based raw materials, the conductive agent added during graphitization accelerates carbon rearrangement and enhances the specific capacity of the material. Simultaneously, the outer coating of metallic conductive agent improves the electronic conductivity of the material and reduces the discharge coefficient (DCR). Consequently, the batteries made using the negative electrode materials of Examples 1 to 3 of this invention possess excellent initial discharge capacity and efficiency.

[0092] (4) Performance testing of pouch batteries

[0093] Using the negative electrode materials of Examples 1 to 3 and Comparative Examples 1 to 4 as negative electrode active materials, and the positive electrode active material ternary material (LiNi) 1 / 3 Co 1 / 3 Mn 1 / 3 A 5Ah pouch cell was assembled from O2, electrolyte, and separator. The separator was Celegard 2400, and the electrolyte was a LiPF6 solution (a 1:1 volume ratio mixture of EC and DEC, with a LiPF6 concentration of 1.3 mol / L). The fabricated pouch cells were labeled A-2, B-2, C-2, D-2, E-2, F-2, and G-2, respectively.

[0094] The cycle performance and rate performance of 5Ah pouch cells prepared using the negative electrode materials of Examples 1 to 3 and Comparative Examples 1 to 4 as negative electrode active materials were tested, and the results are shown in Table 3. The test methods are as follows:

[0095] 4.1) Cyclic performance:

[0096] The battery cycle performance was tested at a charge / discharge rate of 1C / 1C and a voltage range of 2.8V-4.2V at a temperature of 25±3℃; the test results are detailed in Table 3.

[0097] 4.2) Rate performance:

[0098] The battery was charged to 100% SOC using a constant current + constant voltage mode at a 2C rate. The constant current ratio was then calculated as constant current capacity / (constant current capacity + constant voltage capacity). The test results are detailed in Table 3.

[0099] Table 3

[0100]

[0101]

[0102] As can be seen from Table 3, the 5Ah pouch batteries prepared using the negative electrode materials of Examples 1 to 3 as negative electrode active materials exhibit significantly higher cycle performance and rate performance than the comparative examples. The negative electrode materials of Examples 1 to 3 of this invention have low powder conductivity, thereby reducing impedance and improving rate performance; simultaneously, the negative electrode materials of each example have high specific surface area, enhancing their liquid retention and absorption capabilities, thus improving cycle performance.

[0103] The above embodiments are merely preferred embodiments of the present invention and should not be construed as limiting the scope of protection of the present invention. Any non-substantial changes and substitutions made by those skilled in the art based on the present invention shall fall within the scope of protection claimed by the present invention.

Claims

1. A method for preparing a negative electrode material, characterized in that, The negative electrode material is a porous amorphous carbon and conductive agent-coated graphite composite material, and the preparation method includes the following steps: Step S01: Mix coke raw materials with non-metallic conductive agents evenly, pulverize and graphitize them to obtain precursor materials; Step S02: After the adhesive and metal peroxide are mixed evenly, carbon dioxide is introduced for treatment to obtain the coating material; Step S03: Mix the precursor material, the coating material and the metal conductive agent evenly, and perform high-temperature carbonization treatment to obtain the negative electrode material; The mass ratio of the coke raw material to the non-metallic conductive agent is 100:(10-30), and the mass ratio of the binder to the metal peroxide is 100:(1-5); the non-metallic conductive agent is at least one of carbon nanotubes, graphene, carbon fiber, and carbon black; the metal peroxide is at least one of sodium peroxide and potassium peroxide; the metallic conductive agent is at least one of silver nanowires, copper nanowires, and nickel nanowires; and the binder is asphalt. In the process of introducing carbon dioxide, the flow rate of carbon dioxide is 100 SCCM to 500 SCCM, the introduction time is 1 h to 6 h, and the temperature is 1000℃ to 1400℃.

2. The method for preparing the negative electrode material as described in claim 1, characterized in that, The coke raw material is at least one of petroleum coke, needle coke, and coal-associated coke.

3. The method for preparing the negative electrode material as described in claim 1, characterized in that, The mass ratio of the precursor material, the coating material, and the metal conductive agent is 100:(3-10):(0.5-2).

4. A negative electrode material, characterized in that, The negative electrode material is prepared using the method for preparing negative electrode materials as described in any one of claims 1 to 3.

5. A battery, characterized in that, It includes a negative electrode sheet, which includes the negative electrode material as described in claim 4.

Citation Information

Patent Citations

  • Method for preparing graphene composite negative electrode material from modified graphene oxide

    CN105977490A

  • Anode material for lithium-ion power battery and preparation method of anode material

    CN108134087A