Method and apparatus for brushing perovskite layer of thin-film solar cells

By introducing a smoothing structure and inert gas protection into the brush coating device, the problems of brush marks in the brush coating method and the susceptibility of crystallization to erosion in the anti-solvent method are solved, achieving film uniformity and stability. It is suitable for the preparation of large-area flexible films and has the advantages of high efficiency and economy.

CN117160762BActive Publication Date: 2026-11-17HUABI NEW ENERGY TECH (SUZHOU) CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211348446.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-31
Publication Date
2026-11-17
Estimated Expiration
2042-10-31

AI Technical Summary

Technical Problem

In existing technologies, the brush coating method is prone to producing brush marks when preparing perovskite solar cells, resulting in uneven film thickness. Furthermore, the anti-solvent method is susceptible to water and oxygen erosion when preparing large-area flexible films in air, making it difficult to meet commercialization requirements.

Method used

A brush coating device for perovskite layers in thin-film solar cells is used, which combines a smoothing structure and a protective structure to ensure that the solution is evenly spread on the substrate. It is also adapted to the anti-solvent method with a short time window through temperature control and inert gas protection.

Benefits of technology

It improves the quality of thin film formation, reduces brush marks, enhances the performance and stability of solar cells, is suitable for large-area production, reduces the requirements for equipment precision and material utilization, and has the advantages of being economical and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117160762B_ABST
    Figure CN117160762B_ABST
Patent Text Reader

Abstract

This invention provides a brushing apparatus and method for coating a perovskite layer in a thin-film solar cell, relating to the field of solar cell technology. The brushing apparatus for coating the perovskite layer includes a brushing structure for brushing a solution onto a substrate; a smoothing structure is provided on the side of the brushing structure away from the brushing direction on the substrate, and the smoothing structure can reach the substrate to smooth the solution on the substrate. This invention can smooth the solution on the substrate through the smoothing structure, resulting in a uniform spread of the solution on the substrate, a uniform film thickness, which is beneficial for improving the film formation quality and optimizing the subsequent performance and stability of the solar cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of solar cell technology, and specifically relates to a method and apparatus for brushing a perovskite layer in a thin-film solar cell. Background Technology

[0002] A solar cell is a thin film of photoelectric semiconductor that generates electricity directly from sunlight. It is a device that converts light energy into electrical energy directly through the photoelectric effect or photochemical effect. As long as the illuminance conditions are met, it can output voltage and generate current when there is a circuit.

[0003] Perovskite solar cells are solar cells that utilize perovskite-type organometal halide semiconductors as light-absorbing materials. Originally, the term "perovskite" referred specifically to the mineral calcium titanate (CaTiO3), but later it came to encompass crystals with the ABX3 structure and similar crystals collectively known as perovskite minerals. Just as improving efficiency is an effective way to reduce costs in many fields, for perovskite solar cells, increasing photoelectric conversion efficiency can effectively reduce the cost of photovoltaic power generation per unit area. However, even with further improvements in efficiency, single-junction cells struggle to break through the theoretical efficiency limit.

[0004] Larger-area perovskite thin films are crucial for the commercialization of perovskite solar cells. The antisolvent method is advantageous for achieving excellent perovskite active layer crystallization and is therefore widely used in perovskite thin film fabrication. Realizing the antisolvent method for fabricating large-area thin-film perovskite solar cells in air has practical commercial significance.

[0005] For example, patent CN 113410399 A discloses a one-step method for preparing perovskite thin films using an antisolvent, in which polymethyl methacrylate-chlorobenzene antisolvent is added dropwise during the spin-coating process of the perovskite precursor solution. The specific steps are as follows:

[0006] S1: Prepare perovskite precursor solution;

[0007] S2: Add polymethyl methacrylate-chlorobenzene antisolvent dropwise during the spin coating process of the perovskite precursor solution;

[0008] S3: Perform thermal annealing to obtain a perovskite thin film.

[0009] The brush coating method, as one of the conventional methods for preparing perovskite active layers for solar cells, has many advantages.

[0010] For example, CN 113968983 A discloses a method for preparing thin films by layer-by-layer brush coating. The method involves uniformly brushing metal salt solution, solvent, and organic ligand solution onto a functionalized substrate to prepare a thin film.

[0011] Compared to other coating processes and methods, brush coating is not limited by sample size, has a simple preparation process, low equipment cost, and has advantages such as fast synthesis speed, high preparation efficiency, controllable reaction temperature, adjustable film area and thickness, applicability to the preparation of various film materials, low cost, and simple operation.

[0012] However, when using the brush coating method to prepare perovskite solar cells, the brush head inevitably produces brush marks during the coating process due to the material of the brush head, resulting in uneven film thickness. This can lead to problems such as low efficiency and reduced reliability of the subsequent solar cells.

[0013] In addition, in the large-area roll-to-roll preparation process of flexible membranes, the time window suitable for preparation by anti-solvent method is often only a few seconds, and the perovskite precursor liquid is easily corroded by water and oxygen when crystallizing in the air.

[0014] In summary, how to provide a brushing device and method that is suitable for a shorter processing time window in the anti-solvent method and can effectively reduce brush marks generated during the brushing process is a technical problem that urgently needs to be solved. Summary of the Invention

[0015] The purpose of this invention is to overcome the shortcomings of the prior art and provide a brush coating device and method for perovskite layers in thin-film solar cells. This device and method can smooth the solution on the substrate, allowing the solution to spread evenly on the substrate. This method is suitable for preparing large-area perovskite flexible films using the air-solvent method.

[0016] The present invention provides a brush coating apparatus for a perovskite layer of a thin-film solar cell, the brush coating apparatus for a thin-film solar cell perovskite layer including a brush coating structure for brush coating a solution on a substrate;

[0017] A smoothing structure is provided on the side of the brushing structure away from the brushing direction of the substrate. The smoothing structure can reach the substrate and thus smooth the solution on the substrate.

[0018] Furthermore, the brushing structure is a roller brush and / or a bristle brush.

[0019] Furthermore, the brush is made of any one or more of animal hair, plant fibers, silicone, acrylic, spandex, and plastic.

[0020] Furthermore, the brush coating structure is provided with a first protective structure, which can cover the brush coating structure and / or smooth out the solution brushed onto the substrate by the brush coating structure.

[0021] Furthermore, it also includes a liquid storage tank for storing antisolvent solution and / or perovskite precursor solution; the aforementioned brush coating structure is installed on a liquid inlet provided at the lower end of the liquid storage tank; the liquid inlet is provided with a plurality of through holes penetrating the liquid inlet, through which the liquid in the aforementioned liquid storage tank flows to the aforementioned brush coating structure.

[0022] Furthermore, the liquid storage tank is equipped with a flow regulating structure, which is used to control the liquid flow rate in the liquid storage tank.

[0023] Furthermore, it also includes a second protective structure; the second protective structure can at least cover the brush coating structure, or can simultaneously cover the liquid storage tank and the brush coating structure;

[0024] The second protective structure is provided with an air inlet, through which gas can enter the second protective structure;

[0025] A temperature control component is provided on the inner side of the second protective structure.

[0026] Furthermore, the infusion connection port is provided with several through holes that penetrate the infusion connection port, through which the liquid in the aforementioned storage tank flows to the aforementioned brush coating structure.

[0027] The present invention also provides a method for brushing a perovskite layer of a thin-film solar cell based on the brushing device described in any one of the above-mentioned methods, comprising the following steps:

[0028] (1) Obtain a perovskite precursor solution, add the perovskite precursor solution to the first storage tank, connect the brush coating structure to the first storage tank, and the first storage tank quantitatively supplies the precursor solution to the brush coating structure.

[0029] (2) Obtain antisolvent solution, add antisolvent solution to another second liquid storage tank, connect the brush coating structure to the second liquid storage tank, and the second liquid storage tank quantitatively supplies antisolvent solution to the brush coating structure;

[0030] (3) Brush coating structure: The aforementioned perovskite precursor solution and antisolvent solution are brushed onto the substrate to form a film.

[0031] Furthermore, in step (3), the brush coating structure brushes the perovskite precursor solution and the antisolvent solution onto the substrate placed on the temperature control device.

[0032] Furthermore, in step (3), the substrate is selected from any one of a thin film substrate, a polymer substrate, and a glass fiber filter membrane.

[0033] By adopting the above technical solution, this invention, as an example, has the following advantages and positive effects compared with the prior art:

[0034] The ability to smooth the solution on the substrate through a smoothing structure allows for uniform spreading of the solution and consistent film thickness, which improves film formation quality and optimizes the performance and stability of subsequent solar cells. Furthermore, by drying the perovskite solution on the substrate, crystallization in the air is prevented, accommodating the shorter processing time window in the anti-solvent method. This reduces the dependence of roll-to-roll processes on the vertical accuracy and flatness of the flexible substrate, offering advantages such as high material utilization, economic efficiency, environmental friendliness, and high controllability and repeatability.

[0035] In addition, the thin-film solar cell devices prepared using the apparatus and method provided by this invention have stable performance, are suitable for large-area production, and are easy to promote. Attached Figure Description

[0036] Figure 1A A schematic diagram of the smoothed perovskite layer structure for thin-film solar cells provided by the present invention.

[0037] Figure 1B A schematic diagram of the liquid storage tank provided by the present invention.

[0038] Figure 2 This is a schematic diagram of the infusion connection port provided by the present invention.

[0039] Figure 3A A schematic diagram of the first protective structure provided by the present invention.

[0040] Figure 3B A side view of the first protective structure provided by the present invention.

[0041] Figure 4 This is a schematic diagram of the brush coating structure provided by the present invention, which is another embodiment.

[0042] Figure 5 A schematic diagram of the second protective structure provided by the present invention.

[0043] Figure 6 This is a schematic diagram of the overall structure of the brush coating device for the perovskite layer of the thin-film solar cell provided by the present invention.

[0044] Figure 7(a) shows a comparative brush coating effect diagram provided by the present invention.

[0045] Figure 7(b) is a 50X microscope image of comparative Figure 7(a).

[0046] Figure 7(c) shows the brushing effect of the brushing device for the perovskite layer of the thin-film solar cell provided by the present invention.

[0047] Figure 7(d) is a 50X microscope image of Figure 7(c) of the embodiment.

[0048] Explanation of reference numerals in the attached figures:

[0049] The perovskite layer coating device for thin-film solar cells includes a first liquid storage tank 110, a second liquid storage tank 111, a flow regulating structure 120, a liquid inlet 130, a brush bristle fixing port 131, a through hole 132, a first protective structure 140, a coating structure 150, brush bristles 151, a smoothing structure 152; a second protective structure 200, an air inlet 210, and a temperature control component 220. Detailed Implementation

[0050] The technical solutions disclosed in this invention will be described in detail below with reference to the accompanying drawings and specific embodiments.

[0051] Techniques and methods known to those skilled in the art may not be discussed in detail, but where appropriate, such techniques and methods should be considered part of the specification. In all examples shown and discussed herein, any specific values ​​should be interpreted as merely exemplary and not as limitations. Therefore, other examples of exemplary embodiments may have different values.

[0052] Obviously, the described embodiments are only a part of the embodiments of this application, not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of this application without inventive effort are within the scope of protection of this application.

[0053] The accompanying drawings are for illustrative purposes only and are schematic diagrams, not actual images. They should not be construed as limiting the scope of this patent. To better illustrate the embodiments of this utility model, some components in the drawings may be omitted, enlarged, or reduced, and do not represent the actual dimensions of the product. It is understandable to those skilled in the art that some well-known structures and their descriptions may be omitted in the drawings.

[0054] Example

[0055] The present invention provides a brush coating device 100 for a perovskite layer of a thin-film solar cell.

[0056] As one of the typical embodiments, as shown in FIG1, the brushing device for the perovskite layer of the thin-film solar cell includes a brushing structure 150 for brushing a solution onto a substrate.

[0057] A smoothing structure 152 is provided on the side of the brushing structure away from the brushing direction of the substrate. The smoothing structure can reach the substrate and thus smooth the solution on the substrate.

[0058] In this embodiment, the smoothing structure is flush with the upper end of the brushing structure, and its longitudinal length is longer than that of the brushing structure. Therefore, the smoothing structure can reach the substrate when the brushing structure moves on the substrate.

[0059] Of course, other settings are also possible, such as setting it at the lower end of the brushing structure on the side away from the substrate brushing direction, or in other positions, as long as the length of the smoothing structure can reach the substrate.

[0060] Thus, when using the brush coating structure 150 for brush coating, it can smooth the solution on the substrate, allowing the solution to be evenly spread on the substrate, thereby improving the film quality during production.

[0061] Optionally, the smoothing structure is a flexible membrane structure.

[0062] In another implementation, such as Figure 1B As shown, the brush coating device for the perovskite layer of the thin-film solar cell also includes a liquid storage tank for storing an antisolvent solution and / or a perovskite precursor solution.

[0063] The liquid storage tank may include a first liquid storage tank 110 and a second liquid storage tank 111, such as Figure 1B As shown, it can be used to store different solutions separately.

[0064] The liquid storage tank is equipped with a flow regulation structure 120, which is used to control the liquid flow rate in the liquid storage tank.

[0065] As an example rather than a limitation, the flow regulation structure can achieve precise, minute, uniform, and continuous output of fluid using micro-pumps already in use in the prior art.

[0066] Of course, besides using the aforementioned liquid storage tank, other methods can also be used to deliver liquid to the brush-coated structure. For example, in... Figure 1A Based on the existing structure, a conduit and a micro-pump are added. The micro-pump provides power and can regulate the flow rate of the liquid output. The liquid moves to the brush coating structure through the conduit connected to the brush coating structure.

[0067] like Figure 1A or Figure 4 As shown, the brushing structure 150 is a roller brush and / or a bristle brush.

[0068] When the brushing structure 150 is a brush, the brush is made of any one or more of animal hair, plant fiber, silicone, acrylic, spandex and plastic.

[0069] By changing the structure of the brush coating and the type of material used, brush coating structures with different degrees of softness can be obtained, thereby better adapting to different needs in production.

[0070] In practice, the brush coating structure can be selected based on the size of the substrate and the type of solution.

[0071] like Figure 1B As shown, the brush coating structure is installed on the liquid inlet 130 provided at the lower end of the liquid storage tank; through the liquid inlet, the liquid storage tank supplies the perovskite precursor solution and / or antisolvent solution to the brush coating structure.

[0072] The infusion connection port is provided with a plurality of through holes 132 penetrating the infusion connection port 130, through which the liquid in the aforementioned liquid storage tank flows to the aforementioned brush coating structure 150.

[0073] When the brushing structure 150 is a brush, the infusion connection port 130 is also provided with a bristle fixing port 131, into which the bristles can be inserted and fixed. As an optional implementation, such as... Figure 2 As shown, the bristle fixing port 131 and the through hole 132 are arranged at intervals and in parallel.

[0074] like Figure 3A and 3B As shown, the brush coating structure is provided with a first protective structure, which can cover the brush coating structure and protect it.

[0075] As an example rather than a limitation, the first protective structure is a flexible membrane structure.

[0076] In this embodiment, the first protective structure 140 can also be used to smooth the solution brushed onto the substrate. The first protective structure is configured such that the vertical length of one side is shorter than the vertical length of the brushing structure, and the vertical length of the other side is longer than the vertical length of the brushing structure. With this configuration, when the brushing structure is applied, the portion of the brushing structure longer than the first protective structure is applied first, and the portion of the first protective structure longer than the brushing structure follows behind, adhering to the solution brushed onto the brushing structure, thus further smoothing the solution.

[0077] Right now, Figure 3A and 3B The first protective structure in the middle can be used as a smoothing structure.

[0078] Alternatively, based on the smoothing structure on the brush coating structure, a first protective structure with the same smoothing function can be set outside the brush coating structure. By combining the smoothing structure with the first protective structure, the smoothing effect can be enhanced.

[0079] In another embodiment, the brushing structure 150 is a roller brush, the structure of which is as follows: Figure 4 As shown. The remaining settings are the same as when the brush structure is 150 and it is a bristle brush, so they will not be described in detail here.

[0080] like Figure 5As shown, the brush coating device 100 for the perovskite layer of the thin-film solar cell also includes a second protective structure 200.

[0081] The second protective structure can at least cover such as Figure 1A The brush coating structure 150 is shown.

[0082] Alternatively, the second protective structure can simultaneously cover both the liquid storage tank and the brush coating structure 150, such as... Figure 6 As shown.

[0083] The second protective structure is provided with an air inlet 210, through which gas can enter the second protective structure.

[0084] Nitrogen is used as an example, not a limitation. In practice, nitrogen enters the second protective structure through inlet 210. Nitrogen not only plays a protective role in the process, but also helps to level and thin the liquid surface.

[0085] Of course, other inert gases are also acceptable.

[0086] A temperature control component 220 is provided on the inner side of the protective cover.

[0087] By way of example and not limitation, the temperature control component can be installed near the liquid storage tank. This temperature control component is used to control and adjust the temperature of the gas entering the second protective structure, as well as the temperature of the liquid inside the storage tank. In practice, the temperature of the temperature control component can be set within the range of 25-40°C.

[0088] The present invention also provides a method for brushing a perovskite layer for a thin-film solar cell based on the above-described brushing device, comprising the following steps:

[0089] (1) Obtain a perovskite precursor solution, add the perovskite precursor solution to the first storage tank, connect the brush coating structure to the first storage tank, and the first storage tank quantitatively supplies the precursor solution to the brush coating structure 140.

[0090] (2) Obtain antisolvent solution, add antisolvent solution to the second storage tank, connect the brush coating structure to the second storage tank, and the second storage tank quantitatively supplies antisolvent solution to the brush coating structure;

[0091] (3) Brush coating structure: The perovskite precursor solution and antisolvent solution are brushed onto the substrate to form a film.

[0092] In step (3), the brush coating structure applies the perovskite precursor solution and the antisolvent solution to the substrate material placed on the temperature control device.

[0093] In step (3), the substrate is selected from any one of a thin film substrate, a polymer substrate, and a glass fiber filter membrane.

[0094] By way of example and not limitation, the substrate is an ITO flexible film substrate coated with a transport layer interface.

[0095] In practice, the brushing speed of the perovskite precursor solution and antisolvent solution can be adjusted on the substrate material by adjusting the brushing structure to meet different production needs.

[0096] The following provides a specific implementation plan for the above method.

[0097] In this embodiment, the perovskite precursor solution, for example, is (FASnI3). 0.5 (MAPbI3) 0.5 .

[0098] The acquisition method is as follows:

[0099] First, FAI and SnI2 are dissolved in DMSO in a molar ratio of 1:1 to prepare a 1M FASnI3 solution.

[0100] Then, a 1M MAPbI3 solution was prepared by dissolving MAI and PbI2 in DMF at a molar ratio of 1:1.

[0101] Both the FASnI3 and MAPbI3 solutions were stirred overnight at 50°C. Then, the FASnI3 and MAPbI3 solutions were mixed at a molar ratio of 1:1 and stirred at 50°C for another 1 hour. The mixture was then filtered through a 0.22 μm filter, allowed to stand for one hour, and then added to the first storage tank to form a perovskite precursor solution.

[0102] Chlorobenzene was added as an antisolvent to the second storage tank.

[0103] A PEDOT:PSS film was prepared on a cleaned ITO substrate. The ITO substrate was placed on a temperature control device, and the temperature was maintained at 100 degrees Celsius. A solution was brushed onto the PEDOT:PSS layer, adjusting the brushing structure to contact the ITO substrate. In this embodiment, the brushing structure was a bristle brush. The perovskite precursor solution was supplied at a flow rate of 30 μL / min. The bristle brush connected to the first reservoir moved to the left at a speed of 3 mm / s, while another bristle connected to the second reservoir brushed the antisolvent solution behind it at a flow rate of 20 μL / min.

[0104] As can be seen from comparative examples 7(a) and (b), brushing produces many brush marks, resulting in poor brushing effect. As can be seen from 7(c) and (d), the brushing device for coating the perovskite layer of thin-film solar cells provided by this invention significantly reduces the brush marks and significantly improves the brushing effect.

[0105] Within the scope of this disclosure, terms such as “comprising” should be interpreted by default as inclusive or open-ended, rather than exclusive or closed, unless expressly defined as such. All technical, scientific, or other terms shall be interpreted as understood by one of those skilled in the art, unless defined as such. Public terms found in dictionaries should not be interpreted in an overly idealistic or impractical manner in the context of the relevant technical documentation, unless expressly defined as such in this disclosure.

[0106] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the present invention. No reference numerals in the claims should be construed as limiting the scope of the claims.

[0107] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.

Claims

1. A brush coating device for a perovskite layer in a thin-film solar cell, characterized in that: The brushing device for the perovskite layer of the thin-film solar cell includes a brushing structure for brushing a solution onto a substrate; A smoothing structure is provided on the side of the brushing structure away from the brushing direction of the substrate. The smoothing structure can reach the substrate and thus smooth the solution on the substrate. The brush coating structure is provided with a first protective structure, which can cover the brush coating structure and / or smooth out the solution brushed onto the substrate by the brush coating structure. It also includes a liquid storage tank for storing antisolvent solution and / or perovskite precursor solution; the aforementioned brush coating structure is installed on the liquid inlet provided at the lower end of the liquid storage tank; the liquid inlet is provided with a plurality of through holes penetrating the liquid inlet, through which the liquid in the aforementioned liquid storage tank flows to the aforementioned brush coating structure; It also includes a second protective structure; the second protective structure can at least cover the brush coating structure, or can cover both the liquid storage tank and the brush coating structure at the same time; The second protective structure is provided with an air inlet, through which gas can enter the second protective structure; A temperature control component is provided on the inner side of the second protective structure; The liquid storage tank is equipped with a flow regulation structure, which is used to control the liquid flow rate in the liquid storage tank.

2. The brush coating device for the perovskite layer of a thin-film solar cell according to claim 1, characterized in that: The brushing structure is a roller brush and / or a bristle brush.

3. The brush coating device for the perovskite layer of a thin-film solar cell according to claim 2, characterized in that: The brush is made of any one or more of animal hair, plant fiber, silicone, acrylic, spandex and plastic.

4. A method for brushing a perovskite layer for a thin-film solar cell based on the brushing apparatus according to any one of claims 1-3, characterized in that, Includes the following steps: (1) Obtain a perovskite precursor solution, add the perovskite precursor solution to the first storage tank, connect the brush coating structure to the first storage tank, and the first storage tank quantitatively supplies the precursor solution to the brush coating structure. (2) Obtain antisolvent solution, add antisolvent solution to another second liquid storage tank, connect the brush coating structure to the second liquid storage tank, and the second liquid storage tank quantitatively supplies antisolvent solution to the brush coating structure; (3) Brush coating structure: The aforementioned perovskite precursor solution and antisolvent solution are brushed onto the substrate to form a film.

5. The method for brushing the perovskite layer of a thin-film solar cell according to claim 4, characterized in that: In step (3), the brush coating structure applies the perovskite precursor solution and the antisolvent solution to the substrate placed on the temperature control device.

6. The method for brushing the perovskite layer of a thin-film solar cell according to claim 5, characterized in that: In step (3), the substrate is selected from any one of a thin film substrate, a polymer substrate, and a glass fiber filter membrane.

Citation Information

Patent Citations

  • Efficient sheet coating machine for processing lead-acid storage battery grid

    CN110787953A

  • Device and method for preparing perovskite film through hot air flow blade coating

    CN111842044A

  • Diatom mud wallboard coating device and production system

    CN207971020U