A spinel-carbon double-coated lithium-rich manganese-based cathode material and its preparation method
By forming a double-coating structure of spinel layer and carbon layer on the surface of lithium-rich manganese-based cathode material, the problems of insufficient electrochemical performance and cycle stability of the material are solved, achieving efficient electrochemical performance improvement and simplified preparation process.
Patent Information
- Application Number
- CN202311111726.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-31
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-08-31
AI Technical Summary
Lithium-rich manganese-based cathode materials suffer from problems such as low initial coulombic efficiency, poor rate capacity, and severe voltage decay. Furthermore, traditional coating methods lead to lattice expansion and contraction, which affects the material's cycle performance.
A lithium-rich manganese-based cathode material is heat-treated with solid organic acid in an air atmosphere to form a double-coated structure of spinel layer and carbon layer. The melting and decomposition of solid organic acid forms a heterojunction structure on the material surface, improving the lattice matching degree.
It significantly improves the electrochemical performance of materials, such as first-cycle coulombic efficiency, discharge specific capacity, cycle rate and rate performance, simplifies the preparation process and reduces costs.
Smart Images

Figure CN117174893B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to lithium-ion batteries, and in particular to a spinel-carbon double-coated lithium-rich manganese-based cathode material and its preparation method. Background Technology
[0002] The rapid development of the electric vehicle market has led to the emergence of high-energy-density lithium-ion batteries. In current lithium-ion battery systems, the capacity mismatch between the positive and negative electrode materials (the positive electrode capacity is nearly an order of magnitude smaller than the negative electrode capacity) severely hinders the development of lithium-ion batteries. Lithium-rich cathode materials are considered one of the most promising candidates for next-generation rechargeable lithium-ion battery cathode materials due to their outstanding specific capacity. Furthermore, lithium-rich manganese-based cathodes reduce the use of expensive cobalt, offering advantages such as low cost, environmental friendliness, and high thermal stability.
[0003] However, lithium-rich manganese-based cathode materials suffer from inherent problems such as low initial coulombic efficiency, poor rate capacity, and severe voltage decay, hindering their further practical application. These problems need to be addressed as soon as possible to alleviate range anxiety and safety concerns in the electricity consumption market.
[0004] Common improvement methods include coating, doping, morphology control, atmosphere treatment, and surface defect engineering. Atmosphere treatment can introduce oxygen and lithium vacancies by consuming surface Li and O atoms, further limiting surface oxygen release. Simultaneously, oxygen and lithium deficiency helps accelerate lithium-ion transport, thereby improving the material's electrochemical performance. However, the surface layer is still corroded by electrolyte products during cycling, which is detrimental to the material's long-term cycling performance. General coating can improve cycling performance by forming a coating layer resistant to electrolyte products during cycling. However, general coating often suffers from lattice mismatch between the bulk and surface coating layers. During cycling, lithium ion extraction and insertion cause lattice expansion and contraction, leading to cracking or even complete breakage of the coating layer.
[0005] To form a coating layer with a high degree of lattice matching between the bulk and the surface coating, acidification is generally employed, using Li / H exchange on the surface to generate a heterojunction structure with a spinel layer / layered bulk. Furthermore, the generated spinel layer can provide 3D Li... + Diffusion channels can accelerate the diffusion rate of lithium ions, but traditional acidification requires liquid acid or the acid to be dissolved in liquid before adding the cathode material. Then, solvent washing, filtration, drying, or evaporation of the solvent are used to obtain the mixed cathode material. The operation is complicated and time-consuming.
[0006] It should be noted that the information disclosed in the background section above is only for understanding the background of this application, and therefore may include information that does not constitute prior art known to those skilled in the art. Summary of the Invention
[0007] This invention provides a spinel-carbon double-coated lithium-rich manganese-based cathode material and its preparation method.
[0008] The technical solution adopted in this application is as follows: In a first aspect, a method for preparing a spinel-carbon double-coated lithium-rich manganese-based cathode material is provided, comprising the following steps: S1. The mixed powder of lithium-rich manganese-based cathode material and solid organic acid is heat-treated in air atmosphere at a predetermined temperature. During the heat treatment process, the solid organic acid is melted and decomposed, thereby sequentially coating the surface of the lithium-rich manganese-based cathode material with a spinel layer and a carbon layer. S2. After the sample is heat-treated in step S1, it is washed and dried to obtain the spinel-carbon double-coated lithium-rich manganese-based cathode material.
[0009] Preferably, in the mixed powder of step S1, the mass ratio of solid organic acid to lithium-rich manganese-based cathode material is greater than 0 and less than or equal to 1.
[0010] Preferably, in step S1, the range of the predetermined temperature is: at least 50°C above the melting point of the solid organic acid and less than 1000°C.
[0011] Preferably, in step S1, the heat treatment time is 30 min to 7 h; more preferably, the heat treatment time is 3 h to 7 h; more preferably, the heat treatment time is 5 h.
[0012] Preferably, the solid organic acid is at least one of citric acid and tannic acid.
[0013] Preferably, the chemical formula of the lithium-rich manganese-based cathode material is xLi2MnO3•(1–x)LiTMO2, wherein TM is at least one of Ni, Mn, and Co, and 0 < x < 1.
[0014] Preferably, the solid organic acid is citric acid, and the predetermined temperature is 200-400℃.
[0015] Preferably, the preparation method includes the following steps: S1, citric acid and Li 1.2 Mn 0.54 Co 0.13 Ni 0.13 O2 was ground and mixed in a mass ratio greater than 0 and less than or equal to 1 to obtain a mixed powder. Then, under an air atmosphere, the temperature was increased from room temperature to 200-400℃ at a rate of 1-5℃ / min for 30 min-7 h. During the heat treatment, the citric acid underwent melting and decomposition, thereby reacting with Li... 1.2Mn 0.54 Co 0.13 Ni 0.13 The surface of O2 is sequentially coated with a spinel layer and a carbon layer; preferably, the heat treatment temperature is 300 ℃ and the heat treatment is 5 h. S2. After the sample is heat-treated in step S1, it is washed with water, filtered and dried to obtain the spinel layer and carbon layer double-coated lithium-rich manganese-based cathode material.
[0016] In a second aspect, a spinel-carbon double-coated lithium-rich manganese-based cathode material prepared by the preparation method described in the first aspect is provided, comprising a lithium-rich manganese-based cathode material, a spinel layer coated on the surface of the lithium-rich manganese-based cathode material, and a carbon layer coated on the surface of the spinel layer.
[0017] This invention offers the following advantages: It directly heat-treats a mixture of lithium-rich manganese-based cathode material and solid organic acid powder in a solid phase at a predetermined temperature under an air atmosphere. During the heat treatment, the solid organic acid melts and decomposes, thereby sequentially coating the surface of the lithium-rich manganese-based cathode material with a spinel layer and a carbon layer. This preparation method is simple, easy to control, and has low production costs, making it suitable for industrial production. Compared to traditional acidification and atmosphere treatment methods, this invention can introduce a spinel and carbon double-coating structure while generating lithium and oxygen vacancies, significantly improving its electrochemical performance (such as first-cycle coulombic efficiency, discharge specific capacity, cycle rate, and rate performance). Attached Figure Description
[0018] Figure 1 This is a schematic diagram of the structure of a preferred embodiment of the lithium-rich manganese-based cathode material with a spinel layer and a carbon layer double coating. Figure 2 The first charge-discharge curves (0.1C) of the CA2 material of Example 1 and the LLO material of Comparative Example 1 are shown. Figure 3 These are discharge specific capacity and coulombic efficiency curves of the CA2 material of Example 1 and the LLO material of Comparative Example 1 under 1 C cycle. Figure 4 These are the median voltage curves of CA2 material in Example 1 and LLO material in Comparative Example 1 under 1 C cycle. Figure 5 This is a discharge specific capacity diagram of the CA2 material of Example 1 and the LLO material of Comparative Example 1 at different rates. Detailed Implementation
[0019] The embodiments of the present invention will be described in detail below. It should be emphasized that the following description is merely exemplary and not intended to limit the scope and application of the present invention. Unless otherwise specified, the embodiments and features in the embodiments of this application can be combined with each other.
[0020] In this article, room temperature refers to the range of 20-40℃.
[0021] One embodiment of the present invention provides a method for preparing a spinel-carbon double-coated lithium-rich manganese-based cathode material, comprising the following steps: S1. The mixed powder of lithium-rich manganese-based cathode material and solid organic acid is heat-treated in air atmosphere at a predetermined temperature. During the heat treatment process, the solid organic acid is melted and decomposed, thereby sequentially coating the surface of the lithium-rich manganese-based cathode material with a spinel layer and a carbon layer. S2. After the sample is heat-treated in step S1, it is washed and dried to obtain the spinel-carbon double-coated lithium-rich manganese-based cathode material.
[0022] Solid organic acids possess the properties of melting and decomposition. At a predetermined temperature, they melt, encapsulating lithium-rich manganese-based cathode material particles. Simultaneously, the carbon dioxide generated from the decomposition of the solid organic acid reacts with the surface, consuming surface oxygen and lithium atoms and introducing oxygen and lithium vacancies. These vacant surfaces undergo rearrangement at high temperatures, forming a spinel layer between the lithium-rich manganese-based cathode material and the carbon layer. After heat treatment, a heterojunction structure with high lattice matching (mainly LiMn2O4) / layered structure is formed, consisting of a spinel layer / layered body and an outermost carbon layer protecting the internal structure from corrosion. Figure 1 As shown, the formed spinel-carbon double-coated lithium-rich manganese-based cathode material includes a lithium-rich manganese-based cathode material 1, a spinel layer 2 coated on the surface of the lithium-rich manganese-based cathode material, and a carbon layer 3 coated on the surface of the spinel layer. Experimental verification shows that the electrochemical performance (such as first-cycle coulombic efficiency, discharge specific capacity, cycle rate, rate performance, etc.) of the final material obtained by the method of this invention is significantly improved.
[0023] In a preferred embodiment, in the mixed powder of step S1, the mass ratio of solid organic acid to lithium-rich manganese-based cathode material is greater than 0 and less than or equal to 1.
[0024] In a preferred embodiment, in step S1, the range of the predetermined temperature is: at least 50°C above the melting point of the solid organic acid and less than 1000°C.
[0025] In a preferred embodiment, the heat treatment time in step S1 is 30 min to 7 h; preferably, the heat treatment time is 3 h to 7 h, and more preferably, the heat treatment time is 5 h.
[0026] In a preferred embodiment, the solid organic acid is at least one of citric acid and tannic acid.
[0027] In a preferred embodiment, the chemical formula of the lithium-rich manganese-based cathode material is xLi2MnO3•(1–x)LiTMO2, wherein TM is at least one of Ni, Mn, and Co, and 0 < x < 1.
[0028] In a preferred embodiment, the solid organic acid is citric acid, and the predetermined temperature is 200-400°C. Citric acid has a melting point of about 150°C and a decomposition temperature of about 170°C. At the preferred temperature of 200-400°C, citric acid melts and decomposes to produce a heterojunction structure with high lattice matching of a spinel layer / layered structure body and an outermost carbon layer that protects the internal structure from corrosion.
[0029] In a preferred embodiment, the preparation method includes the following steps: S1, citric acid and Li 1.2 Mn 0.54 Co 0.13 Ni 0.13 O2 was ground and mixed in a mass ratio greater than 0 and less than or equal to 1 to obtain a mixed powder. Then, under an air atmosphere, the temperature was increased from room temperature to 200-400℃ at a rate of 1-5℃ / min for 30 min-7 h. During the heat treatment, the citric acid underwent melting and decomposition, thereby reacting with Li... 1.2 Mn 0.54 Co 0.13 Ni 0.13 The surface of O2 is sequentially coated with a spinel layer and a carbon layer; preferably, the heat treatment temperature is 300 ℃ and the heat treatment is 5 h. S2. After the sample is heat-treated in step S1, it is washed with water, filtered and dried to obtain the spinel layer and carbon layer double-coated lithium-rich manganese-based cathode material.
[0030] Another embodiment of the present invention provides a spinel-carbon double-coated lithium-rich manganese-based cathode material prepared by the above preparation method, which includes a lithium-rich manganese-based cathode material, a spinel layer coated on the surface of the lithium-rich manganese-based cathode material, and a carbon layer coated on the surface of the spinel layer.
[0031] The following describes specific embodiments of the present invention.
[0032] Example 1 The preparation method of a spinel-carbon double-coated lithium-rich manganese-based cathode material includes the following steps: 1. Weigh out a certain amount of citric acid and Li 1.2 Mn 0.54 Co 0.13 Ni0.13 O2 (citric acid and Li) 1.2 Mn 0.54 Co 0.13 Ni 0.13 The mass ratio of O2 is 1:4, and the mixture is thoroughly ground and mixed in a mortar and pestle; 2. Transfer the well-ground and mixed sample to a ceramic boat, and heat it from room temperature to 300 ℃ at a heating rate of 5 ℃ / min, and heat it in air atmosphere for 5 hours.
[0033] 3. After heat treatment, the sample is washed with water, filtered, and dried to obtain the final sample. The sample is a carbon layer@spinel layer@lithium-rich manganese-based cathode layer structure, that is, a spinel layer and carbon layer double-coated lithium-rich manganese-based cathode material, which is abbreviated as CA2 material in this example.
[0034] Comparative Example 1 Li without any coating treatment 1.2 Mn 0.54 Co 0.13 Ni 0.13 O2, used as the material in Comparative Example 1, is abbreviated as LLO material.
[0035] The materials of Example 1 and Comparative Example 1 were subjected to a series of tests, as shown in Tables 1 and 2 below. Figure 2-4 As shown, where, Figure 2 The graphs show the first charge-discharge curves (0.1 C) for the two materials. Figure 3 These are discharge specific capacity and coulombic efficiency curves for two materials under 1 C cycling. Figure 4 These are median voltage curves for two materials under 1C cycles. Figure 5 This is a discharge specific capacity diagram of two materials at different discharge rates.
[0036] Table 1: Electrochemical properties of LLO and CA2 materials Table 2: Discharge specific capacity of LLO and CA2 materials at different discharge rates From Table 1 and Table 2 and Figure 2-4 It can be seen that the electrochemical performance of the CA2 material in Example 1 is improved as follows: 1. The first-cycle coulombic efficiency and discharge specific capacity of CA2 material are increased compared to LLO material; 2. The cycling rate of CA2 material has been improved: 1 C (1 C = 200 mA g) -1 Under these conditions, the capacity retention of CA2 material increased and voltage decay was suppressed. 3. Improved rate performance of CA2 material: The discharge specific capacity of CA2 material has been improved under different rate conditions.
[0037] The above description provides a further detailed explanation of the present invention in conjunction with specific / preferred embodiments, and it should not be construed that the specific implementation of the present invention is limited to these descriptions. For those skilled in the art, various substitutions or modifications can be made to these described embodiments without departing from the concept of the present invention, and all such substitutions or modifications should be considered within the scope of protection of the present invention. In the description of this specification, the reference to terms such as "an embodiment," "some embodiments," "preferred embodiment," "example," "specific example," or "some examples," etc., indicates that the specific features, structures, materials, or characteristics described in connection with that embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials, or characteristics described can be combined in any suitable manner in one or more embodiments or examples. Without contradiction, those skilled in the art can combine and integrate the different embodiments or examples described in this specification and the features of different embodiments or examples. Although the embodiments of the present invention and their advantages have been described in detail, it should be understood that various changes, substitutions, and modifications can be made herein without departing from the scope of protection of the patent application.
Claims
1. A method for preparing a spinel-carbon double-coated lithium-rich manganese-based cathode material, characterized in that, Includes the following steps: S1. A mixed powder of lithium-rich manganese-based cathode material and solid organic acid is heat-treated in solid form in air at a predetermined temperature for 30 min to 7 h. During the heat treatment, the solid organic acid melts and decomposes. The carbon dioxide generated by the decomposition reacts with the surface, consuming oxygen and lithium atoms on the surface and introducing oxygen vacancies and lithium vacancies. These vacant surfaces rearrange at high temperature, forming a spinel layer between the lithium-rich manganese-based cathode material and the carbon layer. Thus, the surface of the lithium-rich manganese-based cathode material is sequentially coated with a spinel layer and a carbon layer. The solid organic acid is citric acid, the predetermined temperature is 200-400 °C, and the mass ratio of citric acid to lithium-rich manganese-based cathode material is greater than 0 and less than or equal to 0.
25. S2. After the sample is heat-treated in step S1, it is washed and dried to obtain the spinel-carbon double-coated lithium-rich manganese-based cathode material.
2. The preparation method of the spinel-carbon double-coated lithium-rich manganese-based cathode material as described in claim 1, characterized in that: In step S1, the heat treatment time is 3-7 hours.
3. The preparation method of the spinel-carbon double-coated lithium-rich manganese-based cathode material as described in claim 1, characterized in that: In step S1, the heat treatment time is 5 hours.
4. The preparation method of the spinel-carbon double-coated lithium-rich manganese-based cathode material as described in claim 1, characterized in that: In step S1, the heat treatment temperature is 300 ℃.
5. The method for preparing the spinel-carbon double-coated lithium-rich manganese-based cathode material as described in claim 1, characterized in that: The chemical formula of the lithium-rich manganese-based cathode material is xLi2MnO3•(1–x)LiTMO2, where TM is at least one of Ni, Mn, and Co, and 0 < x < 1.
6. The method for preparing the spinel-carbon double-coated lithium-rich manganese-based cathode material as described in claim 1, characterized in that, The preparation method includes the following steps: S1, citric acid is mixed with Li 1.2 Mn 0.54 Co 0.13 Ni 0.13 O2 in a mass ratio greater than 0 and less than or equal to 0.25 to obtain a mixed powder, then heated from room temperature to 200-400°C at a temperature increase rate of 1-5°C / min under an air atmosphere, and heat treated for 30 min-7 h, during which the citric acid is melted and decomposed, thereby sequentially coating a spinel layer and a carbon layer on the surface of Li 1.2 Mn 0.54 Co 0.13 Ni 0.13 O2. S2. After the sample is heat-treated in step S1, it is washed with water, filtered and dried to obtain the spinel layer and carbon layer double-coated lithium-rich manganese-based cathode material.
Citation Information
Patent Citations
Lithium-rich manganese-based composite positive electrode material and preparation method and application thereof
CN114665069A
Positive electrode material and preparation method thereof, positive electrode plate and secondary battery