A GH3230 alloy material, a GH3230 alloy printing method and its application
By adjusting the composition of GH3230 alloy and optimizing printing process parameters, combined with hot isostatic pressing and solution treatment, the microcrack problem of GH3230 alloy printed parts was solved, and high-performance GH3230 alloy parts were achieved.
Patent Information
- Application Number
- CN202310991414.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2023-07-05
- Filing Date
- 2023-08-08
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-08-08
AI Technical Summary
Existing GH3230 alloy printed parts have a large number of microcracks, which affect their mechanical properties and cannot meet the requirements of QJ/DT 0160044 and Q/GYB 05062 standards.
By adjusting the composition of the GH3230 alloy, controlling the content of C, Si, and Mn elements, and using selective laser melting technology combined with hot isostatic pressing and solution treatment, the printing process parameters, such as laser power, scanning speed, and preheating temperature, were optimized to eliminate microcracks and improve mechanical properties.
It achieves complete densification and a balance of mechanical properties in GH3230 alloy printed parts, with mechanical properties far exceeding standard requirements. It eliminates microcracks and pores and improves the plasticity of printed parts.
Smart Images

Figure CN117187625B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of additive manufacturing (AM) technology, and in particular to a GH3230 alloy material, a GH3230 alloy printing method and its application. Background Technology
[0002] Selective laser melting (SLM) forming technology can directly form complex parts without the use of molds, demonstrating strong technological advantages in the manufacturing of complex structural components. In recent years, this technology has been widely used in the aerospace field. Existing processing methods for GH3230 alloy mainly focus on traditional manufacturing processes such as welding and forging. However, due to their low yield and long production cycle, these methods have long hindered the rapid iteration and upgrading of my country's aerospace equipment. In recent years, with the rapid development of selective laser melting (SLM) technology, a new approach has been provided for the forming of aerospace parts that do not require special molds, are customizable, have short production cycles, and are integrated. GH3230 is often used in the combustion chambers of advanced military aero engines. Due to the limitations of its application scenarios, the requirements for the manufacturing precision and mechanical properties of the parts are extremely stringent. GH3230 not only possesses excellent high-temperature mechanical properties but also exhibits extremely strong oxidation resistance and thermal stability.
[0003] Existing printing processes produce GH3230 parts with numerous microcracks, which significantly negatively impact mechanical properties. Patent CN202110281917.3 provides a method to eliminate microcracks by adding TiB2 powder to GH3230 powder. This method requires high-speed, dual-centrifugal mixing of the two powders and involves parameters related to material mixing (such as rotation speed, time, ratio, and dosage). However, this approach does not address subsequent material processing and cannot meet the high mechanical performance requirements (it does not meet the requirements of standards QJ / DT 0160044 and Q / GYB 05062).
[0004] Given the current deficiencies in the fabrication of GH3230 parts, it is necessary to make improvements. Summary of the Invention
[0005] In view of this, the present invention proposes a GH3230 alloy material, a GH3230 alloy printing method and application, in order to solve the technical problems existing in the prior art.
[0006] In a first aspect, the present invention provides a GH3230 alloy material comprising the following elements: Cr, Fe, C, Mn, Si, Mo, W, Cu, Co, Al, Ti, La, B, P, S, Ni; wherein the mass content of C is 0.06-0.08%, the mass content of Si is 0.3-0.40%, and the mass content of Mn is 0.35-0.50%.
[0007] Preferably, the GH3230 alloy material has a particle size of 15–53 μm.
[0008] Secondly, the present invention also provides a method for printing GH3230 alloy, comprising the following steps:
[0009] Provide the aforementioned GH3230 alloy material;
[0010] The GH3230 alloy material was printed using selective laser melting technology to obtain the GH3230 alloy.
[0011] Preferably, the process parameters controlled during the printing process of the GH3230 alloy are: laser power 75-150W, scanning speed 1000-1400mm / s, track spacing 80-110μm, printing layer thickness 30-40μm, and laser spot diameter 60-80μm.
[0012] Preferably, the GH3230 alloy printing method further includes preheating the printing substrate before printing the GH3230 alloy material, with a preheating temperature of 150-300°C.
[0013] Preferably, in the GH3230 alloy printing method, the scanning strategy used during the printing process is chessboard scanning, and the chessboard size is 800-8000μm.
[0014] Preferably, the GH3230 alloy printing method further includes hot isostatic pressing of the GH3230 alloy after printing the GH3230 alloy material to obtain the GH3230 alloy.
[0015] Preferably, in the GH3230 alloy printing method, the hot isostatic pressing treatment specifically includes: treating the GH3230 alloy at a temperature of 1050-1250℃ and a pressure of 105-160MPa for 1-3 hours.
[0016] Preferably, the GH3230 alloy printing method further includes solution treatment of the GH3230 alloy after hot isostatic pressing.
[0017] Preferably, in the GH3230 alloy printing method, the solution treatment specifically includes: heating the GH3230 alloy to 1100-1230℃ and performing a solution treatment for 0.5-3 hours.
[0018] Preferably, the GH3230 alloy printing method further includes baking the GH3230 alloy material before printing it, wherein the baking temperature is 100-110°C and the baking time is 4-8 hours.
[0019] Thirdly, the present invention also provides an application of the GH3230 alloy material or the GH3230 alloy prepared by the printing method described above in the manufacture of mechanical equipment parts.
[0020] 1. The GH3230 alloy material of the present invention, according to the composition table of GH3230, selects C, Si and Mn contents of 0.06-0.08wt% (standard is 0.05-0.15wt%), 0.3-0.40wt% (standard is 0.25-0.75wt%), and 0.35-0.50wt% (standard is 0.30-1.00wt%), respectively. By controlling the mass content of C, Si and Mn elements, the present invention can reduce the impact of thermal stress generated during the subsequent selective laser melting technology for printing and reduce the sensitivity of the alloy to cracking.
[0021] 2. The GH3230 alloy printing method of the present invention controls the following process parameters during the printing process: laser power 75-150W, scanning speed 1000-1400mm / s, track spacing 80-110μm, printing layer thickness 30-40μm, and laser spot diameter 60-80μm. By adopting the above printing process parameters, the problem of a large number of microcracks in GH3230 alloy printed parts can be eliminated.
[0022] 3. The GH3230 alloy printing method of the present invention further includes preheating the printing substrate before printing the GH3230 alloy material. Preheating the printing substrate reduces the residual stress generated during the printing process and reduces the risk of crack formation.
[0023] 4. The GH3230 alloy printing method of the present invention includes hot isostatic pressing and solution treatment of GH3230 alloy, which can further achieve complete densification and balance of mechanical properties inside the GH3230 alloy printed parts; the GH3230 alloy printed parts prepared by the present invention have no internal defects or only a few microcracks or pores, and the mechanical properties of the printed parts far exceed the requirements of QJ / DT 0160044 and Q / GYB 05062 standards, and the plasticity of the printed parts is optimized compared with the patent CN202110281917.3. Attached Figure Description
[0024] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0025] Figure 1 The image shows a metallographic photograph of the GH3230 alloy after polishing following printing in Example 2.
[0026] Figure 2 The image shows a metallographic photograph of the GH3230 alloy after polishing following printing in Comparative Example 1.
[0027] Figure 3 The image shows a metallographic photograph of the GH3230 alloy after polishing following printing in Example 5.
[0028] Figure 4 Metallographic images of GH3230 alloy after hot isostatic pressing and solution treatment in Example 4, after polishing.
[0029] Figure 5 Metallographic images of GH3230 alloy after hot isostatic pressing and solution treatment in Example 6, after polishing.
[0030] Figure 6 Metallographic images of GH3230 alloy after hot isostatic pressing and solution treatment in Example 7, after polishing.
[0031] Figure 7 The image shows a metallographic photograph of the GH3230 alloy after hot isostatic pressing and solution treatment in Example 8, after polishing. Detailed Implementation
[0032] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0033] To better understand the invention and not to limit its scope, all figures indicating amounts, percentages, and other numerical values used in this application should, in all cases, be understood to be modified by the word "approximately." Therefore, unless specifically stated otherwise, the numerical parameters listed in the specification and appended claims are approximate values and may vary depending on the desired properties being sought. Each numerical parameter should at least be considered as obtained based on reported significant figures and through conventional rounding methods.
[0034] It should be noted that the order of description of the following embodiments is not intended to limit the preferred order of embodiments. Furthermore, in the description of this application, the term "comprising" means "including but not limited to". Various embodiments of the present invention may exist in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a rigid limitation on the scope of the invention; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single digits within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. Additionally, whenever a numerical range is referred to herein, it means including any referenced number (fraction or integer) within the referred range.
[0035] While various embodiments of the invention have been shown and described herein, it will be apparent to those skilled in the art that such embodiments are provided by way of example only. Many modifications, alterations, and alternatives will occur to those skilled in the art without departing from the spirit and essence of the invention. It should be understood that various alternatives to the embodiments of the invention described herein may be employed in the practice of the invention. The appended claims are intended to define the scope of protection of the invention and therefore cover modular compositions, equivalents, or alternatives within the scope of these claims.
[0036] This invention provides a GH3230 alloy material comprising the following elements: Cr, Fe, C, Mn, Si, Mo, W, Cu, Co, Al, Ti, La, B, P, S, and Ni; wherein the mass content of C is 0.05-0.08%, the mass content of Si is 0.25-0.40%, and the mass content of Mn is 0.30-0.50%.
[0037] It should be noted that, according to the composition table of GH3230, the contents of C, Si, and Mn in the GH3230 alloy material of this invention are selected to be 0.06-0.08 wt% (standard is 0.05-0.15 wt%), 0.3-0.40 wt% (standard is 0.25-0.75 wt%), and 0.35-0.50 wt% (standard is 0.30-1.00 wt%), respectively. By controlling the mass content of C, Si, and Mn elements, this application can reduce the impact of thermal stress generated during the subsequent selective laser melting technology for printing and reduce the sensitivity of the alloy to cracking.
[0038] In some embodiments, the GH3230 alloy material comprises the following elements by mass fraction: Cr 21.7%, Fe 0.2%, C 0.05-0.15wt%, Mn 0.30-1.00wt%, Si 0.25-0.75wt%, Mo 2.31%, W 13.64%, Cu ≤0.03%, Co ≤0.03%, Al 0.29%, Ti ≤0.03%, La 0.022%, B 0.009%, P ≤0.005%, S 0.012%, and the balance Ni.
[0039] Specifically, the existing GH3230 alloy includes the following elements by mass fraction: Cr 21.7%, Fe 0.2%, C 0.05~0.15wt%, Mn 0.30~1.00wt%, Si 0.25~0.75wt%, Mo 2.31%, W 13.64%, Cu≤0.03%, Co≤0.03%, Al 0.29%, Ti≤0.03%, La 0.022%, B 0.009%, P≤0.005%, S 0.012%, and the balance Ni.
[0040] Further preferred, the GH3230 alloy material comprises the following elements by mass fraction: Cr 21.7%, Fe 0.2%, C 0.06-0.08%, Mn 0.35-0.50%, Si 0.3-0.40%, Mo 2.31%, W 13.64%, Cu ≤0.03%, Co ≤0.03%, Al 0.29%, Ti ≤0.03%, La 0.022%, B 0.009%, P ≤0.005%, S 0.012%, and the balance Ni.
[0041] In some embodiments, the particle size of the GH3230 alloy material is 15–53 μm.
[0042] Based on the same inventive concept, this invention also provides a method for printing GH3230 alloy, comprising the following steps:
[0043] S1. Provide the above-mentioned GH3230 alloy material;
[0044] S2. Selective laser melting technology is used to print GH3230 alloy material to obtain GH3230 alloy.
[0045] In some embodiments, the process parameters controlled during the printing process are: laser power 75-150W, scanning speed 1000-1400mm / s, track spacing 80-110μm, printing layer thickness 30-40μm, and laser spot diameter 60-80μm.
[0046] Preferably, the process parameters controlled during the printing process are: laser power 125W, scanning speed 1350mm / s, track spacing 80μm, printing layer thickness 30μm, and laser spot diameter 60μm.
[0047] By adopting the above-mentioned printing process parameters, this application can eliminate the problem of numerous microcracks in GH3230 alloy printed parts.
[0048] In some embodiments, the printing substrate is preheated before the GH3230 alloy material is printed, and the preheating temperature is 150-300°C.
[0049] In the above embodiments, it is necessary to preheat the printing substrate. The printing substrate is made of 304 stainless steel, the preheating temperature is 150-300℃, and the preheating time is 5-10 minutes. Preheating the printing substrate reduces the residual stress generated during the printing process and reduces the risk of cracking.
[0050] In some embodiments, a chessboard scanning strategy is used during the printing process, with a chessboard size of 800–8000 μm.
[0051] In the above embodiments, the smaller the chessboard size is, the more overlapping areas of the molten pool, resulting in a larger proportion of heat energy absorbed by the heat-affected zone (HAZ), which may lead to keyhole defects caused by local overmelting of the molten pool. However, the finer the chessboard scanning (i.e., the smaller the chessboard size), the more positive the effect on reducing residual stress. To balance the situation of hole defects and microcracks, a chessboard size of 4000 μm is preferred.
[0052] In some embodiments, after printing GH3230 alloy material to obtain GH3230 alloy, the GH3230 alloy is further subjected to hot isostatic pressing treatment.
[0053] In some embodiments, hot isostatic pressing specifically includes treating the GH3230 alloy at a temperature of 1050-1250°C and a pressure of 105-160 MPa for 1-3 hours.
[0054] Even after optimizing the printing process, some pores and microcracks will inevitably remain inside the GH3230 alloy, but the defect rate is generally less than 0.5%. Hot isostatic pressing is an important means to eliminate pores and cracks in important structural components and improve mechanical properties. Under high temperature and high pressure, the GH3230 alloy material undergoes recovery and recrystallization, which improves its plasticity and creep capacity, enhances the diffusion capacity of atoms and vacancies, and makes it easier to eliminate pores.
[0055] Specifically, in the above embodiments, after the GH3230 alloy is subjected to hot isostatic pressing, the GH3230 alloy is also cooled by furnace cooling.
[0056] In some embodiments, the GH3230 alloy is further subjected to solution treatment after hot isostatic pressing.
[0057] In some embodiments, the solution treatment specifically includes heating the GH3230 alloy to 1100-1230°C and performing a solution treatment for 0.5-3 hours.
[0058] Solution treatment is the most basic and important heat treatment method for high-temperature alloys. There are generally three purposes for solution treatment: First, solution treatment can make the part have a uniform and suitable grain size; second, solution treatment can intensify the movement of atoms and make the microstructure more uniform; third, solution treatment can eliminate or reduce the residual stress in the alloy.
[0059] In the above embodiments, after the GH3230 alloy is solution treated, the GH3230 alloy is also cooled by argon cooling or water cooling.
[0060] In some embodiments, during the solution treatment process, the GH3230 alloy is heated from room temperature to 550-650°C within 80-100 minutes and held at that temperature for 20-40 minutes, and then heated to 1100-1230°C within 80-100 minutes for 0.5-3 hours.
[0061] By performing hot isostatic pressing and solution treatment on GH3230 alloy, the complete internal density and mechanical properties of GH3230 alloy printed parts can be further achieved.
[0062] In some embodiments, before printing the GH3230 alloy material, the GH3230 alloy material is baked, wherein the baking temperature is 100-110°C and the baking time is 4-8 hours.
[0063] In some embodiments, the equipment used by the present invention for printing GH3230 alloy material includes metal additive manufacturing equipment such as Hanbang Technology HBD-150, HBD-280, and HBD-350.
[0064] The GH3230 alloy printing method of this invention can directly form complex parts without the use of molds, featuring high design flexibility, short R&D cycle, and low printing cost. This invention reduces the risk of microcracks and voids in GH3230 alloy printed parts by adding preheating of the printing substrate and optimizing the scanning strategy in the printing process. It also achieves higher performance GH3230 alloy parts by combining hot isostatic pressing and solution treatment processes. The hot isostatic pressing and solution treatment processes are suitable for mass production, allowing for large-scale post-processing of materials per batch, resulting in low cost and easy large-scale promotion. This method supplements the original printing process and improves the mechanical properties. In summary, by combining the optimization of the printing process with the design of hot isostatic pressing and solution treatment, this invention can also eliminate microcracks, and the resulting parts can meet high mechanical performance requirements. The GH3230 alloy printed parts prepared by this invention have no internal microcracks or pores, and the mechanical properties of the printed parts far exceed the requirements of QJ / DT 0160044 and Q / GYB 05062 standards. Compared with the patent CN202110281917.3, the plasticity of the printed parts has been optimized.
[0065] Based on the same inventive concept, the present invention also provides an application of the above-mentioned GH3230 alloy material or the GH3230 alloy prepared by the above-mentioned printing method in the manufacture of mechanical equipment parts.
[0066] Specifically, the aforementioned mechanical equipment components include, but are not limited to, aerospace components, such as aircraft engine combustion chambers, i.e., GH3230 alloy material or the prepared GH3230 alloy can be used to prepare military aircraft engine combustion chambers.
[0067] The following further illustrates the GH3230 alloy material, GH3230 alloy printing method, and application of this application with specific embodiments. This section further describes the content of the present invention in conjunction with specific embodiments, but should not be construed as limiting the present invention. Unless otherwise specified, the technical means used in the embodiments are conventional means well known to those skilled in the art. Unless otherwise specified, the reagents, methods, and equipment used in the present invention are conventional reagents, methods, and equipment in the art.
[0068] Example 1
[0069] This embodiment provides a GH3230 alloy material, comprising the following elements by mass fraction: Cr 21.7%, Fe 0.2%, C 0.06-0.08%, Mn 0.35-0.50%, Si 0.3-0.40%, Mo 2.31%, W 13.64%, Cu 0.03%, Co 0.03%, Al 0.29%, Ti 0.03%, La 0.022%, B 0.009%, P 0.005%, S 0.012%, and the balance Ni;
[0070] The average particle size of the GH3230 alloy material is 30μm.
[0071] Example 2
[0072] This embodiment provides a GH3230 alloy printing method, including the following steps:
[0073] S1. Provide the GH3230 alloy material as described in Example 1;
[0074] S2. Selective laser melting technology is used to print GH3230 alloy material to obtain GH3230 alloy;
[0075] Before printing the GH3230 alloy material, the GH3230 alloy material is baked at a temperature of 105℃ for 6 hours.
[0076] Before printing GH3230 alloy material, the printing substrate is preheated at a temperature of 200℃ for 8 minutes. The printing substrate is made of 304 stainless steel.
[0077] The process parameters controlled during the printing process are: laser power 125W, scanning speed 1350mm / s, track spacing 80μm, printing layer thickness 30μm, and laser spot diameter 60μm.
[0078] During the printing process, a chessboard scanning strategy was selected, with a chessboard size of 4000μm;
[0079] The equipment used for printing and molding is the Hanbang Technology HBD-150 metal additive manufacturing equipment.
[0080] Example 3
[0081] This embodiment provides a GH3230 alloy printing method, including the following steps:
[0082] S1. Provide the GH3230 alloy material as described in Example 1;
[0083] S2. Selective laser melting technology is used to print GH3230 alloy material to obtain GH3230 alloy;
[0084] S3. Solution treatment is performed on the GH3230 alloy in S2;
[0085] Before printing the GH3230 alloy material, the GH3230 alloy material is baked at a temperature of 105℃ for 6 hours.
[0086] Before printing GH3230 alloy material, the printing substrate is preheated at a temperature of 250℃ for 8 minutes. The printing substrate is made of 304 stainless steel.
[0087] The process parameters controlled during the printing process are: laser power 125W, scanning speed 1350mm / s, track spacing 80μm, printing layer thickness 30μm, and laser spot diameter 60μm.
[0088] During the printing process, a chessboard scanning strategy was selected, with a chessboard size of 4000μm;
[0089] The equipment used for printing and molding is the Hanbang Technology HBD-150 metal additive manufacturing equipment;
[0090] The solution treatment specifically includes: heating the GH3230 alloy from room temperature to 600℃ within 90 minutes and holding it at that temperature for 30 minutes, then continuing to heat it to 1180℃ within 90 minutes, performing a solution treatment for 2 hours, and then cooling the GH3230 alloy with argon.
[0091] Example 4
[0092] This embodiment provides a GH3230 alloy printing method, including the following steps:
[0093] S1. Provide the GH3230 alloy material as described in Example 1;
[0094] S2. Selective laser melting technology is used to print GH3230 alloy material to obtain GH3230 alloy;
[0095] S3. The GH3230 alloy obtained in S2 is subjected to hot isostatic pressing treatment.
[0096] S4. Solution treatment is performed on the GH3230 alloy after hot isostatic pressing in S3.
[0097] Before printing the GH3230 alloy material, the GH3230 alloy material is baked at a temperature of 105℃ for 6 hours.
[0098] Before printing GH3230 alloy material, the printing substrate is preheated at a temperature of 250℃ for 8 minutes. The printing substrate is made of 304 stainless steel.
[0099] The process parameters controlled during the printing process are: laser power 125W, scanning speed 1350mm / s, track spacing 80μm, printing layer thickness 30μm, and laser spot diameter 60μm.
[0100] During the printing process, a chessboard scanning strategy was selected, with a chessboard size of 4000μm;
[0101] The equipment used for printing and molding is the Hanbang Technology HBD-150 metal additive manufacturing equipment;
[0102] The hot isostatic pressing process specifically includes: treating the GH3230 alloy at a temperature of 1150℃ and a pressure of 135MPa for 2 hours, and then cooling the GH3230 alloy in the furnace.
[0103] The solution treatment specifically includes: heating the GH3230 alloy from room temperature to 600℃ within 90 minutes and holding it at that temperature for 30 minutes, then continuing to heat it to 1180℃ within 90 minutes, performing a solution treatment for 2 hours, and then cooling the GH3230 alloy with argon.
[0104] Example 5
[0105] This embodiment provides a GH3230 alloy printing method, including the following steps:
[0106] S1. Provide the GH3230 alloy material as described in Example 1;
[0107] S2. Selective laser melting technology is used to print GH3230 alloy material to obtain GH3230 alloy;
[0108] Before printing the GH3230 alloy material, the GH3230 alloy material is baked at a temperature of 105℃ for 6 hours.
[0109] Before printing GH3230 alloy material, the printing substrate is preheated at a temperature of 250℃ for 8 minutes. The printing substrate is made of 304 stainless steel.
[0110] The process parameters controlled during the printing process are: laser power 125W, scanning speed 1350mm / s, track spacing 80μm, printing layer thickness 30μm, and laser spot diameter 60μm.
[0111] During the printing process, a chessboard scanning strategy was selected, with a chessboard size of 4000μm;
[0112] The equipment used for printing and molding is the Hanbang Technology HBD-150 metal additive manufacturing equipment.
[0113] Example 6
[0114] This embodiment provides a GH3230 alloy printing method, including the following steps:
[0115] S1. Provide GH3230 alloy material;
[0116] S2. Selective laser melting technology is used to print GH3230 alloy material to obtain GH3230 alloy;
[0117] S3. The GH3230 alloy obtained in S2 is subjected to hot isostatic pressing treatment.
[0118] S4. Solution treatment is performed on the GH3230 alloy after hot isostatic pressing in S3.
[0119] Before printing the GH3230 alloy material, the GH3230 alloy material is baked at a temperature of 105℃ for 6 hours.
[0120] Before printing GH3230 alloy material, the printing substrate is preheated at a temperature of 250℃ for 8 minutes. The printing substrate is made of 304 stainless steel.
[0121] The process parameters controlled during the printing process are: laser power 150W, scanning speed 1000mm / s, track spacing 80μm, printing layer thickness 30μm, and laser spot diameter 60μm.
[0122] During the printing process, a chessboard scanning strategy was selected, with a chessboard size of 4000μm;
[0123] The equipment used for printing and molding is the Hanbang Technology HBD-150 metal additive manufacturing equipment;
[0124] The hot isostatic pressing process specifically includes: treating the GH3230 alloy at a temperature of 1200℃ and a pressure of 150MPa for 3.5h, and then cooling the GH3230 alloy in the furnace.
[0125] The solution treatment specifically includes: heating the GH3230 alloy from room temperature to 600℃ within 90 minutes and holding it at that temperature for 30 minutes, then continuing to heat it to 1200℃ within 90 minutes, performing a solution treatment for 1 hour, and then cooling the GH3230 alloy with argon.
[0126] The GH3230 alloy material contains the following elements by mass fraction: Cr 21.70%, Mo 2.31%, W 13.64%, Co 0.03%, Fe 0.20%, Si 0.3%, P 0.005%, B 0.009%, Cu 0.03%, Mn 0.35%, Al 0.29%, La 0.022%, Ti 0.03%, O 0.010%, N 0.0029%, C 0.06%, S 0.0012%, with the remainder being Ni.
[0127] Example 7
[0128] This embodiment provides a GH3230 alloy printing method, including the following steps:
[0129] S1. Provide GH3230 alloy material;
[0130] S2. Selective laser melting technology is used to print GH3230 alloy material to obtain GH3230 alloy;
[0131] S3. The GH3230 alloy obtained in S2 is subjected to hot isostatic pressing treatment.
[0132] S4. Solution treatment is performed on the GH3230 alloy after hot isostatic pressing in S3.
[0133] Before printing the GH3230 alloy material, the GH3230 alloy material is baked at a temperature of 105℃ for 6 hours.
[0134] Before printing GH3230 alloy material, the printing substrate is preheated at a temperature of 250℃ for 8 minutes. The printing substrate is made of 304 stainless steel.
[0135] The process parameters controlled during the printing process are: laser power 150W, scanning speed 1050mm / s, track spacing 80μm, printing layer thickness 30μm, and laser spot diameter 60μm.
[0136] During the printing process, a chessboard scanning strategy was selected, with a chessboard size of 4000μm;
[0137] The equipment used for printing and molding is the Hanbang Technology HBD-150 metal additive manufacturing equipment;
[0138] The hot isostatic pressing process specifically includes: treating the GH3230 alloy at a temperature of 1200℃ and a pressure of 150MPa for 3.5h, and then cooling the GH3230 alloy in the furnace.
[0139] The solution treatment specifically includes: heating the GH3230 alloy from room temperature to 600℃ within 90 minutes and holding it at that temperature for 30 minutes, then continuing to heat it to 1200℃ within 90 minutes, performing a solution treatment for 1 hour, and then cooling the GH3230 alloy with argon.
[0140] The GH3230 alloy material contains the following elements by mass fraction: Cr 20.48%, Mo 1.44%, W 13.93%, Co 0.37%, Fe 1.55%, Si 0.35%, P 0.001%, B 0.001%, Cu 0.037%, Mn 0.4%, Al 0.32%, La 0.013%, Ti 0.021%, O 0.029%, N 0.0036%, C 0.07%, S 0.0031%, with the remainder being Ni.
[0141] Example 8
[0142] This embodiment provides a GH3230 alloy printing method, including the following steps:
[0143] S1. Provide GH3230 alloy material;
[0144] S2. Selective laser melting technology is used to print GH3230 alloy material to obtain GH3230 alloy;
[0145] S3. The GH3230 alloy obtained in S2 is subjected to hot isostatic pressing treatment.
[0146] S4. Solution treatment is performed on the GH3230 alloy after hot isostatic pressing in S3.
[0147] Before printing the GH3230 alloy material, the GH3230 alloy material is baked at a temperature of 105℃ for 6 hours.
[0148] Before printing GH3230 alloy material, the printing substrate is preheated at a temperature of 250℃ for 8 minutes. The printing substrate is made of 304 stainless steel.
[0149] The process parameters controlled during the printing process are: laser power 150W, scanning speed 1050mm / s, track spacing 80μm, printing layer thickness 30μm, and laser spot diameter 60μm.
[0150] During the printing process, a chessboard scanning strategy was selected, with a chessboard size of 4000μm;
[0151] The equipment used for printing and molding is the Hanbang Technology HBD-150 metal additive manufacturing equipment;
[0152] The hot isostatic pressing process specifically includes: treating the GH3230 alloy at a temperature of 1200℃ and a pressure of 150MPa for 3.5h, and then cooling the GH3230 alloy in the furnace.
[0153] The solution treatment specifically includes: heating the GH3230 alloy from room temperature to 600℃ within 90 minutes and holding it at that temperature for 30 minutes, then continuing to heat it to 1200℃ within 90 minutes, performing a solution treatment for 1 hour, and then cooling the GH3230 alloy with argon.
[0154] The GH3230 alloy material contains the following elements by mass fraction: Cr 21.66%, Mo 2.26%, W 13.45%, Co 0.03%, Fe 0.20%, Si 0.4%, P 0.005%, B 0.009%, Cu 0.03%, Mn 0.5%, Al 0.30%, La 0.019%, Ti 0.03%, O 0.016%, N 0.0039%, C 0.08%, S 0.0022%, with the remainder being Ni.
[0155] Comparative Example 1
[0156] This comparative example provides a method for printing GH3230 alloy, including the following steps:
[0157] S1. Provide GH3230 alloy material;
[0158] S2. Selective laser melting technology is used to print GH3230 alloy material to obtain GH3230 alloy;
[0159] Before printing the GH3230 alloy material, the GH3230 alloy material is baked at a temperature of 105℃ for 6 hours.
[0160] Before printing GH3230 alloy material, the printing substrate is preheated at a temperature of 200℃ for 8 minutes. The printing substrate is made of 304 stainless steel.
[0161] The process parameters controlled during the printing process are: laser power 125W, scanning speed 1350mm / s, track spacing 80μm, printing layer thickness 30μm, and laser spot diameter 60μm.
[0162] During the printing process, a chessboard scanning strategy was selected, with a chessboard size of 4000μm;
[0163] The equipment used for printing and molding is the Hanbang Technology HBD-150 metal additive manufacturing equipment;
[0164] GH3230 alloy material comprises the following elements by mass fraction: Cr 23.0%, Fe 3.0%, C 0.15%, Mn 0.70%, Si 0.62%, Mo 2.0%, W 14.0%, Cu 0.5%, Co 5.0%, Al 0.3%, Ti 0.1%, La 0.02%, B 0.015%, P 0.03%, S 0.015%, and the balance Ni;
[0165] The average particle size of the GH3230 alloy material is 30μm.
[0166] Comparative Example 2
[0167] This comparative example provides a method for printing GH3230 alloy, including the following steps:
[0168] S1. Provide GH3230 alloy material;
[0169] S2. Selective laser melting technology is used to print GH3230 alloy material to obtain GH3230 alloy;
[0170] Before printing the GH3230 alloy material, the GH3230 alloy material is baked at a temperature of 105℃ for 6 hours.
[0171] Before printing GH3230 alloy material, the printing substrate is preheated at a temperature of 200℃ for 8 minutes. The printing substrate is made of 304 stainless steel.
[0172] The process parameters controlled during the printing process are: laser power 75W, scanning speed 600mm / s, track spacing 80μm, printing layer thickness 30μm, and laser spot diameter 90μm.
[0173] Linear scanning is selected as the scanning strategy during printing;
[0174] The equipment used for printing and molding is the Hanbang Technology HBD-150 metal additive manufacturing equipment;
[0175] GH3230 alloy material comprises the following elements by mass fraction: Cr 23.0%, Fe 3.0%, C 0.15%, Mn 0.70%, Si 0.62%, Mo 2.0%, W 14.0%, Cu 0.5%, Co 5.0%, Al 0.3%, Ti 0.1%, La 0.02%, B 0.015%, P 0.03%, S 0.015%, and the balance Ni;
[0176] The average particle size of the GH3230 alloy material is 30μm.
[0177] Performance testing
[0178] Metallographic photographs (unetched) of the GH3230 alloy after printing and polishing in Example 2 are shown below. Figure 1 As shown; a metallographic photograph (unetched) of the GH3230 alloy after printing and polishing in Comparative Example 1. Figure 2 As shown.
[0179] In both Example 2 and Comparative Example 1, the printing substrates were preheated to 20°C before printing. In Example 2, the mass fractions of C, Mn, and Si in the GH3230 alloy material were 0.08%, 0.50%, and 0.30%, respectively, while in Comparative Example 1, the mass fractions of C, Mn, and Si in the GH3230 alloy material were 0.15%, 0.70%, and 0.62%, respectively. Figures 1-2 It can be seen that the GH3230 alloy obtained in Example 2 has fewer cracks, which shows that by controlling the mass content of C, Si and Mn elements, this application can reduce the impact of thermal stress generated during the printing process and reduce the sensitivity of the alloy to cracking.
[0180] The properties of the GH3230 alloys printed in Example 2 and Comparative Example 1 are shown in Table 1 below.
[0181] Table 1 - Properties of GH3230 Alloy
[0182] <![CDATA[M1]]> <![CDATA[M2]]> <![CDATA[M3]]> <![CDATA[M a ]]> Comparative Example 1 8.3238 8.3236 8.3236 8.3237 Example 2 8.2882 8.2883 8.2877 8.2881 <![CDATA[m1]]> <![CDATA[m2]]> <![CDATA[m3]]> <![CDATA[m a ]]> Comparative Example 1 7.3873 7.3880 7.3880 7.3878 Example 2 7.3636 7.3636 7.3636 7.3636 <![CDATA[ρ l ]]> <![CDATA[ρ0]]> ρ <![CDATA[ρ / ρ 理论 ]]> Comparative Example 1 0.00120 0.99821 8.8684 99.27% Example 2 0.00120 0.99732 8.9317 99.97%
[0183] Table 1 shows the density of GH3230 alloy obtained by the water displacement method. Before testing the density, it is essential to remove any oil or contaminants from the surface of the alloy sample. The density test employs the water displacement method using a high-precision density balance with an accuracy of 0.0001g. The mass M (g) of the alloy sample in air and the mass m (g) in water are rigorously measured, and the temperature of the auxiliary liquid (distilled water) is recorded. The specific formula for calculating the density of the sample is as follows:
[0184] p=M(ρ0-ρ l ) / (Mm)+ρ l
[0185] -ρ0 Auxiliary liquid density (g / cm³) 3 ), -ρ l Air density (0.0012 g / cm³) 3 )
[0186] In Table 1, M1, M2, M3, M a The numbers m1, m2, m3, and m4 represent the masses of the GH3230 alloy samples in Example 2 and Comparative Example 1, respectively, measured four times in air; aThe values represent the masses of the GH3230 alloy samples in Example 2 and Comparative Example 1, respectively, after four tests in water; ρ 理论 This is the theoretical density of GH3230 alloy.
[0187] Metallographic photograph (unetched) of GH3230 alloy after printing and polishing in Example 5 is shown below. Figure 3 As shown. By Figure 1 and Figure 3 The comparison shows that the GH3230 alloy after printing in Example 5 has fewer cracks than the GH3230 alloy after printing in Example 2. This indicates that preheating the printing substrate at a preheating temperature of 150-300°C can reduce the residual stress generated during the printing process and reduce the risk of crack formation.
[0188] The properties of the GH3230 alloy obtained by printing in Example 5 are shown in Table 2 below.
[0189] Table 2 - Properties of GH3230 alloy obtained from printing in Example 5
[0190] <![CDATA[M1]]> <![CDATA[M2]]> <![CDATA[M3]]> <![CDATA[M a ]]> Example 5 8.4014 8.4020 8.4016 8.4017 <![CDATA[m1]]> <![CDATA[m2]]> <![CDATA[m3]]> <![CDATA[m a <!-- 10 -->]]> Example 5 7.4659 7.4663 7.4663 7.4662 <![CDATA[ρ l ]]> <![CDATA[ρ0]]> ρ <![CDATA[ρ / ρ 理论 ]]> Example 5 0.00120 0.99732 8.9473 100.15%
[0191] Table 2 shows the density of the GH3230 alloy printed in Example 5, tested using the water displacement method. The specific testing method is described above. In Table 2, M1, M2, M3, and M... a The numbers m1, m2, m3, and m4 represent the masses of the GH3230 alloy sample from Example 5, measured four times in air; respectively. a The values represent the masses of the GH3230 alloy sample in Example 5, measured four times in water; ρ 理论 This is the theoretical density of GH3230 alloy.
[0192] Metallographic photographs (unetched) of GH3230 alloy after hot isostatic pressing and solution treatment in Example 4 are shown below. Figure 4 As shown. From Figures 3-4 It can be seen from this that Figure 3 A small number of cracks exist at the edges of the GH3230 alloy, and the thermal stress at the edges is relatively large; while Figure 4 It can be seen that the GH3230 alloy has almost no cracks and a smooth surface.
[0193] The mechanical properties of the GH3230 alloy after solution treatment in Example 3 and the GH3230 alloy after hot isostatic pressing and solution treatment in Example 4 were tested. The results are shown in Table 3 below.
[0194] Table 3 - Mechanical properties of GH3230 alloy in Examples 3-4
[0195]
[0196] As shown in Table 3, the GH3230 alloy in Example 4 meets the room temperature tensile test standards of QJ / DT 0160044 and Q / GYB 05062. The room temperature tensile test standards of QJ / DT 0160044 and Q / GYB 05062 are: tensile strength ≥793 MPa, yield strength ≥345 MPa, and elongation ≥40%. However, the elongation of the GH3230 alloy in Example 3 is 31.5%, which is less than 40%. Therefore, the GH3230 alloy in Example 3 does not meet the elongation requirements of QJ / DT 0160044 and Q / GYB 05062.
[0197] Furthermore, the mechanical properties required by QJ / DT 0160044 and Q / GYB 05062 standards, the mechanical properties of GH3230 alloy obtained by ordinary printing, the mechanical properties of GH3230 alloy disclosed in patent CN202110281917.3, and the mechanical properties of GH3230 alloy obtained by printing in Examples 3 and 4 are shown in Table 4 below. All mechanical properties in Table 4 are tensile tests conducted at room temperature.
[0198] Table 4 - Room temperature mechanical properties of different GH3230 alloys
[0199]
[0200]
[0201] As can be seen from Table 2, the GH3230 alloy in Example 4 after hot isostatic pressing and solution treatment has the best comprehensive mechanical properties and can meet the requirements of QJ / DT 0160044 and Q / GYB 05062 standards.
[0202] The GH3230 alloy, according to the chemical composition requirements of "QJ / DT 0160044 Technical Conditions for GH230 Plates and Strips for Aero Engines" and "Q / GYB 05062 Cold-Rolled Sheets and Strips of GH3230 Alloy", includes the following elements by mass fraction: Cr 20.0~24.0%, Fe <3.0%, C 0.05~0.15%, Mn 0.30~1.00%, Si 0.25~0.75%, Mo 1~3%, W 13.0~15%, Cu≤5.0%, Co≤0.03%, Al 0.2~0.5%, Ti≤0.03%, La 0.005~0.050%, B <0.015%, P <0.030%, S <0.005%, with the balance being Ni.
[0203] Metallographic photographs (unetched) of GH3230 alloy after hot isostatic pressing and solution treatment in Examples 6-8 are shown below. Figures 5-7 As shown.
[0204] The GH3230 alloys from Examples 6-8, after undergoing hot isostatic pressing and solution treatment, were tested for elongation after fracture and creep rupture time according to national standards. The results are shown in Table 5 below.
[0205] Table 5 - Properties of GH3230 alloys in Examples 6-8
[0206]
[0207]
[0208] The GH3230 alloys in Examples 6-8, after undergoing hot isostatic pressing and solution treatment, were tested for tensile strength, yield strength, and elongation after fracture according to national standards. The results are shown in Table 6 below.
[0209] Table 6 - Properties of GH3230 alloys in Examples 6-8
[0210]
[0211] As can be seen from Tables 5 and 6, the mechanical properties of the GH3230 alloy in Examples 6 and 8 are lower than those in Example 7. That is, when the C, Si, and Mn contents are at the extreme values, the mechanical properties of the GH3230 alloy are lower than those when the C, Si, and Mn contents are at the intermediate values. Meanwhile, since the high-temperature creep and room-temperature tensile properties of the GH3230 alloy in Examples 6 and 8 are higher than the national standard, the C, Si, and Mn contents in the GH3230 alloy are controlled at 0.06–0.08 wt%, 0.3–0.40 wt%, and 0.35–0.50 wt%, respectively.
[0212] —The chemical composition of GH3230 alloy is required according to the specifications in “QJ / DT 0160044 Technical Conditions for GH230 Plates and Strips for Aero Engines” and “Q / GYB 05062 Cold-rolled Sheets and Strips of GH3230 Alloy”.
[0213] Furthermore, from Figures 5-7 It can be seen that, due to the different contents of Si, Mn and C, the GH3230 alloys in Examples 6 and 8 have a greater tendency to crack, a larger solidification temperature range, and a greater cracking sensitivity compared to the GH3230 alloy in Example 7. Microcracks appear on the metallographic surface, resulting in poor high-temperature creep plasticity and room-temperature tensile plasticity.
[0214] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.
Claims
1. A method for printing GH3230 alloy, characterized in that, Includes the following steps: A GH3230 alloy material is provided, wherein the particle size of the GH3230 alloy material is 15-53 μm, and the GH3230 alloy material comprises the following elements: Cr, Fe, C, Mn, Si, Mo, W, Cu, Co, Al, Ti, La, B, P, S, Ni; wherein the mass content of C is 0.06-0.08%, the mass content of Si is 0.3-0.40%, and the mass content of Mn is 0.35-0.50%. The GH3230 alloy material was printed using selective laser melting technology to obtain the GH3230 alloy. The process parameters controlled during the printing process were: laser power 75-150W, scanning speed 1000-1400mm / s, track spacing 80-110μm, printing layer thickness 30-40μm, and laser spot diameter 60-80μm. Before printing the GH3230 alloy material, the process also includes: preheating the printing substrate at a temperature of 200-250°C. After printing the GH3230 alloy material to obtain the GH3230 alloy, the process further includes: hot isostatic pressing (HIP) treatment of the GH3230 alloy, wherein the HIP treatment includes: treating the GH3230 alloy at a temperature of 1050-1250℃ and a pressure of 105-160MPa for 1-3 hours, and then cooling the GH3230 alloy in the furnace. The hot isostatic pressing treatment of GH3230 alloy further includes: solution treatment of GH3230 alloy, wherein the solution treatment includes: heating GH3230 alloy from room temperature to 550-650℃ within 80-100 min and holding at that temperature for 20-40 min, then continuing to heat to 1100-1230℃ within 80-100 min, solution treatment for 0.5-3 h, and then argon-cooled or water-cooled GH3230 alloy.
2. The GH3230 alloy printing method as described in claim 1, characterized in that, During the printing process, a chessboard scanning strategy is used, with a chessboard size of 800–8000 μm.
3. The GH3230 alloy printing method as described in claim 1, characterized in that, Before printing the GH3230 alloy material, the GH3230 alloy material is baked, wherein the baking temperature is 100-110℃ and the baking time is 4-8h.
Citation Information
Patent Citations
A GH3230 nickel-based superalloy material and its method and application for eliminating microcracks in laser selective melting forming.
CN113061782B
DE160044A
Nickel-base high temperature alloy and manufacturing method, component and application thereof
CN111500898A
Solid solution treatment method for melting GH3230 alloy through laser powder bed and GH3230 alloy