An epitaxial structure and its fabrication method, and a semiconductor device
By using a superlattice buffer layer of alternating BN and AlGaN films in a GaN HEMT device on a Si substrate, the lattice mismatch problem between the Si substrate and GaN is solved, forming a flat epitaxial layer and improving the device's withstand voltage and reliability.
Patent Information
- Application Number
- CN202311132866.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-04
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-09-04
AI Technical Summary
In GaN HEMT devices on Si substrates, the lattice and thermal mismatch between the Si substrate and GaN makes it difficult to grow high-quality epitaxial materials, leading to epitaxial layer warping and cracking, which affects device performance.
A superlattice buffer layer composed of alternating layers of BN and AlGaN films is used to provide compressive stress to counteract tensile stress by utilizing the migration ability and lattice constant characteristics of BN, forming a flat two-dimensional crystalline material and reducing epitaxial layer cracks.
It improves the quality of the epitaxial layer and the withstand voltage of the device, enhances the reliability of the device, reduces cracking of the epitaxial layer, and improves the performance of the device.
Smart Images

Figure CN117199126B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of semiconductor technology, and in particular to an epitaxial structure and its preparation method, and a semiconductor device. Background Technology
[0002] In some Si-based GaN HEMT devices, the significant lattice and thermal mismatch between the Si substrate and GaN makes it difficult to obtain high-quality GaN-based epitaxial materials on large-size Si substrates. In particular, the cooling process after high-temperature growth introduces substantial tensile stress, leading to significant warpage and numerous cracks in the epitaxial layer. To reduce epitaxial layer cracking, related technologies employ superlattice structures composed of AlN / AlGaN to release stress and obtain epitaxial layers with higher crystal quality. However, AlN has poor migration properties, making it difficult to grow good two-dimensional AlN crystalline films. Furthermore, the lattice constant of AlN is close to that of GaN, failing to effectively introduce compressive stress into the subsequent GaN layer. This exacerbates cracking in the epitaxial layer, limiting the epitaxial thickness and consequently restricting the device's breakdown voltage and crystal quality. These problems ultimately lead to leakage current, affecting device performance. Summary of the Invention
[0003] According to a first aspect of the embodiments of this application, an epitaxial structure is provided, comprising: silicon substrate; The epitaxial layer includes a superlattice buffer layer disposed on one side of the silicon substrate, the superlattice buffer layer including alternating layers of BN film and layers of AlGaN film.
[0004] In some embodiments, the thickness of the BN film is less than the thickness of the AlGaN film; the thickness of each BN film ranges from 5 nm to 10 nm; and the thickness of each AlGaN film ranges from 20 nm to 40 nm.
[0005] In some embodiments, the thickness of each BN film layer in the multilayer BN film layer is equal; The thickness of each AlGaN film layer in the multilayer AlGaN film is equal.
[0006] In some embodiments, the bottom layer of the superlattice buffer layer located near the silicon substrate is a BN film, and the top layer of the superlattice buffer layer located away from the silicon substrate is an AlGaN film.
[0007] In some embodiments, the epitaxial structure further includes a withstand layer located on the surface of the superlattice buffer layer opposite to the silicon substrate, wherein the withstand layer is a GaN film. In the top AlGaN film layer located on the side opposite to the silicon substrate, at least the surface material opposite to the silicon substrate is GaN.
[0008] In some embodiments, the epitaxial structure further includes a nucleation layer and a transition layer disposed between the silicon substrate and the superlattice buffer layer, and an insertion layer, a barrier layer, and a P-type enhancement layer disposed sequentially on the withstand voltage layer away from the superlattice buffer layer; wherein the nucleation layer is disposed on the silicon substrate, and the transition layer is disposed on the side of the nucleation layer away from the silicon substrate.
[0009] In some embodiments, the epitaxial layer is formed using metal-organic chemical vapor deposition or molecular beam epitaxy.
[0010] According to a second aspect of the embodiments of this application, a method for preparing an epitaxial structure is provided, comprising: Provide silicon substrates; An epitaxial layer is formed on the silicon substrate; the formation of the epitaxial layer includes forming a superlattice buffer layer, the superlattice buffer layer being located on one side of the silicon substrate; the superlattice buffer layer includes alternating layers of BN film and layers of AlGaN film.
[0011] In some embodiments, forming the superlattice buffer layer includes sequentially forming alternating layers of BN film and layers of AlGaN film; wherein the BN film is formed at high temperature using a mixture of BCl3 or B2H4 and NH3.
[0012] In some embodiments, the thickness of the BN film is less than the thickness of the AlGaN film; the thickness of each BN film ranges from 5 nm to 10 nm; and the thickness of each AlGaN film ranges from 20 nm to 40 nm.
[0013] In some embodiments, the thickness of each BN film layer in the multilayer BN film layer is equal; The thickness of each AlGaN film layer in the multilayer AlGaN film is equal.
[0014] In some embodiments, the bottom layer of the superlattice buffer layer located near the silicon substrate is a BN film, and the top layer of the superlattice buffer layer located away from the silicon substrate is an AlGaN film.
[0015] In some embodiments, after forming a superlattice buffer layer disposed on one side of the silicon substrate, the method for fabricating the epitaxial structure further includes: A pressure-resistant layer is formed on the surface of the superlattice buffer layer opposite to the silicon substrate; the pressure-resistant layer is a GaN film.
[0016] In some embodiments, when forming the AlGaN film layer on the top layer opposite to the silicon substrate, the molar amount of Al is reduced such that in the AlGaN film layer on the top layer opposite to the silicon substrate, at least the surface material opposite to the silicon substrate is GaN.
[0017] In some embodiments, the formation of the epitaxial structure further includes, prior to forming the superlattice buffer layer: A nucleation layer and a transition layer are sequentially formed on the silicon substrate; wherein the nucleation layer is disposed on the silicon substrate, and the transition layer is disposed on the side of the nucleation layer opposite to the silicon substrate; After forming the superlattice buffer layer, the formation of the epitaxial structure further includes: An insertion layer, a barrier layer, and a P-type reinforcement layer are sequentially formed on the pressure-resistant layer away from the superlattice buffer layer.
[0018] In some embodiments, the epitaxial layer is formed using metal-organic chemical vapor deposition or molecular beam epitaxy.
[0019] According to a third aspect of the embodiments of this application, a semiconductor device is provided, the semiconductor device including the epitaxial structure as described above.
[0020] The main technical effects achieved by the embodiments of this application are: The epitaxial structure provided in this application, by setting the superlattice buffer layer as alternating layers of multilayer BN and multilayer AlGaN films, offers advantages over related technologies that use alternating AlN and AlGaN films for forming superlattice buffer layers. BN has better mobility, making it easier to form a flat two-dimensional crystal material. Furthermore, B atoms in BN are smaller than Al and Ga atoms, and the lattice constant of BN is smaller than that of AlN. The BN film in this application can provide greater compressive stress for subsequent epitaxial layers (such as the GaN voltage-resistant layer) to largely offset the tensile stress exerted by the silicon substrate on the epitaxial layer. This results in a flat or slightly convex state for the entire epitaxial layer, which is more conducive to process control during epitaxial layer growth and less prone to cracking. Additionally, because BN has a higher breakdown field strength than AlN, it can further improve the voltage withstand capability of the device with this epitaxial structure. Therefore, compared with the superlattice buffer layer formed by alternating AlN and AlGaN films in related technologies, the superlattice buffer layer formed by alternating multilayer BN and multilayer AlGaN films can provide better stress regulation and increased withstand voltage, which is beneficial to improving the quality of the epitaxial layer and thus improving the reliability of the device with the epitaxial structure. Attached Figure Description
[0021] Figure 1This is a cross-sectional view of the extensional structure provided in an exemplary embodiment of this application; Figure 2 This is a flowchart of a method for preparing an epitaxial structure provided in an exemplary embodiment of this application; Figures 3 to 11 This is a fabrication process diagram of the epitaxial structure provided in an exemplary embodiment of this application. Detailed Implementation
[0022] Exemplary embodiments will now be described in detail, examples of which are illustrated in the accompanying drawings. When the following description relates to the drawings, unless otherwise indicated, the same numerals in different drawings denote the same or similar elements. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with this application. Rather, they are merely examples of apparatuses and methods consistent with some aspects of this application as detailed in the appended claims.
[0023] The terminology used in this application is for the purpose of describing particular embodiments only and is not intended to be limiting of the application. The singular forms “a,” “the,” and “the” used in this application and the appended claims are also intended to include the plural forms unless the context clearly indicates otherwise. It should also be understood that the term “and / or” as used herein refers to and includes any or all possible combinations of one or more of the associated listed items.
[0024] It should be understood that although the terms first, second, third, etc., may be used in this application to describe various information, such information should not be limited to these terms. These terms are only used to distinguish information of the same type from one another. For example, without departing from the scope of this application, first information may also be referred to as second information, and similarly, second information may also be referred to as first information. Depending on the context, the word "if" as used herein may be interpreted as "when," "when," or "in response to determination."
[0025] This application provides an epitaxial structure, a method for fabricating the same, and a semiconductor device. The epitaxial structure includes a silicon substrate and an epitaxial layer. The epitaxial layer includes a superlattice buffer layer disposed on one side of the silicon substrate, and the superlattice buffer layer includes alternating layers of BN films and AlGaN films. The aforementioned epitaxial structure, by setting the superlattice buffer layer as alternating layers of BN and AlGaN films, offers advantages over related technologies that use alternating AlN and AlGaN films to form a superlattice buffer layer. BN has better mobility, making it easier to form a flat two-dimensional crystal material. Furthermore, B atoms in BN are smaller than Al and Ga atoms, and the lattice constant of BN is smaller than that of AlN. The BN film in this application can provide greater compressive stress for subsequent epitaxial layers (such as the GaN voltage-resistant layer) to largely offset the tensile stress exerted by the silicon substrate on the epitaxial layer. This results in a flat or slightly convex state for the entire epitaxial layer, which is more conducive to process control during epitaxial layer growth and less prone to cracking. Additionally, the higher breakdown field strength of BN compared to AlN further improves the voltage withstand capability of the device with this epitaxial structure. Therefore, compared with the superlattice buffer layer formed by alternating AlN and AlGaN films in related technologies, the superlattice buffer layer formed by alternating multilayer BN and multilayer AlGaN films can provide better stress regulation and increased withstand voltage, which is beneficial to improving the quality of the epitaxial layer and thus improving the reliability of the device with the epitaxial structure.
[0026] The epitaxial structure mentioned here can refer to the epitaxial structure of a GaN HEMT device on a Si-based substrate. The semiconductor device can be a GaN HEMT device on a Si-based substrate.
[0027] The following is in conjunction with the appendix Figures 1 to 11 The epitaxial structures and their preparation methods in the embodiments of this application will be described in detail. Unless otherwise specified, the features in the following embodiments may complement or combine with each other.
[0028] Please refer to Figure 1 As shown, the epitaxial structure 100 includes a silicon substrate 10 and an epitaxial layer 20. The epitaxial layer 20 includes a superlattice buffer layer 24 disposed on one side of the silicon substrate 10, and the superlattice buffer layer 24 includes alternating layers of BN film 241 and multiple layers of AlGaN film.
[0029] The lattice constant of BN is 0.25 nm, while that of AlN is 0.31 nm. The lattice constant of AlN is closer to that of GaN (0.313). Compared to the superlattice buffer layer formed by alternating AlN and AlGaN films in related technologies, this epitaxial structure 100 has advantages such as better BN migration ability, making it easier to form a flat two-dimensional crystal material. The B atoms in BN are smaller than those in Al and Ga, and the lattice constant of BN is smaller than that of AlN. The BN film can provide greater compressive stress for other epitaxial films (such as the GaN voltage-resistant layer) to offset the tensile stress of the silicon substrate on the epitaxial layer as much as possible, so that the entire epitaxial layer tends to be flat or slightly convex. This is more conducive to the growth and setting of the epitaxial layer and less prone to breakage. Compared to the superlattice buffer layer formed by alternating AlN and AlGaN films in related technologies, the superlattice buffer layer formed by alternating multilayer BN and multilayer AlGaN films can provide better stress regulation and increased withstand voltage, which is beneficial to improving the quality of the epitaxial layer and thus enhancing the reliability of devices with this epitaxial structure.
[0030] In some embodiments, the thickness of the superlattice buffer layer 24 is preferably set to 3μm-4μm. The number of cycles n of the alternating BN film layer 241 and AlGaN film layer in the superlattice buffer layer 24 is 60 loops-160 loops. Preferably, n is 70 loops-120 loops. Each BN film layer 241 and its corresponding adjacent AlGaN film layer constitute one cycle. For example, one BN film layer 241 and an AlGaN film layer stacked on top of that BN film layer 241 constitute one cycle.
[0031] In some embodiments, the thickness of the BN film 241 is less than the thickness of the AlGaN film 242, which can effectively form a superlattice buffer layer 24, so that the formed superlattice buffer layer 24 has good stress and pressure resistance performance for adjusting the superlattice buffer layer 24 and the entire epitaxial structure 100.
[0032] Through research, the inventors discovered that if the BN film 241 is too thick, it will crack; if the BN film 241 is too thin, it will not play a stress regulation role, and if the BN film 241 is too thin, its resistance to breakdown fields is poor. Further research revealed that in some embodiments, the thickness of each BN film 241 ranges from 5 nm to 10 nm, and the thickness of each AlGaN film 242 ranges from 20 nm to 40 nm. This achieves better stress and pressure resistance performance for adjusting the superlattice buffer layer 24 and the entire epitaxial structure 100.
[0033] In some embodiments, the thickness of each layer of the multilayer BN film 241 is equal, which is more conducive to adjusting the stress and pressure resistance of the superlattice buffer layer 24 and the entire epitaxial structure 100.
[0034] In some embodiments, each AlGaN film 242 of the multilayer AlGaN film 242 has an equal thickness, which further facilitates the adjustment of the stress and pressure resistance of the superlattice buffer layer 24 and the entire epitaxial structure 100.
[0035] In some embodiments, the bottom layer of the superlattice buffer layer 24 located on the side closer to the silicon substrate 10 is a BN film layer 241, and the top layer of the superlattice buffer layer 24 located on the side away from the silicon substrate 10 is an AlGaN film layer 242.
[0036] In some embodiments, the epitaxial structure 100 further includes a pressure-resistant layer 25 located on the surface of the superlattice buffer layer 24 facing away from the silicon substrate 10, wherein the pressure-resistant layer 25 is a GaN film.
[0037] In order to alleviate the degree of lattice mismatch with the upper voltage-resistant layer, reduce the mismatch stress, and make the crystal quality of the upper voltage-resistant layer 25, which is made of GaN, the surface material of the top AlGaN film layer 242 located on the side opposite to the silicon substrate 10 is at least GaN.
[0038] The fact that the surface material facing away from the silicon substrate 10 is GaN can be understood as having only one layer of GaN on the surface, or it can be that a portion of the thickness of the top AlGaN film 242 is GaN. When forming the top AlGaN film 242 on the side facing away from the silicon substrate 10, the molar amount of metallic Al can be gradually reduced (i.e., the amount of Al can be reduced) to eventually form GaN on the top surface of the top AlGaN film 242. This means that in the top AlGaN film 242 on the side facing away from the silicon substrate 10, the surface material facing away from the silicon substrate 10 is at least GaN.
[0039] It should be noted that, in some other embodiments, the top AlGaN film 242 located on the side opposite to the silicon substrate 10 may also be the same AlGaN film as other AlGaN films.
[0040] In some embodiments, the epitaxial structure 100 further includes a nucleation layer and a transition layer 23 disposed between the silicon substrate 10 and the superlattice buffer layer 24, and an insertion layer 26, a barrier layer 27, and a P-type enhancement layer 28 sequentially disposed on the withstand voltage layer 25 away from the superlattice buffer layer 24; wherein the nucleation layer is disposed on the silicon substrate 10, and the transition layer 23 is disposed on the side of the nucleation layer away from the silicon substrate 10.
[0041] The nucleation layer has a two-layer structure, comprising a first layer 21 and a second layer 22. The first layer 21 is an AlN layer, and the second layer 22 is an LT-AlN layer. The transition layer 23 is an AlGaN layer. The withstand layer 25 is a GaN layer. The insertion layer 26 is an AlN layer, used to reduce the accumulated stress of the epitaxial structure. The barrier layer 27 is an AlGaN layer. The p-type reinforcement layer 28 is a p-type GaN layer.
[0042] In some embodiments, each film layer of the epitaxial layer 20 is grown using metal-organic chemical vapor deposition (MOCVD) technology.
[0043] In other embodiments, each layer of the epitaxial layer 20 is grown using molecular beam epitaxy (MBE) technology.
[0044] This application also provides a semiconductor device, which may include the epitaxial structure 100 as described above. It is understood that the semiconductor device may further include a source, a drain, a gate, and a corresponding dielectric layer disposed on the epitaxial structure 100.
[0045] It is understandable that this semiconductor device can be a GaN HEMT device on a Si-based substrate.
[0046] Please refer to Figure 2 As shown, this application provides a method for preparing an epitaxial structure 100, which may include the following steps S101 and S103: In step S101, a silicon substrate is provided; In step S103, an epitaxial layer is formed on the silicon substrate; the formation of the epitaxial layer includes forming a superlattice buffer layer, the superlattice buffer layer being located on one side of the silicon substrate; the superlattice buffer layer includes alternating layers of BN film and layers of AlGaN film.
[0047] The following is combined Figures 3 to 11 As shown, the preparation method of the above-mentioned epitaxial structure 100 is described in detail.
[0048] like Figure 3 As shown, in step S101, a silicon substrate 10 is provided.
[0049] like Figures 4 to 6 As shown, after step S101 and before forming the superlattice buffer layer 24 in step S103, the formation of the epitaxial structure 100 further includes the following steps: A nucleation layer and a transition layer 23 are sequentially formed on the silicon substrate 10; wherein the nucleation layer is disposed on the silicon substrate 10, and the transition layer 23 is disposed on the side of the nucleation layer opposite to the silicon substrate 10.
[0050] The nucleation layer here includes a first layer 21 and a second layer 22. The first layer 21 is an AlN layer, and the second layer 22 is an LT-AlN layer. The transition layer 23 is an AlGaN layer.
[0051] Please combine Figure 7 As shown, the formation of the epitaxial layer 20 includes the formation of a superlattice buffer layer 24, which is located on one side of the silicon substrate 10; the superlattice buffer layer 24 includes alternating layers of BN film 241 and AlGaN film 242.
[0052] The formation of the superlattice buffer layer 24 includes the sequential formation of alternating layers of BN film 241 and AlGaN film 242.
[0053] The BN film 241 can be formed at high temperature using a mixture of BCl3 and NH3 gases. Alternatively, the BN film 241 can be formed at high temperature using a mixture of B2H4 and NH3 gases.
[0054] When forming the BN film 241, the growth temperature of the BN film 241 can be controlled at 800℃-1100℃, the duration of introducing the boron source (such as BCl3 or B2H4) can be controlled at 10S-50S, and the duration of introducing the nitrogen source (such as NH3) can be controlled at 10S-80S. Preferably, the duration of introducing the nitrogen source (such as NH3) is longer than that of introducing the boron source (such as BCl3 or B2H4), which can better nitride the boron atoms, thereby better forming hexagonal boron nitride crystals and thus better forming the BN film 241. In some embodiments, the thickness of the superlattice buffer layer 24 is preferably set at 3μm-4μm. The number of cycles n of the alternating BN film 241 and AlGaN film in the superlattice buffer layer 24 is 60 loops-160 loops. Preferably, n is 70 loops-120 loops. Each BN film layer 241 and its corresponding adjacent AlGaN film layer constitute a cycle. For example, a BN film layer 241 and an AlGaN film layer stacked on top of that BN film layer 241 constitute a cycle.
[0055] In some embodiments, the thickness of the BN film 241 is set to be less than the thickness of the AlGaN film 242, which can effectively form the superlattice buffer layer 24, so that the formed superlattice buffer layer 24 has good stress and pressure resistance performance for adjusting the superlattice buffer layer 24 and the entire epitaxial structure 100.
[0056] Through research, the inventors discovered that if the BN film 241 is too thick, it will crack; if the BN film 241 is too thin, it will not play a stress regulation role, and if the BN film 241 is too thin, its resistance to breakdown fields is poor. Further research revealed that in some embodiments, the thickness of each BN film layer ranges from 5 nm to 10 nm. The thickness of each AlGaN film layer 242 ranges from 20 nm to 40 nm, resulting in better stress and pressure resistance performance of the superlattice buffer layer 24 and the entire epitaxial structure 100.
[0057] In some embodiments, the thickness of each layer of the multilayer BN film 241 is equal, which is more conducive to adjusting the stress and pressure resistance of the superlattice buffer layer 24 and the entire epitaxial structure 100.
[0058] In some embodiments, the thickness of each AlGaN film 242 in the multilayer AlGaN film 242 is equal, which further facilitates the adjustment of stress and pressure resistance of the superlattice buffer layer 24 and the entire epitaxial structure 100.
[0059] In some embodiments, the bottom layer of the superlattice buffer layer 24 located on the side closer to the silicon substrate 10 is a BN film layer 241, and the top layer of the superlattice buffer layer 24 located on the side away from the silicon substrate 10 is an AlGaN film layer 242.
[0060] Please combine Figure 8 As shown, in some embodiments, after forming the superlattice buffer layer 24 disposed on one side of the silicon substrate 10, the method for fabricating the epitaxial structure 100 further includes: A pressure-resistant layer 25 is formed on the surface of the superlattice buffer layer 24 on the side opposite to the silicon substrate 10; the pressure-resistant layer 25 is a GaN film.
[0061] In some embodiments, when forming the AlGaN film 242 on the top layer located on the side opposite to the silicon substrate 10, the molar amount of Al is reduced, so that in the AlGaN film 242 on the top layer located on the side opposite to the silicon substrate 10, at least the surface material opposite to the silicon substrate 10 is GaN. This can alleviate the degree of lattice mismatch, reduce mismatch stress, and make the crystal quality of the GaN-material-based withstand layer 25 better.
[0062] The statement that the surface material at least away from the silicon substrate 10 is GaN can be understood as having only one layer of GaN on the surface, or it can be that part of the thickness of the top AlGaN film 242 is GaN.
[0063] Preferably, when forming the top AlGaN film 242 located on the side opposite to the silicon substrate 10, the molar amount of metal Al can be gradually reduced (i.e., the amount of Al is reduced, or the proportion of Al is reduced) to eventually form GaN on the top surface of the top AlGaN film 242. This means that in the top AlGaN film 242 located on the side opposite to the silicon substrate 10, at least the surface material opposite to the silicon substrate 10 is GaN.
[0064] It should be noted that in some other embodiments, when forming the top AlGaN film 242 located on the side opposite to the silicon substrate 10, the molar amount of Al may not be reduced, and the same AlGaN film layer as other AlGaN film layers may be formed.
[0065] Please combine Figures 9 to 11 As shown, in step S103, after forming the superlattice buffer layer 24, the formation of the epitaxial structure 100 further includes: An insertion layer 26, a barrier layer 27, and a P-type reinforcement layer 28 are sequentially formed on the pressure-resistant layer 25 away from the superlattice buffer layer 24.
[0066] The pressure-resistant layer 25 is a GaN layer. The insertion layer 26 is an AlN layer, used to reduce the cumulative stress of the epitaxial structure. The barrier layer 27 is an AlGaN layer. The p-type reinforcement layer 28 is a p-type GaN layer.
[0067] It is understood that, in some embodiments, each film layer of the epitaxial layer 20 is grown using metal-organic chemical vapor deposition (MOCVD) technology.
[0068] In other embodiments, each layer of the epitaxial layer 20 is grown using molecular beam epitaxy (MBE) technology.
[0069] It should be noted that the dimensions of layers and regions may be exaggerated in the accompanying drawings for clarity. Furthermore, it is understood that when an element or layer is referred to as being "on" another element or layer, it can be directly on the other element, or there may be intermediate layers. Additionally, it is understood that when an element or layer is referred to as being "below" another element or layer, it can be directly below the other element, or there may be more than one intermediate layer or element. Furthermore, it is also understood that when a layer or element is referred to as being "between" two layers or two elements, it can be the only layer between the two layers or two elements, or there may be more than one intermediate layer or element. Similar reference numerals throughout indicate similar elements.
[0070] Other embodiments of this application will readily occur to those skilled in the art upon consideration of the specification and practice of the disclosure herein. This application is intended to cover any variations, uses, or adaptations of this application that follow the general principles of this application and include common knowledge or customary techniques in the art not disclosed herein. The specification and examples are to be considered exemplary only, and the true scope and spirit of this application are indicated by the following claims.
[0071] It should be understood that this application is not limited to the precise structure described above and shown in the accompanying drawings, and various modifications and changes can be made without departing from its scope. The scope of this application is limited only by the appended claims.
Claims
1. An epitaxial structure, characterized in that, include: silicon substrate; An epitaxial layer, the epitaxial layer including a superlattice buffer layer disposed on one side of the silicon substrate, the superlattice buffer layer including alternating layers of BN film and layers of AlGaN film; The bottom layer of the superlattice buffer layer located near the silicon substrate is a BN film, and the top layer of the superlattice buffer layer located away from the silicon substrate is an AlGaN film. The epitaxial structure also includes a pressure-resistant layer located on the surface of the superlattice buffer layer opposite to the silicon substrate, wherein the pressure-resistant layer is a GaN film layer; In the top AlGaN film layer located on the side opposite to the silicon substrate, at least the surface material opposite to the silicon substrate is GaN; The thickness of the BN film is less than that of the AlGaN film; the thickness of each BN film ranges from 5 nm to 10 nm; the thickness of each AlGaN film ranges from 20 nm to 40 nm.
2. The epitaxial structure as described in claim 1, characterized in that, The thickness of each layer of the multilayer BN film is equal. The thickness of each AlGaN film layer in the multilayer AlGaN film is equal.
3. The epitaxial structure as described in claim 1, characterized in that, The epitaxial structure further includes a nucleation layer and a transition layer disposed between the silicon substrate and the superlattice buffer layer, and an insertion layer, a barrier layer, and a P-type enhancement layer disposed sequentially on the withstand voltage layer away from the superlattice buffer layer; wherein the nucleation layer is disposed on the silicon substrate, and the transition layer is disposed on the side of the nucleation layer away from the silicon substrate.
4. The epitaxial structure as described in any one of claims 1 to 3, characterized in that, The epitaxial layer is formed using metal-organic chemical vapor deposition or molecular beam epitaxy.
5. A method for preparing an epitaxial structure, characterized in that, include: Provide silicon substrates; An epitaxial layer is formed on the silicon substrate; the formation of the epitaxial layer includes forming a superlattice buffer layer, the superlattice buffer layer being located on one side of the silicon substrate; the superlattice buffer layer includes alternating layers of BN film and layers of AlGaN film; The bottom layer of the superlattice buffer layer located near the silicon substrate is a BN film, and the top layer of the superlattice buffer layer located away from the silicon substrate is an AlGaN film. After forming a superlattice buffer layer on one side of the silicon substrate, the method for fabricating the epitaxial structure further includes: A voltage-resistant layer is formed on the surface of the superlattice buffer layer opposite to the silicon substrate; the voltage-resistant layer is a GaN film. When forming the top AlGaN film layer located on the side opposite to the silicon substrate, the molar amount of Al is reduced, such that in the top AlGaN film layer located on the side opposite to the silicon substrate, at least the surface material opposite to the silicon substrate is GaN; The thickness of the BN film is less than that of the AlGaN film; the thickness of each BN film ranges from 5 nm to 10 nm; the thickness of each AlGaN film ranges from 20 nm to 40 nm.
6. The method for preparing the epitaxial structure as described in claim 5, characterized in that, The formation of the superlattice buffer layer includes the sequential formation of alternating layers of BN film and AlGaN film; wherein the BN film is formed at high temperature using a mixture of BCl3 or B2H4 and NH3.
7. The method for preparing the epitaxial structure as described in claim 5, characterized in that, The thickness of each layer of the multilayer BN film is equal. The thickness of each AlGaN film layer in the multilayer AlGaN film is equal.
8. The method for preparing the epitaxial structure as described in claim 5, characterized in that, Before forming the superlattice buffer layer, the following is also included: A nucleation layer and a transition layer are sequentially formed on the silicon substrate; wherein the nucleation layer is disposed on the silicon substrate, and the transition layer is disposed on the side of the nucleation layer opposite to the silicon substrate; After forming the superlattice buffer layer, the process further includes: An insertion layer, a barrier layer, and a P-type reinforcement layer are sequentially formed on the pressure-resistant layer away from the superlattice buffer layer.
9. The method for preparing the epitaxial structure according to any one of claims 5 to 8, characterized in that, The epitaxial layer is formed using metal-organic chemical vapor deposition or molecular beam epitaxy.
10. A semiconductor device, characterized in that, The semiconductor device includes an epitaxial structure as described in any one of claims 1 to 4.
Citation Information
Patent Citations
Epitaxial substrate for electronic devices and manufacturing method therefor
CN102318049A