Cross-linked polymer electrolytes, composite membrane electrolytes and their preparation methods, composite cathodes, composite anodes, lithium-ion batteries

By cross-linking polyphenol monomers with polyethers to form a cross-linked polymer electrolyte, combined with inorganic electrolyte particles, the problems of low room temperature ionic conductivity and insufficient mechanical strength of lithium batteries are solved, achieving efficient lithium-ion transport and improved battery performance.

CN117199498BActive Publication Date: 2026-11-17CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202210615273.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-06-01
Publication Date
2026-11-17
Estimated Expiration
2042-06-01

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention relates to the field of lithium-ion batteries, and discloses a cross-linked polymer electrolyte, a composite membrane electrolyte, a method for preparing the same, a composite positive electrode, a composite negative electrode, and a lithium-ion battery. The cross-linked polymer electrolyte comprises a polymer matrix, a lithium salt, and inorganic electrolyte particles. The polymer matrix is ​​obtained by cross-linking polyphenol monomers with polyether. Based on the total weight of the cross-linked polymer electrolyte, it comprises 50-70 wt% polymer matrix, 10-25 wt% lithium salt, and 20-35 wt% inorganic electrolyte particles. The cross-linked polymer electrolyte utilizes a cross-linked network formed by polyphenol monomers and polyether to enhance the mechanical strength of the cross-linked polymer electrolyte. The polyphenol monomers not only provide binding sites for lithium ions but also improve the lithium ion transport rate. The cross-linking effect of polyphenols on polyether effectively inhibits polyether crystallization and improves the room temperature ionic conductivity of the cross-linked polymer electrolyte.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion batteries, specifically to a cross-linked polymer electrolyte, a composite membrane electrolyte and its preparation method, a composite positive electrode, a composite negative electrode, and a lithium-ion battery. Background Technology

[0002] Compared to other energy storage devices, lithium batteries offer advantages such as high voltage, high energy density, excellent cycle life, and low self-discharge rate, making them widely used in various mobile electronic devices and the automotive industry. As living standards improve, people have increasingly stringent requirements for energy storage devices. However, traditional lithium batteries contain flammable and explosive organic electrolytes, posing safety risks such as leakage, combustion, and even explosions during use, seriously threatening personal safety and property. Therefore, the development of a new generation of lithium batteries is urgently needed.

[0003] All-solid-state lithium batteries, due to their use of electrolytes, possess high stability and safety performance, and are considered a key development direction for next-generation lithium batteries. Furthermore, electrolytes, due to their excellent mechanical properties, can effectively suppress the growth of dendrites on the surface of lithium metal electrodes, thus holding significant application value in the field of high-energy-density lithium metal batteries. Among polymer electrolytes, polyethers are the most commonly used and most effective polymers. Polyethers have excellent lithium salt dissolution capabilities and facilitate lithium-ion transport through the movement of flexible chain segments. However, due to their high crystallinity, polyether-based polymer electrolytes generally have low conductivity (only 10 at room temperature). -5 It has poor mechanical properties and elongation at break (S / cm), and its mechanical properties and elongation at break are also poor.

[0004] Therefore, designing a polyphenol / polyether cross-linked solid electrolyte with high ionic conductivity has significant theoretical and practical value. Summary of the Invention

[0005] The purpose of this invention is to overcome the problems of low room temperature ionic conductivity, poor cycle stability and poor mechanical strength in the prior art, and to provide a cross-linked polymer electrolyte, a composite membrane electrolyte and its preparation method, a composite positive electrode, a composite negative electrode and a lithium-ion battery. The cross-linked polymer electrolyte has low crystallinity, high room temperature ionic conductivity and high mechanical strength.

[0006] To achieve the above objectives, the first aspect of the present invention provides a cross-linked polymer electrolyte, characterized in that the cross-linked polymer electrolyte comprises a polymer matrix, a lithium salt, and inorganic electrolyte particles;

[0007] The polymer matrix is ​​obtained by crosslinking polyphenolic monomers with polyethers;

[0008] Based on the total weight of the cross-linked polymeric electrolyte, the cross-linked polymeric electrolyte comprises 50-70 wt% polymer matrix, 10-25 wt% lithium salt, and 20-35 wt% inorganic electrolyte particles.

[0009] A second aspect of the present invention provides a method for preparing the above-mentioned cross-linked polymer electrolyte, characterized in that the preparation method includes:

[0010] In the presence of a solvent, polyphenol monomers, polyethers, lithium salts, and inorganic electrolyte particles are mixed and the pH is adjusted to 7-10 to carry out an in-situ crosslinking reaction, thereby obtaining a crosslinked polymer electrolyte.

[0011] A third aspect of the present invention provides a composite membrane electrolyte, characterized in that the composite membrane electrolyte comprises the above-mentioned cross-linked polymer electrolyte and a porous support material;

[0012] The mass ratio of the cross-linked polymer electrolyte to the porous support material is 0.3-0.8:1.

[0013] A fourth aspect of the present invention provides a method for preparing the above-mentioned composite membrane electrolyte, characterized in that the preparation method includes:

[0014] In the presence of a solvent, polyphenol monomers, polyethers, lithium salts, and inorganic electrolyte particles are mixed and the pH is adjusted to 7-10. The mixture is then brought into contact with a porous support material to undergo an in-situ crosslinking reaction, resulting in a composite membrane electrolyte.

[0015] A fifth aspect of the present invention provides a composite positive electrode, characterized in that the composite positive electrode is prepared by the following method:

[0016] In the presence of a solvent, polyphenol monomers, polyethers, lithium salts, and inorganic electrolyte particles are mixed and the pH is adjusted to 7-10. The mixture is then brought into contact with the positive electrode sheet to undergo an in-situ crosslinking reaction, resulting in a composite positive electrode.

[0017] A sixth aspect of the present invention provides a composite negative electrode, characterized in that the composite negative electrode is prepared by the following method:

[0018] In the presence of a solvent, polyphenol monomers, polyethers, lithium salts, and inorganic electrolyte particles are mixed and the pH is adjusted to 7-10. The mixture is then brought into contact with the negative electrode sheet to undergo an in-situ crosslinking reaction, resulting in a composite negative electrode.

[0019] The seventh aspect of the present invention provides a lithium-ion battery, characterized in that the lithium-ion battery comprises one of the above-mentioned cross-linked polymer electrolyte, composite membrane electrolyte, composite positive electrode and composite negative electrode.

[0020] Through the above technical solutions, the cross-linked polymer electrolyte, composite membrane electrolyte and its preparation method, composite positive electrode, composite negative electrode, and lithium-ion battery provided by the present invention can achieve the following beneficial effects:

[0021] (1) A cross-linked network is formed by polymerizing polyphenol monomers and polyethers. The polyphenol monomers not only provide binding sites for lithium ions but also enhance the lithium ion transport rate. At the same time, the polyphenol monomers can effectively inhibit the crystallization of polyethers by cross-linking with polyethers, and the transport performance of lithium ions in the cross-linked network can be further improved by adding inorganic electrolyte particles.

[0022] (2) The composite membrane electrolyte containing the cross-linked polymer electrolyte and supporting material can effectively improve mechanical strength while ensuring that the ionic conductivity does not decrease;

[0023] (3) The above-mentioned cross-linked polymer electrolyte forms a composite electrode with the positive or negative electrode, which can effectively reduce the interfacial impedance. The lithium-ion battery prepared by the composite electrode has high coulombic efficiency and capacity retention. Detailed Implementation

[0024] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0025] The first aspect of the present invention provides a cross-linked polymer electrolyte, characterized in that the cross-linked polymer electrolyte comprises a polymer matrix, a lithium salt, and inorganic electrolyte particles;

[0026] The polymer matrix is ​​obtained by crosslinking polyphenolic monomers with polyethers;

[0027] Based on the total weight of the polymeric electrolyte, the cross-linked polymeric electrolyte comprises 50-70 wt% polymer matrix, 10-25 wt% lithium salt, and 20-35 wt% inorganic electrolyte particles.

[0028] In this invention, a cross-linking network is formed by polyphenol monomers and polyethers. The polyphenol monomers not only provide binding sites for lithium ions but also enhance the lithium ion transport rate. Simultaneously, the cross-linking effect of the polyphenols on the polyethers effectively inhibits polyether crystallization and improves the room-temperature ionic conductivity of the cross-linked polymer electrolyte.

[0029] According to the present invention, the cross-linked polymer electrolyte comprises 55-65 wt% polymer matrix, 15-18 wt% lithium salt and 25-30 wt% inorganic electrolyte particles.

[0030] In this invention, the cross-linked polymer electrolyte prepared has the best overall performance when the polymer matrix, lithium salt, and inorganic electrolyte particles meet the above-mentioned ranges.

[0031] According to the present invention, the polyphenolic monomer is selected from at least one of gallic acid, ellagic acid, tannic acid, catechin, epigallocatechin gallate, epigallocatechin gallate, pyrogallol, quercetin, morin, naringenin, rutin, naringin, phloroglucinol and resveratrol.

[0032] According to the present invention, the polyether is a functional group-terminated polyether, wherein the functional group is selected from at least one of acyl chloride, epoxy and amino groups.

[0033] In this invention, the polyether is selected from at least one of diamino polyethylene glycol, epoxy-terminated polyethylene glycol, and polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer.

[0034] Furthermore, the number-average molecular weight of the functional group-terminated polyether is 1×10⁻⁶. 2 -1×10 6 Da.

[0035] According to the present invention, the lithium salt is selected from at least one of lithium hexafluorophosphate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(trifluoromethanesulfonic acid)imide, and lithium bis(oxalato)borate.

[0036] According to the present invention, the inorganic electrolyte particles are selected from Li 1.3 Al 0.3 Ti 1.7 (PO4)3、 La 0.51 Li 0.34 TiO 2.94 Li7La3Zr2O 12 Li 1.07 Al 0.69 Ti 1.46 (PO4)3, Li 1.5 Al 0.5 Ge 1.5 (PO4)3、 Li 10 GeP2S 12 Li 3.25 Ge 0.25 P 0.75 S4, Li7P3S 11 and Li 3.25 P 0.95 At least one of S4.

[0037] In this invention, the transport performance of lithium ions in the cross-linked network is improved by adding inorganic electrolyte particles, thereby further improving the room temperature ionic conductivity of the cross-linked polymer electrolyte.

[0038] A second aspect of the present invention provides a method for preparing the above-mentioned cross-linked polymer electrolyte, characterized in that the preparation method includes:

[0039] In the presence of a solvent, polyphenol monomers, polyethers, lithium salts, and inorganic electrolyte particles are mixed and the pH is adjusted to 7-10 to carry out an in-situ crosslinking reaction, thereby obtaining a crosslinked polymer electrolyte.

[0040] In this invention, the polyphenolic monomers are derived from plant extracts and can react with polyethers in water, enabling green production.

[0041] In this invention, the types of polyphenol monomers, polyethers, lithium salts, and inorganic electrolyte particles are all the same as those in the first aspect of this invention, and will not be repeated here.

[0042] According to the present invention, based on the total amount of polyphenol monomers, polyethers, lithium salts and inorganic electrolyte particles, the amount of polyphenol monomers is 5-25 wt%, the amount of polyethers is 45-65 wt%, the amount of lithium salts is 10-25 wt%, and the amount of inorganic electrolyte particles is 20-35 wt%.

[0043] In this invention, there is no particular limitation on the method of pH adjustment; it can be a conventional method in the art, such as using lithium hydroxide or hydrochloric acid to adjust the pH value of the mixed solution.

[0044] In this invention, in order to obtain better results, the pH-adjusted mixed solution is stirred and dispersed evenly at room temperature, and then the air in the mixed solution is removed by ultrasound.

[0045] In this invention, the room temperature is a temperature conventionally understood in the art, such as 15-30°C, and should not be construed as a limitation by those skilled in the art.

[0046] In this invention, the crosslinking reaction is preferably carried out in a polytetrafluoroethylene mold.

[0047] According to the present invention, the conditions for the crosslinking reaction include: reacting at a temperature of 50-80°C for 2-5 hours.

[0048] In order to obtain better results, the preparation method further includes: subjecting the product obtained by the crosslinking reaction to a first drying, washing and a second drying.

[0049] In this invention, there are no particular limitations on the washing conditions and methods. They can be conventional washing methods in the art, as long as they can remove residual unreacted monomers and solvents. For example, anhydrous ethanol can be used to wash 2-3 times.

[0050] According to the present invention, the conditions for the first drying and the second drying each independently include: vacuum drying at 100-120°C for 1-3 hours.

[0051] Furthermore, the drying method is not particularly limited, but vacuum drying is preferred in this invention.

[0052] According to the present invention, the solvent is selected from at least one of dimethylacetamide, dimethylformamide, methanol, ethanol, isopropanol, tert-butanol, ethyl acetate, acetone, glycerol and water.

[0053] A third aspect of the present invention provides a composite membrane electrolyte, characterized in that the composite membrane electrolyte comprises the above-mentioned cross-linked polymer electrolyte and a porous support material;

[0054] The mass ratio of the cross-linked polymer electrolyte to the porous material is 0.3-0.8:1.

[0055] In this invention, when the mass ratio of the cross-linked polymer electrolyte to the porous material meets the above-mentioned range, both the ionic conductivity and mechanical strength are high.

[0056] In this invention, the mass ratio of the cross-linked polymer electrolyte to the porous material is 0.4-0.6:1.

[0057] According to the present invention, the porous support material is selected from at least one of polyethylene diaphragm, polypropylene diaphragm, polyester nonwoven fabric, polyimide nonwoven fabric, polypropylene nonwoven fabric and polyamide nonwoven fabric.

[0058] According to the present invention, the thickness of the porous support material is 20-100 micrometers and the pore size is 0.1-5 micrometers.

[0059] Furthermore, the porous support material has a thickness of 30-50 micrometers and a pore size of 0.5-2 micrometers.

[0060] A fourth aspect of the present invention provides a method for preparing the above-mentioned composite membrane electrolyte, characterized in that the preparation method includes:

[0061] In the presence of a solvent, polyphenol monomers, polyethers, lithium salts, and inorganic electrolyte particles are mixed and the pH is adjusted to 7-10. The mixture is then brought into contact with a porous support material to undergo an in-situ crosslinking reaction, resulting in a composite membrane electrolyte.

[0062] In this invention, the types and amounts of the polyphenol monomers, polyethers, lithium salts, and inorganic electrolyte particles are the same as in the second aspect of this invention, and will not be repeated here.

[0063] A fifth aspect of the present invention provides a composite positive electrode, characterized in that the composite positive electrode is prepared by the following method:

[0064] In the presence of a solvent, polyphenol monomers, polyethers, lithium salts, and inorganic electrolyte particles are mixed and the pH is adjusted to 7-10. The mixture is then brought into contact with the positive electrode sheet to undergo an in-situ crosslinking reaction, resulting in a composite positive electrode.

[0065] In this invention, the composite positive electrode comprises a cross-linked polymer electrolyte and a positive electrode sheet, wherein the cross-linked polymer electrolyte is the cross-linked polymer electrolyte provided in the first aspect of this invention.

[0066] Furthermore, the mass ratio of the cross-linked polymer electrolyte to the positive electrode is 0.01-0.5:1.

[0067] To achieve better results, the mass ratio of the cross-linked polymer electrolyte to the positive electrode is 0.05-0.3:1.

[0068] According to the present invention, the positive electrode sheet is composed of a positive electrode material and an aluminum foil, wherein the positive electrode material is selected from at least one of lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, nickel-manganese materials, nickel-cobalt-manganese ternary materials, and sulfur-containing materials.

[0069] In this invention, the types and amounts of the polyphenol monomers, polyethers, lithium salts, and inorganic electrolyte particles are the same as in the second aspect of this invention, and will not be repeated here.

[0070] A sixth aspect of the present invention provides a composite negative electrode, characterized in that the composite negative electrode is prepared by the following method:

[0071] In the presence of a solvent, polyphenol monomers, polyethers, lithium salts, and inorganic electrolyte particles are mixed and the pH is adjusted to 7-10. The mixture is then brought into contact with the negative electrode sheet to undergo an in-situ crosslinking reaction, resulting in a composite negative electrode.

[0072] In this invention, the composite negative electrode comprises a cross-linked polymer electrolyte and a negative electrode sheet, wherein the cross-linked polymer electrolyte is the cross-linked polymer electrolyte provided in the first aspect of this invention.

[0073] Furthermore, the mass ratio of the cross-linked polymer electrolyte to the negative electrode is 0.01-0.5:1.

[0074] To achieve better results, the mass ratio of the cross-linked polymer electrolyte to the positive electrode is 0.05-0.3:1.

[0075] According to the present invention, the negative electrode sheet is composed of a negative electrode material and copper foil, wherein the negative electrode material is selected from at least one of lithium metal sheet, graphite, soft carbon, hard carbon and silicon material.

[0076] In this invention, the types and amounts of the polyphenol monomers, polyethers, lithium salts, and inorganic electrolyte particles are the same as in the second aspect of this invention, and will not be repeated here.

[0077] The seventh aspect of the present invention provides a lithium-ion battery, characterized in that the lithium-ion battery comprises one of the above-mentioned cross-linked polymer electrolyte, composite membrane electrolyte, composite positive electrode and composite negative electrode.

[0078] In this invention, the lithium-ion battery contains any one of the above-mentioned cross-linked polymer electrolyte, composite membrane electrolyte, composite positive electrode, and composite negative electrode.

[0079] In this invention, the polymer electrolyte forms a composite electrode with the positive or negative electrode, which effectively reduces the gap between the electrolyte and the electrode and lowers the interface resistance.

[0080] In this invention, since the phenolic hydroxyl groups in the polyphenol monomers are fixed in the cross-linked network, they will not migrate during battery operation. This can significantly reduce the accumulation of anions on the electrode surface, weaken the polarization voltage caused by concentration polarization, and further improve the cycle stability of the lithium battery.

[0081] The present invention will be described in detail below through embodiments. In the following embodiments,

[0082] The crystallinity of cross-linked polymer electrolytes and composite membrane electrolytes was determined by XRD.

[0083] The tensile strength of the cross-linked polymer electrolyte and the composite membrane electrolyte was measured by a universal tensile testing machine.

[0084] The room temperature ionic conductivity of the cross-linked polymer electrolyte and the composite membrane electrolyte was measured by an electrochemical workstation method.

[0085] The thickness of the porous support material was measured using a thickness gauge.

[0086] The pore size of the porous support material was measured using a mercury porosimeter.

[0087] The coulombic efficiency of lithium-ion batteries was measured using a blue electric cycle tester.

[0088] The discharge capacity retention rate of lithium-ion batteries was measured using a Blue Electric Cycling Tester.

[0089] The chemical reagents and instruments used in the embodiments and comparative examples of this invention are all commercially available products.

[0090] I. Preparation of Cross-linked Polymer Electrolytes

[0091] Example 1-1

[0092] (1) Mix 4g of tannic acid, 10g of diamino polyethylene glycol (number average molecular weight 20,000 Da), 4g of lithium perchlorate, and 6g of Li 1.3 Al 0.3 Ti 1.7 (PO4) was added to 100 mL of water, and the pH of the reaction solution was adjusted to 9 using lithium hydroxide solution. The mixture was stirred and sonicated at 20 °C to remove air, resulting in a mixed solution.

[0093] (2) Pour the above mixed solution into a polytetrafluoroethylene mold and react at 60°C for 2.5 h to obtain a crosslinked product. Place it in a vacuum oven and dry at 110°C for 1 h to obtain a crosslinked polymer electrolyte matrix.

[0094] (3) The prepared cross-linked polymer electrolyte matrix was washed three times with anhydrous ethanol to remove the unreacted monomers remaining in the membrane. Finally, it was placed in a vacuum oven and dried at 100°C for 1 hour to obtain the cross-linked polymer electrolyte.

[0095] The cross-linked polymer electrolyte contains a polymer matrix of 58.3 wt%, a lithium salt of 16.7 wt%, and inorganic electrolyte particles of 25 wt%.

[0096] The crystallinity, tensile strength, and room temperature ionic conductivity of the cross-linked polymer electrolyte are shown in Table 1.

[0097] Examples 1-2

[0098] Consistent with Example 1-1, except that the amount of tannic acid used is 4g, the amount of diamino polyethylene glycol used is 12g, the amount of lithium perchlorate used is 4g, and the amount of Li... 1.3 Al 0.3 Ti 1.7 The amount of (PO4) used was 6g, so that the content of polymer matrix in the prepared cross-linked polymer electrolyte was 61.5wt%, the content of lithium salt was 15.4wt%, and the content of inorganic electrolyte particles was 23.1wt%.

[0099] The crystallinity, tensile strength, and room temperature ionic conductivity of the cross-linked polymer electrolyte are shown in Table 1.

[0100] Examples 1-3

[0101] Consistent with Example 1-1, except that tannic acid is replaced with gallic acid and diamino polyethylene glycol is replaced with polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer (number average molecular weight 5800 Da).

[0102] The cross-linked polymer electrolyte contains a polymer matrix of 58.3 wt%, a lithium salt of 16.7 wt%, and inorganic electrolyte particles of 25 wt%.

[0103] The crystallinity, tensile strength, and room temperature ionic conductivity of the cross-linked polymer electrolyte are shown in Table 1.

[0104] Examples 1-4

[0105] Consistent with Example 1-1, except that the amount of tannic acid used is 6g, the amount of diamino polyethylene glycol used is 11.5g, the amount of lithium perchlorate used is 3g, and Li... 1.3 Al 0.3 Ti 1.7 The amount of (PO4) used was 6g. The cross-linked polymer electrolyte prepared contained a polymer matrix content of 66wt%, a lithium salt content of 11.3wt%, and an inorganic electrolyte particle content of 22.7wt%.

[0106] The crystallinity, tensile strength, and room temperature ionic conductivity of the cross-linked polymer electrolyte are shown in Table 1.

[0107] Comparative Example 1-1

[0108] Consistent with Example 1-1, except that the polyphenol monomers are replaced with an equal amount of glycerol triglycidyl ether.

[0109] The crystallinity, tensile strength, and room temperature ionic conductivity of the obtained cross-linked polymer electrolyte are shown in Table 1.

[0110] Comparative Examples 1-2

[0111] Consistent with Example 1-1, except that it does not contain inorganic electrolyte particles.

[0112] The crystallinity, tensile strength, and room temperature ionic conductivity of the obtained cross-linked polymer electrolyte are shown in Table 1.

[0113] Comparative Examples 1-3

[0114] Same as Example 1-1, except that the amount of tannic acid used is 10g, the amount of diamino polyethylene glycol used is 5g, the amount of lithium perchlorate used is 1g, and the amount of Li... 1.3 Al 0.3 Ti 1.7 The amount of (PO4) used is 10g, so that the content of polymer matrix in the prepared cross-linked polymer electrolyte is 37.7wt%, the content of lithium salt is 3.8wt%, and the content of inorganic electrolyte particles is 38.4wt%.

[0115] The crystallinity, tensile strength, and room temperature ionic conductivity of the cross-linked polymer electrolyte are shown in Table 1.

[0116] Table 1

[0117]

[0118] As can be seen from the results in Table 1, Examples 1-1 to 1-4, which fall within the scope of protection of this invention, have lower crystallinity and higher room temperature ionic conductivity. Among them, the cross-linked polymer electrolytes prepared in Examples 1-2 to 1-3, which meet the preferred technical solutions of this invention, have significantly better effects, with a crystallinity not exceeding 36% and a room temperature ionic conductivity not less than 0.58 mS / cm.

[0119] However, the comparative examples 1-1 to 1-3, which do not meet the technical requirements of this invention, have higher crystallinity and very low room temperature conductivity.

[0120] II. Preparation of Composite Membrane Electrolytes

[0121] Example 2-1

[0122] S1, 2.5g epigallocatechin gallate, 8g epoxy-terminated polyethylene glycol (number average molecular weight 10,000 Da), 4.5g lithium bis(oxalato)borate and 5g Li 10 GeP2S 12 Add to 100 mL of ethanol, adjust the pH of the reaction solution to 9 using lithium hydroxide solution, stir and sonicate at 20 °C to remove air from the solution, and obtain a mixed solution;

[0123] S2. Pour the above mixed solution into a polytetrafluoroethylene mold containing polyester nonwoven fabric (70 micrometers thick, 5 micrometers average pore size), react at 60°C for 2.5 hours, and then place it in a vacuum oven and dry at 110°C for 2 hours to obtain the composite membrane electrolyte matrix.

[0124] S3. The prepared electrolyte matrix is ​​washed three times with anhydrous ethanol. Finally, the washed polymer electrolyte is placed in a vacuum oven and dried at 100°C for 1 hour to evaporate excess ethanol, thus obtaining the polymer electrolyte of the porous material membrane.

[0125] The mass ratio of the composite membrane electrolyte to the porous material is 0.3:1.

[0126] The crystallinity, tensile strength, and room temperature ionic conductivity of the polymer electrolyte in the porous material membrane are shown in Table 2.

[0127] Example 2-2

[0128] S1. Combine 2.5g epigallocatechin gallate, 8g epoxy-terminated polyethylene glycol (number average molecular weight 20,000 Da), 4.5g lithium bis(trifluoromethanesulfonic acid)imide, and 5g Li7P3S. 11 Add to 100 mL of dimethylacetamide, adjust the pH of the reaction solution to 9 using lithium hydroxide solution, stir and sonicate at 20 °C to remove air from the solution, and obtain a mixed solution;

[0129] S2. Pour the above mixed solution into a polytetrafluoroethylene mold containing a polyethylene diaphragm (thickness 25 micrometers, pore size 0.6 micrometers), react at 60°C for 2.5 hours, and then place it in a vacuum oven and dry at 110°C for 2 hours to obtain a composite diaphragm electrolyte matrix.

[0130] S3. The prepared composite membrane electrolyte matrix was washed three times with anhydrous ethanol to remove unreacted monomers and dimethylacetamide remaining in the membrane. Finally, the washed polymer was placed in a vacuum oven and dried at 100°C for 1 hour to obtain the composite membrane electrolyte.

[0131] The mass ratio of the composite membrane electrolyte to the porous material is 0.6:1; the crystallinity, tensile strength and room temperature ionic conductivity of the composite membrane electrolyte are shown in Table 2.

[0132] Example 2-3

[0133] Similar to Example 2-1, except that the polyester nonwoven fabric has a thickness of 15 micrometers and a pore size of 0.6 micrometers.

[0134] The mass ratio of the polymer electrolyte to the porous material is 1.8:1; the crystallinity, tensile strength and room temperature ionic conductivity of the composite membrane electrolyte are shown in Table 2.

[0135] Examples 2-4

[0136] S1. Mix 4g tannic acid, 10g diamino polyethylene glycol (number average molecular weight 20,000 Da), 4g lithium perchlorate, and 6g Li 1.3 Al 0.3 Ti 1.7 (PO4) was added to 100 mL of water, and the pH of the reaction solution was adjusted to 9 using lithium hydroxide solution. The solution was stirred and sonicated at 20 °C to remove air from the solution, resulting in a mixed solution.

[0137] S2, Same as Example 2-1;

[0138] S3, same as Example 2-1.

[0139] The mass ratio of the composite membrane electrolyte to the porous material is 0.5:1.

[0140] The crystallinity, tensile strength, and room temperature ionic conductivity of the composite membrane electrolyte are shown in Table 2.

[0141] Comparative Example 2-1

[0142] Consistent with Example 2-1, except that the amount of epigallocatechin gallate was 4g, the amount of epoxy-terminated polyethylene glycol (number average molecular weight 20,000 Da) was 2g, and the amount of lithium bis(oxalate)borate was 3g. 10 GeP2S 12 2g, wherein the mass ratio of the polymer electrolyte to the porous material is 0.9:1.

[0143] The crystallinity, tensile strength, and room temperature ionic conductivity of the obtained composite membrane electrolyte are shown in Table 2.

[0144] Comparative Example 2-2

[0145] Similar to Example 2-1, except that the pH of the reaction solution was adjusted to 11.

[0146] The crystallinity, tensile strength, and room temperature ionic conductivity of the obtained composite membrane electrolyte are shown in Table 2.

[0147] Table 2

[0148]

[0149] Table 2 shows that the polymer electrolytes of porous material membranes prepared in Examples 2-1 to 2-4 have high mechanical strength, low crystallinity, high room temperature ionic conductivity, and high mechanical strength due to the addition of porous support materials. Among them, the polymer electrolytes of porous material membranes prepared in Examples 2-4 have good mechanical strength and high room temperature ionic conductivity, compared with the cross-linked polymer electrolytes prepared in Example 1-1, due to the addition of porous support materials.

[0150] III. Fabrication of Composite Electrodes and Lithium-ion Batteries

[0151] The following examples will be used to describe the preparation of composite electrodes (composite positive electrode and composite negative electrode).

[0152] Example 3-1

[0153] a. Mix 9g tannic acid, 6g diamino polyethylene glycol (number average molecular weight 100,000 Da), 3.75g lithium hexafluorophosphate, and 5g La 0.51 Li 0.34 TiO 2.94Add to 100 mL of water, adjust the pH of the reaction solution to 9 using lithium hydroxide solution, stir and sonicate at 20 °C to remove air from the solution, and obtain a mixed solution;

[0154] b. Pour the above mixed solution into a polytetrafluoroethylene mold with a lithium iron phosphate positive electrode sheet containing aluminum foil at the bottom, react at 60°C for 2.5 h, and then place it in a vacuum oven and dry at 110°C for 1 h to obtain a composite positive electrode matrix containing a cross-linked polymer electrolyte.

[0155] c. The prepared composite cathode matrix containing cross-linked polymer electrolyte is washed three times with anhydrous ethanol to remove unreacted monomers remaining in the membrane. Finally, the washed cross-linked polymer electrolyte matrix is ​​placed in a vacuum oven and dried at 100°C for 2 hours to obtain composite cathode P1.

[0156] In the composite positive electrode P1, the mass ratio of the cross-linked polymer electrolyte to the positive electrode sheet is 0.2:1.

[0157] Example 3-2

[0158] The method is consistent with that in Example 3-1, except that the amount of tannic acid used is 18g, the amount of diamino polyethylene glycol is 12g, the amount of lithium hexafluorophosphate is 7.5g, and La... 0.51 Li 0.34 TiO 2.94 The amount of material used was 10g, and a composite positive electrode P2 was obtained, wherein the mass ratio of cross-linked polymer electrolyte to positive electrode sheet was 0.4:1.

[0159] Example 3-3

[0160] The method is consistent with that in Example 3-1, except that the amount of tannic acid used is 0.09 g, the amount of diamino polyethylene glycol used is 0.06 g, the amount of lithium hexafluorophosphate used is 0.038 g, and the amount of La... 0.51 Li 0.34 TiO 2.94 The amount of [agent] used was 0.05g, and a composite positive electrode P3 was obtained, wherein the mass ratio of cross-linked polymer electrolyte to positive electrode sheet was 0.002:1.

[0161] Examples 3-4

[0162] a. Mix 9g of tannic acid, 4g of epoxy-terminated polyethylene glycol (number average molecular weight 20,000 Da), 2.5g of lithium hexafluoroarsenate, and 6g of Li7La3Zr2O. 12 Add to 100 mL of water, adjust the pH of the reaction solution to 8 using lithium hydroxide solution, stir and sonicate at 20 °C to remove air from the solution, and obtain a mixed solution;

[0163] b. Pour the above mixed solution into a polytetrafluoroethylene mold with a graphite negative electrode sheet containing copper foil at the bottom, react at 70°C for 3.5 h, and then place it in a vacuum oven and dry at 110°C for 1 h to obtain a composite negative electrode matrix containing cross-linked polymer electrolyte and copper foil.

[0164] c. The prepared composite negative electrode matrix containing cross-linked polymer electrolyte and copper foil is washed three times with anhydrous ethanol to remove unreacted monomers remaining in the membrane. Finally, the washed cross-linked polymer electrolyte is placed in a vacuum oven and dried at 100°C for 2 hours to obtain the composite negative electrode N1.

[0165] In the composite negative electrode N1, the mass ratio of cross-linked polymer electrolyte to negative electrode sheet is 0.35:1.

[0166] The following application examples will be used to describe the fabrication of lithium-ion batteries.

[0167] Application Example 1

[0168] The cross-linked polymer electrolyte prepared in Example 1, the graphite negative electrode containing copper foil, and the positive electrode containing aluminum foil were stacked to obtain a lithium-ion battery C1.

[0169] The coulombic efficiency and discharge capacity retention of lithium-ion battery C1 are shown in Table 3.

[0170] Application Example 2

[0171] Similar to Application Example 1, except that the cross-linked polymer electrolyte was replaced with the composite membrane electrolyte prepared in Examples 2-4, resulting in lithium-ion battery C2.

[0172] The coulombic efficiency and discharge capacity retention of lithium-ion battery C2 are shown in Table 3.

[0173] Application Example 3

[0174] Similar to Application Example 1, except that the cross-linked polymer electrolyte and the positive electrode containing aluminum foil of lithium cobalt oxide were replaced with the composite positive electrode P1 prepared in Example 3-1 to obtain lithium-ion battery C3.

[0175] The coulombic efficiency and discharge capacity retention of lithium-ion battery C3 are shown in Table 3.

[0176] Application Example 4

[0177] Similar to Application Example 1, except that the cross-linked polymer electrolyte and the lithium cobalt oxide cathode containing aluminum foil were replaced with the composite cathode P2 prepared in Example 3-2, resulting in lithium-ion battery C4.

[0178] The coulombic efficiency and discharge capacity retention of lithium-ion battery C4 are shown in Table 3.

[0179] Application Example 5

[0180] Similar to Application Example 1, except that the cross-linked polymer electrolyte and the graphite anode sheet containing copper foil were replaced with the composite anode N1 prepared in Examples 3-4, resulting in lithium-ion battery C5.

[0181] The coulombic efficiency and discharge capacity retention of lithium-ion battery C5 are shown in Table 3.

[0182] Application Example 6

[0183] Similar to Application Example 1, except that the cross-linked polymer electrolyte and the positive electrode containing aluminum foil of lithium cobalt oxide were replaced with the composite positive electrode P3 prepared in Example 3-3, resulting in lithium-ion battery C6.

[0184] The coulombic efficiency and discharge capacity retention of lithium-ion battery C6 are shown in Table 3.

[0185] Application Example 7

[0186] Similar to Application Example 1, except that the cross-linked polymer electrolyte is replaced with the polymer electrolyte of the porous material membrane prepared in Examples 2-3, to obtain the lithium-ion battery C7.

[0187] The coulombic efficiency and discharge capacity retention of lithium-ion battery C7 are shown in Table 3.

[0188] Comparative Application Examples 1 to 3

[0189] Similar to Application Example 1, except that the cross-linked polymer electrolyte prepared in Example 1-1 was replaced with the cross-linked polymer electrolytes prepared in Comparative Examples 1-1, 1-2 and 1-3, to obtain lithium-ion batteries DC1 to DC3.

[0190] Table 3 shows the coulombic efficiency and discharge capacity retention of lithium-ion batteries DC1 to DC3.

[0191] Comparative Application Example 4

[0192] Similar to Application Example 2, except that the cross-linked polymer electrolyte prepared in Examples 2-4 was replaced with the polymer electrolyte of the porous material membrane prepared in Comparative Example 2-1, to obtain the lithium-ion battery DC4.

[0193] The coulombic efficiency and discharge capacity retention of the lithium-ion battery DC4 are shown in Table 3.

[0194] Test case

[0195] The lithium-ion batteries prepared by Application Examples 1-5 and Comparative Application Examples 1 to 4 were tested for coulombic efficiency and discharge capacity. The cycling conditions were: 100 cycles at 0.1C rate at 25°C. The results are shown in Table 3.

[0196] Table 3

[0197]

[0198]

[0199] Table 3 shows that lithium-ion batteries containing the composite cathode prepared in Example 3-1 or the composite electrode prepared in Example 3-3 exhibit high coulombic efficiency and discharge capacity, demonstrating excellent electrochemical performance. This is because the composite electrode prepared using the in-situ method can effectively reduce the void between the electrolyte and the electrode, lower the interfacial resistance, and thus improve the coulombic efficiency and discharge capacity of the battery.

[0200] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A cross-linked polymer electrolyte, characterized in that, The cross-linked polymer electrolyte comprises a polymer matrix, a lithium salt, and inorganic electrolyte particles; The polymer matrix is ​​obtained by crosslinking polyphenolic compounds with polyethers; Based on the total weight of the cross-linked polymer electrolyte, the cross-linked polymer electrolyte comprises 50-70 wt% polymer matrix, 10-25 wt% lithium salt, and 20-35 wt% inorganic electrolyte particles; The polyether is a functional group-terminated polyether, wherein the functional group is selected from at least one of acyl chloride, epoxy and amino groups; The polyphenolic compounds are selected from at least one of gallic acid, ellagic acid, tannic acid, catechin, epigallocatechin gallate, epigallocatechin gallate, pyrogallol, quercetin, morin, naringenin, rutin, naringin, phloroglucinol, and resveratrol.

2. The cross-linked polymer electrolyte according to claim 1, wherein, The cross-linked polymer electrolyte comprises a polymer matrix of 55-65 wt%, a lithium salt of 15-18 wt%, and inorganic electrolyte particles of 25-30 wt%, with the total content of the polymer matrix, lithium salt, and inorganic electrolyte particles not exceeding 100 wt%.

3. The cross-linked polymer electrolyte according to claim 1 or 2, wherein, The number-average molecular weight of the functional group-terminated polyether is 1×10⁻⁶. 2 -1×10 6 Da.

4. The cross-linked polymer electrolyte according to claim 1 or 2, wherein, The lithium salt is selected from at least one of lithium hexafluorophosphate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(trifluoromethanesulfonic acid)imide, and lithium bis(oxalato)borate.

5. The cross-linked polymer electrolyte according to claim 1 or 2, wherein, The inorganic electrolyte particles are selected from Li 1.3 Al 0.3 Ti 1.7 (PO4)3, La 0.51 Li 0.34 TiO 2.94 Li7La3Zr2O 12 Li 1.07 Al 0.69 Ti 1.46 (PO4)3, Li 1.5 Al 0.5 Ge 1.5 (PO4)3, Li 10 GeP2S 12 Li 3.25 Ge 0.25 P 0.75 S4, Li7P3S 11 and Li 3.25 P 0.95 At least one of S4.

6. A method for preparing a cross-linked polymer electrolyte according to any one of claims 1-5, characterized in that, The preparation method includes: In the presence of a solvent, polyphenolic compounds, polyethers, lithium salts, and inorganic electrolyte particles are mixed and the pH is adjusted to 7-10 to carry out an in-situ crosslinking reaction, thereby obtaining a crosslinked polymer electrolyte.

7. The preparation method according to claim 6, wherein, Based on the total amount of polyphenolic compounds, polyethers, lithium salts and inorganic electrolyte particles, the amount of polyphenolic compounds is 5-25 wt%, the amount of polyethers is 45-65 wt%, the amount of lithium salts is 10-25 wt%, and the amount of inorganic electrolyte particles is 20-35 wt%.

8. The preparation method according to claim 6, wherein, The solvent is selected from at least one of dimethylacetamide, dimethylformamide, methanol, ethanol, isopropanol, tert-butanol, ethyl acetate, acetone, glycerol, and water.

9. The preparation method according to claim 6, wherein, The conditions for the crosslinking reaction include reacting at a temperature of 50-80℃ for 2-5 hours.

10. A composite membrane electrolyte, characterized in that, The composite membrane electrolyte comprises the cross-linked polymer electrolyte and the porous support material as described in any one of claims 1-5; The mass ratio of the cross-linked polymer electrolyte to the porous support material is 0.3-0.8:

1.

11. The composite membrane electrolyte according to claim 10, wherein, The porous support material is selected from at least one of polyethylene diaphragm, polypropylene diaphragm, polyester nonwoven fabric, polyimide nonwoven fabric, polypropylene nonwoven fabric, and polyamide nonwoven fabric.

12. The composite membrane electrolyte according to claim 10 or 11, wherein, The thickness of the porous support material is 20-100 micrometers, and the pore size is 0.1-5 micrometers.

13. A method for preparing a composite membrane electrolyte according to any one of claims 10-12, characterized in that, The preparation method includes: In the presence of a solvent, polyphenolic compounds, polyethers, lithium salts, and inorganic electrolyte particles are mixed and the pH is adjusted to 7-10. The mixture is then brought into contact with a porous support material to undergo an in-situ crosslinking reaction, resulting in a composite membrane electrolyte.

14. A composite positive electrode, characterized in that, The composite positive electrode comprises the cross-linked polymer electrolyte and positive electrode sheet as described in any one of claims 1-5; The composite cathode is prepared according to the following method: In the presence of a solvent, polyphenolic compounds, polyethers, lithium salts, and inorganic electrolyte particles are mixed and the pH is adjusted to 7-10. The mixture is then brought into contact with the positive electrode to undergo an in-situ crosslinking reaction, resulting in a composite positive electrode.

15. A composite negative electrode, characterized in that, The composite negative electrode comprises the cross-linked polymer electrolyte and negative electrode sheet as described in any one of claims 1-5; The composite negative electrode is prepared according to the following method: In the presence of a solvent, polyphenolic compounds, polyethers, lithium salts, and inorganic electrolyte particles are mixed and the pH is adjusted to 7-10. The mixture is then brought into contact with the negative electrode sheet to undergo an in-situ crosslinking reaction, resulting in a composite negative electrode.

16. A lithium-ion battery, characterized in that, The lithium-ion battery comprises one of the following: the cross-linked polymer electrolyte according to any one of claims 1-5, the composite membrane electrolyte according to any one of claims 10-12, the composite positive electrode according to claim 14, and the composite negative electrode according to claim 15.

Citation Information

Patent Citations

  • Fixed electrolyte and lithium-based battery using the same

    CN103165936A

  • Composite solid-state electrolyte, solid-state battery and preparation method of solid-state battery

    CN111244537A