TOPCon batteries and their formation methods

By forming a doped crystalline silicon layer in the TOPCon cell and optimizing its structure, the problems of light absorption in the polycrystalline silicon layer and transport resistance in the silicon nitride layer were solved, thereby improving the efficiency and stability of the solar cell.

CN117293219BActive Publication Date: 2026-11-10JINKO SOLAR (SHANGRAO) CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311146365.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-09-06
Publication Date
2026-11-10
Estimated Expiration
2043-09-06

AI Technical Summary

Technical Problem

In traditional TOPCon solar cells, the small band gap of the polycrystalline silicon layer leads to parasitic photoabsorption, and the large lateral transport resistance of the silicon nitride layer limits the improvement of cell efficiency.

Method used

A doped source layer is formed on the surface of the initial crystalline silicon layer, and a doped crystalline silicon layer is formed through a diffusion process. The thickness and structure of the doped crystalline silicon layer are adjusted by an oxidation process to form an electrostatic field to reduce the carrier recombination rate. A mask layer is used to protect key parts and avoid light absorption and contact stability issues.

Benefits of technology

It improves the photoelectric conversion efficiency of solar cells, increases the fill factor and short-circuit current, reduces the carrier recombination rate, and improves the stability and light absorption utilization of the cells.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117293219B_ABST
    Figure CN117293219B_ABST
Patent Text Reader

Abstract

This application relates to the field of solar cell technology, providing a TOPCon cell and a method for forming the same. The method includes: forming a tunneling layer and an initial crystalline silicon layer sequentially stacked on a substrate surface; forming a doped source layer containing doped ions on the surface of the initial crystalline silicon layer; forming a mask layer on the surface of the doped source layer; using a diffusion process to diffuse doped ions from the doped source layer into the initial crystalline silicon layer, thereby transforming the initial crystalline silicon layer into a doped crystalline silicon layer, the doped crystalline silicon layer comprising a first portion and a second portion; using an oxidation process to transform a portion of the second portion into an oxide layer; removing the oxide layer and the mask layer; forming a passivation layer on the surface of the doped crystalline silicon layer; and forming grid lines on the surface of the passivation layer, the grid lines being directly opposite the first portion and penetrating the passivation layer along the substrate thickness direction to make electrical contact with the first portion, thereby improving the performance of the solar cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of solar cell technology, and in particular to a TOPCon cell and a method for forming the same. Background Technology

[0002] With the continuous development of solar cell technology, more and more photovoltaic manufacturers are beginning to deploy TOPCon cell technology. Traditional TOPCon solar cells use a tunneling oxide layer and a polycrystalline silicon layer on the back for passivation contacts. This structure allows majority carriers to penetrate the oxide layer while blocking minority carriers, thus achieving selective carrier passage and reducing surface recombination and metal recombination. However, the small band gap of the polycrystalline silicon layer results in strong parasitic absorption of light, which limits further improvements in TOPCon cell efficiency. Furthermore, the use of silicon nitride layers in traditional TOPCon solar cells leads to a high lateral transport resistance, which is also detrimental to performance improvement. Summary of the Invention

[0003] This application provides a TOPCon cell and a method for forming the same, which at least helps to improve the performance of solar cells.

[0004] According to some embodiments of this application, one aspect of this application provides a method for forming a TOPCon battery, comprising: providing a substrate; forming a tunneling layer and an initial crystalline silicon layer sequentially stacked on the surface of the substrate; forming a doped source layer on the surface of the initial crystalline silicon layer, the doped source layer containing doped ions; forming a mask layer on the surface of the doped source layer, the mask layer including multiple sub-mask layers; employing a diffusion process to diffuse doped ions in the doped source layer into the initial crystalline silicon layer, thereby transforming the initial crystalline silicon layer into a doped crystalline silicon layer, the doped crystalline silicon layer including a first portion and a second portion, the first portion facing the sub-mask layers, the second portion facing the gap between adjacent sub-mask layers; employing an oxidation process to transform a portion of the second portion into an oxide layer; removing the oxide layer and the mask layer; forming a passivation layer on the surface of the doped crystalline silicon layer; forming a gate line on the surface of the passivation layer, the gate line facing the first portion, and the gate line penetrating the passivation layer along the thickness direction of the substrate and making electrical contact with the first portion.

[0005] In some embodiments, the temperature of the diffusion process is higher than that of the oxidation process, the pressure of the diffusion process is lower than that of the oxidation process, the oxygen flow rate of the diffusion process is lower than that of the oxidation process, and the nitrogen flow rate of the diffusion process is higher than that of the oxidation process.

[0006] In some embodiments, the process conditions for the diffusion process include: a temperature of 880–950°C, a pressure of 50–250 mbar, an oxygen flow rate of 0–1000 sccm, and a nitrogen flow rate of 500–4000 sccm; the process conditions for the oxidation process include: a process temperature of 50–800°C, a pressure of 250–900 mbar, an oxygen flow rate of 200–5000 sccm, and a nitrogen flow rate of 0–3000 sccm.

[0007] In some embodiments, during the process of converting a portion of the second thickness into an oxide layer using an oxidation process, the temperature of the oxidation process is gradually reduced.

[0008] In some embodiments, the thickness of the mask layer is 2 nm to 8 nm in the direction perpendicular to the substrate surface.

[0009] In some embodiments, the ratio of the thickness of the oxide layer to the thickness of the doped silicon layer in a direction perpendicular to the substrate surface is 0.4 to 0.6.

[0010] According to some embodiments of this application, this application also provides a TOPCon battery, which is prepared using any of the TOPCon battery formation methods described in the above embodiments, comprising: a substrate; a tunneling layer located on the surface of the substrate; a doped silicon layer located on the surface of the tunneling layer away from the substrate, the doped silicon layer comprising a first portion and a second portion, wherein the height of the first portion relative to the substrate surface is higher than the height of the second portion relative to the substrate surface in a direction perpendicular to the substrate surface; a passivation layer located on the surface of the doped silicon layer away from the tunneling layer; and a gate line located on the surface of the passivation layer away from the doped silicon layer, the gate line being directly opposite the first portion and penetrating the passivation layer along the thickness direction of the substrate to make electrical contact with the first portion.

[0011] In some embodiments, the thickness ratio of the first portion to the second portion is 4:1 to 5:1 in the direction perpendicular to the substrate surface.

[0012] In some embodiments, the thickness of the second portion is 15 nm to 25 nm in a direction perpendicular to the substrate surface.

[0013] In some embodiments, the ratio of the doped ion concentration in the first portion to the doped ion concentration in the second portion is 0.9:1 to 1:1.

[0014] The technical solution provided in this application has at least the following advantages:

[0015] The TOPCon cell formation method provided in this application provides a tunneling layer on the substrate surface that can chemically passivate the substrate, increasing the interface state density and promoting the recombination of photogenerated carriers. This increases the fill factor, short-circuit current, and open-circuit voltage of the solar cell, thereby improving its photoelectric conversion efficiency. After forming the initial crystalline silicon layer, a doped source layer with doped ions is first formed on the surface of the initial crystalline silicon layer. Then, a mask layer is formed on the surface of the doped source layer, followed by a diffusion process. In the subsequent diffusion process, the doped ions in the doped source layer diffuse into the initial crystalline silicon layer, transforming it into a doped crystalline silicon layer. The doped crystalline silicon layer can have a field passivation effect, forming an electrostatic field in the direction from the doped crystalline silicon layer towards the substrate. This causes minority carriers to escape, reducing their concentration and lowering the carrier recombination rate at the substrate interface. The mask layer includes multiple sub-mask layers, the positions of which correspond to the positions of the electrode regions on the substrate. In the oxidation process, the first part I of the doped silicon layer is covered by the sub-mask layer, while the second part II of the doped silicon layer is exposed. Only a portion of the thickness of the second part II is oxidized into an oxide layer, and the first part I is protected by the mask layer. Thus, for the doped silicon layer, the thickness of the second part II is reduced in the direction perpendicular to the substrate surface, which can reduce the parasitic absorption effect of the doped silicon layer. Meanwhile, the thickness of the first part I remains unchanged. Therefore, when the passivation layer and gate lines are subsequently formed, the gate lines corresponding to the positions of the first part I will not directly contact the tunneling layer due to the excessive thinness of the first part I when they burn through the passivation layer and make electrical contact with the first part I, thus improving the stability of the solar cell. Attached Figure Description

[0016] One or more embodiments are illustrated by way of example with corresponding pictures in the accompanying drawings. These illustrations do not constitute a limitation on the embodiments. Unless otherwise stated, the pictures in the accompanying drawings do not constitute a limitation on scale. In order to more clearly illustrate the technical solutions in the embodiments of this application or in the conventional technology, the drawings used in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0017] Figures 1 to 10 This is a schematic diagram of the structure corresponding to each step of a method for forming a TOPCon battery provided in an embodiment of this application. Detailed Implementation

[0018] The doped polycrystalline silicon layer in TOPCon solar cells exhibits optical parasitic effects, which reduces the utilization rate of incident light. To mitigate the light absorption effect of TOPCon cells, laser ablation can be used to thin the doped polycrystalline silicon layer in the non-metallic regions, thereby reducing the thickness of the doped polycrystalline silicon in the non-metallic areas and thus reducing the light absorption effect of the doped polycrystalline silicon layer. However, because laser ablation thinning has relatively high energy, it can easily cause significant damage to the film layer, and may even lead to microcracks and mechanical damage.

[0019] According to some embodiments of this application, one embodiment of this application provides a method for forming a TOPCon cell to improve the performance of solar cells.

[0020] The embodiments of this application will now be described in detail with reference to the accompanying drawings. However, those skilled in the art will understand that many technical details have been provided in the embodiments of this application to facilitate a better understanding of the application. However, the technical solutions claimed in this application can be implemented even without these technical details and various variations and modifications based on the following embodiments.

[0021] Figures 1 to 10 The following is a structural diagram showing the various steps of a method for forming a TOPCon battery according to an embodiment of this application. The method for forming a TOPCon battery according to this embodiment will be described in detail below with reference to the accompanying drawings.

[0022] refer to Figure 1 Provides a base of 100.

[0023] The material of the substrate 100 can be an elemental semiconductor material, such as silicon or germanium silicon. The elemental semiconductor material can be in a single crystal state, a polycrystalline state, an amorphous state, or a microcrystalline state (a state that simultaneously possesses a single crystal state and an amorphous state is called a microcrystalline state). For example, silicon can be at least one of single crystal silicon, polycrystalline silicon, amorphous silicon, or microcrystalline silicon.

[0024] The substrate 100 can also be a compound semiconductor material. Common compound semiconductor materials include, but are not limited to, silicon germanide, silicon carbide, gallium arsenide, indium gallium arsenide, perovskite, cadmium telluride, and copper indium selenide.

[0025] The substrate 100 can be an N-type semiconductor substrate or a P-type semiconductor substrate. The N-type semiconductor substrate is doped with an N-type dopant element, which can be any one of group V elements such as phosphorus (P), bismuth (Bi), antimony (Sb), or arsenic (As). The P-type semiconductor substrate is doped with a P-type dopant element, which can be any one of group III elements such as boron (B), aluminum (Al), gallium (Ga), or gallium (In).

[0026] The substrate may have a front and a back side. In some embodiments, the solar cell is a single-sided cell, in which case the front side of the substrate can serve as the light-receiving surface to receive incident light, and the back side serves as the back-lighting surface. In some embodiments, the solar cell is a bifacial cell, in which case both the front and back sides of the substrate can serve as light-receiving surfaces to receive incident light.

[0027] In some embodiments, a texturing process can be applied to at least one surface of the substrate's light-receiving or back-light-receiving side to form a textured structure, such as a pyramidal textured surface, on at least one surface of the substrate's light-receiving or back-light-receiving side. This can enhance the absorption and utilization rate of incident light on the substrate's light-receiving or back-light-receiving side, thereby improving the efficiency of the solar cell.

[0028] Typically, a solar cell has an electrode region, and the grid lines of the solar cell are located in the electrode region. The grid lines are used to collect the electrical energy generated by the solar cell and transmit the electrical energy to the outside world. Therefore, in Figure 1 The substrate 100 is divided into alternating electrode regions 103 and non-electrode regions 104, and the positions of the grid lines correspond to the electrode regions 103 of the substrate 100.

[0029] refer to Figure 2 or Figure 3 A tunneling layer 110 and an initial crystalline silicon layer 120 are formed sequentially on the surface of the substrate 100.

[0030] In some embodiments, reference Figure 2 A tunneling layer 110 and an initial crystalline silicon layer 120 can be formed on the back surface of the substrate 100.

[0031] In some embodiments, reference Figure 3 Furthermore, a tunneling layer 110 and an initial crystalline silicon layer 120 can be formed on the light-receiving surface of the substrate 100. The substrate 100 may include a substrate 101 and an emitter 102. The substrate 101 has a front side and a back side, with the front side being the light-receiving surface and the back side being the back light-receiving surface. The emitter 102 is located on the front side of the substrate 101, the tunneling layer 110 is located on the surface of the emitter 102 away from the substrate 101, and the initial crystalline silicon layer 120 is located on the surface of the tunneling layer 110 away from the emitter 102.

[0032] The tunneling layer 110 can achieve a chemical passivation effect. Due to the presence of interface state defects on the surface of the substrate 100, the tunneling layer 110 can saturate the dangling bonds on the surface of the substrate 100, reduce the defect state density on the surface of the substrate 100, and reduce the recombination centers on the surface of the substrate 100 to reduce the carrier recombination rate. This results in a larger interface state density on the surface of the substrate 100. The increase in interface state density will promote the recombination of photogenerated carriers, increase the fill factor, short-circuit current, and open-circuit voltage of the solar cell, and thus improve the photoelectric conversion efficiency of the solar cell.

[0033] In some embodiments, the material of the tunneling layer 110 may be at least one of silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, or magnesium fluoride.

[0034] In some embodiments, the thickness of the tunneling layer 110 in the direction perpendicular to the surface of the substrate 100 can be 1 nm to 2 nm, such as 1 nm, 1.2 nm, 1.4 nm, 1.6 nm, 1.8 nm or 2 nm, etc. A thinner tunneling layer 110 can more effectively reduce contact recombination.

[0035] In some embodiments, the initial crystalline silicon layer 120 may be intrinsic polycrystalline silicon or intrinsic amorphous silicon, etc.

[0036] refer to Figure 4 A doped source layer 130 is formed on the surface of the initial crystalline silicon layer 120, and the doped source layer 130 contains doped ions.

[0037] In some embodiments, if the substrate 100 contains N-type doped ions, then the doped ions in the doped source layer 130 are N-type doped ions; if the substrate 100 contains P-type doped ions, then the doped ions in the doped source layer 130 are P-type doped ions. That is, the type of doped ions in the doped source layer 130 is the same as the type of doped ions in the substrate 100.

[0038] If the dopant ions in the doped source layer 130 are N-type dopant ions, trimethyl borate, tripropyl borate, boron tribromide, or anhydrous trimethyl borate can be used as deposition sources. The deposition sources can decompose to produce boron oxide, which is deposited on the surface of the initial crystalline silicon layer 120. If the dopant ions in the doped source layer 130 are P-type dopant ions, phosphorus oxychloride can be used as a deposition source. The phosphorus pentoxide produced by the decomposition of phosphorus oxychloride will be deposited on the surface of the initial crystalline silicon layer 120.

[0039] refer to Figure 5 A mask layer 140 is formed on the surface of the doped source layer 130. The mask layer 140 includes multiple sub-mask layers 141. The multiple sub-mask layers 141 can be arranged parallel to each other, and the positions of the sub-mask layers 141 are directly opposite the positions of the electrode regions 103.

[0040] In some embodiments, chemical vapor deposition (CVD), plasma-enhanced vapor deposition (PECVD), atomic layer deposition (ALD), plasma-enhanced atomic layer deposition (PEALD), or physical vapor deposition (PVD) may be employed.

[0041] In some embodiments, the material of the mask layer 140 may be silicon oxide, silicon nitride, silicon oxynitride, and silicon carbide nitride, etc.

[0042] refer to Figure 6A diffusion process is used to diffuse dopant ions from the doped source layer 130 into the initial silicon layer 120, thereby transforming the initial silicon layer 120 into a doped silicon layer 121. The doped silicon layer 121 includes a first part I and a second part II. The first part I is directly opposite to the sub-mask layer 141, and the second part II is directly opposite to the gap between adjacent sub-mask layers 141. That is, the first part is directly opposite to the electrode region, and the second part is directly opposite to the non-electrode region.

[0043] In some embodiments, the conditions of the diffusion process may include: a process temperature of 880°C to 950°C, such as 880°C, 890°C, 900°C, 910°C, 920°C, 930°C, 940°C, or 950°C; a constant pressure of 50 mbar to 250 mbar, such as 50 mbar, 80 mbar, 100 mbar, 120 mbar, 150 mbar, 180 mbar, 200 mbar, 220 mbar, 240 mbar, or 250 mbar; and a nitrogen flow rate of 500 sccm to 4000 sccm. sccm, such as 500sccm, 800sccm, 1000sccm, 1500sccm, 2000sccm, 2500sccm, 3000sccm, 3500sccm or 4000sccm; oxygen flow rate in the range of 0sccm to 1000sccm, such as 0sccm, 100sccm, 200sccm, 300sccm, 400sccm, 500sccm, 600sccm, 700sccm, 800sccm, 900sccm or 1000sccm.

[0044] The doped ions in the doped source layer 130 are diffused into the initial crystalline silicon layer 120 through a diffusion process, so that the initial crystalline silicon layer 120 is transformed into a doped crystalline silicon layer 121. The doped crystalline silicon layer 121 can have a field passivation effect. An electrostatic field can be formed in the direction from the self-doped crystalline silicon layer 121 to the substrate 100, causing minority carriers to escape, thereby reducing the concentration of minority carriers and reducing the carrier recombination rate at the interface of the substrate 100. This, in turn, increases the open-circuit voltage, short-circuit current and fill factor of the solar cell, thereby improving the photoelectric conversion efficiency of the solar cell.

[0045] In some embodiments, the dopant ion concentration of the first portion I of the doped silicon layer 121 can be greater than the dopant ion concentration within the substrate 100, and the dopant ion concentration of the second portion II of the doped silicon layer 121 is greater than the dopant ion concentration within the substrate 100. In this way, a sufficiently high potential barrier can be formed along the direction of the doped silicon layer 121 toward the substrate 100, allowing majority carriers in the substrate 100 to pass through the tunneling layer 110 into the doped silicon layer 121, thereby improving the efficiency of the solar cell.

[0046] In some embodiments, the ratio of the dopant ion concentration in the first part I to the dopant ion concentration in the second part II is 0.9:1 to 1:1, for example, 0.9:1, 0.92:1, 0.94:1, 0.96:1, 0.98:1, or 1:1. It is understood that if the mask layer 140 is located on the surface of the first part I during the diffusion process, it may affect the diffusion process, resulting in a lower dopant ion concentration in the first part I compared to the second part II. However, by controlling the thickness of the mask layer 140, the ratio of the dopant ion concentration in the first part I to the dopant ion concentration in the second part II can be kept within an appropriate range to avoid affecting the performance of the doped silicon layer 121.

[0047] refer to Figure 7 An oxidation process is used to transform a portion of the second part II into an oxide layer 150. This reduces the remaining thickness of the second part II in the direction perpendicular to the surface of the substrate 100.

[0048] In some embodiments, the conditions of the oxidation process may include: a process temperature of 50–800°C, such as 50°C, 100°C, 200°C, 400°C, 600°C, or 800°C; a pressure of 250 mbar–900 mbar, such as 250 mbar, 300 mbar, 400 mbar, 600 mbar, 800 mbar, or 900 mbar; an oxygen flow rate of 200 sccm–5000 sccm, such as 200 sccm, 500 sccm, 1000 sccm, 2000 sccm, 3000 sccm, 4000 sccm, or 5000 sccm; and a nitrogen flow rate of 0 sccm–3000 sccm, such as 0 sccm, 500 sccm, 1000 sccm, 1500 sccm, 2000 sccm, 2500 sccm, or 3000 sccm.

[0049] In some embodiments, the temperature of the diffusion process is higher than that of the oxidation process, the pressure of the diffusion process is lower than that of the oxidation process, the oxygen flow rate of the diffusion process is lower than that of the oxidation process, and the nitrogen flow rate of the diffusion process is higher than that of the oxidation process. Since the diffusion process requires dopant ions within the doped source layer 130 to diffuse into the initial silicon layer 120, while the oxidation process only requires a portion of the second part II of the doped silicon layer 121 to be converted into an oxide layer 150, the diffusion process requires a higher temperature to propel the dopant ions inward compared to the oxidation process. Conversely, the oxidation process requires oxygen to diffuse into the second part II to react with it and form the oxide layer 150, requiring higher pressure and oxygen concentration than the diffusion process, allowing for a corresponding reduction in nitrogen concentration.

[0050] In some embodiments, during the oxidation process to transform a portion of the second portion II of a certain thickness into an oxide layer 150, the temperature of the oxidation process is gradually reduced. That is, after the diffusion process is completed, the oxidation process can be carried out directly without providing a heat source, thereby reducing the cost required to provide a heat source.

[0051] If the dopant ion is boron ion, the oxide layer 150 can be borosilicate glass; if the dopant ion is phosphorus ion, the oxide layer 150 can be phosphosilicate glass.

[0052] In some embodiments, the ratio of the thickness of the oxide layer 150 to the thickness of the doped silicon layer 121 in a direction perpendicular to the surface of the substrate 100 is 0.4 to 0.6, for example, 0.4, 0.45, 0.5, 0.55, or 0.6. It is understood that in the oxidation process, a portion of the second part II of the thickness of the doped silicon layer 121 is converted into the oxide layer 150, while the remaining second part II remains as the doped silicon layer 121. This second part II needs sufficient thickness to ensure adequate field passivation. Simultaneously, the remaining thickness of the second part II of the doped silicon layer 121 thins at the intersection with the first part I, reducing the absorption of incident light by the doped silicon layer 121, thereby improving the utilization rate of incident light by the solar cell and increasing the efficiency of the solar cell.

[0053] Understandably, the thickness of the mask layer 140 can affect the diffusion and masking processes. If the mask layer 140 is too thick, during the diffusion process, some dopant ions in the region of the doped source layer 130 directly opposite the mask layer 140 may not diffuse into the initial silicon layer 120. If the mask layer 140 is too thin, during the oxidation process, a portion of the first portion I may be oxidized, resulting in a reduction in the thickness of the first portion I along the direction perpendicular to the surface of the substrate 100. Therefore, the thickness of the mask layer 140 needs to be adjusted within an appropriate range. Specifically, along the direction perpendicular to the surface of the substrate 100, the thickness of the mask layer 140 can be 2nm to 8nm, for example, 2nm, 3nm, 4nm, 5nm, 6nm, 7nm, or 8nm.

[0054] refer to Figure 8 Remove oxide layer 150 and mask layer 140.

[0055] In some embodiments, the oxide layer 150 and the mask layer 140 can be removed simultaneously in the same process step. In some embodiments, the oxide layer 150 can be removed first, followed by the mask layer 140. In some embodiments, the mask layer 140 can be removed first, followed by the oxide layer 150. The order in which the oxide layer 150 and the mask layer 140 are removed is not limited.

[0056] In some embodiments, after the oxidation process and before removing the oxide layer 150 and the mask layer 140, a cleaning process may be included, in which the oxide layer 150 and the mask layer 140 can protect the remaining doped silicon layer 121 and prevent the doped silicon layer from being contaminated by the cleaning process.

[0057] In some embodiments, the cleaning solution used in the cleaning process can be SC-1 cleaning solution (composed of ammonium hydroxide, hydrogen peroxide and water), SC-2 cleaning solution (composed of hydrochloric acid, hydrogen peroxide and water), SPM cleaning solution (composed of sulfuric acid, hydrogen peroxide and water) or DHF (composed of hydrofluoric acid, hydrogen peroxide and water).

[0058] refer to Figure 9 A passivation layer 160 is formed on the surface of the doped silicon layer 121. The passivation layer 160 can prevent the surface of the solar cell from being oxidized or corroded, thus avoiding solar cell failure and improving the lifespan of the solar cell. In addition, the passivation layer 160 can also increase the refractive index of the solar cell surface, improve the light absorption capacity of the solar cell, and thereby improve the photoelectric conversion efficiency of the solar cell.

[0059] In some embodiments, the material of the passivation layer 160 may be silicon nitride, silicon oxynitride, or a composite material of silicon nitride and silicon oxynitride.

[0060] In some embodiments, the passivation layer 160 can be a single-layer structure or a multi-layer structure. For a multi-layer structure, the materials of different layers can be different from each other, or some layers can be made of the same material but different from the materials of other layers. For example, the passivation layer 160 can be a multi-layer structure composed of silicon nitride and aluminum oxide layers.

[0061] refer to Figure 10 A grid line 170 is formed on the surface of the passivation layer 160, directly opposite the first portion I, and the grid line 170 penetrates the passivation layer 160 along the thickness direction of the substrate 100 and makes electrical contact with the first portion I. The grid line 170 can be used to collect the electrical energy generated by the solar cell and transmit the electrical energy to the outside world.

[0062] In some embodiments, the material of the gate line 170 includes at least one of aluminum, nickel, silver, copper, gold, and graphite-based conductive materials.

[0063] The TOPCon cell formation method provided in this application embodiment can achieve a chemical passivation effect by forming a tunneling layer 110 on the surface of the substrate 100, thereby increasing the interface state density on the surface of the substrate 100, promoting the recombination of photogenerated carriers, increasing the fill factor, short-circuit current, and open-circuit voltage of the solar cell, and improving the photoelectric conversion efficiency of the solar cell. After forming the initial crystalline silicon layer 120, a doped source layer 130 with doped ions is first formed on the surface of the initial crystalline silicon layer 120, and then a mask layer 140 is formed on the surface of the doped source layer 130. Then, a diffusion process is performed. In the subsequent diffusion process, the doped ions in the doped source layer 130 will diffuse into the initial crystalline silicon layer 120, so that the initial crystalline silicon layer 120 is transformed into a doped crystalline silicon layer 121. The doped crystalline silicon layer 121 can have a field passivation effect. An electrostatic field can be formed in the direction from the doped crystalline silicon layer 121 to the substrate 100, causing minority carriers to escape, thereby reducing the concentration of minority carriers and reducing the carrier recombination rate at the interface of the substrate 100. The mask layer 140 includes multiple sub-mask layers 141, the positions of which correspond to the positions of the electrode regions 103 of the substrate 100. In the oxidation process, the first part I of the doped silicon layer 121 is covered by the sub-mask layer 141, and the second part II of the doped silicon layer 121 is exposed. Only a portion of the thickness of the second part II is oxidized into an oxide layer 150, while the first part I is protected by the mask layer 140. Thus, for the doped silicon layer 121, the thickness of the second part II is reduced in the direction perpendicular to the surface of the substrate 100, which can reduce the parasitic absorption effect of the doped silicon layer 121. The thickness of the first part I remains unchanged. When the passivation layer 160 and the gate line 170 are subsequently formed, the gate line 170 corresponding to the position of the first part I will not directly contact the tunneling layer 110 due to the excessive thinness of the first part I when it burns through the passivation layer 160 and makes electrical contact with the first part I, thereby improving the stability of the solar cell.

[0064] According to some embodiments of this application, another embodiment of this application provides a TOPCon battery, which can be fabricated using the TOPCon battery formation method provided in the above embodiments to improve the efficiency of solar cells. It should be noted that the parts that are the same as or corresponding to the above embodiments can be referred to the corresponding descriptions of the foregoing embodiments, and will not be described in detail below.

[0065] The TOPCon battery provided in this embodiment will be described in detail below with reference to the accompanying drawings.

[0066] refer to Figure 10A TOPCon cell includes: a substrate 100; a tunneling layer 110 located on the surface of the substrate 100; a doped silicon layer 121 located on the surface of the tunneling layer 110 away from the substrate 100, the doped silicon layer 121 including a first portion I and a second portion II, wherein the height of the first portion I relative to the surface of the substrate 100 is higher than the height of the second portion II relative to the surface of the substrate 100 in a direction perpendicular to the surface of the substrate 100; a passivation layer 160 located on the surface of the doped silicon layer 121 away from the tunneling layer 110; and a gate line 170 located on the surface of the passivation layer 160 away from the doped silicon layer 121, the gate line 170 being directly opposite the first portion I and penetrating the passivation layer 160 along the thickness direction of the substrate 100 to make electrical contact with the first portion I.

[0067] In some embodiments, the thickness ratio of the first portion I to the second portion II in the direction perpendicular to the surface of the substrate 100 is 4:1 to 5:1, for example, 4:1, 4.2:1, 4.5:1, 4.7:1, 4.9:1, or 5:1. In the direction perpendicular to the surface of the substrate 100, the thickness of the first portion I is greater than the thickness of the second portion II. For the second portion II, a thinner thickness can reduce the parasitic absorption effect of the doped silicon layer 121; for the first portion I, a thicker thickness can prevent the gate line 170 from penetrating the passivation layer 160 and the first portion I from directly contacting the tunneling layer 110, thus improving the stability of the solar cell. However, the thicknesses of the first portion I and the second portion II need to be within an appropriate range. The thickness of the first portion I cannot be too large to avoid increasing the parasitic absorption effect, and the thickness of the second portion II cannot be too small to avoid failing to achieve the field passivation effect.

[0068] In some embodiments, the thickness of the second portion II in the direction perpendicular to the surface of the substrate 100 is 15 nm to 25 nm, for example, 15 nm, 17.5 nm, 20 nm, 22.5 nm, or 25 nm. When the thickness of the second portion II is within an appropriate range, the second portion II can have a field passivation effect and also avoid the problem of parasitic absorption in the second portion II.

[0069] In some embodiments, the ratio of doped ion concentration in the first part I to that in the second part II is 0.9:1 to 1:1, for example, 0.9:1, 0.92:1, 0.94:1, 0.96:1, 0.98:1, or 1:1. It is understood that when a TOPCon cell is fabricated using the above-described method, the mask layer 140 is located on the surface of the first part I during the diffusion process, which may affect the diffusion process. This could result in the doped ion concentration in the first part I being lower than that in the second part II. However, by controlling the thickness of the mask layer 140, the ratio of doped ion concentration in the first part I to that in the second part II can be kept within an appropriate range to avoid affecting the performance of the doped silicon layer 121.

[0070] The TOPCon cell provided in this application embodiment has a tunneling layer 110 on the surface of the substrate 100. The tunneling layer 110 can perform chemical passivation, increasing the interface state density on the surface of the substrate 100, thereby promoting the recombination of photogenerated carriers, increasing the fill factor, short-circuit current, and open-circuit voltage of the solar cell, and thus improving the photoelectric conversion efficiency of the solar cell. In the direction perpendicular to the surface of the substrate 100, the thickness of the first part I is greater than the thickness of the second part II. For the second part II, the thinner thickness can reduce the parasitic absorption effect of the doped crystalline silicon layer 121; for the first part I, the thicker thickness can prevent the grid line 170 from penetrating the passivation layer 160 and the first part I from directly contacting the tunneling layer 110, thereby improving the stability of the solar cell.

[0071] Those skilled in the art will understand that the above embodiments are specific examples of implementing this application, and in practical applications, various changes can be made in form and detail without departing from the spirit and scope of this application.

Claims

1. A method for forming a TOPCon battery, characterized in that, include: Provide a base; A tunneling layer and an initial crystalline silicon layer are formed sequentially on the surface of the substrate; A doped source layer is formed on the surface of the initial crystalline silicon layer, and the doped source layer contains doped ions. A mask layer is formed on the surface of the doped source layer, the mask layer comprising multiple sub-mask layers; A diffusion process is used to diffuse the doped ions in the doped source layer into the initial silicon layer, so that the initial silicon layer is transformed into a doped silicon layer. The doped silicon layer includes a first part and a second part. The first part is directly opposite the sub-mask layer, and the second part is directly opposite the gap between adjacent sub-mask layers. An oxidation process is used to convert a portion of the second part of its thickness into an oxide layer; Remove the oxide layer and the mask layer; A passivation layer is formed on the surface of the doped silicon layer; A gate line is formed on the surface of the passivation layer, the gate line is directly opposite the first portion, and the gate line penetrates the passivation layer along the thickness direction of the substrate and makes electrical contact with the first portion.

2. The method for forming a TOPCon battery according to claim 1, characterized in that, The temperature of the diffusion process is higher than that of the oxidation process, the pressure of the diffusion process is lower than that of the oxidation process, the oxygen flow rate of the diffusion process is lower than that of the oxidation process, and the nitrogen flow rate of the diffusion process is higher than that of the oxidation process.

3. The method for forming a TOPCon battery according to claim 2, characterized in that, The diffusion process conditions include: a temperature of 880–950°C, a pressure of 50–250 mbar, an oxygen flow rate of 0–1000 sccm, and a nitrogen flow rate of 500–4000 sccm; the oxidation process conditions include: a process temperature of 50–800°C, a pressure of 250–900 mbar, an oxygen flow rate of 200–5000 sccm, and a nitrogen flow rate of 0–3000 sccm.

4. The method for forming a TOPCon battery according to claim 2, characterized in that, During the oxidation process, as the second portion of a certain thickness is converted into an oxide layer, the temperature of the oxidation process is gradually reduced.

5. The method for forming a TOPCon battery according to claim 1, characterized in that, The thickness of the mask layer is 2 nm to 8 nm in a direction perpendicular to the surface of the substrate.

6. The method for forming a TOPCon battery according to claim 1, characterized in that, In a direction perpendicular to the substrate surface, the ratio of the thickness of the oxide layer to the thickness of the doped silicon layer is 0.4 to 0.

6.

7. A TOPCon battery, prepared using the method for forming a TOPCon battery as described in any one of claims 1 to 6, characterized in that, include: Base; A tunneling layer located on the surface of the substrate; A doped silicon layer is located on the surface of the tunneling layer away from the substrate. The doped silicon layer includes a first portion and a second portion, wherein, in a direction perpendicular to the substrate surface, the height of the first portion relative to the substrate surface is greater than the height of the second portion relative to the substrate surface. A passivation layer is located on the surface of the doped silicon layer away from the tunneling layer; A gate line is located on the surface of the passivation layer away from the doped silicon layer. The gate line is directly opposite the first portion and penetrates the passivation layer along the thickness direction of the substrate, making electrical contact with the first portion.

8. The TOPCon battery according to claim 7, characterized in that, In the direction perpendicular to the surface of the substrate, the thickness ratio of the first portion to the second portion is 4:1 to 5:

1.

9. The TOPCon battery according to claim 8, characterized in that, The thickness of the second portion is 15 nm to 25 nm in a direction perpendicular to the surface of the substrate.

10. The TOPCon battery according to claim 7, characterized in that, The ratio of the doped ion concentration in the first part to the doped ion concentration in the second part is 0.9:1 to 1:1.

Citation Information

Patent Citations

  • Passivation contact structure, solar cell and preparation method

    CN115312608A

  • Topcon solar cell and preparation method thereof

    CN116130530A