A polypeptide linker for the complete conversion of PET plastic into TPA, its preparation method and application

By forming nanoparticles through the self-assembly of peptide linkers, and combining them with PET hydrolase and MHET hydrolase, the problems of complex enzyme modification and difficulty in utilizing intermediates in the biodegradation of PET plastics are solved, realizing the efficient and complete conversion of PET plastics into TPA, and improving degradation efficiency and enzyme stability.

CN117384300BActive Publication Date: 2026-11-17THE NAT CENT FOR NANOSCI & TECH NCNST OF CHINA
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202311317984.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-12
Publication Date
2026-11-17
Estimated Expiration
2043-10-12

AI Technical Summary

Technical Problem

Existing technologies for the biodegradation of PET plastics involve complex and costly enzyme modifications, and the intermediate oligomers generated during enzyme degradation are difficult to utilize directly, making it impossible to achieve efficient closed-loop recycling of PET plastics.

Method used

Nanoparticles are formed by the self-assembly of peptide linkers and combined with PET hydrolase and MHET hydrolase to form a multi-enzyme complex. Through hydrogen bonding interactions, 100% of PET plastic is converted into monomer TPA.

Benefits of technology

It improved the degradation efficiency of PET plastic by 23 times, realizing the complete conversion of PET plastic into the directly usable monomer TPA. No intermediates were generated during the degradation process, and the degradation rate and enzyme stability were significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117384300B_ABST
    Figure CN117384300B_ABST
Patent Text Reader

Abstract

This invention provides a polypeptide linker for the complete conversion of PET plastic to TPA, its preparation method, and its application. The polypeptide linker comprises a polypeptide M targeting MHET hydrolase, a linker peptide, and a polypeptide P targeting PET hydrolase, sequentially linked together, with polypeptide M located at the N-terminus and polypeptide P at the C-terminus. The sequence of polypeptide M targeting MHET hydrolase includes any of the sequences shown in SEQ ID No. 1 to 3, the sequence of polypeptide P targeting PET hydrolase includes any of the sequences shown in SEQ ID No. 4 to 7, and the linker peptide includes any one of the polypeptides shown in SEQ ID No. 8 to 17, polytyrosine, or polyproline. Compared to physically blended PET hydrolase and MHET hydrolase, the multi-enzyme complex provided by this invention improves degradation efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of biodegradable plastics, and relates to a polypeptide linker for the complete conversion of PET plastic into TPA, its preparation method, and its application. Background Technology

[0002] Plastics are widely used due to their low cost, especially polyesters such as PET. However, the recycling and reuse of PET is far below the production level. Currently, approximately 80% of waste plastics worldwide are disposed of in landfills or left to decay naturally in the environment each year. Components of waste plastics can infiltrate crops, animals, and even marine life, ultimately entering the human body through the food chain, posing a serious threat to the natural environment and human health. Currently, plastic degradation is mainly achieved through mechanical or chemical degradation pathways. Mechanical degradation involves pre-treating plastics into small microplastics and then melting and reshaping them; however, mechanical degradation has drawbacks such as reduced product properties and uncleanliness. Chemical degradation mainly includes solution-based methods such as hydrolysis, alcoholysis, ammonolysis, and saccharification. Current hydrolysis methods are simple, but they also suffer from energy consumption and significant environmental pollution. Hydrolysis is generally carried out in the presence of acids or alkalis through heating or microwave radiation, requiring high temperatures (200–250°C) and certain pressures (1.4–2 MPa), necessitating a long reaction time to ensure complete degradation, and only 4% of PET is successfully recycled. In the recycling and processing of polyester waste plastics, how to economically, environmentally, and efficiently degrade PET into small molecules such as terephthalic acid is an urgent problem to be solved.

[0003] Biodegradation is a promising, efficient, and environmentally friendly method for degrading PET. Several microorganisms and keratinases have already been developed for PET degradation. A. Marty's group obtained highly catalytically active and thermally stable ICCG through site-directed mutagenesis of LCC keratinase, which can degrade 90% of PET powder within 10 hours. However, this high degradation efficiency requires high degradation temperatures, resulting in high energy consumption. Therefore, scientists are dedicated to finding enzymes with high degradation efficiency at room temperature for PET degradation. In 2016, Yoshida discovered *Ideonella sakaiensis*, the only bacterium to date capable of degrading PET with high enzyme activity. Further research revealed that the main active components in *Ideonella sakaiensis* responsible for degradation are the secreted enzyme PETase and the membrane protease MHETase. This bacterium adheres to PET plastic via the secreted PETase, degrading PET into the intermediate terephthalic acid monohydroxyethyl ester (MHET). MHET is then degraded by MHETase on the outer surface of the bacterial membrane into monomeric small molecules of terephthalic acid (TPA) and ethylene glycol (EG). Since the wild-type enzymes IsPETase and IsMHETase have low catalytic efficiency for PET, some studies have been conducted to engineer these wild-type enzymes to improve their degradation activity.

[0004] CN202210400007.7 discloses an engineered enzyme complex for efficiently degrading PET plastic, its preparation method, and its applications, belonging to the field of biotechnology. The engineered enzyme complex consists of RIAD and RIDD, IsPETase, MHETase, and hydrophobin4. Through the specific and strong in vitro binding of RIAD and RIDD, IsPETase, MHETase, and hydrophobin4 are brought closer together spatially. MHETase can degrade MHET, which causes substrate inhibition of IsPETase, while hydrophobin4 pulls the complex towards the PET plastic surface, thereby significantly improving the degradation environment of IsPETase. The engineered enzyme complex provided by this invention can efficiently degrade PET plastic at room temperature, with a degradation efficiency approximately 5 times higher than that of IsPETase, which currently has the highest degradation rate through directed evolution.

[0005] CN202110803574.2 discloses a method for degrading PET plastic using the synergistic effect of two enzymes. The method involves placing PET plastic in a mixed enzyme solution of PETase and MHETase, and reacting the enzymes at 30°C for 48 hours. The enzyme activity ratio of PETase to MHETase is 3:1. This method can rapidly degrade PET plastic into terephthalic acid and ethylene glycol monomers. Compared with the bacterial strain *Ideonella sakaiensis* and the use of the degrading enzymes alone, the degradation rate is significantly improved. The reaction conditions are mild, the process is safe, and there is no secondary pollution. In particular, by constructing a recombinant *E. coli* strain expressing both MHETase and PETase enzymes after codon optimization of the PETase and MHETase genes, and expressing them under optimized conditions, the degradation rate of PET can be further improved.

[0006] CN201710963873.6, belonging to the field of microbial genetic engineering technology, addresses the challenge of degrading PET plastic by providing a PET hydrolase expression unit, a recombinant DNA vector for *E. coli* based on this unit capable of effectively secreting and expressing PET hydrolase, and its applications. The recombinant DNA vector provided by this invention can effectively achieve secretory expression of PET hydrolase in *E. coli* host bacteria. Its culture medium exhibits significant lipase bioactivity, enabling the degradation of PET plastic films during continuous culture. This provides a promising genetic engineering approach for the biodegradation of PET plastic.

[0007] However, the engineered enzymes or microorganisms constructed through genetic engineering or protein engineering in the three published patents mentioned above are technically complex and costly to operate, and existing bioengineering technologies still cannot avoid protein misfolding and disordered spatial structures. More importantly, the process of enzymes degrading PET plastic into monomers inevitably generates a large number of intermediate oligomers, which cannot be directly reused to manufacture virgin plastics or upgraded to create higher-value products.

[0008] Therefore, developing an enzyme that can efficiently degrade PET plastic in situ and convert it into a single product that can be directly utilized is crucial for the closed-loop recycling of PET plastic. Summary of the Invention

[0009] To address the shortcomings of existing technologies, the present invention aims to provide a polypeptide linker for the complete conversion of PET plastic into TPA, its preparation method, and its application.

[0010] To achieve this objective, the present invention adopts the following technical solution:

[0011] In a first aspect, the present invention provides a polypeptide linker for achieving complete conversion of PET plastic into TPA. The polypeptide linker comprises a polypeptide M targeting MHET hydrolase, a linker peptide, and a polypeptide P targeting PET hydrolase, which are sequentially linked, wherein polypeptide M is located at the N-terminus and polypeptide P is located at the C-terminus. The sequence of the polypeptide M targeting MHET hydrolase includes any of the sequences shown in SEQ ID No. 1 to 3, the sequence of the polypeptide P targeting PET hydrolase includes any of the sequences shown in SEQ ID No. 4 to 7, and the linker peptide includes any one of the polypeptides shown in any of the sequences shown in SEQ ID No. 8 to 17, polytyrosine, or polyproline.

[0012] The PET is polyethylene terephthalate, and the TPA is terephthalic acid. In neutral aqueous solution, the peptide linkers can self-assemble into β-sheet nanoparticles through hydrogen bonding interactions between different peptide targeting sequences M and P. When the nanoparticles are mixed with PET hydrolase and MHET hydrolase, the nanoparticles can specifically bind to PET hydrolase and MHET hydrolase and undergo β-sheet-mediated co-assembly, forming a multi-enzyme complex, due to the self-recognition between identical peptide sequences from the protein and the nanoparticles.

[0013] During the degradation of PET plastic, the multi-enzyme complex formed by the polypeptide linker, PET hydrolase, and MHET hydrolase can shorten the distance between PET hydrolase and MHET hydrolase, and rapidly degrade the product MHET produced by PET hydrolase into monomer TPA by MHET hydrolase, achieving 100% conversion of PET plastic into monomer TPA; moreover, compared with the blended PET hydrolase and MHET hydrolase, the multi-enzyme complex increases the PET degradation efficiency by 23 times.

[0014] SEQ ID No. 1:TTVTTMLLASVALAAC.

[0015] SEQ ID No.2: FATIAT.

[0016] SEQ ID No. 3: PLVAWV.

[0017] SEQ ID No. 4: AVLGGLMAV.

[0018] SEQ ID No. 5: TVGAIAI.

[0019] SEQ ID No. 6: GFVVITI.

[0020] SEQ ID No.7: TLIFAC.

[0021] SEQ ID No. 8: PGP.

[0022] SEQ ID No. 9: GPG.

[0023] SEQ ID No. 10: PPP.

[0024] SEQ ID No. 11: GGG.

[0025] SEQ ID No. 12: (PGP)n.

[0026] SEQ ID No. 13: (GPG)n.

[0027] SEQ ID No. 14: (PPP)n.

[0028] SEQ ID No. 15: (GGG)n.

[0029] SEQ ID No. 16: (GSGSGS)n.

[0030] SEQ ID No. 17: P(G)nP.

[0031] Preferably, n is 2-5, for example 2, 3, 4, 5.

[0032] Preferably, the polytyrosine contains 5 to 12 tyrosine residues, for example, 5, 6, 7, 8, 9, 10, 11 or 12.

[0033] Preferably, the polyproline contains 5 to 12 proline residues, for example, 5, 6, 7, 8, 9, 10, 11 or 12.

[0034] Preferably, the sequence of the polypeptide M that targets and recognizes MHET hydrolase is the sequence shown in SEQ ID No. 3.

[0035] Preferably, the sequence of the polypeptide P that targets and recognizes PET hydrolase is the sequence shown in SEQ ID No. 6.

[0036] Preferably, the sequence of the linker peptide is the sequence shown in SEQ ID No. 8.

[0037] Preferably, the PET hydrolase includes any one of IsPETase, DuraPETase, ThermoPETase, FAST-PETase, PETase-EK30, or HotPETase, and is more preferably IsPETase.

[0038] Preferably, the MHET hydrolase includes IsMHETase, Exo-MHETase, and MHETase. R411K / S416A / F424I MHETase S416A / R411Q / F424N IsMHETase is further preferred.

[0039] Preferably, the target recognition sequence M, the linker peptide, and the target recognition sequence P are covalently coupled via amide condensation.

[0040] Preferably, the polypeptide linker comprises a compound represented by Formula I.

[0041]

[0042] Secondly, the present invention provides a nanoparticle prepared by the following method: synthesizing a polypeptide linker by chemical synthesis, and then performing self-assembly in a self-assembly buffer to form a nanoparticle.

[0043] The preparation method described in this invention is technically mature, has a high success rate, and is easily mastered by those skilled in the art. It promotes the production and use of related products and creates conditions for the mass production of products and their application in actual clinical medicine.

[0044] Preferably, the chemical synthesis method includes solid-phase synthesis.

[0045] Preferably, the self-assembly buffer comprises any one of water, phosphate buffer, Tris-HCl buffer, or HEPES buffer, and more preferably phosphate buffer.

[0046] Preferably, the pH of the self-assembly buffer solution is 7.0 to 8.0, such as 7.0, 7.1, 7.2, 7.3, 7.4, 7.5, 7.6, 7.7, 7.8, 7.9, 8.0, etc. Other specific values ​​within the above range can be selected, and will not be elaborated here.

[0047] Preferably, the spatial structure of the nanoparticles includes any one or a combination of at least two of α-helices, β-sheets, or β-hairpins, and more preferably β-sheets.

[0048] Preferably, the diameter of the nanoparticles is 10-30 nm, such as 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, 18 nm, 19 nm, 20 nm, 21 nm, 22 nm, 23 nm, 24 nm, 25 nm, 26 nm, 27 nm, 28 nm, 29 nm, 30 nm, etc. Other specific values ​​within the above range can be selected, and will not be elaborated here.

[0049] Preferably, the driving force of the assembly includes any one or a combination of at least two of hydrogen bonds, van der Waals forces, or π-π interactions, for example, it can be hydrogen bonds, van der Waals forces, π-π interactions, or a combination of van der Waals forces and π-π interactions.

[0050] Thirdly, the present invention provides a multi-enzyme complex for the complete conversion of PET plastic into TPA, characterized in that the multi-enzyme complex comprises PET hydrolase, MHET hydrolase and nanoparticles; the three components in the multi-enzyme complex are arranged in a sandwich configuration and / or an encapsulation configuration, wherein the sandwich configuration is in which the nanoparticles are located between the PET hydrolase and the MHET hydrolase, and the encapsulation configuration is in which the nanoparticles encapsulate the PET hydrolase and the MHET hydrolase in one space.

[0051] In this invention, the polypeptide linker for achieving 100% conversion of PET plastic to TPA is obtained by linking two sequences, targeted assembly peptide P and targeted assembly peptide M, together with a linker peptide. Targeted assembly peptide M is located at the N-terminus, and targeted assembly peptide P at the C-terminus. The mass spectrometry characterization of the polypeptide linker is as follows: Figure 1 As shown, this polypeptide linker can self-assemble into nanoparticles with a β-sheet structure. These nanoparticles can specifically recognize and bind to two enzymes, IsPETase and IsMHETase, to form self-assembly-mediated protein-peptide aggregates. From a catalytic perspective, these protein-peptide aggregates can achieve a one-step conversion of PET into the monomer TPA.

[0052] Preferably, the diameter of the multi-enzyme complex is 29-49 nm, such as 29 nm, 30 nm, 31 nm, 32 nm, 33 nm, 34 nm, 35 nm, 36 nm, 37 nm, 38 nm, 39 nm, 40 nm, 41 nm, 42 nm, 43 nm, 44 nm, 45 nm, 46 nm, 47 nm, 48 nm, 49 nm, etc. Other specific values ​​within the above range can be selected, and will not be elaborated here.

[0053] Preferably, the binding affinity between the nanoparticles and PET hydrolase is 0.07 μM to 4.35 μM, such as 0.07 μM, 0.1 μM, 0.5 μM, 1 μM, 1.5 μM, 2 μM, 2.5 μM, 3 μM, 3.5 μM, 4 μM, 4.35 μM, etc. Other specific values ​​within the above range can be selected, and will not be elaborated here.

[0054] Preferably, the binding affinity of the nanoparticles to MHET hydrolase is 0.1 μM to 20.6 μM, for example, 0.1 μM, 1 μM, 2 μM, 3 μM, 4 μM, 5 μM, 6 μM, 7 μM, 8 μM, 9 μM, 10 μM, 11 μM, 12 μM, 13 μM, 14 μM, 15 μM, 16 μM, 17 μM, 18 μM, 19 μM, 20 μM, 20.6 μM, etc. Other specific values ​​within the above range can be selected, and will not be elaborated here.

[0055] Preferably, the molar ratio of the polypeptide linker, PET hydrolase, and MHET hydrolase is (75-200):1:1, wherein the specific point values ​​in (75-200) can be selected from 75, 85, 95, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, etc. Other specific point values ​​within the above range can be selected, and will not be elaborated here.

[0056] Preferably, the concentration of the polypeptide linker is no greater than 500 μM, such as 100 μM, 150 μM, 200 μM, 250 μM, 300 μM, 350 μM, 400 μM, 450 μM, 500 μM, etc. Other specific values ​​within the above range can be selected, and will not be elaborated here.

[0057] Preferably, the PET hydrolase includes any one of IsPETase, DuraPETase, ThermoPETase, FAST-PETase, PETase-EK30, or HotPETase, and is more preferably IsPETase.

[0058] Preferably, the MHET hydrolase includes IsMHETase, Exo-MHETase, and MHETase. R411K / S416A / F424I or MHETase S416A / R411Q / F424N Any one of them, more preferably IsMHETase.

[0059] Fourthly, the present invention provides the application of the polypeptide linker described in the first aspect, the nanoparticles described in the second aspect, or the multi-enzyme complex described in the third aspect in the degradation of PET plastics.

[0060] In this invention, the polypeptide linker that enables 100% conversion of PET plastic to TPA, after forming nanoparticles, can specifically recognize and bind to two enzymes, IsPETase and IsMHETase, forming self-assembly-mediated protein-peptide aggregates through hydrogen bonding interactions. From a catalytic perspective, the presence of the polypeptide linker enabling 100% conversion of PET plastic to TPA results in the formation of protein-peptide aggregates, allowing for the one-step conversion of PET to TPA.

[0061] The polypeptide linker that enables 100% conversion of PET plastic into TPA can achieve complete degradation of PET plastic; the preparation method is mature, can be mass-produced, and has extremely high application value.

[0062] In this invention, the PET plastic includes amorphous PET plastic powder, amorphous PET plastic film, and highly crystalline PET plastic sheet.

[0063] Compared with the prior art, the present invention has the following beneficial effects:

[0064] (1) The polypeptide linker that enables 100% conversion of PET plastic to TPA according to the present invention remains in a particulate state in a neutral solution. When IsPETase and IsMHETase enzymes are present, the polypeptide nanoparticles that enable 100% conversion of PET plastic to TPA specifically recognize and bind to the two enzymes IsPETase and IsMHETase, and form a self-assembled protein polypeptide aggregate by means of hydrogen bond interaction.

[0065] (2) The polypeptide protein aggregate that enables 100% conversion of PET plastic to TPA not only shortens the spatial distance between IsPETase and IsMHETase but also increases the contact between IsPETase and the substrate, allowing IsMHETase to rapidly degrade MHET produced by IsPETase, thereby completely degrading PET plastic into monomeric TPA in one step. Compared to physically blended IsPETase and IsMHETase, the polypeptide linker that enables 100% conversion of PET plastic to TPA can increase the degradation rate by approximately 23 times. The polypeptide linker that enables 100% conversion of PET plastic to TPA can also improve enzyme stability by 10 days.

[0066] (3) The preparation method of the polypeptide that achieves 100% conversion of PET plastic into TPA is mature, can be mass-produced, promotes the promotion and use of the product, and has broad application prospects. Attached Figure Description

[0067] Figure 1This is an ESI-MS characterization image of the polypeptide linker prepared in Example 1 of the present invention, which achieves 100% conversion of PET plastic into TPA.

[0068] Figure 2 The image shows the Fourier transform infrared (FTIR) spectrum of the polypeptide linker used in Example 1 of this invention to achieve 100% conversion of PET plastic into TPA.

[0069] Figure 3 These are transmission electron microscope (TEM) images (scale bar = 100 nm) of the polypeptide linker that achieves 100% conversion of PET plastic to TPA as described in Embodiment 1 of the present invention. Image a is a TEM image of the nanoparticle structure of the polypeptide linker, and image b is a magnified view of the TEM image of the nanoparticle structure of the polypeptide linker in image a.

[0070] Figure 4 The results are obtained by dynamic light scattering instrumentation of the polypeptide linker that achieves 100% conversion of PET plastic to TPA as described in Example 1 of this invention, in phosphate buffer at pH 7.5 for 0 h to 4 h.

[0071] Figure 5 The results are experimental results of the binding force between the polypeptide linker that achieves 100% conversion of PET plastic to TPA as described in Example 1 of this invention and the enzymes IsPETase and IsMHETase.

[0072] Figure 6 This is a transmission electron microscope image (scale bar = 100 nm) of the polypeptide linker that enables 100% conversion of PET plastic to TPA as described in Example 1 of this invention, co-assembled with enzymes IsPETase and IsMHETase.

[0073] Figure 7 The results are obtained by dynamic light scattering instrumentation after the polypeptide linker that achieves 100% conversion of PET plastic to TPA as described in Example 1 of this invention is co-assembled with enzymes IsPETase and IsMHETase and then placed in phosphate buffer at pH 7.5 for 0 to 4 hours.

[0074] Figure 8 This is the result of the polypeptide linker, which achieves 100% conversion of PET plastic into TPA as described in Example 1 of the present invention, completely converting PET plastic into TPA monomer.

[0075] Figure 9 This is the result of the polypeptide linker enhancing enzyme stability described in Example 1 of the present invention, which achieves 100% conversion of PET plastic into TPA.

[0076] Figure 10AThis is an image (scale bar = 5 μm) showing the degradation effect of enzyme on PET film when the polypeptide linker that enables 100% conversion of PET plastic to TPA as described in Example 1 of this invention is absent.

[0077] Figure 10B This is an image (scale bar = 5 μm) showing the degradation effect of enzyme on PET film in the presence of the polypeptide linker that enables 100% conversion of PET plastic to TPA as described in Example 1 of this invention.

[0078] Figure 11 This is the result of the macroscopic effect of enzyme degradation on PET film in the presence of the polypeptide linker that enables 100% conversion of PET plastic to TPA as described in Example 1 of the present invention. Detailed Implementation

[0079] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.

[0080] Where specific techniques or conditions are not specified in the examples, they shall be performed in accordance with the techniques or conditions described in the literature in this field, or in accordance with the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased through legitimate channels.

[0081] Wang resin and amino acids were purchased from Jier Biochemical (Shanghai) Co., Ltd.

[0082] Hexahydropyridine, N,N-dimethylformamide, N-methylmorpholine, hydrazine hydrate, triisopropylsilane and trifluoroacetic acid were purchased from Sinopharm Chemical Reagent Beijing Co., Ltd.

[0083] Fluorescein isothiocyanate (FITC) was purchased from Chuangrong Technology (Guangzhou) Co., Ltd.

[0084] The IsPETase plasmid was derived from Addgene.

[0085] IsMHETase plasmid was purchased from Jiman Company;

[0086] DH5α competent cells were purchased from Beijing Tuoying Times Technology Co., Ltd.

[0087] BL21(DE3) competent cells were purchased from Beijing TransGen Biotech Co., Ltd.

[0088] Tryptone and yeast powder were purchased from Beijing Coolplay Technology Co., Ltd.

[0089] The nickel column packing for His labels was purchased from Beijing Coollab Technology Co., Ltd.

[0090] The protease inhibitor was purchased from Solarbio.

[0091] The gravity-type protein purification empty column was purchased from Sangon Biotech (Shanghai) Co., Ltd.

[0092] Amorphous PET powder was purchased from Sigama-Aldrich;

[0093] The amorphous PET film was purchased from Goodfellow, UK.

[0094] The highly crystalline PET sheets are from Wahaha bottled water packaging bottles.

[0095] Example 1

[0096] This embodiment synthesizes a polypeptide linker that enables 100% conversion of PET plastic into TPA. The polypeptide linker that enables 100% conversion of PET plastic into TPA includes a targeting assembly peptide M, a linking peptide, and a targeting assembly peptide P connected in sequence.

[0097] The amino acid sequence of the targeted assembly peptide M is shown in SEQ ID No. 3, the amino acid sequence of the linking peptide is shown in SEQ ID No. 8, and the amino acid sequence of the targeted assembly peptide P is shown in SEQ ID No. 6.

[0098] SEQ ID No. 3: PLVAWV;

[0099] SEQ ID No. 6: GFVVITI;

[0100] SEQ ID No. 8: PGP.

[0101] The molecular structure of the polypeptide linker that enables 100% conversion of PET plastic into TPA is shown in Formula I:

[0102]

[0103] The method for preparing polypeptide linkers that enable 100% conversion of PET plastic into TPA includes the following steps:

[0104] (1) Design targeted assembly peptide P and targeted assembly peptide M;

[0105] (2) Connect the two sequences of the target assembly peptide P and the target assembly peptide M together with a linker peptide, with the target assembly peptide M at the N-terminus and the target assembly peptide P at the C-terminus.

[0106] (3) Synthesize polypeptide linkers that enable 100% conversion of PET plastic into TPA by solid-phase synthesis.

[0107] A polypeptide linker was synthesized to achieve 100% conversion of PET plastic into TPA using a solid-phase synthesis method.

[0108] Wang resin with a modification density of 0.35 mM (isoleucine I-terminus immobilized on the resin, N-terminus protected by Fmoc) was used. The N-terminal Fmoc protection was removed using a 1:4 volume ratio of hexahydropyridine and N,N-dimethylformamide, and the success of deprotection was verified using the ninhydrin test. The amino acid and benzotriazole-N,N,N',N'-tetramethylurea hexafluorophosphate were weighed at 10 times the molar mass of the first amino acid. Then, a coupling agent (a 5:95 volume ratio of N-methylmorpholine and N,N-dimethylformamide) was added and stirred until dissolved. The solution was transferred to a peptide synthesis tube and reacted for 45 min. The above steps were repeated to link all remaining amino acids via condensation reactions.

[0109] The peptide resin was washed into the peptide synthesis tube using N,N-dimethylformamide. The synthesized peptide was then removed from the resin using a trifluoroacetic acid solution containing 2.5% water and 2.5% triisopropylsilane, simultaneously removing the side chain protection of the amino acids. The trifluoroacetic acid was removed by rotary evaporation. The crude peptide product was precipitated with anhydrous diethyl ether, washed, and dried to obtain a cationic therapeutic peptide, an assembled peptide, and a β-D-glucopyranose conjugate.

[0110] The obtained polypeptide conjugates were characterized by ESI-MS, and the results are as follows: Figure 1 As shown.

[0111] As shown in the figure, the mass spectrum of the obtained product is as follows:

[0112] C 78 H 122 N 16 O 20 [M+2H] 2+ 833.0, [M+H] + :1664.95.Found ESI-MS:m / z 833.4,1665.0.

[0113] The above results indicate that the polypeptide linker for achieving 100% conversion of PET plastic to TPA was successfully prepared.

[0114] Example 2

[0115] This embodiment verifies the assembly structure and morphology of the polypeptide linker prepared in Example 1, which enables 100% conversion of PET plastic into TPA, under neutral conditions.

[0116] The polypeptide linker that achieves 100% conversion of PET plastic to TPA was dissolved in phosphate buffer at pH 7.5 and characterized using Fourier transform infrared spectroscopy. The results are as follows: Figure 2 As shown.

[0117] Depend on Figure 2 It can be seen that in the Fourier transform infrared spectrum at 1627 cm⁻¹ -1 The characteristic peak of the β-sheet assembly structure was observed at 1534 cm⁻¹. -1 The peak at 1693 cm⁻¹ is a characteristic peak of the amide second band of the β-sheet. -1 The peak at this point is a characteristic peak of the antiparallel β-sheet, indicating that in a slightly acidic buffer system with a pH of 7.5, the polypeptide linker that enables 100% conversion of PET plastic to TPA can form a β-sheet structure.

[0118] Furthermore, the morphology of the peptide linker that achieves 100% conversion of PET plastic to TPA was observed in phosphate buffer at pH 7.5 using transmission electron microscopy (lanthanum hexaboride transmission electron microscope, Tecnai G2 20S-TWIN(T-20), FEI Corporation, USA). The resulting morphology image of the peptide linker nanoparticles that achieve 100% conversion of PET plastic to TPA is shown in the figure below. Figure 3 As shown in Figures a and b.

[0119] Depend on Figure 3 It can be seen that in a neutral buffer system, the polypeptide linkers that achieve 100% conversion of PET plastic into TPA aggregate to form nanoparticles of about 11 nm, demonstrating that the β-sheet structure in different neutral environments exhibits hydrogen bond-assisted self-assembly properties.

[0120] In addition, the particle size distribution of the polypeptide linker nanoparticles that achieve 100% conversion of PET plastic to TPA was monitored over time in a neutral buffer system at pH 7.5 using dynamic light scattering. The results are as follows: Figure 4 As shown.

[0121] Depend on Figure 4 It can be seen that, with the extension of time, after 4 hours in the neutral buffer system, the size of the peptide linker nanoparticles that achieve 100% conversion of PET plastic to TPA is stably distributed at around 20 nm. This proves that in the neutral buffer system, the peptide linkers that achieve 100% conversion of PET plastic to TPA are assembled into uniform and stable nanoparticles.

[0122] Example 3

[0123] This embodiment verifies that the polypeptide linker prepared in Example 1, which enables 100% conversion of PET plastic to TPA, undergoes co-assembly in the presence of both IsMHETase and IsPETase enzymes.

[0124] The peptide linker that enables 100% conversion of PET plastic into TPA first self-assembles into bispecific nanoparticles in a neutral solution. Then, the nanoparticles specifically bind to IsMHETase and IsPETase, and the three together assemble into protein-peptide aggregates.

[0125] To demonstrate that the peptide can bind to both IsMHETase and IsPETase, the binding affinity of the peptide linker that enables 100% conversion of PET plastic to TPA with the two enzymes IsPETase and IsMHETase was measured using a micro-thermal surge experiment. A 2 mM stock solution of the peptide linker that enables 100% conversion of PET plastic to TPA was prepared and serially diluted to 16 concentration gradients: 1 mM, 0.5 mM, 0.25 mM, 0.125 mM, 0.0625 mM, 0.3125 mM, 0.015625 mM, 0.0078125 mM, 0.00390625 mM, 0. Sixteen concentrations of peptide solutions with enzymatic degradation activity against PET plastic were incubated with 400 nM of Cy5-labeled IsPETase or IsMHETase. The mixed samples were aspirated using a capillary tube, and the affinity was tested using a micro-thermal surge experiment (Monolith NT.115 instrument, Nano Tmeper, Germany). The results are as follows: Figure 5 As shown.

[0126] Depend on Figure 5 It was found that the polypeptide linker achieving 100% conversion of PET plastic to TPA interacts with both enzymes, IsPETase and IsMHETase, with dissociation constants (Kd) in the low micromolar or even nanomolar range. In contrast, the polypeptide linker achieving 100% conversion of PET plastic to TPA rarely binds to the control protein bovine serum albumin, indicating that the polypeptide linker selectively binds to both enzymes, IsPETase and IsMHETase.

[0127] To demonstrate that the polypeptide linker achieving 100% conversion of PET plastic to TPA is a protein-peptide aggregate assembled with two enzymes, IsPETase and IsMHETase, the morphology of the polypeptide linker achieving 100% conversion of PET plastic to TPA was observed in phosphate buffer at pH 7.5 using transmission electron microscopy (Lanium hexaboride transmission electron microscope, Tecnai G2 20S-TWIN(T-20), FEI Corporation, USA). The morphology of the polypeptide linker nanoparticles achieving 100% conversion of PET plastic to TPA is shown in the image below. Figure 6 As shown.

[0128] Depend on Figure 6 It can be seen that in a neutral buffer system, the polypeptide linkers that achieve 100% conversion of PET plastic to TPA aggregate to form nanoparticles of about 29 nm, proving that the polypeptide linkers that achieve 100% conversion of PET plastic to TPA are protein polypeptide aggregates assembled together with two enzymes, IsPETase and IsMHETase.

[0129] In addition, the particle size distribution of the polypeptide linker nanoparticles that achieve 100% conversion of PET plastic to TPA was monitored over time in a neutral buffer system at pH 7.5 using dynamic light scattering. The results are as follows: Figure 7 As shown.

[0130] Depend on Figure 7 It can be seen that, with the extension of time, after 4 hours in the neutral buffer system, the size of the peptide linker nanoparticles that achieve 100% conversion of PET plastic to TPA is stably distributed at around 40 nm. This proves that in the neutral buffer system, the peptide linkers that achieve 100% conversion of PET plastic to TPA are assembled into uniform and stable nanoparticles.

[0131] Example 4

[0132] This embodiment verifies that the polypeptide linker prepared in Example 1 is completely degraded into monomer TPA in one step.

[0133] The application of the peptide linker in converting 100% of PET plastic to TPA was verified using amorphous PET powder and amorphous PET membrane. A 200 μM solution of the peptide linker was prepared and added to enzymes IsPETase and IsMHETase, then incubated with amorphous PET powder for 24 hours. The supernatant was collected, and the composition and content of degradation products (including BHET, MHET, and TPA) in the supernatant were detected by high-performance liquid chromatography (Shimadzu, Japan). The results are as follows: Figure 8 As shown.

[0134] Depend on Figure 8It is evident that adding the polypeptide linker that enables 100% conversion of PET plastic to TPA to the enzyme for PET plastic degradation results in a degradation efficiency 20 times higher than that of the enzyme alone, and the synergistic coefficient also increases from 4.5 to 84. Compared to the degradation products of the enzyme alone, which consist of the intermediate product MHET and monomeric TPA, the presence of the polypeptide linker ensures that the degradation products only contain monomeric TPA, without the intermediate product MHET. This indicates that the addition of the polypeptide linker significantly enhances the enzyme's activity in degrading PET, and can completely degrade PET plastic to monomeric TPA in one step. For IsPETase enzyme alone, the addition of the polypeptide linker also significantly improves the degradation efficiency of IsPETase enzyme.

[0135] To further verify the enhanced enzyme stability of the polypeptide linker for achieving 100% conversion of PET plastic to TPA, a 200 μM solution of the polypeptide linker was prepared and added to the enzymes IsPETase and IsMHETase. The solution was then incubated with amorphous PET powder for 10 days. Supernatants were collected at 12 hours, 1 day, 2 days, 3 days, 4 days, 5 days, 6 days, 7 days, 8 days, 9 days, and 10 days. The composition and content of degradation products (including BHET, MHET, and TPA) in the supernatant were detected using high-performance liquid chromatography (Shimadzu, Japan). The results are as follows: Figure 9 As shown.

[0136] Depend on Figure 9 It is known that when the polypeptide linker that enables 100% conversion of PET plastic to TPA is added to the enzyme to degrade PET plastic, the degradation activity lasts for 10 days, and the degradation effect is 23 times higher than that of the enzyme alone. The enzyme alone loses its activity on the first day. The degradation rate per unit time also proves that the addition of the polypeptide linker that enables 100% conversion of PET plastic to TPA makes the degradation efficiency much higher than that of the enzyme alone, and there is only a slight decrease within 10 days. This indicates that the addition of the polypeptide linker that enables 100% conversion of PET plastic to TPA significantly enhances the long-term stability of the enzyme that degrades PET.

[0137] In addition, the effect of the polypeptide linker in converting 100% of PET plastic into TPA was observed using an amorphous PET membrane, and the results are shown in Figures 10 and 11.

[0138] Depend on Figure 10A It is evident that, compared to the slight irregular grooves on the surface of PET film caused by enzyme degradation alone, the addition of peptide linkers, which enables 100% conversion of PET plastic into TPA, results in significant erosion and porosity on the PET film surface. Figure 10B As shown. The top right corner shows the smooth surface of the untreated PET film. Furthermore, by... Figure 11 It is known that by increasing the concentration of the polypeptide linkers and enzymes that enable 100% conversion of PET plastic into TPA, the amorphous PET film is completely degraded after 7 days of degradation.

[0139] In summary, this invention provides a polypeptide linker for achieving 100% conversion of PET plastic to TPA, which can self-assemble into nanoparticles in a neutral solution. These nanoparticles can specifically target the enzymes IsMHETase and IsPETase, co-assembling with both enzymes. The nanoparticles not only shorten the spatial distance between IsPETase and IsMHETase but also increase the contact between IsPETase and the substrate, enabling IsMHETase to rapidly degrade MHET produced by IsPETase, thereby completely degrading PET plastic into monomeric TPA in one step. Compared to physically blended IsPETase and IsMHETase, the polypeptide linker provided by this invention can increase the degradation rate of PET plastic by approximately 23 times. Furthermore, the presence of the polypeptide linker enhances enzyme stability. The preparation method is mature and efficient, with broad application prospects.

[0140] The applicant declares that this invention illustrates, through the above embodiments, a polypeptide linker for the complete conversion of PET plastic into TPA, its preparation method, and its application. However, this invention is not limited to the above embodiments, meaning that this invention does not necessarily rely on the above embodiments for implementation. Those skilled in the art should understand that any improvements to this invention, equivalent substitutions of raw materials for the product, addition of auxiliary components, and selection of specific methods all fall within the protection and disclosure scope of this invention.

[0141] The preferred embodiments of the present invention have been described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solution of the present invention, and these simple modifications all fall within the protection scope of the present invention.

[0142] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not describe the various possible combinations separately.

Claims

1. A polypeptide linker enabling complete conversion of PET plastic to TPA, characterized in that, The polypeptide linker comprises a polypeptide M targeting MHET hydrolase, a linker peptide, and a polypeptide P targeting PET hydrolase, which are sequentially linked, with polypeptide M located at the N-terminus and polypeptide P located at the C-terminus. The sequence of polypeptide M targeting MHET hydrolase is shown in SEQ ID No. 3, the sequence of polypeptide P targeting PET hydrolase is shown in SEQ ID No. 6, and the sequence of the linker peptide is shown in SEQ ID No.

8. The PET hydrolase is IsPETase, and the MHET hydrolase is IsMHETase.

2. The polypeptide linker to achieve complete conversion of PET plastic to TPA according to claim 1, wherein, The target recognition sequence M, the linker peptide, and the target recognition sequence P are covalently coupled through amide condensation.

3. The polypeptide linker to achieve complete conversion of PET plastic to TPA according to claim 1, wherein, The polypeptide linker includes the compound shown in Formula I; 。 4. A nanoparticle, characterized in that, The nanoparticles are prepared by the following method: synthesizing the polypeptide linker according to any one of claims 1-3 by chemical synthesis, and then performing self-assembly in self-assembly buffer to form nanoparticles.

5. The nanoparticle of claim 4, wherein, The self-assembly buffer includes any one of water, phosphate buffer, Tris-HCl buffer, or HEPES buffer.

6. The nanoparticle of claim 5, wherein, The self-assembly buffer is a phosphate buffer.

7. The nanoparticle of claim 4, wherein, The pH of the self-assembly buffer solution is 7.0~8.

0.

8. The nanoparticles according to claim 4, characterized in that, The spatial structure of the nanoparticles is β-sheet.

9. The nanoparticle of claim 4, wherein, The diameter of the nanoparticles is 10~30 nm.

10. A multi-enzyme complex for achieving complete conversion of PET plastic to TPA, characterized in that, The multi-enzyme complex includes PET hydrolase, MHET hydrolase and nanoparticles according to any one of claims 4-9; the three components in the multi-enzyme complex are arranged in a sandwich configuration and / or an encapsulation configuration, wherein the sandwich configuration is in which the nanoparticles are located between the PET hydrolase and the MHET hydrolase, and the encapsulation configuration is in which the nanoparticles encapsulate the PET hydrolase and the MHET hydrolase in one space. The PET hydrolase is IsPETase, and the MHET hydrolase is IsMHETase.

11. The multi-enzyme complex for achieving complete conversion of PET plastic into TPA according to claim 10, wherein, The diameter of the multi-enzyme complex is 29-49 nm.

12. The multi-enzyme complex for achieving complete conversion of PET plastic into TPA as claimed in claim 10, wherein, The binding affinity of the nanoparticles to PET hydrolase is 0.07 μM ~ 4.35 μM.

13. The multi-enzyme complex for achieving complete conversion of PET plastic into TPA as claimed in claim 10, wherein, The binding affinity of the nanoparticles to MHET hydrolase is 0.1 μM ~ 20.6 μM.

14. The multi-enzyme complex for the complete conversion of PET plastic to TPA according to claim 10, characterized in that, The molar ratio of the nanoparticles, PET hydrolase, and MHET hydrolase is (75-200):1:

1.

15. The multi-enzyme complex for the complete conversion of PET plastic to TPA according to claim 10, characterized in that, The concentration of the nanoparticles is no greater than 500 μM.

16. The use of a polypeptide linker according to any one of claims 1-3, a nanoparticle according to any one of claims 4-9, or a multi-enzyme complex according to any one of claims 10-15 in the degradation of PET plastics.

Citation Information

Patent Citations

  • Genetic engineering strain for degrading PET (polyethylene terephthalate) plastics

    CN107794252A

  • Method for degrading PET plastics by utilizing synergistic effect of two enzymes

    CN113549244A

  • Engineering enzyme compound for efficiently degrading PET (Polyethylene Terephthalate) plastic as well as preparation method and application of engineering enzyme compound

    CN114941004A

  • Method for screening targeted-self-assembled polypeptide

    CN116223811A

  • Nanoparticles based method for screening enzyme or microorganism

    US20220056387A1