A high sound absorption ceramic plate that can be used in tunnels and a preparation method thereof
By using raw materials such as river and lake sludge powder, talc powder and activated coal gangue, combined with nanofibers and specific gelling agents, high sound-absorbing ceramic panels are prepared, which solves the problems of existing technology in terms of noise reduction, fire resistance level and sound absorption frequency bandwidth. It achieves high sound absorption performance and comprehensive performance improvement in medium and low frequency environments.
Patent Information
- Application Number
- CN202311521017.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-15
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-11-15
AI Technical Summary
Existing sound-absorbing materials for tunnels have deficiencies in noise reduction effect, fire resistance level, surface strength and sound absorption frequency bandwidth, making it difficult to meet the comprehensive performance requirements in complex environments.
It uses river and lake sludge powder, talc powder and activated coal gangue as raw materials, combined with SiO2 nanofibers, polyvinylpyrrolidone and sodium tripolyphosphate as dispersants, glycerin epoxy resin and carbomer as gelling agents, hydrogen peroxide and carbonization Microsilica powder is used as a foaming agent to prepare high sound-absorbing ceramic panels through ball milling, dispersion, gelation and foaming injection molding processes.
It significantly improves the sound absorption coefficient in medium and low frequency environments, improves the compressive strength and fire resistance of ceramic plates, and meets the noise control needs in tunnels. At the same time, the material cost is low and it is easy to be industrialized.
Smart Images

Figure CN117417178B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of tunnel noise reduction and sound absorption materials, and in particular to a high-sound-absorbing ceramic plate that can be used in tunnels and a preparation method thereof. The plate can be used for noise control in various complex and special environments such as highway tunnels, road tunnels, high-speed rail tunnels, subway tunnels, and lake bottom tunnels. Background Art
[0002] The adverse effects of traffic noise on people and the surrounding environment have garnered widespread public attention. Tunnels are semi-enclosed structures, where sound waves undergo multiple propagation and reflection. Traffic noise propagates through tunnels through a pronounced acoustic waveguide effect, resulting in slow attenuation of noise inside the tunnel and significantly higher noise intensity than outside. Especially for highway and road tunnels over 1,000 meters in length, the noise intensity inside the tunnel is high, affecting a wide area, with long reverberation times and poor speech intelligibility. Furthermore, the noise radiation level at the tunnel entrance is also high. The high-decibel, long-reverberation noise environment within tunnels not only seriously impacts the efficiency of public address systems in disseminating evacuation information during emergency response, but also causes driver anxiety and stress, impacting their concentration and reaction speed, and increasing driving safety risks. The unattenuated transmission of the clamorous noise within road tunnels to the tunnel entrance radiates to the outside world, severely disrupting the daily lives and work of noise-sensitive buildings such as residential buildings, educational institutions, and hospitals. Furthermore, the strong noise within tunnels can severely affect the hearing and communication of tunnel maintenance workers. Therefore, tunnel noise has always been an important factor affecting tunnel emergency evacuation, driving safety, and environmental comfort.
[0003] Tunnels have stringent requirements for sound-absorbing decorative materials. They must possess comprehensive properties, including fire resistance, fire resistance, moisture resistance, corrosion resistance, aging resistance, environmental aesthetics, and ease of construction. In recent years, a series of specialized tunnel-specific sound-absorbing panels have emerged, including CEMCOM panels, perforated FC panels (fiber cement panels), and foam ceramics. However, existing tunnel-specific sound-absorbing materials have limitations. Perforated FC panels have low fire resistance and poor noise reduction performance, foam ceramics and expanded perlite have low surface strength, and microporous sound-absorbing tiles have a narrow absorption band. Therefore, there is a need to research new sound-absorbing materials that offer superior sound absorption and noise reduction performance while meeting the comprehensive requirements for fire resistance, fire resistance, moisture resistance, corrosion resistance, aging resistance, environmental aesthetics, and ease of construction within tunnel spaces. Summary of the Invention
[0004] Based on the problems and needs in the above-mentioned technology, the present application provides a high-sound-absorbing ceramic plate that can be used in tunnels and a preparation method thereof, aiming to alleviate problems such as high intensity, long reverberation time, and low speech clarity of traffic noise in tunnels. The ceramic plate has a hard surface, corrosion resistance, and non-flammability, as well as high sound absorption coefficient and wide sound absorption frequency band.
[0005] In the first aspect, the present invention discloses a high sound absorption ceramic plate that can be used in tunnels, which adopts the following technical solution:
[0006] A high-sound-absorbing ceramic plate that can be used in tunnels. The ceramic plate is made of the following components in parts by mass: 50-80 parts of river and lake silt powder, 10-15 parts of talc, 5-40 parts of activated coal gangue, 1-2 parts of a dispersant, 3-4 parts of a gelling agent, and 2-4 parts of a foaming agent; the dispersant comprises a composite of SiO2 nanofibers, polyvinyl pyrrolidone, and sodium tripolyphosphate.
[0007] By adopting the above technical solution, river and lake silt powder, talcum powder and activated coal gangue are used as raw materials. Coal gangue and river and lake silt are both solid waste resources, and talcum powder is also a low-priced and widely available raw material. SiO2 nanofibers, polyvinyl pyrrolidone and sodium tripolyphosphate are added as a dispersant. Polyvinyl pyrrolidone is a dispersing component with excellent water solubility. The addition of SiO2 nanofibers has a multi-level entanglement structure, which increases the contact area between the dispersant and the raw materials, providing more contact points and tortuous noise dissipation paths. The addition of sodium tripolyphosphate forms a charge layer attached to the surface of the SiO2 nanofibers during the hydrolysis process, which helps to improve the viscous friction dissipation performance between the SiO2 nanofibers and the raw material components, so that sound waves are continuously reflected and dissipated in the system. The ceramic plate obtained can achieve a higher sound absorption coefficient in a medium and low frequency environment. In addition, in addition to helping with the dispersion effect, the excess sodium tripolyphosphate is hydrolyzed to form phosphate, which reacts with CaO in the activated coal gangue, helping to improve the compressive strength of the ceramic plate.
[0008] Preferably, the volume ratio of the SiO2 nanofibers: polyvinyl pyrrolidone: sodium tripolyphosphate is (1-2): (3-4): (2-4).
[0009] As a further preference, the volume ratio of SiO2 nanofibers, polyvinyl pyrrolidone and sodium tripolyphosphate is 1:(1.5~4):2.
[0010] Preferably, the volume ratio of SiO2 nanofibers and sodium tripolyphosphate in the dispersant is 50-70%, and the volume ratio of sodium tripolyphosphate in the dispersant is above 30-45%.
[0011] Preferably, the activated coal gangue is prepared by heating the coal gangue to 750-800° C. within 30-45 minutes, keeping the temperature for 45-60 minutes, and then cooling.
[0012] By adopting the above technical solution, the coal gangue is rapidly heated and calcined, the organic components inside the coal gangue are volatilized, and bubble pores are formed inside the coal gangue to obtain activated coal gangue. The bubble pores as a microporous structure help to improve the sound absorption performance of the ceramic plate; the microporous structure inside the activated coal gangue and the pore structure inside the ceramic plate form a resonant cavity structure, which helps to improve the sound absorption performance of the ceramic plate.
[0013] Preferably, the gelling agent comprises a combination of glycerol epoxy resin and sodium alginate or carbomer.
[0014] By adopting the above technical solution, sodium alginate and carbomer contain a large number of carboxyl groups and hydroxyl groups in their own molecules, which can form hydrogen bonds with water molecules, thereby enhancing the interaction between molecules and forming a colloid; the glycerol epoxy resin molecular structure contains a large number of epoxy groups and benzene ring structures, and has excellent heat resistance, which helps to effectively gel and solidify in the later sintering process; among them, the combination of glycerol epoxy resin and carbomer is the best, because the gelation speed of carbomer is relatively slow, which is conducive to providing sufficient time for the dispersant to be evenly dispersed during the slurry stirring process.
[0015] Preferably, the foaming agent comprises a mixture of hydrogen peroxide and silicon carbide powder in a volume ratio of 1:(1-2).
[0016] By adopting the above technical solution, the foaming agent is hydrogen peroxide and silicon carbide micropowder mixed in a ratio of 1: (1~2). The hydrogen peroxide foams and releases gas during the slurry stirring process. During the sintering process of the ceramic plate, the fusible components in the silicon carbide micropowder will melt into a liquid phase, and during sintering, the gas will be trapped in the liquid phase to form pores, thereby promoting the formation of resonant bubbles inside the ceramic plate, which is beneficial to improving the sound absorption performance of the ceramic plate in medium and low frequency environments.
[0017] In a second aspect, the present application discloses a method for preparing a high-sound-absorbing ceramic plate that can be used in tunnels, using the following technical solution:
[0018] A method for preparing a high-sound-absorbing ceramic plate that can be used in tunnels comprises the following steps: mixing river and lake silt powder, talcum powder, and activated coal gangue, adding deionized water, a dispersant, and a gelling agent, and ball milling to obtain a mixed slurry with a solid content of 45-80%; adding a foaming agent to the mixed slurry, heating and stirring in a water bath, foaming and injection molding, cooling and drying, and sintering.
[0019] Preferably, the method for preparing the ceramic plate comprises the following steps:
[0020] (1) Mix river and lake silt powder, talcum powder, and activated coal gangue to obtain raw materials;
[0021] (2) Mix the raw materials, dispersant, and gelling agent, add 45-80% by mass of deionized water, place in a ball mill, and after the slurry is fully ball-milled, take out the slurry for use;
[0022] (3) Add sodium hydroxide to the slurry to adjust the pH to 9.5-10, then add a foaming agent, heat and stir in a water bath until the slurry is fully foamed;
[0023] (4) The fully foamed slurry is injected into the mold, placed and microwave-dried for 4 to 8 hours, and then demolded to obtain a ceramic green body;
[0024] (5) The green body is sintered, the temperature gradient is set, the green body is cooled, and the green body is taken out. The high sound absorption ceramic plate that can be used in the tunnel is completed.
[0025] Preferably, the temperature during sintering is controlled with a temperature gradient of 0-300°C, 300-800°C, and 800-1150°C.
[0026] In summary, this application has the following beneficial effects:
[0027] 1. The formula of this application uses river and lake silt powder, talcum powder and activated coal gangue as raw materials. Coal gangue and river and lake silt are solid waste resources. Talc powder is also a low-cost and widely available raw material. The addition of SiO2 nanofibers, polyvinyl pyrrolidone and sodium tripolyphosphate as a dispersant helps to fully disperse the slurry. The ceramic plate produced can achieve a high sound absorption coefficient in a medium and low frequency (500-2000Hz) environment.
[0028] 2. The foaming agent of the present application is a mixture of hydrogen peroxide and silicon carbide powder, which is conducive to promoting the formation of a stable and uniform resonant pore structure inside the ceramic plate, thereby improving the sound absorption performance of the ceramic plate in medium and low frequency environments;
[0029] 3. This application uses a compound of glycerol epoxy resin and carbomer as a gelling agent. Carbomer has a slow gelling speed and a high viscosity after gelling. During the slurry preparation process, it helps to provide sufficient dispersion time for the dispersant. Glycerol epoxy resin helps to improve the heat resistance of the gelling agent and also plays an excellent curing and cross-linking role during the sintering process, thereby promoting the improvement of the compressive strength and sound absorption performance of the ceramic plate.
[0030] 4. The main raw materials of this application are all inorganic components. The fire resistance grade of the prepared ceramic plate reaches Class A. It also has the comprehensive properties of moisture resistance, corrosion resistance, aging resistance, environmental protection and beautiful appearance.
[0031] 5. In the ceramic plate formula of the present application, whether it is the main raw materials or chemical agents such as dispersants, foaming agents, gelling agents, etc., the cost is low, the sources are easily available, and they are easy to industrialize and produce. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a sample photo of the ceramic plate used to illustrate Example 2.
[0033] Figure 2 It is a microscopic morphology diagram of the ceramic plate of Example 2.
[0034] Figure 3 It is a graph showing the sound absorption curves of Examples 1-5 and Comparative Example 1.
[0035] Figure 4 It is a graph showing the sound absorption curves of Examples 6-8 and Comparative Examples 1-2. DETAILED DESCRIPTION
[0036] In order to make the invention objectives, technical solutions and beneficial technical effects of this application more clear, this application will be described in detail below. It should be noted that the various aspects, features, implementation methods and advantages described in this application can be compatible and / or can be combined together.
[0037] Unless otherwise specified, the meanings of the technical terms in this specification are the same as those generally understood by those skilled in the art.
[0038] The present invention is based on the resource recycling of river and lake silt solid waste. The solid waste river and lake silt is used as the main material. The river and lake silt is dried, crushed and sieved to obtain river and lake silt powder. Activated coal gangue and talcum powder are added to the river and lake silt powder. Activated coal gangue is also one of the solid wastes. Talc powder is a commonly used auxiliary filler on the market. The river and lake silt powder, activated coal gangue and talcum powder are compounded as raw materials. The raw materials are widely available and low in price. The present invention aims to study how to make full use of solid waste and recycle solid waste to prepare sound-absorbing ceramic plates with a high sound absorption coefficient in a medium and low frequency environment of 500~2000Hz, thereby solving special environmental noise control problems such as the strong wind noise pressure caused by the fast forward speed of vehicles in tunnels.
[0039] In addition, based on the low-cost and efficient treatment of solid waste, the main raw materials, dispersants, foaming agents, gelling agents and other chemical agents in this application are all low-cost and easily available ingredients, and are easy to industrialize.
[0040] The invention relates to a high sound absorption ceramic plate that can be used in tunnels and a preparation method thereof.
[0041] The present invention is described in detail below.
[0042] In a first aspect, the present application provides a high sound absorption ceramic plate that can be used in tunnels, using the following technical solution:
[0043] A high-sound-absorbing ceramic plate that can be used in tunnels. The ceramic plate is made of the following components in parts by mass: 50-80 parts of river and lake silt powder, 10-15 parts of talc, 5-40 parts of activated coal gangue, 1-2 parts of a dispersant, 3-4 parts of a gelling agent, and 2-4 parts of a foaming agent; the dispersant comprises a composite of SiO2 nanofibers, polyvinyl pyrrolidone, and sodium tripolyphosphate.
[0044] Preferably, the ingredients include 60-70 parts of river and lake silt powder, 12-14 parts of talc, 20-30 parts of activated coal gangue, 1.3-1.7 parts of dispersant, 3.2-3.6 parts of gelling agent, and 2.5-3.5 parts of foaming agent.
[0045] In some specific embodiments, the river and lake silt is silt discarded from river and lake dredging, and after drying and crushing, the particle size is less than 15 μm; the chemical composition of the silt includes the following components in mass percentage: SiO2 76.8%-78.1%, Al2O3 10.3%-11.9%, Fe2O3 4.6%-5.1%, K2O 2.1%-2.5%, CaO 1.2%-1.6%, MgO 0.4%-0.9%, TiO2 0.8%-1.0%, SO3 0.1%-0.6%, P2O5 0.10%-0.12%, MnO 0.14%-0.17%, ZrO2 0.05%-0.08%, Cl 0.02%-0.04%, V2O5 0-0.03%, SrO 0.01%-0.02%, Cr2O30.01%-0.02%, ZnO0.01%-0.02%, Rb2O 0.007%-0.017%, Y2O30.00 5%-0.01%, NbO 0-0.002%, CuO 0-0.006%.
[0046] In some specific embodiments, the cumulative content of talc powder with a particle size of less than 30 μm is greater than 90% of the talc powder.
[0047] In some specific embodiments, the activated coal gangue is selected from activated coal gangue powder with an average particle size of less than 1 mm; the commercially available coal gangue powder is heated to 750°C within 30 minutes, kept warm for 45 minutes, and then air-cooled at 10-20°C for 15-30 minutes to obtain activated coal gangue powder; during the rapid heating process, the organic components in the coal gangue powder are volatilized, and bubble pores are formed inside the coal gangue, which helps to improve the reaction activity and sound absorption performance of the coal gangue powder of the present application.
[0048] In some specific embodiments, the dispersant is selected from SiO2 nanofibers, polyvinyl pyrrolidone, and sodium tripolyphosphate, mixed in a volume ratio of (1-2): (3-4): (2-4). For example, the volume ratio is 1:3:2, 1:3:4, 1:3.5:2, 1:3.5:4, 1:4:2, 1:4:4, 1.5:3:2, 1.5:3:4, 1.5:4:2, 1.5:4:4, 2:3:2, 2:3:4, 2:4:2, and 2:4:4. When the volume ratio of SiO2 nanofibers and sodium tripolyphosphate in the dispersant is 50% or greater, and the volume ratio of sodium tripolyphosphate in the dispersant is greater than 30%, the dispersant helps to evenly disperse the slurry, thereby improving the sound absorption performance of the sound-absorbing ceramic panel.
[0049] In some specific embodiments, the gelling agent comprises a combination of glycerol epoxy resin and sodium alginate or carbomer. Preferably, the gelling agent is a combination of glycerol epoxy resin and carbomer in a volume ratio of 1:1. Carbomer has a slow gelation rate and a high viscosity after gelation, which helps provide sufficient dispersion time for the dispersant during slurry preparation. Furthermore, glycerol epoxy resin has excellent heat resistance and can perform excellent curing and cross-linking during the sintering process, thereby ensuring the reactive activity of the gelling agent during sintering.
[0050] In some embodiments, the foaming agent is selected from a mixture of hydrogen peroxide and silicon carbide micropowder; preferably, the foaming agent comprises hydrogen peroxide and silicon carbide micropowder in a volume ratio of 1:(1-2). Hydrogen peroxide hydrolysis produces a large amount of gas. During the slurry preparation process, this gas facilitates the infiltration of gas between the river and lake silt powder, talcum powder, and activated coal gangue, as well as within each component, acting as an "emulsification" agent, promoting the uniform dispersion of the river and lake silt powder and activated coal gangue in the slurry. During the subsequent sintering process, this also facilitates the formation of uniform pores within the ceramic plate. During sintering, the fusible components in the silicon carbide micropowder melt into a liquid phase, where gas is trapped to form pores. This promotes the formation of resonant pores within the ceramic plate, thereby improving the sound absorption performance of the ceramic plate in low- and medium-frequency environments. When the volume ratio of hydrogen peroxide to silicon carbide powder is 2:1, more gas is generated during the slurry preparation process, which easily forms a "bubble" phenomenon with the bubbles in the later fusible areas, thereby reducing the compressive strength and sound absorption performance of the ceramic plate to a certain extent.
[0051] In a second aspect, the present application provides a method for preparing a high-sound-absorbing ceramic plate that can be used in tunnels, using the following technical solution:
[0052] A method for preparing a high-sound-absorbing ceramic plate that can be used in tunnels comprises the following steps:
[0053] (1) Ball milling, dispersion, and gelation:
[0054] Mixing river and lake silt powder, talcum powder, and activated coal gangue to obtain raw materials;
[0055] (2) Mix the raw materials, dispersant, and gelling agent, add 45-80% by mass of deionized water, place in a ball mill, and mill at a speed of 300-500 rpm for 2-6 hours. Take the slurry for later use;
[0056] (3) Heating and stirring in a water bath to produce foam:
[0057] Add sodium hydroxide to the slurry of step (2), adjust the pH to 9.5-10, then add a foaming agent, heat in a water bath to maintain 65-70°C, and stir at a speed of 200-800 rpm for 2-4 minutes until the slurry is fully foamed;
[0058] (4) Injection molding and drying:
[0059] The fully foamed slurry in step (3) is injected into an acrylic mold, allowed to stand, cooled and formed, placed in a microwave oven, and microwave-dried for 4 to 8 hours before demoulding to obtain a ceramic embryo body;
[0060] (5) The green embryo obtained in step (4) is placed in a crucible, placed in a sintering furnace, sintered and solidified, the temperature is set to a gradient, and cooled and taken out. The high sound absorption ceramic plate that can be used in tunnels is completed.
[0061] In some embodiments, the alkalinity is suitably 9.5-10, preferably 9.6, 9.7, 9.8, 9.9 or a range consisting of any two of the above values; if the alkalinity is too high, the foaming performance will be affected.
[0062] In some specific embodiments, microwave drying for 4 to 8 hours is microwave drying at medium heat for 3 to 5 hours, and microwave drying at high heat for 1 to 3 hours; as an example, microwave drying at medium heat is 3 hours, 3.5 hours, 4 hours, 4.5 hours, 5 hours, or within the range of any two of the above values; microwave drying at high heat is 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, or within the range of any two of the above values.
[0063] In some specific embodiments, the temperature control during sintering is as follows: the temperature gradient is 0-300° C., keeping warm for 1 hour, 300-800° C., keeping warm for 1 hour, 800-1150° C., keeping warm for 1 hour. Example
[0064] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0065] Examples 1 to 5
[0066] The following is described using Example 1 as an example:
[0067] Example 1:
[0068] This embodiment provides a high-sound-absorbing ceramic plate that can be used in tunnels, comprising the following components: 50 kg of river and lake silt powder, 10 kg of talcum powder, 5 kg of activated coal gangue, 1 kg of dispersant, 3 kg of gelling agent, and 2 kg of foaming agent;
[0069] In this embodiment, the average particle size of talc is 10-30 μm; the activated coal gangue is selected from coal gangue powder with a CaO content of nearly 4% and a particle size of 80-120 μm, and the coal gangue powder is heated to 750° C. within 30 minutes, kept warm for 45 minutes, and then cooled to obtain the activated coal gangue; the dispersant is selected from SiO2 nanofiber: polyvinyl pyrrolidone: sodium tripolyphosphate in a volume ratio of 1:3:2; the gelling agent is selected from glycerol epoxy resin and carbomer 940 in a volume ratio of 1:1; the foaming agent is selected from hydrogen peroxide and silicon carbide micropowder in a volume ratio of 1:1;
[0070] In this embodiment, a high sound absorption ceramic plate that can be used in tunnels is prepared according to the following steps:
[0071] (1) Treatment of river and lake silt:
[0072] Drying, crushing and sieving the river and lake silt to obtain river and lake silt powder;
[0073] (2) Ball milling, dispersion, and gelation:
[0074] Mix the river and lake silt powder, talcum powder and activated coal gangue from step (1) to obtain a raw material;
[0075] (3) Mix the raw materials, dispersant, and gelling agent, add 45-50% by mass of deionized water, place in a ball mill, and mill at a speed of 400 rpm for 4 h. Take the slurry for later use;
[0076] (4) Heating and stirring in a water bath to produce foam:
[0077] Add 4% by mass of sodium hydroxide solution to the slurry in step (3), adjust the pH to 10, then add a foaming agent, heat in a water bath to maintain 75°C, and stir at a speed of 400 rpm for 4 minutes until the slurry is fully foamed;
[0078] (5) Injection molding and drying:
[0079] The fully foamed slurry in step (4) is injected into an acrylic mold, allowed to stand, cooled and formed, placed in a microwave oven, dried at medium microwave heat for 4 hours, dried at high microwave heat for 2 hours, and then demolded to obtain a ceramic green body;
[0080] (6) The green embryo obtained in step (5) is placed in a crucible, placed in a sintering furnace, sintered and solidified, with a heating rate of 5°C / min and a temperature gradient of 0-300°C, kept warm for 1 hour, 300-800°C, kept warm for 1 hour, 800-1150°C, kept warm for 1 hour, cooled and taken out, and the production of a high sound-absorbing ceramic plate that can be used in tunnels is completed.
[0081] As shown in Table 1, the main difference between Examples 1 to 5 is the different contents of the components used in the ceramic plate.
[0082] Table 1 Content of components used in ceramic plates (kg)
[0083] sample River and lake silt powder talcum powder Activated coal gangue dispersants Gelling agent foaming agent Deionized water Example 1 50 10 5 1 3 2 56 Example 2 60 12 10 1.2 3.2 2.4 75 Example 3 70 13 25 1.2 3.2 2.4 92 Example 4 75 14 25 1.8 3.8 3.4 102 Example 5 80 15 40 2 4 4 115
[0084] Example 6:
[0085] A high sound-absorbing ceramic plate that can be used in tunnels, which differs from Example 2 in that the volume ratio of SiO2 nanofibers, polyvinyl pyrrolidone, and sodium tripolyphosphate in the dispersant is different. In this embodiment, the volume ratio of SiO2 nanofibers, polyvinyl pyrrolidone, and sodium tripolyphosphate is 1:3.5:2.
[0086] Example 7
[0087] A high sound-absorbing ceramic plate that can be used in tunnels, which differs from Example 2 in that the volume ratio of SiO2 nanofibers, polyvinyl pyrrolidone, and sodium tripolyphosphate in the dispersant is different. In this embodiment, the volume ratio of SiO2 nanofibers, polyvinyl pyrrolidone, and sodium tripolyphosphate is 1:4:2.
[0088] Example 8
[0089] A high sound-absorbing ceramic plate that can be used in tunnels, which differs from Example 2 in that the volume ratio of SiO2 nanofibers, polyvinyl pyrrolidone, and sodium tripolyphosphate in the dispersant is different. In this embodiment, the volume ratio of SiO2 nanofibers, polyvinyl pyrrolidone, and sodium tripolyphosphate is 2:3:4.
[0090] Comparative Example 1:
[0091] A high sound-absorbing ceramic plate that can be used in tunnels, which differs from Example 2 in that the volume ratio of SiO2 nanofibers, polyvinyl pyrrolidone, and sodium tripolyphosphate in the dispersant is different. In this embodiment, the volume ratio of SiO2 nanofibers, polyvinyl pyrrolidone, and sodium tripolyphosphate is 0.5:3:2.
[0092] Comparative Example 2:
[0093] A high sound-absorbing ceramic plate that can be used in tunnels, which differs from Example 2 in that the volume ratio of SiO2 nanofibers, polyvinyl pyrrolidone, and sodium tripolyphosphate in the dispersant is different. In this embodiment, the volume ratio of SiO2 nanofibers, polyvinyl pyrrolidone, and sodium tripolyphosphate is 2.5:3:2.
[0094] Comparative Example 1:
[0095] A sound-absorbing ceramic plate, which differs from Example 2 in that the components of the ceramic plate are different. This comparative example uses the following components in parts by mass: 60 kg of river and lake silt powder, 12 kg of talcum powder, 10 kg of coal gangue, 1.2 kg of dispersant, 3.2 kg of gelling agent, and 2.4 kg of foaming agent; 75 kg of deionized water; wherein the dispersant is ammonium polyacrylate; the gelling agent is sodium alginate; and the foaming agent is triethanolamine lauryl sulfate and cocamidopropyl betaine compounded in a volume ratio of 1:1. The preparation method is consistent with that of Example 2.
[0096] Detection methods:
[0097] Sound absorption coefficient: Normal incidence sound absorption coefficient, the measurement standard is GB / T 18696.2-2002;
[0098] Compressive strength: Mechanical testing was performed using an SHK-A104 compressive strength testing machine in accordance with GB / T 4740-1999.
[0099] Porosity: Tested in accordance with BS EN ISO 9237 using the gas volume method using Mecanum PHI equipment.
[0100] Table 2 Mechanical properties and sound absorption properties of ceramic plates in Examples and Comparative Examples
[0101] sample Compressive strength (MPa) Porosity (%) Sound absorption coefficient at 500Hz Sound absorption coefficient at 800Hz Sound absorption coefficient at 1000Hz Sound absorption coefficient at 1500Hz Sound absorption coefficient at 2000Hz Example 1 8.6 96.7 0.45 0.88 0.93 0.87 0.72 Example 2 8.9 97 0.38 0.78 0.90 0.98 0.83 Example 3 7.7 92.4 0.32 0.60 0.72 0.99 0.92 Example 4 7.5 95.8 0.37 0.78 0.93 0.89 0.69 Example 5 7.4 93.1 0.30 0.59 0.80 0.97 0.79 Example 6 8.5 95.4 0.39 0.82 0.92 0.82 0.78 Example 7 7.9 93.6 0.20 0.48 0.73 0.98 0.80 Example 8 9.0 94.6 0.38 0.70 0.86 0.97 0.79 Comparative Example 1 8.2 92.5 0.42 0.70 0.81 0.90 0.82 Comparative Example 2 7.7 94.5 0.37 0.60 0.73 0.93 0.95 Comparative Example 1 7.3 82.5 0.50 0.56 0.55 0.54 0.56
[0102] Combined with Examples 1 to 5 and Comparative Example 1 and Table 2 and Figure 1-3 The test results show that the formula of this application uses river and lake silt powder, talcum powder and activated coal gangue as raw materials, and adds SiO2 nanofiber, polyvinyl pyrrolidone and sodium tripolyphosphate as dispersants, adds glycerol epoxy resin and carbomer 940 as gelling agents, and adds hydrogen peroxide and silicon carbide micropowder as foaming agents, which helps to fully disperse, gel, foam and injection mold the slurry. The ceramic plate obtained can achieve a higher sound absorption coefficient in the medium and low frequencies of 500~2000Hz.
[0103] In Example 2 and Example 4, the amount of river and lake silt powder added to the slurry is more than 34%, the amount of dispersant added is 0.76%, the amount of gelling agent added is more than 1.75%, and the amount of foaming agent added is more than 1.5%. The prepared sound-absorbing ceramic plates are well-formed and have high compressive strength, especially in medium and low frequency environments. The sound absorption performance is the best, and it is suitable for environments in tunnels where the traffic noise intensity is high, the reverberation time is long, and the speech clarity is low.
[0104] However, the dispersant, gelling agent and foaming agent used in Comparative Example 1 are different from those in the present application, and the coal gangue has not been activated. The ceramic plate prepared cannot quickly increase the sound absorption coefficient in a medium and low frequency environment. Therefore, the formula of the present application can realize the resource utilization of river and lake silt and coal gangue solid waste, and prepare sound-absorbing ceramic plates through gel foaming injection molding, so that the ceramic plates can achieve high sound absorption characteristics in a medium and low frequency environment. At the same time, the raw materials are low-cost and environmentally friendly components, and also have corrosion-resistant and non-flammable properties.
[0105] Combined with Example 2, Examples 6-8, Comparative Examples 1-2 and Table 2 and Figure 4 The test results show that SiO2 nanofibers, polyvinyl pyrrolidone and sodium tripolyphosphate are compounded in a ratio of 1: (1.5~4): 2, and the resulting sound-absorbing ceramic board has excellent sound absorption performance and can quickly reach a peak value in a 600-1200Hz environment; while in Comparative Example 1-2, the rate of increase of the sound absorption coefficient in 600-1200Hz decreases, and the peak value that can be achieved also decreases, indicating that the volume ratio of SiO2 nanofibers and sodium tripolyphosphate in the dispersant is 50-70%, and the volume ratio of sodium tripolyphosphate in the dispersant is 30-45%. The dispersant can evenly disperse the slurry, thereby promoting the improvement of sound absorption performance; at the same time, excess sodium tripolyphosphate is hydrolyzed to form phosphate, which reacts with CaO in the activated coal gangue, helping to improve the compressive strength of the ceramic board.
Claims
1. A high sound absorption ceramic plate that can be used in tunnels. Features: The ceramic plate is made of the following components by weight: 50-80 parts of river and lake sludge powder, 10-15 parts of talcum powder, 5-40 parts of activated coal gangue, 1-2 parts of dispersant, 3-4 parts of gelling agent, and 2-4 parts of foaming agent; the dispersant includes SiO 2 A composite of nanofibers, polyvinyl pyrrolidone and sodium tripolyphosphate; The gelling agent includes a composition of glycerol epoxy resin and sodium alginate or carbomer; The foaming agent comprises a mixture of hydrogen peroxide and silicon carbide powder compounded in a volume ratio of 1:(1-2); Among them, SiO 2 The volume ratio of nanofiber: polyvinyl pyrrolidone: sodium tripolyphosphate is (1~2): (3~4): (2~4).
2. A high sound absorption ceramic plate that can be used in tunnels according to claim 1, Features: The activated coal gangue is prepared by heating the coal gangue to 750-800° C. within 30-45 minutes, keeping the temperature for 45-60 minutes, and then cooling.
3. A method for preparing a high sound absorption ceramic plate that can be used in tunnels according to any one of claims 1 to 2, It is characterized in that The method comprises the following steps: mixing river and lake sludge powder, talcum powder and activated coal gangue, adding deionized water, dispersant and gelling agent for ball milling to obtain a mixed slurry with a solid content of 45-80%; adding a foaming agent to the mixed slurry, heating in a water bath, stirring for foaming injection molding, cooling and drying, and sintering.
4. The method for preparing a high sound absorption ceramic plate that can be used in tunnels according to claim 1, It is characterized in that The steps include: (1) Mix river and lake silt powder, talcum powder and activated coal gangue to obtain raw materials; (2) Mix the raw materials, dispersant and gelling agent, add deionized water, and place in a ball mill for ball milling. After the slurry is fully ball milled, take out the slurry for use; (3) Add sodium hydroxide to the slurry to adjust the pH to 9.5-10, then add a foaming agent, heat and stir in a water bath until the slurry is fully foamed; (4) injecting the fully foamed slurry into a mold, placing it in a mold, and microwave drying it for 4 to 8 hours before demolding it to obtain a ceramic green body; (5) The ceramic green body is sintered, the temperature gradient is set, the green body is cooled, and the green body is taken out, thereby completing the production of a high sound absorption ceramic plate that can be used in a tunnel.
5. A method for preparing a high sound absorption ceramic plate that can be used in tunnels according to claim 4, Features: The temperature control during sintering has a temperature gradient of 0~300℃, 300~800℃, and 800~1150℃.