A double-layer composite solid electrolyte and its preparation process and application
By using a double-layer structure composite solid electrolyte in lithium-ion batteries and using a double-layer structure of active fillers and inert fillers, the poor cycle performance problem caused by lithium dendrites is solved, and efficient lithium ion transmission and stability is achieved. in high voltage electrolyte materials.
Patent Information
- Application Number
- CN202311379570.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-24
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-10-24
AI Technical Summary
The growth of lithium dendrites inside solid electrolytes in lithium-ion batteries leads to poor circulation performance and reduces the cycle life of lithium-ion batteries. The current technology has low conductivity and insufficient stability, making it difficult to effectively solve interface problems.
A double-layer structure composite solid electrolyte is used, the main layer is filled with active filler Li6.3La3Zr1.65W0.35O12, and the modification layer is filled with inert filler Al2O3, which is prepared by hot solvent coating to form a distinct double-layer structure to enhance lithium ion transmission. Performance and stability.
It significantly improves the cycle stability and electrochemical performance of lithium-ion batteries, has excellent rate performance and long cycle stability, and has an electrochemical window >5 V, suitable for high-voltage electrolyte materials.
Smart Images

Figure CN117423892B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of batteries, and in particular relates to a double-layer composite solid electrolyte and a preparation process and application thereof. Background Art
[0002] Solid electrolytes are used to replace traditional liquid electrolytes in lithium-ion batteries to fundamentally solve the safety problems of lithium-ion batteries. Composite solid electrolytes with high ionic conductivity have great development potential due to their excellent flexibility and have attracted widespread attention.
[0003] During the cycle of lithium-ion batteries, the growth of lithium dendrites inside the solid electrolyte can easily lead to poor cycle performance of lithium-ion batteries and reduce the cycle life of lithium-ion batteries. Specifically, the instability of the electrolyte / electrode interface causes the interface concentration difference, which promotes the growth of dendritic lithium dendrites perpendicular to the interface under the influence of the external electric field, and eventually pierces the electrolyte, causing the lithium-ion battery to short-circuit, and ultimately leading to the failure of the lithium-ion battery.
[0004] Prior art: Chinese patent authorization announcement No. CN110518277B discloses a solid electrolyte, a preparation method thereof, and a solid-state battery containing the solid electrolyte. The solid electrolyte includes a positive electrode interface layer, an intermediate layer, and a negative electrode interface layer. In the positive electrode interface layer, the intermediate layer, and the negative electrode interface layer, the polymer is one or more of polyoxymethylene, polyvinylidene fluoride, polymethyl methacrylate, polyethylene oxide, or polypropylene oxide, and the inorganic powder is one or more of inert filler nano-SiO2, Al2O3, TiO2 particles, BaTiO3, and molecular sieves, or one or more of active fillers LiAlO2, LLZTO, LAGP, LLTO, and LGPS. The preparation method adopts scraping film formation, and the prepared composite solid electrolyte has excellent bending resistance and windability, and the electrochemical window is 4.8V. The core is to design the gradient between different layers so that different layers have different properties and play different roles to solve the interface problem.
[0005] Chinese patent application publication number CN114497718A discloses a room temperature high-voltage polymer electrolyte and a preparation method and a battery thereof, wherein the polymer electrolyte comprises at least a first electrolyte layer and a second electrolyte layer stacked in layers, both of which are composited with a polymer, a lithium salt, an ionic liquid, and a filler, wherein the first polymer is selected from one or more of polyvinylidene fluoride, poly(vinylidene fluoride-hexafluoropropylene), polyacrylonitrile, and polycarbonate, the second polymer is selected from polyethylene oxide, and the first inorganic filler and the second inorganic filler independently include an inert filler without ionic conductivity and an inert filler with ionic conductivity. At least one of the active fillers; the inert filler includes at least one of silicon dioxide, aluminum oxide, cerium oxide, and titanium dioxide; the active filler includes at least one of lithium fast ion conductor solid electrolyte, sodium fast ion conductor solid electrolyte, perovskite solid electrolyte, and garnet solid electrolyte. The preparation method adopts a scraping method and a casting method. Its purpose is to resist electrochemical oxidation, improve stability, and solve the problem of low conductivity of existing double-layer polymer electrolytes. The core is to add ionic liquid into the electrolyte layer, increase the concentration of free lithium ions, assist lithium ion diffusion, and improve the conductivity of the electrolyte.
[0006] The purpose of the present invention is to develop another composite solid electrolyte and its preparation process and battery, so as to improve the lithium ion transmission performance and stability of the solid electrolyte, thereby improving the cycle performance of the lithium ion battery. Summary of the invention
[0007] Purpose of the invention: In order to overcome the above shortcomings, the purpose of the present invention is to provide a double-layer composite solid electrolyte and its preparation process and application. The solid electrolyte adopts a double-layer composite structure that combines the characteristics of active fillers and inert fillers. The main layer is filled with active fillers to provide excellent lithium ion transmission performance, and the modified layer is filled with inert fillers to provide high lithium stability. It is applied to solid-state lithium metal batteries and exhibits excellent battery performance, with broad application prospects.
[0008] The objective of the present invention is achieved through the following technical solutions:
[0009] A double-layer composite solid electrolyte, the solid electrolyte is a double-layer structure composed of a composite polymer layer 1 filled with active fillers as a main layer and a composite polymer layer 2 filled with inert fillers as a modifying layer; wherein the composite polymer layer 1 includes active fillers, polycaprolactone, and lithium salts, and the composite polymer layer 2 includes inert fillers, polycaprolactone, and lithium salts.
[0010] The solid electrolyte described in the present invention is reasonably designed and adopts a double-layer composite structure combining the characteristics of active fillers and inert fillers. The main layer is a composite polymer layer one filled with active fillers, and the modified layer is a composite polymer layer two filled with inert fillers. The polymer matrix is polycaprolactone. The main layer and the modified layer are clearly layered and in close contact. The main layer provides excellent lithium ion transmission performance and the modified layer provides high lithium stability, showing excellent electrochemical performance, excellent rate performance and long cycle stability, and the electrochemical window is >5 V. It can be used as an ideal high-voltage electrolyte material in solid-state lithium metal batteries.
[0011] Furthermore, in the above-mentioned double-layer structure composite solid electrolyte, the main layer is a composite polymer layer one prepared by mixing an active filler with polycaprolactone and a lithium salt through a hot solvent coating method; the modification layer is a composite polymer layer two prepared by mixing an inert filler with polycaprolactone and a lithium salt and coating the mixture on the surface of the main layer through a hot solvent coating method.
[0012] The main layer and the modified layer of the solid electrolyte are coated on the surface of the main layer by a hot solvent coating method, and a double-layer structure is formed after drying, so that the main layer and the modified layer are clearly layered and in close contact.
[0013] Furthermore, in the above-mentioned double-layer composite solid electrolyte, the active filler is Li 6.3 LqCy 1.65 W 0.35 O 12 , the inert filler is Al2O3, and the lithium salt is LiTFSI.
[0014] The present invention selects Li 6.3 LqCy 1.65 W 0.35 O 12 As active filler, Li 6.3 LqCy 1.65 W 0.35 O 12 This makes the solid electrolyte have higher ionic conductivity, but its instability to lithium promotes the growth of lithium dendrites during the cycling of lithium-ion batteries.
[0015] The present invention selects Al2O3 as an inert filler. The solid electrolyte filled with Al2O3 has excellent lithium stability, promotes uniform deposition of lithium ions, and thus inhibits the growth of lithium dendrites. However, its low ionic conductivity limits its rate cycle. 6.3 LqCy 1.65 W 0.35 O 12It not only reduces the crystallinity of polycaprolactone and improves the ionic conductivity of the main layer, but also forms a continuous lithium ion transmission channel in the composite polymer layer 1 due to its own ionic conductivity, further improving the lithium ion transmission performance of the main layer. The Li-Al-O layer formed by the lithiation reaction between Al2O3 in the modified layer and the surface of the lithium negative electrode promotes the uniform deposition of lithium ions, effectively inhibits the growth of lithium dendrites, and improves the interface problem.
[0016] Therefore, the use of a double-layer composite solid electrolyte that combines the characteristics of active fillers and inert fillers not only achieves excellent ionic conductivity but also lithium stability, significantly improving the cycle stability of lithium-ion batteries.
[0017] Furthermore, in the above-mentioned double-layer composite solid electrolyte, the active filler is added in an amount of 20-50% of the total mass of the active filler, polycaprolactone and lithium salt, and the number average molecular weight of the polycaprolactone is 10000-100000 g·mol -1 The lithium-oxygen ratio Li:O of the lithium salt and polycaprolactone is 1:1-100.
[0018] Furthermore, in the above-mentioned double-layer composite solid electrolyte, the amount of the inert filler added is 5-30% of the total mass of the inert filler, polycaprolactone and lithium salt, and the number average molecular weight of the polycaprolactone is 10000-100000 g·mol -1 The lithium-oxygen ratio Li:O of the lithium salt and polycaprolactone is 1:1-100.
[0019] Furthermore, in the above-mentioned double-layer composite solid electrolyte, the amount of the active filler added is 35% of the total mass of the active filler, polycaprolactone and lithium salt, and the number average molecular weight of the polycaprolactone is 80000 g·mol -1 The lithium-oxygen ratio Li:O of the lithium salt and polycaprolactone is 1:20.
[0020] Furthermore, in the above-mentioned double-layer composite solid electrolyte, the inert filler is added in an amount of 20% of the total mass of the inert filler, polycaprolactone and lithium salt, and the number average molecular weight of the polycaprolactone is 80000 g·mol -1 The lithium-oxygen ratio Li:O of the lithium salt and polycaprolactone is 1:20.
[0021] The present invention also relates to a preparation process of the double-layer composite solid electrolyte, comprising the following steps:
[0022] S1: polycaprolactone and lithium salt are mixed, a solvent is added, and the mixture is stirred at a temperature of 50-70°C until the polycaprolactone is completely dissolved; then, an active filler that has been fully dried in a vacuum drying oven is added, and the stirring is continued, and the stirring process is accompanied by ultrasonic treatment to obtain a composite polymer layer 1 slurry, and the composite polymer layer 1 slurry is evenly coated on a glass plate, and the coated glass plate is placed in a ventilated place to dry for 10-30 hours to obtain a composite polymer layer 1, and the composite polymer layer 1 is cut to obtain a main body layer with a thickness of 0-100 μm;
[0023] S2: Mix polycaprolactone and lithium salt, add solvent, and stir at a temperature of 50-70°C until polycaprolactone is completely dissolved; then, add inert filler and continue stirring, and the stirring process is accompanied by ultrasonic treatment to obtain a composite polymer layer two slurry, and the composite polymer layer two slurry is evenly coated on the surface of the main layer. After coating, place it in a ventilated place to dry for 10-30 hours to obtain a composite polymer layer two, and then cut to obtain a solid electrolyte; wherein the thickness of the modified layer is 0-10 μm.
[0024] The preparation process of the double-layer composite solid electrolyte of the present invention is simple in technology and suitable for industrial production.
[0025] Furthermore, in the preparation process of the double-layer composite solid electrolyte, the solvent in steps S1 and S2 is dimethyl carbonate; the stirring is performed at a temperature of 60° C. in steps S1 and S2; the coating is performed by scraper coating in steps S1 and S2; and the drying is performed in a ventilated place for 24 hours in steps S1 and S2.
[0026] The present invention also relates to the application of the double-layer structure composite solid electrolyte, and the above-mentioned solid electrolyte is applied to a solid-state lithium metal battery; the solid electrolyte is assembled with a positive electrode and a negative electrode to obtain a solid-state lithium metal battery.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] (1) The double-layer composite solid electrolyte disclosed in the present invention has a reasonable design. The solid electrolyte adopts a double-layer structure of a main layer and a modified layer. The main layer and the modified layer are respectively made of active fillers and inert fillers as inorganic fillers, polycaprolactone as a polymer matrix, and are mixed with lithium salts and prepared by a hot solvent coating method. The main layer provides excellent lithium ion transmission performance and the modified layer provides high lithium stability.
[0029] (2) The double-layer composite solid electrolyte disclosed in the present invention uses Li 6.3 LqCy 1.65 W 0.35 O 12 , inert fillers are selected as Al2O3, Li6.3 LqCy 1.65 W 0.35 O 12 Not only does it reduce the crystallinity of polycaprolactone and improve the ionic conductivity of the main layer, but its own ionic conductivity also forms a continuous lithium ion transmission channel in the composite polymer layer 1, further improving the lithium ion transmission performance of the main layer; the Li-Al-O layer formed by the lithiation reaction between Al2O3 in the modified layer and the surface of the lithium negative electrode promotes the uniform deposition of lithium ions, effectively inhibits the growth of lithium dendrites, and improves the interface problem;
[0030] (3) The preparation process of the double-layer composite solid electrolyte disclosed in the present invention is simple and can be prepared on a large scale. The main layer and the modified layer are coated on the surface of the main layer by a hot solvent coating method, and a double-layer structure is formed after drying, so that the main layer and the modified layer are clearly layered and in close contact;
[0031] (4) Application of the double-layer composite solid electrolyte disclosed in the present invention. The solid electrolyte can be used as an ideal high-voltage electrolyte material in solid-state lithium metal batteries. When used in solid-state lithium metal batteries, it exhibits excellent battery performance: 1. The rate test at 0.1~1 C at 60°C shows that its discharge capacity decays less with increasing rate and has a higher discharge capacity; 2. The long cycle test shows that when the capacity is cycled for 300 cycles at 1 C at 60°C, the capacity retention rate is above 95%, which has excellent long cycle stability; 3. The ionic conductivity of the solid electrolyte reaches 3.62×10 -5 S cm -1 , the lithium ion transference number is 0.55, and its electrochemical stability window is >5 V. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a flow chart of the preparation process of Comparative Examples 1-3 of the double-layer composite solid electrolyte of the present invention;
[0033] Figure 2 This is a flow chart of the preparation process of Example 1 of the double-layer composite solid electrolyte of the present invention;
[0034] Figure 3 The internal structure of the battery of Example 2 of the application of the double-layer composite solid electrolyte of the present invention;
[0035] Figure 4 The temperature-dependent ionic conductivity diagram of Comparative Examples 1-3 of the double-layer composite solid electrolyte of the present invention;
[0036] Figure 5 This is a temperature-dependent ionic conductivity diagram of Example 1 of the double-layer composite solid electrolyte of the present invention;
[0037] Figure 6 This is a rate performance diagram of 0.1~1 C at 60°C for Example 2 of the application of the double-layer structure composite solid electrolyte of the present invention;
[0038] Figure 7 This is a long cycle curve of Example 2 of the application of the double-layer structure composite solid electrolyte of the present invention at 60°C and 1°C for 300 cycles;
[0039] Figure 8 This is a SEM image of the surface of the lithium negative electrode after cycling in Example 2 of the application of the double-layer composite solid electrolyte of the present invention. DETAILED DESCRIPTION
[0040] The following is a comparison of Examples 1-3, Example 1, and Example 2 in combination with specific experimental data and the attached Figure 1-8 , the technical solutions in the embodiments of the present invention are clearly and completely described. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the protection scope of the present invention.
[0041] The following comparative examples 1, 2 and 3 provide a single-layer solid electrolyte.
[0042] Comparative Example 1
[0043] like Figure 1 As shown, in Comparative Example 1, the main layer 1 is used as a single-layer solid electrolyte, and its preparation process includes the following steps:
[0044] (1) First, weigh 0.57 g of a molecule with a number average molecular weight of 80,000 g·mol -1 0.144 g of LiTFSI with a lithium-oxygen ratio of Li:O=1:20 was weighed into a clean beaker, 1 mL of dimethyl carbonate was added, and a magnetic stirrer was used to stir at a constant temperature (60°C) until the polycaprolactone was completely dissolved;
[0045] (2) Then, according to the doping amount of 25 wt.%, 0.238 g of Li 6.3 LqCy 1.65 W 0.35 O 12 , add to the above solution, continue to stir evenly, and the stirring process is accompanied by ultrasonic treatment;
[0046] (3) Finally, the stirred composite polymer layer 1 slurry was evenly coated on a glass plate using a scraper, and the scraper was set to 500 μm. The coated glass plate was placed in a ventilated place to dry for 24 h to obtain a composite polymer layer 1; the composite polymer layer 1 was cut into discs with a diameter of 19 mm using a slicer to obtain a single-layer solid electrolyte of Comparative Example 1 with a thickness of 70 μm.
[0047] Comparative Example 2
[0048] like Figure 1 As shown, in Comparative Example 2, the main layer 1 is used as a single-layer solid electrolyte, and its preparation process includes the following steps:
[0049] (1) First, weigh 0.57 g of a molecule with a number average molecular weight of 80,000 g·mol -1 0.144 g of LiTFSI with a lithium-oxygen ratio of Li:O=1:20 was weighed into a clean beaker, 1 mL of dimethyl carbonate was added, and a magnetic stirrer was used to stir at a constant temperature (60°C) until the polycaprolactone was completely dissolved;
[0050] (2) Then, according to the doping amount of 35 wt.%, 0.3844 g of Li 6.3 LqCy 1.65 W 0.35 O 12 , add to the above solution, continue to stir evenly, and the stirring process is accompanied by ultrasonic treatment;
[0051] (3) Finally, the stirred composite polymer layer 1 slurry was evenly coated on a glass plate using a scraper, and the scraper was set to 500 μm. The coated glass plate was placed in a ventilated place to dry for 24 h to obtain a composite polymer layer 1; the composite polymer layer 1 was cut into discs with a diameter of 19 mm using a slicer to obtain a single-layer solid electrolyte of Comparative Example 2 with a thickness of 70 μm.
[0052] Comparative Example 3
[0053] like Figure 1 As shown, in Comparative Example 3, the main layer 1 is used as a single-layer solid electrolyte, and its preparation process includes the following steps:
[0054] (1) First, weigh 0.57 g of a molecule with a number average molecular weight of 80,000 g·mol -1 0.144 g of LiTFSI with a lithium-oxygen ratio of Li:O=1:20 was weighed into a clean beaker, 1 mL of dimethyl carbonate was added, and a magnetic stirrer was used to stir at a constant temperature (60°C) until the polycaprolactone was completely dissolved;
[0055] (2) Then, according to the doping amount of 45 wt.%, 0.5842 g of Li 6.3 LqCy 1.65 W 0.35 O 12 , add to the above solution, continue to stir evenly, and the stirring process is accompanied by ultrasonic treatment;
[0056] (3) Finally, the stirred slurry was evenly coated on a glass plate with a scraper set to 500 μm. The coated glass plate was placed in a ventilated place to dry for 24 h to obtain a composite polymer layer 1. The composite polymer layer 1 was cut into discs with a diameter of 19 mm with a slicer to obtain a single-layer solid electrolyte of Comparative Example 3 with a thickness of 70 μm.
[0057] The following Example 1 provides a double-layer composite solid electrolyte.
[0058] Example 1
[0059] like Figure 2 As shown, Example 1 is a double-layer composite solid electrolyte prepared by using a composite polymer layer 1 filled with active fillers as the main layer 1 and a composite polymer layer 2 filled with inert fillers as the modified layer 2, and its preparation process includes the following steps:
[0060] S1: First, weigh 0.57 g of a molecule with a number average molecular weight of 80,000 g·mol -1 0.144 g of LiTFSI with a lithium oxygen ratio of Li:O=1:20 was weighed and placed in a clean beaker. 1 mL of dimethyl carbonate was added and stirred at a constant temperature (60°C) with a magnetic stirrer until the polycaprolactone was completely dissolved. Then, 0.3844 g of Li 2 O 2 hydrated with water was weighed and dried in a vacuum oven at a doping amount of 35 wt.%. 6.3 LqCy 1.65 W 0.35 O 12 , add to the above solution, continue to stir evenly, and the stirring process is accompanied by ultrasonic treatment; finally, the stirred composite polymer layer 1 slurry is evenly coated on the glass plate with a scraper, and the scraper is set to 500 μm. The coated glass plate is placed in a ventilated place to dry for 24 hours to obtain the main layer 1;
[0061] S2: First, weigh 0.57 g of a number average molecular weight of 80,000 g·mol -10.144 g of LiTFSI with a lithium-oxygen ratio of Li:O=1:20 was weighed and placed in a clean beaker, 1 mL of dimethyl carbonate was added, and a magnetic stirrer was used to stir at a constant temperature (60°C) until the polycaprolactone was completely dissolved; then, 0.1785 g of Al2O3 was weighed according to an addition amount of 20 wt.%, added to the above solution, and continued to stir evenly, and the stirring process was accompanied by ultrasonic treatment; finally, the stirred composite polymer layer 2 slurry was evenly coated on the surface of the dried main layer 1 with a scraper, and the scraper was set to 100 μm, and the coated glass plate was placed in a ventilated place to dry for 24 h; finally, it was cut into discs with a diameter of 19 mm using a slicer to obtain the double-layer composite solid electrolyte of Example 1, with a main layer thickness of 70 μm and a modified layer thickness of 5 μm.
[0062] The following Example 2 provides a solid-state lithium metal battery.
[0063] Example 2
[0064] like Figure 3 As shown, Example 2 is a lithium iron phosphate positive electrode ( Figure 3 LiFePO4) and lithium anode ( Figure 3 Limental in), double-layer composite solid electrolyte of Example 1 ( Figure 3 Middle 6.3 LqCy 1.65 W 0.35 O 12 A solid-state lithium metal battery assembled with Composite Polymer Layer as the main layer 1 and LiOH / Al2O3 Composite Polymer Layer as the modification layer 2).
[0065] Effect verification
[0066] The single-layer solid electrolytes of Comparative Examples 1-3 and the double-layer composite solid electrolyte of Example 1 were tested. The test results are as follows: Figure 4 , 5 shown.
[0067] Among them, Figure 4 The temperature-dependent ionic conductivity diagram shows: Comparative Example 1 (Li 6.3 LqCy 1.65 W 0.35 O 12 The ionic conductivity of the doping amount is 25 wt.%) is 2.40×10 -6 S cm -1 , Comparative Example 2 (Li 6.3 LqCy 1.65 W 0.35 O12 The ionic conductivity of the doping amount is 35wt.%) is 7.94×10 -6 S cm -1 , Comparative Example 3 (Li 6.3 LqCy 1.65 W 0.35 O 12 The ionic conductivity of the doping amount is 45wt.%) is 1.78×10 -6 S cm -1 , indicating that when the Li 6.3 LqCy 1.65 W 0.35 O 12 When the incorporation amount is 35 wt.%, the performance is the best.
[0068] Among them, Figure 5 The temperature-dependent ionic conductivity diagram shows that the ionic conductivity of the double-layer composite solid electrolyte of Example 1 reaches 3.62×10 -5 S cm -1 , which is better than the single-layer solid electrolytes of Comparative Examples 1 to 3. The lithium ion transference number of the double-layer composite solid electrolyte of Example 1 is 0.55, and its electrochemical stability window is >5 V, which can be used as an ideal electrolyte for high-voltage materials.
[0069] The solid-state lithium metal battery of Example 2 was subjected to a performance test. The test results are as follows: Figure 6 , 7 , as shown in Figure 8.
[0070] The 0.1~1 C rate performance test results of the solid-state lithium metal battery of Example 2 are as follows: Figure 6 As shown by Figure 6 It can be obtained that the rate cycling of the all-solid-state lithium metal battery of Example 2 at 0.1~1 C shows that with the increase of the rate, its discharge specific capacity decays slightly and slowly.
[0071] Among them, the long cycle curve of the solid-state lithium metal battery of Example 2 at 1 C for 300 cycles is as follows: Figure 7 As shown by Figure 7 It can be obtained that the capacity retention rate of the all-solid-state lithium metal battery of Example 2 is 95% after 300 cycles at 1 C, and the coulombic efficiency is stable at more than 99%.
[0072] The SEM image of the lithium negative electrode surface of the solid-state lithium metal battery after cycling in Example 2 is as follows: Figure 8 As shown by Figure 8 It can be obtained that the surface of the lithium negative electrode is dense and flat after the cycle, indicating that a dense oxide film is formed on the surface of the lithium negative electrode, which can effectively inhibit the growth of lithium dendrites, thereby improving the cycle stability and service life of the battery.
[0073] In summary, compared with the solid electrolytes and batteries in the prior art, the double-layer structure composite solid electrolyte and the solid-state lithium metal battery prepared by the present invention have better performance, excellent rate performance and long cycle stability, and the electrochemical window is >5 V, and can be used as an ideal high-voltage electrolyte material in solid-state lithium metal batteries.
[0074] The present invention has many specific application paths, and the above is only a preferred embodiment of the present invention. It should be pointed out that the above embodiments are only used to illustrate the present invention, and are not used to limit the protection scope of the present invention. For those of ordinary skill in the art, several improvements can be made without departing from the principle of the present invention, and these improvements should also be regarded as the protection scope of the present invention.
Claims
1. A double-layer composite solid electrolyte, characterized in that: The solid electrolyte is a double-layer structure composed of a composite polymer layer 1 filled with active fillers as a main layer (1) and a composite polymer layer 2 filled with inert fillers as a modification layer (2); wherein the composite polymer layer 1 comprises active fillers, polycaprolactone, and lithium salt, and the composite polymer layer 2 comprises inert fillers, polycaprolactone, and lithium salt. The thickness of the main layer (1) is 70 μm, and the thickness of the modification layer (2) is 5 μm. The main layer (1) is a composite polymer layer 1 prepared by mixing active fillers with polycaprolactone and lithium salt by a hot solvent coating method; the modification layer (2) is a composite polymer layer 2 prepared by mixing inert fillers with polycaprolactone and lithium salt by a hot solvent coating method and coating the surface of the main layer (1). The active filler is Li 6.3 Ln3Z 1.65 W 0.35 O 12 , the inert filler is Al2O3, and the lithium salt is LiTFSI.
2. The double-layer composite solid electrolyte according to claim 1, characterized in that: The active filler is added in an amount of 20-50% of the total mass of the active filler, polycaprolactone and lithium salt, and the number average molecular weight of the polycaprolactone is 10000-100000 g·mol -1 The lithium-oxygen ratio Li:O of the lithium salt and polycaprolactone is 1:1-100.
3. The double-layer composite solid electrolyte according to claim 1, characterized in that: The inert filler is added in an amount of 5-30% of the total mass of the inert filler, polycaprolactone and lithium salt, and the number average molecular weight of the polycaprolactone is 10000-100000 g·mol -1 The lithium-oxygen ratio Li:O of the lithium salt and polycaprolactone is 1:1-100.
4. The double-layer composite solid electrolyte according to claim 2, characterized in that: The active filler is added in an amount of 35% of the total mass of the active filler, polycaprolactone and lithium salt, and the number average molecular weight of the polycaprolactone is 80000 g·mol -1 The lithium-oxygen ratio Li:O of the lithium salt and polycaprolactone is 1:
20.
5. The double-layer composite solid electrolyte according to claim 3, characterized in that: The inert filler is added in an amount of 20% of the total mass of the inert filler, polycaprolactone and lithium salt, and the number average molecular weight of the polycaprolactone is 80000 g·mol -1 The lithium-oxygen ratio Li:O of the lithium salt and polycaprolactone is 1:
20.
6. A process for preparing a double-layer composite solid electrolyte according to any one of claims 1 to 5, characterized in that: The steps include: S1: polycaprolactone and lithium salt are mixed, a solvent is added, and the mixture is stirred at a temperature of 50-70°C until the polycaprolactone is completely dissolved; then, an active filler that has been fully dried in a vacuum drying oven is added, and the stirring is continued, and the stirring process is accompanied by ultrasonic treatment to obtain a composite polymer layer 1 slurry, and the composite polymer layer 1 slurry is evenly coated on a glass plate, and the coated glass plate is placed in a ventilated place to dry for 10-30 hours to obtain a composite polymer layer 1, and the composite polymer layer 1 is cut to obtain a main layer (1); S2: polycaprolactone and lithium salt are mixed, a solvent is added, and the mixture is stirred at a temperature of 50-70°C until the polycaprolactone is completely dissolved; then, an inert filler is added and the stirring is continued, and the stirring process is accompanied by ultrasonic treatment to obtain a composite polymer layer II slurry, and the composite polymer layer II slurry is evenly coated on the surface of the main layer (1). After coating, the mixture is placed in a ventilated place to dry for 10-30 hours to obtain a composite polymer layer II, and then cut to obtain a solid electrolyte.
7. The preparation process of a double-layer composite solid electrolyte according to claim 6, characterized in that: The solvent in steps S1 and S2 is dimethyl carbonate; the stirring is carried out at a temperature of 60° C. in steps S1 and S2; the coating in steps S1 and S2 is carried out by scraper coating; and the drying is carried out in a ventilated place for 24 hours in steps S1 and S2.
8. The use of a double-layer composite solid electrolyte according to any one of claims 1 to 5, characterized in that: The solid electrolyte is applied to a solid-state lithium metal battery; the solid electrolyte is assembled with a positive electrode and a negative electrode to obtain a solid-state lithium metal battery.