Production technology of multi-layer cylinder with ribbed tubes for high modulus polypropylene integrated pump station
Through the ribbed tube multi-layer cylinder production process of high-modulus polypropylene integrated pump station, combined with block copolymerized polypropylene, styrene-butadiene transparent impact resin and other materials and reinforced materials, the problem of polypropylene cylinders in the existing technology has been solved. The problem of poor body and ring stiffness has been solved by achieving high bending resistance and improving ring stiffness, making it suitable for integrated pump stations.
Patent Information
- Application Number
- CN202311422443.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-31
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-10-31
AI Technical Summary
The existing integrated pump station cylinder material has problems such as non-degradability, non-recyclability, poor corrosion resistance and durability, electrical conductivity and safety hazards. In addition, the polypropylene material has poor ring stiffness and is easily deformed and damaged.
The ribbed tube multi-layer cylinder production process of the high-modulus polypropylene integrated pump station is used, by configuring block copolymer polypropylene, styrene-butadiene transparent impact resin, composite filler, paraffin, and 2-naphthylphosphate monosodium Salt and 2,2'-methylenebis(4,6-di-tert-butylphenyl) sodium phosphate and other components are combined with reinforcing materials and hot press annealing process to prepare high bending resistance and ring stiffness. Polypropylene barrel.
It achieves a significant improvement in the high modulus, bending resistance and ring stiffness of the polypropylene cylinder, which is suitable for integrated pump stations, solves the corrosion resistance and safety hazards of traditional materials, and improves the physical deformation resistance of the material. and mechanical properties.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of new materials, and in particular to a production process for a ribbed tube multilayer cylinder of a high modulus polypropylene integrated pump station. Background Art
[0002] Integrated pumping station is equipment for lifting and draining sewage, rainwater, drinking water, wastewater, etc. Currently, the types of integrated pumping station cylinder materials on the market mainly include fiberglass, stainless steel, carbon steel, polypropylene, etc.
[0003] The existing patent with authorization announcement number CN 102730952 B provides a glass tempering furnace and a glass tempering method, the main process method of which is to produce glass fiber reinforced plastics; however, the glass fiber reinforced plastics are non-degradable, non-recyclable, and environmentally unfriendly; and although metal materials such as stainless steel and carbon steel are not easy to deform, they have poor corrosion resistance and durability, and the materials are conductive and have safety hazards; although the current polypropylene material is corrosion-resistant, the ring stiffness of the material preparation cylinder is poor, and it is easy to deform and damage.
[0004] Therefore, a high modulus polypropylene integrated pump station cylinder structure is designed and prepared, so that the polypropylene cylinder has higher bending resistance and ring stiffness, and can better withstand external force and maintain its shape; in view of this, we propose a ribbed tube multi-layer cylinder production process for high modulus polypropylene integrated pump station. Summary of the invention
[0005] The purpose of the present invention is to solve the deficiencies mentioned in the above background technology and provide a production process for a ribbed tube multilayer cylinder of a high modulus polypropylene integrated pump station.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0007] The production process of the ribbed tube multilayer cylinder of the high modulus polypropylene integrated pump station, the specific production process steps of the cylinder are:
[0008] Step 1: preparing and mixing high modulus polypropylene barrel wall raw material components, mixing and extruding and granulating through a screw extruder to prepare a composite raw material masterbatch;
[0009] Step 2: Dry the composite raw material masterbatch, and inject the composite raw material masterbatch melt into the cylinder mold for preparing the cylinder lining through an injection molding machine;
[0010] The composite raw material masterbatch is based on polypropylene, and the polypropylene base material is block copolymer polypropylene. The specific mass proportions of each component are: 100 parts of block copolymer polypropylene, 24-28 parts of styrene-butadiene transparent impact-resistant resin, 6-7 parts of high-density polyethylene, 9-11 parts of composite filler, 2-4 parts of paraffin wax, 1.8-2 parts of 2-naphthyl phosphate monosodium salt, 0.2-0.3 parts of 2,2'-methylene bis (4,6-di-tert-butylphenyl) sodium phosphate, and 0.4-0.6 parts of calcium stearate;
[0011] Step 3: Cool and demould the barrel liner, rotate the barrel liner, and apply tackifying resin on the surface of the barrel liner;
[0012] Step 4: Continuously wind the reinforcement material on the surface of the cylinder lining to form a reinforcement layer, and then coat the tackifying resin on the reinforcement layer again;
[0013] Step 5: insert the structure of step 4 into the cylinder mold for preparing the cylinder outer lining, and inject the composite raw material masterbatch molten material into the mold through injection molding by an injection molding machine;
[0014] Step six: Cool and demould, apply hot pressing annealing process and then naturally cool to room temperature to obtain a ribbed tube multilayer cylinder of a high modulus polypropylene integrated pump station. The specific steps of the hot pressing annealing process are: place the demoulding cylinder at an ambient temperature of 110-125°C, and seal it with 8-12MPa air pressure, maintain the pressure for 1.5-2h, cool it naturally, and then release the pressure and take it out.
[0015] Preferably, the cylinder adopts {A(CBC)} n A layered structure;
[0016] Wherein: A is the inner lining or outer lining of the cylinder made of composite raw material masterbatch;
[0017] B is a reinforcing rib layer; C is a tackifying resin; and n is a positive integer value of 1, 2, or 3.
[0018] Preferably, the mass fraction ratio of the butadiene-styrene transparent impact-resistant resin to the high-density polyethylene is set to 4:1.
[0019] Preferably, the composite filler comprises a hydroxyl-containing inorganic filler and hexagonal boron nitride with a particle size of 5-15 μm and an equal mass ratio, and the hydroxyl-containing inorganic filler comprises talc powder, calcined kaolin and mica powder in a mass ratio of 2-2.5:1:1.
[0020] Preferably, the hydroxyl-containing inorganic filler is subjected to a modification process, and the specific process steps are: drying the hydroxyl-containing inorganic filler, preparing an anhydrous ethanol modification solution containing 0.8-1.2wt% of n-octyltriethoxysilane, immersing the hydroxyl-containing inorganic filler and stirring for 30-40 minutes, and drying at 110-120°C.
[0021] Preferably, the composite raw material masterbatch extrusion granulation production process is specifically as follows: after mixing the raw materials of each component, the extrusion granulation is carried out through a twin-screw extruder, and seven temperature sections are set in sequence to 200±1℃, 205±1℃, 220±1℃, 235±5℃, 235±5℃, 230±5℃, and 205±5℃, the screw feeding speed is 20r / min; the main engine screw speed is 200r / min.
[0022] Preferably, the specific production process of the injection molding process of the injection molding machine is: setting three injection molding temperature intervals in sequence: 225±2°C, 215±2, 205±2°C, and setting the injection pressure to 120-135MPa and holding the pressure for 30-60S.
[0023] Preferably, the production process of the reinforcement material is as follows: adding 3-8% by mass of nano silicon powder to glass raw materials, and controlling the particle size of the nano silicon powder to be 35-100 nm;
[0024] The temperature is raised to 1100-1250°C for melt blending, and the fiber diameter is controlled to be 20-35 μm by fiber drawing.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The production process of the ribbed tube multilayer cylinder of the high modulus polypropylene integrated pump station can produce and prepare a high modulus polypropylene multilayer cylinder with good bending resistance and ring stiffness, which is suitable for the integrated pump station; the cylinder structure can strengthen and improve the physical deformation resistance of the polypropylene material itself by combining high-density polyethylene, styrene-butadiene transparent impact-resistant resin and composite filler;
[0027] Importantly, in this production process, the monosodium 2-naphthyl phosphate and sodium 2,2'-methylenebis(4,6-di-tert-butylphenyl) phosphate can cross-link with the hydroxyl-containing inorganic filler and the chemical structure of the polypropylene substrate, solving the problem of poor compatibility of traditional fillers while enabling them to obtain a cross-linked connecting bond structure, thereby improving the material modulus; and the hot pressing annealing process applied at the end of the production process can further improve the crystallinity of polypropylene and the adhesion effect of the intermediate tackifying resin, increase the mechanical properties of the overall structure, and facilitate obtaining a stable high modulus structure. DETAILED DESCRIPTION
[0028] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. In the absence of conflict, the embodiments in this application and the features in the embodiments can be combined with each other. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work belong to the scope of protection of the present invention.
[0029] The present invention describes the above technical solution in detail through the following embodiments:
[0030] Example 1
[0031] The production process of the multi-layer cylinder with ribbed tubes of the high modulus polypropylene integrated pump station. The cylinder of this embodiment adopts a multi-layer structure of cylinder inner lining-thickening resin-reinforcing rib layer-thickening resin-cylinder outer lining. The specific production process of the cylinder includes the preparation of composite raw material masterbatch of the cylinder inner lining and the cylinder outer lining.
[0032] The composite raw material masterbatch is based on polypropylene, specifically block copolymer polypropylene. The components of the high modulus polypropylene cylinder wall raw material are weighed according to the following proportions:
[0033] Block copolymer polypropylene SB9310: 100 parts;
[0034] Butadiene-styrene transparent impact-resistant resin KR03: 28 parts;
[0035] High density polyethylene DMDA8008: 7 parts;
[0036] Composite filler: 10.5 parts;
[0037] Paraffin 10#: 3 parts;
[0038] 2-Naphthyl phosphate monosodium salt: 2 parts;
[0039] Sodium 2,2'-methylenebis(4,6-di-tert-butylphenyl)phosphate: 0.3 parts;
[0040] Calcium stearate: 0.5 parts.
[0041] The composite filler includes a hydroxyl-containing inorganic filler and hexagonal boron nitride with a particle size of 15 μm and a mass ratio of 1:1, and the hydroxyl-containing inorganic filler includes talc powder of Dongguan Jinxin Powder Technology Co., Ltd., calcined kaolin of Shijiazhuang Yitian Mineral Products Co., Ltd., and mica powder of Guangzhou Yifeng Chemical Technology Co., Ltd. in a mass ratio of 2:1:1; it should be noted that the hydroxyl-containing inorganic filler in this embodiment is subjected to a modification treatment process, and the specific process steps are: drying the hydroxyl-containing inorganic filler, preparing an anhydrous ethanol modification solution containing 1wt% of n-octyltriethoxysilane, controlling the material-liquid ratio to 1:2, immersing the hydroxyl-containing inorganic filler and stirring for 30 minutes, and drying at 110°C for 8 hours.
[0042] First of all, it should be noted that the composite filler added in this embodiment can increase the modulus of polypropylene. Its physical enhancement as a filler is well known. Although inorganic fillers can significantly improve the ring stiffness of the matrix resin, there are obvious problems in the filler filling process: filler particles are prone to agglomeration, blending is prone to incompatibility, and uniformity is hindered. Therefore, dispersion problems and interface compatibility problems need to be considered. Therefore, most of them currently use silane coupling agents for surface modification to reduce the surface polarity of the filler. However, the two only eliminate or reduce the polar repulsive force, and there is no bonding connection relationship to improve the overall structural stability.
[0043] Therefore, it is worthwhile to explain the production process in detail. The production process of the multi-layer cylinder with ribs of the high modulus polypropylene integrated pump station of this embodiment has outstanding creativity in that the modified talcum powder, calcined kaolin and mica powder used in the composite filler all have rich hydroxyl structures on the surface; at the same time, polypropylene also contains chemical functional group structures such as hydroxyl groups. The key point is that in this production process, 2-naphthyl phosphate monosodium salt and 2,2'-methylene bis (4,6-di-tert-butylphenyl) phosphate sodium both contain multiple active phosphate groups, which can react with polypropylene and hydroxyl-containing Chemical cross-linking structures occur between inorganic fillers; different from the traditional polarity elimination process, a cross-linking structure is creatively obtained between the filler and polypropylene, which can cooperate with the modified structure to reduce the polar repulsive force, and then increase the modulus of the cylinder material; the purpose of blending butadiene transparent impact-resistant resin KR03 produced by Chevron Philips in South Korea and high-density polyethylene DMDA8008 produced by Dushanzi Petrochemical is to improve the mechanical properties of the matrix and the modulus of the material itself, and calcium stearate is used to cross-link the molecular chains between it and polypropylene, promote crystallization during hot melt injection molding, and increase stiffness and modulus strength.
[0044] The production process of the reinforcement material is as follows: use 325 mesh high boron glass powder raw material from Hebei Xinxu Mineral Products Co., Ltd., and add 8% by mass of nano silicon powder DK-Si-001 from Beijing Dekedaojin Technology Co., Ltd.; heat to 1250°C for melt blending, draw and fiberize to control the fiber diameter to 30μm, and 120 strands are combined into yarn.
[0045] The above components are mixed, extruded and granulated through a twin-screw extruder to prepare a composite raw material masterbatch; the extrusion granulation production process is specifically as follows: the HT-30 twin-screw extruder is used to mix and extrude the raw materials of the various components, and seven temperature sections are set in sequence at 200°C, 205°C, 220°C, 235°C, 235°C, 230°C, and 205°C, and the screw feeding speed is 20r / min; the main engine screw speed is 200r / min, and the granulation is dried at 80°C for 12 hours before use, because the increase of fillers in the raw material components and the addition of butadiene transparent impact-resistant resin KR03 and high-density polyethylene will increase the hot-melt glass transition temperature, and the above temperature sections can fully hot-melt the mixed raw materials.
[0046] Then, a CJ80E injection molding machine was used for injection molding, and three injection molding temperature intervals were set in sequence: 225°C, 215°C, and 205°C, and the injection pressure was set to 135MPa and the pressure holding time was 60S. In the injection molding process, the composite raw material masterbatch melt was first injected into the barrel mold for preparing the barrel lining, cooled and demolded, the barrel lining was rotated, and ExxonMobil Chemical Escorez 1102 tackifying resin was coated on the surface of the barrel lining; reinforcing materials were continuously wound on the surface of the barrel lining to form a reinforcing rib layer, and ExxonMobil Chemical Escorez 1102 tackifying resin was coated on the reinforcing rib layer again; then it was inserted into the barrel mold for preparing the barrel lining, and the barrel lining was obtained by injection molding again through the injection molding machine.
[0047] After cooling, demoulding is performed and a hot pressing annealing process is applied. The specific steps of the hot pressing annealing process are: placing the demoulding cylinder at an ambient temperature of 115°C and sealing it with an air pressure of 8MPa. After maintaining the pressure for 2 hours, naturally cooling it and then releasing the pressure to obtain a ribbed tube multi-layer cylinder of a high modulus polypropylene integrated pump station.
[0048] It should be explained that the creative hot pressing annealing process is also an important factor affecting the modulus performance of the polypropylene. The purpose of the hot pressing annealing process is to make the molecular chains entangled with each other and secondary crystallized by applying temperature and hot pressing, thereby improving the internal crystallinity between molecules, which is beneficial to improving the modulus. At the same time, the hot pressing annealing process temperature of this embodiment is lower than the hot melting temperature of the cylinder, close to the hot melting temperature of the Escorez 1102 tackifying resin. Under hot pressing conditions, the bonding strength of the connecting layer can be increased, which is beneficial to obtaining a stable overall cylinder structure.
[0049] Example 2
[0050] The production process of the ribbed tube multilayer cylinder of the high modulus polypropylene integrated pump station of this embodiment is different from that of Example 1 only in that the modification process of the hydroxyl-containing inorganic filler in this embodiment adopts an anhydrous ethanol modification solution containing 10wt% of n-octyltriethoxysilane, and other conditions are the same.
[0051] Example 3
[0052] The production process of the ribbed tube multilayer cylinder of the high modulus polypropylene integrated pump station of this embodiment is different from that of Example 1 only in that the composite filler of this embodiment does not contain hexagonal boron nitride, and other conditions are the same.
[0053] Example 4
[0054] The production process of the ribbed tube multilayer cylinder of the high modulus polypropylene integrated pump station of this embodiment is different from that of Example 1 only in that 35 parts by mass of butadiene transparent impact-resistant resin KR03 is provided in this embodiment, and other conditions are the same.
[0055] Example 5
[0056] The production process of the ribbed tube multilayer cylinder of the high modulus polypropylene integrated pump station of this embodiment is different from that of Example 1 only in that this embodiment is provided with only 35 parts by mass of high-density polyethylene DMDA8008, and other conditions are the same.
[0057] Comparative Example 1
[0058] The production process of the ribbed tube multilayer cylinder of the high modulus polypropylene integrated pump station in this comparative example is different from that in Example 1 only in that: this comparative example does not add 2-naphthyl phosphate monosodium salt and 2,2'-methylene bis(4,6-di-tert-butylphenyl) sodium phosphate, and other conditions are the same.
[0059] Comparative Example 2
[0060] The production process of the ribbed tube multilayer cylinder of the high modulus polypropylene integrated pump station in this comparative example is different from that in Example 1 only in that no composite filler is added in this comparative example, and other conditions are the same.
[0061] Comparative Example 3
[0062] The production process of the ribbed tube multilayer cylinder of the high modulus polypropylene integrated pump station in this comparative example is different from that in Example 1 only in that the hot pressing annealing process is not applied in this comparative example, and other conditions are the same.
[0063] Comparative Example 4
[0064] The production process of the ribbed tube multilayer cylinder of the high modulus polypropylene integrated pump station in this comparative example is different from that in Example 1 in that: this comparative example adopts a blank control, the composite raw material masterbatch only uses block copolymer polypropylene, no other components are added, and no hot pressing annealing process is applied, and other conditions are the same.
[0065] According to Examples 1-5 and Comparative Examples 1-4, test specimens were prepared to test and determine the modulus performance, with specific reference to ASTM D 790-03 "Standard Test Method for Flexural Properties of Unreinforced and Reinforced Plastics and Electrical Insulating Materials 1"; the recommended specimen size was 127×12.7×3.2 mm, and in order to facilitate testing, the cylinder lining-tackifying resin-reinforcement rib layer-tackifying resin-cylinder lining were 1.3 mm, 0.1 mm, 0.4 mm, 0.1 mm, and 1.3 mm thick respectively; the support span-depth ratio was 16;
[0066] The test extreme value is when the specimen is deformed until the outer surface of the specimen breaks, or until the maximum strain reaches 5.0%, whichever occurs first. The elastic modulus of each specimen is tested. The specific data are as follows: Table 1 and Table 2:
[0067] Table 1:
[0068]
[0069] Table 2:
[0070]
[0071] First, from the comparison of the test data of the samples in Table 1 and Table 2, it can be seen that the elastic modulus is a physical quantity that describes the bending resistance of a material under stress. The layered cylinder structure has a significantly higher elastic modulus than traditional polypropylene. The elastic modulus is directly proportional to the ring stiffness of the cylinder. The higher the elastic modulus, the stronger the ring stiffness. That is, the multi-layer cylinder used as an integrated pump station has better anti-deformation ability.
[0072] Specifically, the data of Example 2 show that the concentration of the modified solution also affects the modulus. Considering that the excessive modified concentration reacts chemically with the filler surface during the modification process, the sites for cross-linking of the phosphate group in the component are reduced or decreased, thereby weakening the cross-linking structural relationship with polypropylene. Therefore, sufficient modification will not improve the modulus, and Example 1 is preferred; Example 3 illustrates that the filler added in an appropriate amount plays a role in improving the modulus, and its hexagonal boron nitride has high hardness physical properties; Examples 4 and 5 illustrate that both butadiene transparent impact-resistant resin KR03 and high-density polyethylene have the ability to significantly improve the modulus, but their single setting cannot achieve the most effective effect, although the gap is not obvious, the ratio of Example 1 can be preferred;
[0073] Comparative Example 2 shows that the two components affect the modulus, and the combination of Comparative Example 2 shows that the modulus changes greatly without adding composite fillers; Comparative Example 3 shows that the hot pressing annealing process has a smaller impact, but it is indispensable and has important significance for further improving the peak value; among them, Comparative Examples 1-3 show that the conditions of each comparative example have an impact on the modulus compared with Comparative Example 4, and the best effect can be obtained by coordinated cooperation, and Example 1 is preferred.
[0074] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
Claims
1. The production process of multi-layer ribbed tube cylinder of high modulus polypropylene integrated pump station is characterized by: The specific production process steps of the cylinder are: Step 1: preparing and mixing high modulus polypropylene barrel wall raw material components, mixing and extruding and granulating through a screw extruder to prepare a composite raw material masterbatch; Step 2: Dry the composite raw material masterbatch, and inject the composite raw material masterbatch melt into the cylinder mold for preparing the cylinder lining through an injection molding machine; The composite raw material masterbatch is based on polypropylene, and the polypropylene base material is block copolymer polypropylene. The specific mass proportions of each component are: 100 parts of block copolymer polypropylene, 24-28 parts of styrene-butadiene transparent impact-resistant resin, 6-7 parts of high-density polyethylene, 9-11 parts of composite filler, 2-4 parts of paraffin wax, 1.8-2 parts of 2-naphthyl phosphate monosodium salt, 0.2-0.3 parts of 2,2'-methylene bis (4,6-di-tert-butylphenyl) sodium phosphate, and 0.4-0.6 parts of calcium stearate; The composite filler comprises a hydroxyl-containing inorganic filler and hexagonal boron nitride with a particle size of 5-15 μm and an equal mass ratio, wherein the hydroxyl-containing inorganic filler comprises talc powder, calcined kaolin and mica powder with a mass ratio of 2-2.5:1:1; Step 3: Cool and demould the barrel liner, rotate the barrel liner, and apply tackifying resin on the surface of the barrel liner; Step 4: Continuously wind the reinforcement material on the surface of the cylinder lining to form a reinforcement layer, and then coat the tackifying resin on the reinforcement layer again; Step 5: insert the structure of step 4 into the cylinder mold for preparing the cylinder outer lining, and inject the composite raw material masterbatch molten material into the mold through injection molding by an injection molding machine; Step six: Cool and demould, apply hot pressing annealing process and then naturally cool to room temperature to obtain a ribbed tube multilayer cylinder of a high modulus polypropylene integrated pump station. The specific steps of the hot pressing annealing process are: place the demoulding cylinder at an ambient temperature of 110-125°C, and seal it with 8-12MPa air pressure, maintain the pressure for 1.5-2h, cool it naturally, and then release the pressure and take it out.
2. The process for producing a ribbed tube multilayer cylinder of a high modulus polypropylene integrated pump station according to claim 1, characterized in that: The cylinder adopts {A(CBC)} n A layered structure; Wherein: A is the inner lining or outer lining of the cylinder made of composite raw material masterbatch; B is a reinforcing rib layer; C is a tackifying resin; and n is a positive integer value of 1, 2, or 3.
3. The process for producing a ribbed tube multilayer cylinder of a high modulus polypropylene integrated pump station according to claim 1, characterized in that: The mass fraction ratio of the transparent butadiene-styrene impact-resistant resin to the high-density polyethylene is set to 4:
1.
4. The process for producing a ribbed tube multilayer cylinder of a high modulus polypropylene integrated pump station according to claim 1, characterized in that: The modification process of the hydroxyl-containing inorganic filler comprises the following specific steps: drying the hydroxyl-containing inorganic filler, preparing an anhydrous ethanol modification solution containing 0.8-1.2wt% of n-octyltriethoxysilane, immersing the hydroxyl-containing inorganic filler and stirring for 30-40 minutes, and drying at 110-120°C.
5. The process for producing a ribbed tube multilayer cylinder of a high modulus polypropylene integrated pump station according to claim 1, characterized in that: The composite raw material masterbatch extrusion granulation production process is specifically as follows: the raw materials of each component are mixed and then extruded and granulated through a twin-screw extruder, seven temperature sections are set in sequence to 200±1°C, 205±1°C, 220±1°C, 235±5°C, 235±5°C, 230±5°C, and 205±5°C, the screw feeding speed is 20r / min; the main engine screw speed is 200r / min.
6. The process for producing a ribbed tube multilayer cylinder of a high modulus polypropylene integrated pump station according to claim 1, characterized in that: The specific production process of the injection molding process of the injection molding machine is: setting three injection molding temperature intervals in sequence: 225±2℃, 215±2, 205±2℃, and setting the injection pressure to 120-135MPa and holding the pressure for 30-60S.
7. The process for producing a ribbed tube multilayer cylinder of a high modulus polypropylene integrated pump station according to claim 1, characterized in that: The production process of the reinforcement material is as follows: adding 3-8% of the mass fraction of the glass raw materials to the glass raw materials, and controlling the particle size of the nano silicon powder to 35-100nm; The temperature is raised to 1100-1250°C for melt blending, and the fiber diameter is controlled to be 20-35 μm by fiber drawing.
Citation Information
Patent Citations
Glass tempering furnace and glass tempering method
CN102730952B
Fiber reinforced thermoplastic compound pipeline and manufacturing technology thereof
CN104534187A
High-rigidity polypropylene composition
CN106893204A
Polypropylene corrugated pipe composite material and preparation method of composite polypropylene corrugated pipe
CN111040307A