Adhesives, insulating films using them, and battery modules
By using a binder containing adhesives, curing agents, solvents, and cyclic oligosaccharides, safety issues during the use of power batteries have been resolved, the vibration and impact resistance of battery modules has been improved, the risk of short circuits within the battery pack has been reduced, and vehicle safety has been enhanced.
Patent Information
- Application Number
- CN202280040507.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-26
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-05-26
AI Technical Summary
During use, due to the uncertainty of vehicle driving scenarios and impacts, power batteries are prone to collisions and impacts between battery cells and between battery cells and other components, which can lead to safety accidents.
An adhesive comprising an adhesive, a curing agent, a solvent, and 20-50% by weight of cyclic oligosaccharides is used to prepare an insulating film and to bond battery cells and battery cells to end plates/side plates, thereby enhancing the vibration resistance and impact resistance of the battery module.
It significantly improves the vibration and shock resistance of the battery module, reduces short circuits within the battery pack, and enhances the safety performance of the vehicle during operation.
Smart Images

Figure CN117480673B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of adhesive technology, and more particularly to an adhesive, an insulating film using the same, and a battery module. Background Technology
[0002] Lithium-ion power batteries are mainly used in electric vehicles. The common assembly form is: battery modules are composed of battery cells and accessories, and battery packs are composed of battery modules and accessories. These are then installed on the vehicle to provide power. Due to the uncertainty of vehicle driving scenarios and possible collisions, collisions and impacts can easily occur between battery cells within the battery module and between battery cells and other components, which can lead to safety accidents.
[0003] Therefore, how to solve the safety issues of power batteries during use is an urgent problem to be solved in this field. Summary of the Invention
[0004] This application is made in view of the above-mentioned problems, and its purpose is to provide an adhesive, an insulating film using the same, and a battery module, which aims to improve the problem of adhesive failure and improve the vibration resistance and shock resistance of the battery module.
[0005] The first aspect of this application provides an adhesive comprising:
[0006] The adhesive, curing agent, solvent, and 20% to 50% by weight of cyclic oligosaccharides, based on the total weight of the adhesive.
[0007] In any embodiment, the adhesive of this application comprises:
[0008] 5% to 50% by weight of adhesive, optionally 20% to 40% by weight;
[0009] 20% to 50% by weight of cyclic oligosaccharides, optionally 25% to 35% by weight;
[0010] 0.5% to 10% by weight of curing agent, optionally 1% to 5% by weight; 10% to 40% by weight of solvent, optionally 15% to 35% by weight; each based on the total weight of the adhesive.
[0011] In any embodiment, the cyclic oligosaccharides in the binder of this application are selected from one or more of α-cyclodextrin, β-cyclodextrin and γ-cyclodextrin.
[0012] In any embodiment, the adhesive in the adhesive of this application is selected from one or more of polyvinyl acetate, polyvinyl alcohol, chlorinated polyethylene, polyisobutylene, cellulose ester and polyacrylic acid; optionally, the number average molecular weight of the adhesive is 1,000-90,000, and optionally 5,000-50,000.
[0013] In any embodiment, the curing agent in the adhesive of this application is a polyamide curing agent.
[0014] In any embodiment, the solvent in the adhesive of this application is selected from one or more of carbon tetrachloride, ethyl acetate, methyl formate, ethanol, and toluene; optionally, the solvent is toluene.
[0015] In any embodiment, the adhesive of this application further comprises cellulose, the cellulose being selected from one or more of hydroxypropyl methylcellulose, methylcellulose, ethylcellulose, hydroxyethylcellulose, hydroxypropylcellulose and carboxymethylcellulose. Optionally, the cellulose content is from 2% to 25% by weight, or optionally from 3% to 20% by weight, based on the total weight of the adhesive.
[0016] A second aspect of this application provides an insulating film, including a base film and an organic coating on at least one surface of the base film, the organic coating including the adhesive described in the first aspect of this application, the thickness of the organic coating being 90μm-300μm, optionally 100μm-200μm.
[0017] In any embodiment, the base film is made of a polymer selected from at least one of the following polymers: polyethylene, polyvinyl chloride, polypropylene, and polyethylene terephthalate.
[0018] In any embodiment, the base film is a polyethylene terephthalate film, and the base film is hydroxylated.
[0019] A third aspect of this application provides a battery module, including side-by-side battery cells and end plates and side plates surrounding the battery cells, wherein the battery module satisfies at least one of the following conditions:
[0020] The battery casing of the battery cell is covered with the insulating film of the second aspect of this application;
[0021] The battery cells are bonded together, between the battery cells and the side plate, and between the battery cells and the end plate by the adhesive of the first aspect of this application.
[0022] A fourth aspect of this application provides a battery pack, including the battery module of the third aspect of this application, wherein the battery pack serves as a power source for an electrical device.
[0023] This application develops an adhesive with excellent bonding ability, shock resistance, and impact resistance. Battery modules using the adhesive exhibit significantly improved vibration resistance and impact resistance, significantly reduced short circuits within the battery pack, and significantly improved vehicle safety during operation.
[0024] The adhesive of this application may be used in battery packs in the following ways: Firstly, the adhesive is used as a coating component to prepare an insulating film, which is then wrapped around the surface of the battery cell casing to provide insulation and shock resistance. Secondly, during battery module assembly, the adhesive acts as an adhesive to bond the battery cells and the battery cells / battery cells to end plates / battery cells to side plates, further enhancing the robustness and shock resistance of the battery module. Battery packs using the aforementioned adhesive exhibit significantly improved vibration resistance and impact resistance, significantly reduced short circuits within the battery pack, and significantly improved vehicle safety. Attached Figure Description
[0025] Figure 1 The image shows the infrared spectrum of the base film of the insulating film according to one embodiment of this application.
[0026] Figure 2 This is an insulating film according to one embodiment of the present application, wherein the adhesive of the present application is coated on one side of the base film.
[0027] Figure 3 This is a schematic diagram of a battery module composed of battery cells according to an embodiment of this application, wherein the outer shell of the battery cells is covered with an insulating film.
[0028] Figure 4 This is a schematic diagram of a battery module assembled into a battery pack according to one embodiment of this application. Detailed Implementation
[0029] The following detailed description, with appropriate reference to the accompanying drawings, specifically discloses embodiments of the adhesive, insulating film using the adhesive, and power battery device of this application. However, unnecessary details may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided to enable those skilled in the art to fully understand this application and are not intended to limit the subject matter of the claims.
[0030] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60-120 and 80-110 are listed for a specific parameter, it is expected that ranges of 60-110 and 80-120 are also included. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5. In this application, unless otherwise stated, the numerical range "ab" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0-5" indicates that all real numbers between "0-5" have been listed in this article; "0-5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0031] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0032] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.
[0033] Unless otherwise specified, the terms "comprising" and "including" as used in this application can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.
[0034] Unless otherwise specified, the term "or" is inclusive in this application. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, the condition "A or B" is satisfied by any of the following conditions: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0035] To increase the stability of individual battery cells within the battery module, adhesives are typically used to bond the cells together when assembling the module. End plates and side plates are then secured to the cells using adhesives. Secondly, to enhance insulation between battery cells, an insulating film is applied to the surface of each cell's casing. However, during vehicle use, the battery pack is subjected to various vibrations over extended periods, which can cause the adhesive to detach, leading to displacement of the battery cells within the module. This, in turn, can damage the insulating film on the cell casing, resulting in short circuits between the cells and potentially causing a vehicle safety incident.
[0036] Based on the above-mentioned technical problems, this application focuses on increasing the bonding ability, shock resistance, and impact resistance between individual battery cells within the battery module. It develops an adhesive that combines excellent bonding ability with shock resistance and impact resistance. Battery modules using the adhesive exhibit significantly improved vibration resistance and impact resistance, significantly reduced short circuits within the battery pack, and significantly improved vehicle safety during operation.
[0037] [Adhesive]
[0038] Based on this, a first aspect of this application provides an adhesive comprising:
[0039] The adhesive, curing agent, solvent, and 20% to 50% by weight of cyclic oligosaccharides, based on the total weight of the adhesive.
[0040] The adhesive of this application may be used in battery packs in the following ways: Firstly, the adhesive is used as a coating component to prepare an insulating film, which is then wrapped around the surface of the battery cell casing to provide insulation and shock resistance. Secondly, during battery module assembly, the adhesive acts as an adhesive to bond the battery cells and the battery cells / battery cells to end plates / battery cells to side plates, further enhancing the robustness and shock resistance of the battery module. Battery packs using the aforementioned adhesive exhibit significantly improved vibration resistance and impact resistance, significantly reduced short circuits within the battery pack, and significantly improved vehicle safety.
[0041] Unbound by any particular theory, it is now believed that cyclic oligosaccharides, composed of several glucose units linked by 1,4-glycosidic bonds, possess a hollow cylindrical three-dimensional cyclic structure. This three-dimensional cyclic structure allows the cyclic oligosaccharide molecules to withstand repeated micro-strains in different directions without structural disintegration. The inner edge of the cyclic oligosaccharide ring is mainly composed of CH bonds, exhibiting hydrophobicity. These hydrophobic cavities can embed long-chain polymer compounds, further decomposing micro-stresses by forming a cross-linked network. Therefore, this cyclic oligosaccharide can improve the adhesion performance of binders under long-term vibration and impact strain, thereby giving battery modules excellent shock resistance and impact resistance.
[0042] In some embodiments, the adhesive of this application includes:
[0043] 5% to 50% by weight of adhesive, optionally 20% to 40% by weight;
[0044] 20% to 50% by weight of cyclic oligosaccharides, optionally 25% to 35% by weight;
[0045] 0.5% to 10% by weight of curing agent, optionally 1% to 5% by weight; 10% to 40% by weight of solvent, optionally 15% to 35% by weight; each based on the total weight of the adhesive.
[0046] In some embodiments, the content of the cyclic oligosaccharide is 20% to 50% by weight, optionally 25% to 35% by weight, and more preferably 28% to 32% by weight, based on the total weight of the binder.
[0047] Both excessively high and low levels of cyclic oligosaccharides can significantly reduce the adhesive's bonding effectiveness under prolonged vibration and impact strain. Only when the content is within a suitable range can the adhesive maintain good bonding performance and avoid failure under prolonged vibration and impact strain.
[0048] In some embodiments, the cyclic oligosaccharide has the following general formula:
[0049]
[0050] The R is selected from one or more of hydrogen atom, NH2, C1-C6 alkyl, C1-C6 alkyl carbonyl and C1-C6 alkyl hydroxyl, and n is an integer from 0 to 6, optionally an integer from 1 to 3; optionally, the cyclic oligosaccharide is selected from one or more of α-cyclodextrin, β-cyclodextrin and γ-cyclodextrin.
[0051] In this application, it is understood that “C1-C6 alkyl” refers to a straight-chain or branched hydrocarbon having 1 to 6 carbon atoms, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, pentyl, 1-methylbutyl, 2-methylbutyl, 3-methylbutyl, 1,2-dimethylpropyl, 1,1-dimethylpropyl, 2,2-dimethylpropyl, 1-ethylpropyl, hexyl, 1-methylpentyl, 2-methylpentyl, 3-methylpentyl, 4-methylpentyl, 1,2-dimethylpropyl, 1,3-dimethylbutyl, 1,4-dimethylbutyl, 2,3-dimethylbutyl, 1,1-dimethylbutyl, 2,2-dimethylbutyl, 3,3-dimethylbutyl, 1,1,2-trimethylpropyl, 1,2,2-trimethylpropyl, 1-ethylbutyl, and 2-ethylbutyl. Alkyl groups having 1 to 4 carbon atoms may also be selected, such as, in particular, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, or tert-butyl.
[0052] The different types of cyclic oligosaccharides can be purchased directly or synthesized directly using existing technologies.
[0053] In this application, it can be understood that "integers from 0 to 6" refers to integers of 0, 1, 2, 3, 4, 5, and 6.
[0054] In some embodiments, β-cyclodextrin with 7 glucose monomer molecules and γ-cyclodextrin with 8 glucose monomer molecules can also provide good vibration and impact strain resistance.
[0055] Furthermore, when the cyclic oligosaccharide is α-cyclodextrin, the corresponding number of glucose monomer molecules is 6, and its cavity size allows some long-chain polymers to pass through. When the number of glucose monomer molecules increases, its cavity size becomes larger, and the vibration resistance and impact strain resistance of cyclodextrin are correspondingly weakened. Therefore, α-cyclodextrin can provide better vibration resistance and impact strain resistance.
[0056] In some embodiments, the adhesive content is 20% to 50% by weight, optionally 25% to 40% by weight, and also optionally 26% to 35% by weight, based on the total weight of the adhesive.
[0057] By further adjusting the weight ratio of the adhesive within a suitable range, the bonding performance of the adhesive can be further improved, thereby enhancing the vibration resistance and strain resistance of the corresponding battery module.
[0058] In some embodiments, the adhesive is selected from one or more of polyvinyl acetate, polyvinyl alcohol, perchlorate, polyisobutylene, cellulose ester and polyacrylic acid.
[0059] In some embodiments, the number average molecular weight of the adhesive is 1,000-90,000, optionally 5,000-50,000, or even 5,500-20,000.
[0060] Maintaining the molecular weight distribution of the adhesive within a reasonable range ensures better adhesive uniformity and synergistic effects with other components, resulting in superior bonding and seismic performance. Conversely, low molecular weights weaken the bonding between adhesive molecules and between adhesive molecules and other components, rendering the adhesive ineffective. Conversely, excessively high molecular weights limit further enhancement of bonding performance, failing to significantly improve adhesive properties. In this application, the molecular weight range of the adhesive can be selected as 5500-20000.
[0061] In this application, the number average molecular weight was determined by gel permeation chromatography (GPC) according to GB / T 21863-2008 "Gel permeation chromatography (GPC) with tetrahydrofuran as eluent" (equivalent to German standard DIN 55672-1:2007 "Gel permeation chromatography (GPC) Part 1: with tetrahydrofuran (THF) as eluent").
[0062] In some embodiments, the degree of polymerization of the adhesive is 100-2000, optionally 200-1000, and more preferably 300-600.
[0063] Maintaining the degree of polymerization of adhesive molecules within a reasonable range results in better adhesive uniformity, better synergy with other components of the adhesive, and better adhesive bonding and seismic performance.
[0064] In some embodiments, the viscosity of the adhesive is 5000 mPa·s-15000 mPa·s.
[0065] When the viscosity of the adhesive is too low, the adhesive exhibits Newtonian fluid properties, resulting in poor film-forming properties and making it prone to missed coating during application. When the viscosity is too high, the adhesive has poor dispersibility and is prone to agglomeration, which also affects film-forming properties and leads to missed coating.
[0066] In this application, the viscosity of the adhesive can be tested at 25°C using a rotational method according to standard GB / T 10247-2008. The specific operation of this standard is as follows: Fill a beaker or sample container with the sample to be tested, ensuring no air bubbles are introduced; if necessary, vacuum to eliminate air bubbles. If the sample is volatile or hygroscopic, seal the beaker or sample container during the isothermal process. Place the prepared beaker or sample container in the isothermal bath, ensuring sufficient time to reach the specified temperature. Select a suitable rotor so that the reading is between 20% and 90% of the maximum range. For a 63# rotor, the following conditions should be met: 1000 mPa·s ≤ viscosity ≤ 10000 mPa·s, 20% ≤ torque percentage ≤ 90%. If the viscosity result is unsuitable, use a 64# rotor instead, which should simultaneously meet the following conditions: 10000 mPa·s < viscosity, 20% ≤ torque percentage ≤ 90%. During the test, the rotor groove should be flush with the slurry surface. Turn on the motor, and after 5 minutes when the instrument viscosity reading stabilizes, stop the motor. After the rotor stops, turn the motor on again to perform a second test. Repeat this process until the deviation of the two consecutive test data from the average value is no more than 3%. The result is the average of the two measurements.
[0067] In some embodiments, the adhesive composition further comprises cellulose, which is selected from one or more of hydroxypropyl methylcellulose, methylcellulose, ethylcellulose, hydroxyethylcellulose, hydroxypropylcellulose, and carboxymethylcellulose. Cellulose primarily functions as a crosslinking agent in the adhesive of this application, enabling organic molecules such as adhesives, cyclic oligosaccharides, and curing agents to crosslink through cellulose, further increasing the adhesive's bonding and shock-resistant properties.
[0068] In some embodiments, the cellulose content is 2% to 25% by weight, optionally 3% to 20% by weight, optionally 5% to 15% by weight, or optionally 8% to 12% by weight, based on the total weight of the binder.
[0069] In some embodiments, the cellulose is hydroxypropyl methylcellulose, which has hydroxyl, propyl, and methyl functional groups on its cellulose chain. The variety of functional groups enhances the cross-linking effect of nanocellulose in the binder, giving the binder good adhesion.
[0070] In some embodiments, the number-average molecular weight of the cellulose is 10,000-30,000, optionally 15,000 to 25,000.
[0071] In some embodiments, the cellulose is nanocellulose with a particle size Dv50 of 10nm-100nm, optionally 30nm-70nm.
[0072] When the Dv50 of nanocellulose is too low, it is not easy to disperse evenly in the binder system, which affects the cross-linking effect and thus the bonding performance and shock resistance of the binder. When the Dv50 of nanocellulose is too high, it is not easy to form a network structure with other polymer components in the binder system, which affects the cross-linking effect.
[0073] Furthermore, the Dv50 of nanocellulose is the same as that of α-cyclodextrin (typically 30-70 nm).
[0074] In this application, the particle size Dv50 of the nanocellulose can be determined using a laser particle size analyzer (such as a Malvern Master Size 3000) in accordance with standard GB / T 19077.1-2016. The physical definition of Dv50 is as follows:
[0075] Dv50: The particle size corresponding to a cumulative volume distribution percentage of 50%.
[0076] Those skilled in the art will understand that cellulose of other particle sizes can also be used, and ground to the desired particle size as needed, and the methods of grinding the particles are also well known to those skilled in the art.
[0077] Regardless of any theory, the inventors believe that cellulose can bind to the outer edge of cyclic oligomers through hydrogen bonding, and then form a cross-linked network through intermolecular interactions and adhesives and curing agents, thereby enabling the adhesive to maintain good bonding performance under long-term vibration and impact strain conditions.
[0078] In some embodiments, the weight ratio of adhesive: cyclic oligosaccharide: cellulose is (1.5-4):(1.5-5):1, optionally (2-3.5):(2-3.5):1, and further optionally (2.5-3.3):(2.5-3.3):1.
[0079] In some embodiments, the curing agent is a polyamide curing agent, such as Versamid 125 curing agent. Compared to other types of curing agents, amide curing agents have better curing properties and can impart good adhesion to the composition even in humid environments.
[0080] In some embodiments, the curing agent content is from 0.5% to 10% by weight, optionally from 1% to 5% by weight, and more preferably from 1.5% to 4% by weight, based on the total weight of the adhesive.
[0081] In some embodiments, the solvent is selected from one or more of carbon tetrachloride, ethyl acetate, methyl formate, ethanol, and toluene.
[0082] In some embodiments, the solvent is toluene. The components of the adhesive exhibit good dispersion in a toluene solution, resulting in optimal coating performance.
[0083] In some embodiments, the solvent content is 10% to 40% by weight, optionally 15% to 35% by weight, or 20% to 30% by weight, based on the total weight of the adhesive.
[0084] Solvents can promote the dispersion of components and the occurrence of cross-linking reactions. After coating, the solvent gradually evaporates, causing the binder to have an adhesive effect.
[0085] [Insulating film]
[0086] A second aspect of this application provides an insulating film comprising a base film and an organic coating on at least one surface of the base film, the organic coating comprising the adhesive described in the first aspect of this application, the organic coating having a thickness of 90 μm-300 μm, optionally 100 μm-200 μm.
[0087] In some embodiments, the base film is made of a polymer selected from at least one of the following polymers: polyethylene, polyvinyl chloride, polypropylene, and polyethylene terephthalate.
[0088] In this application, the coating method can be a method conventionally used in the art, such as a doctor blade casting method, with the doctor blade gap adjusted to 50 μm to 260 μm, or optionally 100 μm to 200 μm.
[0089] In some embodiments, the base film is a polymer film made of a polymer with a number average molecular weight of 20,000 to 30,000.
[0090] In some embodiments, the thickness of the base film is 50 μm to 300 μm, optionally 80 μm to 200 μm.
[0091] In some embodiments, the base film is hydroxylated.
[0092] In this application, the hydroxylation treatment can be performed as follows: a hydroxylating agent is coated onto the membrane surface (coating thickness can be 100-300 μm), and then reacted at 10℃-50℃, optionally 20℃-30℃, for 1 to 20 minutes, optionally 5 to 15 minutes. The treated surface is then washed with deionized water to remove the hydroxylating agent (e.g., using pH test paper to determine the membrane surface pH value; a pH value of 7.0 to 7.5 is considered to indicate that the hydroxylating agent has been removed). The hydroxylating agent can be one or more of 10 wt% to 60 wt% NaOH solution and 10 wt% to 60 wt% KOH solution; optionally, the hydroxylating agent is 10 wt% to 60 wt% NaOH solution, optionally 20 wt% to 40 wt% NaOH solution.
[0093] In some embodiments, the base film may also be pretreated before hydroxylation, such as by surface washing with ethanol and deionized water.
[0094] Introducing hydroxyl groups under alkaline conditions can avoid the influence of residual hydroxylation reagents on cyclodextrin molecules; a reasonable selection of the concentration range of the alkaline hydroxylation solution can also avoid damage to the base film.
[0095] In some embodiments, the base film is made of polyethylene terephthalate (PET). PET films have high chemical stability, but the PET molecular chain lacks hydrophilic groups, resulting in poor compatibility with most polymers. Hydroxylation treatment in an alkaline solution can improve the reactivity of the film surface, which is beneficial for the adhesive to adhere well to the PET film.
[0096] See Figure 2 It is the insulating film of this application, wherein the adhesive A of this application is coated on one side of the base film B.
[0097] [Battery Module]
[0098] A third aspect of this application provides a battery module comprising side-by-side battery cells and end plates and side plates surrounding the battery cells.
[0099] In some implementations, see Figure 3 , Figure 3 The battery module is composed of six battery cells arranged side by side, and the battery casing of each battery cell is covered with an insulating film according to the second aspect of this application.
[0100] In some implementations, see Figure 3 The battery module is bonded together with the battery cells, between the battery cells and the side plate S, and between the battery cells and the end plate E by the adhesive of the first aspect of this application.
[0101] This application does not impose any particular restrictions on the shape of the battery cell; it can be cylindrical, square, or any other arbitrary shape.
[0102] In some implementations, the battery module may contain one or more battery cells, and the specific number can be selected by those skilled in the art based on the application and capacity of the battery module.
[0103] In some embodiments, the above-mentioned battery modules can also be assembled into a battery pack, see [link to relevant documentation]. Figure 4 The battery pack may contain one or more battery modules, and the specific number can be selected by those skilled in the art based on the application and capacity of the battery pack.
[0104] The battery pack can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include, but is not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.
[0105] [Example]
[0106] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in the art or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.
[0107] Unless otherwise specified, all operations in this application are performed at room temperature (25°C) and normal pressure (101 kPa).
[0108] Example 1-1
[0109] Preparation of adhesives
[0110] The adhesive was prepared by mixing 30% by weight of polyacrylic acid (purchased from Maclean, P890197), 30% by weight of α-cyclodextrin (purchased from Maclean, C804818), 10% by weight of hydroxypropyl methylcellulose (purchased from Maclean, H811095), 28% by weight of toluene, and 2% by weight of Versamid 125 curing agent to obtain the adhesive of Example 1.
[0111] Preparation of insulating film
[0112] Step 1: Pre-treat the PET base film (100μm thick). Use ethanol as a cleaning agent, treat at room temperature (25℃, the same below) for 15 minutes, then rinse 3 times with deionized water, and air dry at room temperature.
[0113] Step 2: Hydroxylate the pretreated PET base film. The specific method is as follows: evenly coat both sides of the PET base film with a 30% by weight NaOH solution, react at room temperature for 10 minutes, rinse with deionized water until the surface of the PET base film is neutral (the pH value of the washing solution is 7.0 when measured with pH test paper), and air dry at room temperature.
[0114] Step 3: Apply the above adhesive evenly to both sides of the PET base film using a doctor blade (using a doctor blade casting machine, with the doctor blade gap adjusted to 125μm), with an organic layer thickness of 125μm.
[0115] Thus, the insulating film of Example 1 was obtained.
[0116] [Battery Module Fabrication]
[0117] 1. Prepare the end plates of the battery module and press them firmly on the assembly equipment; 2. Clean the battery cells, side plates, and end plates; 3. Cover the surface of the battery cells with insulating film (except for the top where the connection part of the battery cell is located); 4. Assemble the 6 battery cells according to... Figure 3 5. Arrange the battery cells side by side as shown, so that the battery cells are attached to each other and to the end plate; 6. Prepare the side plate assembly and attach the side plate to the sides of the 6 battery cells; 7. After assembly, the battery module for testing is obtained.
[0118] Examples 1-2
[0119] Except for the preparation of the adhesive, in which polyacrylic acid: α-cyclodextrin: hydroxypropyl methylcellulose: toluene: Versamid 125 = 40%: 20%: 10%: 28%: 2% by weight, the other preparation steps are the same as in Example 1-1.
[0120] Examples 1-3
[0121] Except for the preparation of the adhesive, in which polyacrylic acid: α-cyclodextrin: hydroxypropyl methylcellulose: toluene: Versamid 125 = 10%: 50%: 10%: 28%: 2% by weight, the other preparation steps are the same as in Example 1-1.
[0122] Comparative Example 1-1
[0123] Except for the preparation of the adhesive, in which polyacrylic acid: α-cyclodextrin: hydroxypropyl methylcellulose: toluene: Versamid 125 = 60%: 0%: 10%: 28%: 2% by weight, the other preparation steps are the same as in Examples 1-1.
[0124] Comparative Examples 1-2
[0125] Except for the preparation of the adhesive, in which polyacrylic acid: α-cyclodextrin: hydroxypropyl methylcellulose: toluene: Versamid 125 = 10%: 55%: 5%: 28%: 2% by weight, the other preparation steps are the same as in Example 1-1.
[0126] Example 2-1
[0127] Except for the preparation of the adhesive, in which polyacrylic acid: β-cyclodextrin: hydroxypropyl methylcellulose: toluene: Versamid 125 = 35%: 25%: 10%: 28%: 2% by weight, the other preparation steps are the same as in Example 1-1.
[0128] Example 2-2
[0129] Except for the preparation of the adhesive, in which polyacrylic acid: β-cyclodextrin: hydroxypropyl methylcellulose: toluene: Versamid 125 = 25%: 35%: 10%: 28%: 2%, the other preparation steps are the same as in Examples 1-1.
[0130] Comparative Examples 1-3
[0131] Except for the preparation of the adhesive, in which polyacrylic acid: α-cyclodextrin: hydroxypropyl methylcellulose: toluene: Versamid 125 = 0%: 60%: 10%: 28%: 2% by weight, the other preparation steps are the same as in Example 1-1.
[0132] Example 3-1
[0133] Except for the preparation of the adhesive, in which polyacrylic acid: γ-cyclodextrin: hydroxypropyl methylcellulose: toluene: Versamid 125 = 30%: 30%: 10%: 28%: 2% by weight, the other preparation steps are the same as in Example 1-1.
[0134] Example 3-2
[0135] Except for the preparation of the adhesive, in which polyacrylic acid: γ-cyclodextrin: hydroxypropyl methylcellulose: toluene: Versamid 125 = 30%: 30%: 2%: 28%: 10% by weight, the other preparation steps are the same as in Example 1-1.
[0136] Example 3-3
[0137] Except for the preparation of the adhesive, in which polyacrylic acid: γ-cyclodextrin: hydroxypropyl methylcellulose: toluene: Versamid 125 = 30%: 30%: 25%: 13%: 2% by weight, the other preparation steps are the same as in Example 1-1.
[0138] Examples 3-4
[0139] Except for the preparation of the adhesive, in which polyacrylic acid: γ-cyclodextrin: hydroxypropyl methylcellulose: toluene: Versamid 125 = 30%: 30%: 0%: 28%: 12% by weight, the other preparation steps are the same as in Example 1-1.
[0140] Examples 3-5
[0141] Except for the preparation of the adhesive, in which polyacrylic acid: γ-cyclodextrin: hydroxypropyl methylcellulose: toluene: Versamid 125 = 10%: 30%: 30%: 28%: 2% by weight, the other preparation steps are the same as in Examples 1-1.
[0142] Comparative Examples 1-4
[0143] The battery cell casing is only covered with a PET base film, and acrylic structural adhesive (brand: 3M, model: DP8805NS) is used between the battery cells in the battery module and between the battery cells and the end plates and side plates.
[0144] Comparative Examples 1-5
[0145] Except for the step of “Preparation of Insulating Film”, where the base film was not treated in the first and second steps, the other preparation steps are the same as in Example 1-1.
[0146] Example 4-1
[0147] Except for the preparation of the insulating film, where the thickness of the organic coating is 90 μm, the other preparation steps are the same as in Example 1-1.
[0148] Example 4-2
[0149] Except for the preparation of the insulating film, where the thickness of the organic coating is 280 μm, the other preparation steps are the same as in Example 1-1.
[0150] Comparative Examples 1-6
[0151] Except for the preparation of the insulating film, where the thickness of the organic coating is 350 μm, the other preparation steps are the same as in Example 1-1.
[0152] Comparative Examples 1-7
[0153] Except for the preparation of the insulating film, where the thickness of the organic coating is 50 μm, the other preparation steps are the same as in Example 1-1.
[0154] [Battery module vibration resistance and impact resistance test]
[0155] The battery modules corresponding to all the above embodiments and comparative examples were tested using a universal testing machine (MTS, model: CDT1100).
[0156] Vibration strain test in different directions: Vibration strain was applied to the battery module in the x, y, and z directions respectively (see...) Figure 3 The vibration conditions were set as follows: vibration frequency range of 100-1500Hz, high-frequency vibration duration of 8 hours, and vibration acceleration range of 0-100m / s². 2 After the test, the battery module was disassembled and the frequency change of the individual battery cells in the battery pack before and after vibration was recorded. The smaller the rate of change, the better the vibration resistance of the battery module.
[0157] Impact strain test in different directions: Impact strain was applied to the battery module in the x, y, and z directions respectively. The impact conditions were set as follows: vibration frequency range of 100-1500Hz, high-frequency impact duration of 6ms, and impact acceleration range of 0-500m / s². 2 After the test, the battery module was disassembled, and the frequency change of the individual battery cells in the tested battery module before and after the impact was recorded. The smaller the rate of change, the better the impact resistance.
[0158] The criteria for judging the shock resistance performance of the battery module in this application are as follows:
[0159] If the frequency change rate of a single battery cell in the x, y, and z directions before and after vibration is within ±3%, the battery module is considered to have excellent vibration resistance.
[0160] If the frequency change rate of a single battery cell in the x, y, and z directions before and after vibration is within ±10%, the battery module is considered to have good vibration resistance.
[0161] If the frequency change rate of a single battery cell in the x, y, and z directions before and after vibration is within ±10% in two or fewer of the three directions, the vibration resistance of the battery module is considered to be average.
[0162] If the frequency change rate of a single battery cell in the x, y, and z directions is greater than ±10% in three directions, or the frequency change rate in at least one direction is greater than 20% before and after vibration, the battery module is considered to have poor vibration resistance.
[0163] If the frequency change rate of a single battery cell in the x, y, and z directions is within ±8% before and after the impact, the battery module is considered to have excellent impact resistance.
[0164] If the frequency change rate of a single battery cell in the x, y, and z directions is within ±20% before and after the impact, the battery module is considered to have good impact resistance.
[0165] If the frequency change rate of a single battery cell in the x, y, and z directions before and after the impact is within ±20% in two or fewer directions, the impact resistance of the battery module is considered to be average.
[0166] If the frequency change rate of a single battery cell in the x, y, and z directions is greater than ±20% in three directions or greater than 30% in at least one direction before and after the impact, it is considered to have poor impact resistance.
[0167] Table 1. Preparation parameters, product parameters, and performance parameters for the examples and comparative examples.
[0168]
[0169]
[0170] [Data Analysis]:
[0171] Table 1 shows the examples and comparative examples, which investigated the vibration resistance and impact resistance of the battery module of this application from the perspectives of the amount of cyclic oligosaccharides, the amount of adhesive, the amount of cellulose, whether the base film is hydroxylated, and the thickness of the insulating film, as detailed below:
[0172] The impact of cyclic polymers on the vibration resistance and impact resistance of battery modules
[0173] A comprehensive analysis of Examples 1-1 to 1-3 and Comparative Examples 1-1 to 1-2 shows that when the content of cyclic polymer in the adhesive of this application is 20-50% by weight, the vibration resistance and impact resistance of the battery module are excellent. Because the impact resistance conditions are more stringent, the content of polyacrylic acid in Examples 1-3 is 10% by weight. At this ratio, the adhesive performance of the adhesive is slightly weaker, so its impact resistance is good.
[0174] In the comparative examples, the content of cyclic polymers was outside the appropriate range. In Comparative Example 1-1, the content of cyclic polymers was 0% by weight, which could not increase the adhesive's resistance to vibration and impact. In Comparative Example 1-2, the proportion of cyclic polymers was too high and the proportion of polyacrylic acid was too low, resulting in poor adhesive performance. Although it had some vibration resistance, it could not pass the impact resistance test.
[0175] The impact of adhesives on the vibration resistance and impact resistance of battery modules
[0176] Through comprehensive analysis of Examples 2-1 to 2-3 and Comparative Examples 1-3, it can be seen that when the polyacrylic acid content in the adhesive of this application is 20-40% by weight, the adhesive exhibits excellent vibration resistance and impact resistance. In Comparative Examples 1-3, the polyacrylic acid content is 0% by weight, and the adhesive bonding effect is very poor, so its vibration resistance and impact resistance are poor.
[0177] The impact of cellulose on the vibration resistance and impact resistance of battery modules
[0178] A comprehensive comparison of Examples 3-1 to 3-5 shows that the appropriate proportion of cellulose in the adhesive of this application is 2-25% by weight. Within this range, the adhesive exhibits excellent or good vibration resistance and impact resistance. In Examples 3-4, the proportion of cellulose is 0% by weight, and the adhesive bonding effect is slightly weak, so its impact resistance is average. In Examples 3-5, the proportion of cellulose is 30% by weight and the proportion of polyacrylic acid is 10% by weight. The proportion of cellulose is too high and the proportion of polyacrylic acid is too low. Cellulose cannot play a role in strengthening the bonding, so its impact resistance is average.
[0179] Analysis of Insulating Film Thickness Variation
[0180] A comprehensive comparison of Examples 4-1 to 4-2 and Comparative Examples 1-6 and 1-7 reveals that the suitable thickness of the organic coating on the insulating film of this application is 90-280 μm. The battery module with the battery cell covered by the insulating film exhibits good vibration resistance and impact resistance. When the thickness of the insulating film is further reduced to 50 μm (Comparative Example 1-7), the adhesive layer is too thin and affects its bonding effect. When the thickness is increased to 350 μm (Comparative Example 1-6), the adhesive layer is too thick and is prone to bonding failure. Under both of these ratios, the vibration resistance and impact resistance of the adhesive are generally average.
[0181] As shown in Comparative Examples 1-4, the battery modules obtained by bonding battery cells together using conventional acrylic structural adhesive have poor impact and vibration resistance.
[0182] As shown in Comparative Examples 1-5, when the base film is not hydroxylated, the impact and vibration resistance of the corresponding battery modules are generally poor. Figure 1 As shown, in the infrared spectrum of the adhesive in Example 1-1, at 3600 cm⁻¹ -1 A distinct absorption vibration peak of hydroxyl groups was observed at the wavenumber, while the unhydroxylated binders of Comparative Examples 1-5 showed a peak at 3600 cm⁻¹. -1 At the wavenumber, there is only a weak hydroxyl absorption vibration peak, and the presence of more hydroxyl functional groups is beneficial for the bonding between the binder component in the organic coating and the hydroxyl groups on the surface of the base film.
Claims
1. A battery module, comprising side-by-side battery cells and end plates and side plates surrounding the battery cells, wherein, The battery cell casing is covered with an insulating film; The insulating film includes a base film and an organic coating on at least one surface of the base film, the organic coating including an adhesive, the organic coating having a thickness of 90 μm-300 μm; the base film is a film made of polyethylene terephthalate, and the base film is hydroxylated. The binder comprises an adhesive, a curing agent, a solvent, and 20% to 50% by weight of a cyclic oligosaccharide, based on the total weight of the binder; the cyclic oligosaccharide is selected from one or more of α-cyclodextrin, β-cyclodextrin, and γ-cyclodextrin.
2. The battery module according to claim 1, wherein, The adhesive comprises: 5% to 50% by weight of adhesives; 20% to 50% by weight of cyclic oligosaccharides; 0.5% to 10% by weight of curing agent; 10% to 40% by weight of solvent; Each is based on the total weight of the adhesive.
3. The battery module according to claim 2, wherein, The adhesive comprises: 20% to 40% by weight of adhesives; 25% to 35% by weight of cyclic oligosaccharides; 1% to 5% by weight of curing agent; 15% to 35% by weight of solvent; Each is based on the total weight of the adhesive.
4. The battery module according to any one of claims 1 to 3, wherein, The adhesive is selected from one or more of polyvinyl acetate, polyvinyl alcohol, perchlorate, polyisobutylene, cellulose ester and polyacrylic acid.
5. The battery module according to claim 4, wherein, The number average molecular weight of the adhesive is 1,000-90,000.
6. The battery module according to claim 5, wherein, The number average molecular weight of the adhesive is 5,000-50,000.
7. The battery module according to claim 1, wherein, The curing agent is a polyamide-based curing agent.
8. The battery module according to claim 1, wherein, The solvent is selected from one or more of carbon tetrachloride, ethyl acetate, methyl formate, ethanol, and toluene.
9. The battery module according to claim 8, wherein, The solvent is toluene.
10. The battery module according to claim 1, wherein, The binder further comprises cellulose, which is selected from one or more of hydroxypropyl methylcellulose, methylcellulose, ethylcellulose, hydroxyethylcellulose, hydroxypropylcellulose, and carboxymethylcellulose.
11. The battery module according to claim 10, wherein, The cellulose content is 2% to 25% by weight, based on the total weight of the binder.
12. The battery module according to claim 11, wherein, The cellulose content is from 3% to 20% by weight, based on the total weight of the binder.
13. The battery module according to claim 1, wherein, The thickness of the organic coating is 100 μm-200 μm.
14. The battery module according to claim 1, wherein, The battery cells are bonded together, between the battery cells and the side plate, and between the battery cells and the end plate by the adhesive.
15. A battery pack comprising the battery module according to any one of claims 1-14, wherein the battery pack serves as a power source for an electrical device.
Citation Information
Patent Citations
Bonding coating slurry, diaphragm and lithium ion battery