A preparation method and application of a low-alkali, high-nickel ternary cathode material

By mixing large-particle lithium-rich cathode materials with small-particle lithium-deficient materials and annealing sintering, the problem of residual lithium on the surface of high-nickel cathode materials is solved, the process is simplified, and the electrochemical performance and capacity are improved, making it suitable for high-energy power batteries.

CN117497686BActive Publication Date: 2026-11-17GEM WUXI ENERGY MATERIAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311445761.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-01
Publication Date
2026-11-17
Estimated Expiration
2043-11-01

AI Technical Summary

Technical Problem

Existing technologies involve numerous and costly processes when removing residual lithium from the surface of high-nickel cathode materials, resulting in poor electrochemical performance, safety hazards, and reduced capacity of lithium-ion batteries.

Method used

Large-particle lithium-rich cathode material A is mixed with small-particle lithium-deficient material B, and then annealed and sintered in an oxygen-containing atmosphere, followed by multiple stirring and sintering processes. By mixing and lithium replenishment, residual alkali is reduced and the activity of the material is improved.

Benefits of technology

It simplifies the process, reduces production costs, improves the initial charge-discharge specific capacity, initial efficiency, and cycle stability of the material, and enhances electrochemical performance, making it suitable for high-energy power battery applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117497686B_ABST
    Figure CN117497686B_ABST
Patent Text Reader

Abstract

This invention relates to the field of lithium-ion battery cathode material preparation technology, and in particular to a method for preparing a low-alkali, high-nickel ternary cathode material and its application. The preparation method of this invention includes: 1) mixing a first precursor, a first additive, and a first lithium salt, followed by a first sintering to obtain cathode material A; mixing a second precursor, a second additive, and a second lithium salt, followed by a second sintering to obtain cathode material B; wherein the particle size D50 of the first precursor is 15-20 μm; and the particle size D50 of the second precursor is 1-5 μm; 2) mixing cathode material A and cathode material B to obtain a mixed cathode material; 3) annealing and sintering the mixed cathode material from step 2) in an oxygen-containing atmosphere, and then subjecting the annealed and sintered product to at least two stirring and sintering treatments to obtain the low-alkali, high-nickel ternary cathode material. This method can reduce residual alkali and enhance the electrochemical performance of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion battery cathode material preparation technology, and in particular to a method for preparing a low-alkali, high-nickel ternary cathode material and its application. Background Technology

[0002] Lithium-ion batteries, as a new energy source, have been widely used in the market due to their advantages such as high energy density, long cycle life, stable battery voltage, no memory effect, environmental friendliness, and low cost. Currently, based on market needs, the energy density requirements for lithium-ion batteries are increasing, leading to the development of LiNi batteries with higher energy density. x Co y Mn z O2 (x>0.8) ternary materials have attracted much attention, but during storage, these materials are prone to reacting with CO2 and H2O in the air, generating residual alkalis such as Li2CO3 and LiOH on the material surface. The generation of these residual alkalis not only makes it easier for them to react with polyvinylidene fluoride (PVDF) during electrode homogenization, increasing the slurry viscosity and leading to gelation, but also increases gas production during electrochemical reactions, posing a safety hazard to the battery.

[0003] Currently, the most effective method for removing residual lithium from the surface of high-nickel cathode materials is water washing. This involves removing residual alkali during the washing process, including introducing additives or weak acids. However, water washing is a complex process, time-consuming, energy-intensive, and requires expensive equipment. The wastewater treatment also incurs significant costs. Furthermore, the washing process removes lithium from the near-surface lattice of the high-nickel cathode material. + / H + Ion exchange leads to a decrease in capacity and a deterioration in electrochemical performance. Summary of the Invention

[0004] Therefore, the technical problem to be solved by the present invention is to overcome the defects of existing methods for removing residual lithium from the surface of high-nickel cathode materials, which involve many steps, high costs, low capacity and poor electrochemical performance of the cathode materials. The present invention provides a method for preparing low-residual-base high-nickel ternary cathode materials and their applications.

[0005] This invention provides a method for preparing a low-alkali, high-nickel ternary cathode material, comprising the following steps:

[0006] 1) The first precursor, the first additive, and the first lithium salt are mixed and then subjected to a first sintering to obtain cathode material A; the second precursor, the second additive, and the second lithium salt are mixed and then subjected to a second sintering to obtain cathode material B; wherein the particle size D50 of the first precursor is 15-20 μm; and the particle size D50 of the second precursor is 1-5 μm.

[0007] 2) Mix cathode material A and cathode material B to obtain a mixed cathode material;

[0008] 3) The mixed cathode material in step 2) is annealed and sintered in an oxygen-containing atmosphere, and then the annealed and sintered product is stirred and sintered at least twice to obtain the low residual alkali and high nickel ternary cathode material.

[0009] Preferably, in step 3), the annealed and sintered product is subjected to stirring and sintering treatment at least 2-3 times.

[0010] Preferably, in step 1), the first additive and the second additive are each independently selected from at least one of ZrO2, WO3, MoO3, TiO2, Y2O3, Mg(OH)2, Al2O3, TiO2, and H3BO3;

[0011] The first precursor and the second precursor are each independently selected from at least one of nickel-cobalt-manganese composite oxide, nickel-cobalt-aluminum composite oxide, nickel-cobalt-manganese composite hydroxide, and nickel-cobalt-aluminum hydroxide.

[0012] Optionally, the first precursor is selected from Ni 0.90 Co 0.05 Mn 0.05 (OH)2;

[0013] Optionally, the second precursor is selected from Ni 0.8 Co 0.1 Mn 0.1 (OH)2.

[0014] Preferably, in step 1), the mass ratio of the first precursor, the first additive, and the first lithium salt is 1:(0.005-0.006):(0.450-0.470);

[0015] The mass ratio of the second precursor, the second additive, and the second lithium salt is 1:(0.005-0.006):(0.270-0.360);

[0016] In step 1), the molar ratio n of lithium to transition metal elements in cathode material A is... Li / n 过渡 >1.00;

[0017] In the cathode material B, the molar ratio n of lithium to transition metal elements is... Li / n 过渡 <1.00.

[0018] The lithium ratio described in this invention refers to the ratio of the molar amount of metallic Li to the molar amount of the transition metal. The transition metal or transition metal element described in this invention includes metallic Ni, metallic Co, and doped metal Q. The molar amount n of the transition metal element... 过渡 It is the sum of the molar amounts of metallic Ni, metallic Co, and doped metallic Q.

[0019] Preferably, the general formula of the positive electrode material A is Li. a Ni x Co y Q 1-x-y O2, where Q is Mn or Al, 1.00 < a < 1.03, 0.8 ≤ x ≤ 1, 0 ≤ y ≤ 0.2;

[0020] The cathode material B is selected from Li b Ni x Co y Q 1-x-y O2, where Q is Mn or Al, 0.6 < b < 1, 0.8 ≤ x ≤ 1, 0 ≤ y ≤ 0.2.

[0021] Preferably, in step 1), the first lithium salt and the second lithium salt are each independently selected from lithium hydroxide;

[0022] The present invention does not specifically limit the selection of lithium hydroxide. Anhydrous lithium hydroxide or lithium hydroxide hydrate can be selected. Optionally, the lithium hydroxide is selected from LiOH·H2O.

[0023] In step 1), the first sintering temperature is 700-900℃, and the first sintering time is 8-15h;

[0024] The second sintering temperature is 700-900℃, and the second sintering time is 8-15h;

[0025] The first sintering is carried out in an oxygen-containing atmosphere;

[0026] The second sintering is carried out in an oxygen-containing atmosphere.

[0027] Preferably, the mixing speed in step 2) is 150-250 r / min, and the mixing time is 10 min-20 min.

[0028] Optionally, in step 2), the molar percentage of nickel in the cathode material B, excluding lithium, is lower than that in the cathode material A, excluding lithium.

[0029] Preferably, the added mass m of the positive electrode material B and the added mass R of the positive electrode material A in step 2) satisfy the following relationship:

[0030] m = R * x1 / M * M B / {1-(x2 / M)*[M 过渡 / (1-x2)]}*β,1.01≤β≤1.2;

[0031] In the formula, x1 is the percentage of residual lithium in cathode material A as detected;

[0032] x2 represents the lithium mass percentage of cathode material B;

[0033] M is the molar mass of lithium, expressed in mol / g;

[0034] M 过渡 The molar mass of the transition metal in cathode material B is expressed in mol / g.

[0035] M B The molar mass of cathode material B is expressed in mol / g.

[0036] m is the mass of cathode material B added, in grams;

[0037] R represents the added mass of cathode material A, in grams.

[0038] Preferably, 1.05≤β≤1.2.

[0039] In the above formula, β is a correction coefficient, R*x1 / M is the total residual lithium molar amount of cathode material A with mass R; 1-(x2 / M)*[M 过渡 [ / (1-x2)] represents the total molar percentage of lithium deficiency in cathode material B.

[0040] The method for determining the residual lithium mass percentage x1 of cathode material A in this invention is not specifically limited; conventional methods in the art can be used. Typically, without limitation, 10g of cathode material A is dissolved in 1L of water and stirred at 200rpm for 30min. The supernatant is then filtered to obtain the supernatant. The mass of lithium in the supernatant is detected by inductively coupled plasma (ICP), and the residual lithium mass percentage of cathode material A is calculated as: mass of lithium in supernatant / mass of cathode material A * 100%.

[0041] Preferably, the annealing and sintering temperature in step 3) is 500-700℃, the annealing and sintering time is 6-10h, and the heating rate of the annealing and sintering is 2-5℃ / min.

[0042] Optionally, the oxygen concentration of the sintering atmosphere during the annealing and sintering is 90-100%.

[0043] Preferably, in step 3), the stirring speed is 150-250 r / min and the stirring time is 10 min-20 min.

[0044] In step 3), the product after annealing and sintering is subjected to at least two stirring and sintering processes, wherein the sintering temperature is 500-700℃ and the sintering time is 6-10h.

[0045] This invention provides a method for preparing the low-alkali, high-nickel ternary cathode material described above, and its application in lithium-ion batteries.

[0046] The technical solution of this invention has the following advantages:

[0047] 1. The present invention provides a method for preparing a low-alkali, high-nickel ternary cathode material, comprising the following steps: 1) mixing a first precursor, a first additive, and a first lithium salt and then performing a first sintering to obtain cathode material A; mixing a second precursor, a second additive, and a second lithium salt and then performing a second sintering to obtain cathode material B; wherein the particle size D50 of the first precursor is 15-20 μm; and the particle size D50 of the second precursor is 1-5 μm; 2) mixing cathode material A and cathode material B to obtain a mixed cathode material; 3) annealing and sintering the mixed cathode material in step 2) in an oxygen-containing atmosphere, and then subjecting the annealed and sintered product to at least two stirring and sintering treatments to obtain the low-alkali, high-nickel ternary cathode material. This invention employs a mixture of large-particle, lithium-rich cathode material A and small-particle, lithium-deficient material B for lithium replenishment. This reduces residual alkali while increasing the capacity of the small-particle cathode material B. Firstly, the lithium-deficient small-particle cathode material B, acting as a secondary sintering reactant, replenishes lithium vacancies in its structure with residual lithium from cathode material A during annealing and sintering. This significantly reduces the accumulation of residual lithium on the surface of the large-particle cathode material A, lowering the residual alkali on the surface of the high-nickel cathode material. Simultaneously, lithium replenishment is performed on the small-particle cathode material B, increasing its capacity and improving the overall material's compaction density, thereby enhancing its overall energy density and activity. The annealing process of this scheme includes repeated mixing and annealing after annealing and sintering. This allows the residual lithium on the surface of the large-particle cathode material A to fully contact and be fully absorbed by the small-particle cathode material B during the continuous remixing process. On the other hand, the repeated mixing and annealing process also allows some of the residual lithium on the surface of the large-particle cathode material A to re-enter the crystal structure of the large-particle cathode material A, thereby reducing residual alkali and improving the overall activity of the material. The low-alkali, high-nickel ternary cathode material prepared by the method of this invention has a uniform Li distribution and a low residual alkali content, which is basically the same as the residual alkali content of the material obtained by water washing to remove residual alkali. The method of this invention can achieve a similar residual alkali removal effect as water washing, but avoids the side reactions caused by water washing, enhances the overall activity of the material, and thus increases the electrochemical performance of the material, such as the initial charge-discharge specific capacity, initial efficiency, and cycle stability. At the same time, even after boric acid coating, the cathode material obtained by this invention still has excellent cycle performance compared with the cathode material obtained by water washing to remove residual alkali.

[0048] 2. The method for preparing low residual alkali and high nickel ternary cathode material provided by the present invention is suitable for high-compact, high-capacity cathode materials with mixed secondary spheres of varying sizes. It is also applicable to high-capacity, long-cycle cathodes with mixed secondary sphere single crystals. The lithium-ion battery with mixed sizes constructed by the present invention has a high compaction density, which can optimize the overall performance of the battery and is suitable for fields requiring high-energy power batteries.

[0049] 3. The preparation method of low residual alkali and high nickel ternary cathode material provided by the present invention can fully and effectively consume the residual lithium on the surface of large cathode material by using small-particle cathode material with low lithium content, while simplifying the process flow, realizing the waterless washing process of ultra-high nickel cathode material, reducing production costs. The preparation method of the present invention is simple and easy to implement and is convenient for industrialization. Attached Figure Description

[0050] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0051] Figure 1 SEM image of the low residual alkali and high nickel ternary cathode material prepared in Example 3 of this invention after boric acid coating;

[0052] Figure 2 SEM image of the ternary cathode material prepared by Comparative Example 3 of this invention after boric acid coating;

[0053] Figure 3 Comparison of cycle capacity retention rates between the low residual alkali and high nickel ternary cathode material of Example 3 and the ternary cathode material prepared in Comparative Example 3 after boric acid coating. Detailed Implementation

[0054] The following embodiments are provided to better understand the present invention and are not limited to the preferred embodiments described. They do not constitute a limitation on the content and scope of protection of the present invention. Any product that is the same as or similar to the present invention, derived by any person under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the protection scope of the present invention.

[0055] For experiments not specifically described in the examples, the procedures or conditions should be followed according to the conventional experimental procedures described in the literature in this field. Reagents or instruments whose manufacturers are not specified are all commercially available conventional reagent products.

[0056] Example 1

[0057] This embodiment provides a method for preparing a low-residue, high-nickel ternary cathode material, including the following steps:

[0058] 1) 2000g of Ni with a D50 of 15.0μm 0.90 Co 0.05 Mn 0.05A mixture of (OH)₂, 10.06 g ZrO₂, and 922.51 g LiOH·H₂O was sintered at 780 °C for 10 h in an oxygen atmosphere to obtain cathode material A. Inductively coupled plasma atomic emission spectrometry (ICP) analysis revealed that the chemical formula of cathode material A is Li₂. 1.015 Ni 0.9 Co 0.05 Mn 0.05 O2; 1000g of Ni with a D50 of 3.0μm 0.8 Co 0.1 Mn 0.1 After mixing (OH)₂ with 5.02g ZrO₂ and 348.56g LiOH·H₂O, the mixture was sintered at 780℃ for 10h under an oxygen atmosphere to obtain cathode material B. Inductively coupled plasma atomic emission spectrometry (ICP) analysis revealed that the chemical formula of cathode material B is Li₂. 0.75 Ni 0.8 Co 0.1 Mn 0.1 O2;

[0059] 2) According to inductively coupled plasma detection (ICP), the residual lithium mass percentage of cathode material A is x1 = 1.17%, and the lithium mass percentage of cathode material B is x2 = 5.44%. Taking 800g of cathode material A, the mass of cathode material B is m = R*x1 / M*M. B / {1-(x2 / M)*[M 过渡 / (1-x2)]}*β, β=1.01, m=(800*1.17% / 6.94)*95.55 / {1-5.44% / 6.94*[58.345 / (1-5.44%)]}*1.01g=130.18g, that is, 130.18g of positive electrode material B and 800g of positive electrode material A are mixed in a high-speed mixer at a mixing speed of 150r / min and a mixing time of 15min to obtain mixed positive electrode material;

[0060] 3) The mixed cathode material from step 2) is annealed and sintered in an oxygen-containing atmosphere in a rotary kiln at 650°C for 8 hours. The heating rate during annealing and sintering is 3°C / min. Then, the annealed and sintered product is stirred and sintered three times. The stirring speed in the three stirring and sintering steps is 150 r / min, the stirring time is 15 min, and the sintering temperature in the three stirring and sintering steps is 650°C and the sintering time is 8 hours to obtain the low residual alkali and high nickel ternary cathode material.

[0061] Example 2

[0062] This embodiment provides a method for preparing a low-residue, high-nickel ternary cathode material, including the following steps:

[0063] 1) 2000g of Ni with a D50 of 15.0μm 0.90 Co 0.05 Mn 0.05 A mixture of (OH)₂, 10.06 g ZrO₂, and 922.51 g LiOH·H₂O was sintered at 780 °C for 10 h in an oxygen atmosphere to obtain cathode material A. Inductively coupled plasma atomic emission spectrometry (ICP) analysis revealed that the chemical formula of cathode material A is Li₂. 1.015 Ni 0.9 Co 0.05 Mn 0.05 O2; 1000g of Ni with a D50 of 3.0μm 0.8 Co 0.1 Mn 0.1 After mixing (OH)₂ with 5.02g ZrO₂ and 348.56g LiOH·H₂O, the mixture was sintered at 780℃ for 10h under an oxygen atmosphere to obtain cathode material B. Inductively coupled plasma atomic emission spectrometry (ICP) analysis revealed that the chemical formula of cathode material B is Li₂. 0.75 Ni 0.8 Co 0.1 Mn 0.1 O2;

[0064] 2) According to inductively coupled plasma detection (ICP), the residual lithium mass percentage of cathode material A is x1 = 1.17%, and the lithium mass percentage of cathode material B is x2 = 5.44%. Taking 800g of cathode material A, the mass of cathode material B is m = R*x1 / M*M. B / {1-(x2 / M)*[M 过渡 / (1-x2)]}*β, β=1.03, m=(800*1.17% / 6.94)*95.55 / {1-5.44% / 6.94*[58.345 / (1-5.44%)]}*1.03g=132.75g, that is, 132.75g of positive electrode material B and 800g of positive electrode material A are mixed in a high-speed mixer at a mixing speed of 250r / min and a mixing time of 15min to obtain mixed positive electrode material;

[0065] 3) The mixed cathode material from step 2) is annealed and sintered in an oxygen-containing atmosphere in a rotary kiln at 650°C for 8 hours. The heating rate during annealing and sintering is 3°C / min. Then, the annealed and sintered product is stirred and sintered three times. The stirring speed in the three stirring and sintering steps is 250 r / min, the stirring time is 15 min, and the sintering temperature in the three stirring and sintering steps is 650°C and the sintering time is 8 hours to obtain the low residual alkali and high nickel ternary cathode material.

[0066] Example 3

[0067] This embodiment provides a method for preparing a low-residue, high-nickel ternary cathode material, including the following steps:

[0068] 1) 2000g of Ni with a D50 of 15.0μm 0.90 Co 0.05 Mn 0.05 A mixture of (OH)₂, 10.06 g ZrO₂, and 922.51 g LiOH·H₂O was sintered at 780 °C for 10 h in an oxygen atmosphere to obtain cathode material A. Inductively coupled plasma atomic emission spectrometry (ICP) analysis revealed that the chemical formula of cathode material A is Li₂. 1.015 Ni 0.9 Co 0.05 Mn 0.05 O2; 1000g of Ni with a D50 of 3.0μm 0.8 Co 0.1 Mn 0.1 After mixing (OH)₂ with 5.02g ZrO₂ and 348.56g LiOH·H₂O, the mixture was sintered at 780℃ for 10h under an oxygen atmosphere to obtain cathode material B. Inductively coupled plasma (ICP) detection revealed that the chemical formula of cathode material B is Li₂. 0.75 Ni 0.8 Co 0.1 Mn 0.1 O2;

[0069] 2) According to inductively coupled plasma detection (ICP), the residual lithium mass percentage of cathode material A is x1 = 1.17%, and the lithium mass percentage of cathode material B is x2 = 5.44%. Taking 800g of cathode material A, the mass of cathode material B is m = R*x1 / M*M. B / {1-(x2 / M)*[M 过渡 / (1-x2)]}*β, β=1.05, m=(800*1.17% / 6.94)*95.55 / {1-5.44% / 6.94*[58.345 / (1-5.44%)]}*1.05g=135.33g, that is, 135.33g of positive electrode material B and 800g of positive electrode material A are mixed in a high-speed mixer at a mixing speed of 200r / min and a mixing time of 15min to obtain mixed positive electrode material;

[0070] 3) The mixed cathode material from step 2) is annealed and sintered in an oxygen-containing atmosphere in a rotary kiln at 650°C for 8 hours. The heating rate during annealing and sintering is 3°C / min. Then, the annealed and sintered product is stirred and sintered three times. The stirring speed in the three stirring and sintering steps is 200 r / min, the stirring time is 15 min, and the sintering temperature in the three stirring and sintering steps is 650°C and the sintering time is 8 hours to obtain the low residual alkali and high nickel ternary cathode material.

[0071] Example 4

[0072] This embodiment provides a method for preparing a low-residue, high-nickel ternary cathode material, including the following steps:

[0073] 1) 2000g of Ni with a D50 of 15.0μm 0.90 Co 0.05 Mn 0.05 After mixing (OH)₂ with 10.06 g ZrO₂ and 922.51 g LiOH·H₂O, the mixture was sintered at 780 °C for 10 h in an oxygen atmosphere to obtain cathode material A. Inductively coupled plasma (ICP) detection revealed that the chemical formula of cathode material A is Li₂. 1.015 Ni 0.9 Co 0.05 Mn 0.05 O2; 1000g of Ni with a D50 of 3.0μm 0.8 Co 0.1 Mn 0.1 After mixing (OH)₂ with 5.02g ZrO₂ and 348.56g LiOH·H₂O, the mixture was sintered at 780℃ for 10h under an oxygen atmosphere to obtain cathode material B. Inductively coupled plasma atomic emission spectrometry (ICP) analysis revealed that the chemical formula of cathode material B is Li₂. 0.75 Ni 0.8 Co 0.1 Mn 0.1 O2;

[0074] 2) According to inductively coupled plasma detection (ICP), the residual lithium mass percentage of cathode material A is x1 = 1.17%, and the lithium mass percentage of cathode material B is x2 = 5.44%. Taking 800g of cathode material A, the mass of cathode material B is m = R*x1 / M*M. B / {1-(x2 / M)*[M 过渡 / (1-x2)]}*β, β=1.07, m=(800*1.17% / 6.94)*95.55 / {1-5.44% / 6.94*[58.345 / (1-5.44%)]}*1.07g=137.91g, that is, 137.91g of cathode material B and 800g of cathode material A are mixed in a high-speed mixer at a mixing speed of 190r / min and a mixing time of 15min to obtain mixed cathode material;

[0075] 3) The mixed cathode material from step 2) is annealed and sintered at 650°C for 8 hours in an oxygen-containing atmosphere in a rotary kiln. The heating rate during annealing and sintering is 3°C / min. Then, the annealed and sintered product is stirred and sintered three times. The stirring speed during the three stirring and sintering steps is 190 r / min, the stirring time is 15 min, and the sintering temperature during the three stirring and sintering steps is 650°C for 8 hours to obtain the low residual alkali and high nickel ternary cathode material.

[0076] Example 5

[0077] This embodiment provides a method for preparing a low-residue, high-nickel ternary cathode material, including the following steps:

[0078] 1) 2000g of Ni with a D50 of 15.0μm 0.90 Co 0.05 Mn 0.05 After mixing (OH)₂ with 10.06 g ZrO₂ and 922.51 g LiOH·H₂O, the mixture was sintered at 780 °C for 10 h in an oxygen atmosphere to obtain cathode material A. Inductively coupled plasma (ICP) detection revealed that the chemical formula of cathode material A is Li₂. 1.015 Ni 0.9 Co 0.05 Mn 0.05 O2; 1000g of Ni with a D50 of 3.0μm 0.8 Co 0.1 Mn 0.1 After mixing (OH)₂ with 5.02g ZrO₂ and 348.56g LiOH·H₂O, the mixture was sintered at 780℃ for 10h under an oxygen atmosphere to obtain cathode material B. Inductively coupled plasma atomic emission spectrometry (ICP) analysis revealed that the chemical formula of cathode material B is Li₂. 0.75 Ni 0.8 Co 0.1 Mn 0.1 O2;

[0079] 2) According to inductively coupled plasma detection (ICP), the residual lithium mass percentage of cathode material A is x1 = 1.17%, and the lithium mass percentage of cathode material B is x2 = 5.44%. Taking 800g of cathode material A, the mass of cathode material B is m = R*x1 / M*M. B / {1-(x2 / M)*[M 过渡 / (1-x2)]}*β, β=1.09, m=(800*1.17% / 6.94)*95.55 / {1-5.44% / 6.94*[58.345 / (1-5.44%)]}*1.09g=140.49g, that is, 140.49g of cathode material B and 800g of cathode material A are mixed in a high-speed mixer at a mixing speed of 230r / min and a mixing time of 15min to obtain mixed cathode material;

[0080] 3) The mixed cathode material from step 2) is annealed and sintered in an oxygen-containing atmosphere in a rotary kiln at 650°C for 8 hours. The heating rate during annealing and sintering is 3°C / min. Then, the annealed and sintered product is stirred and sintered three times. The stirring speed during the three stirring and sintering steps is 230 r / min, the stirring time is 15 min, and the sintering temperature during the three stirring and sintering steps is 650°C for 8 hours to obtain the low residual alkali and high nickel ternary cathode material.

[0081] Example 6

[0082] This embodiment provides a method for preparing a low-residue, high-nickel ternary cathode material, including the following steps:

[0083] 1) 2000g of Ni with a D50 of 17.0μm 0.90 Co 0.05 Mn 0.05 A mixture of (OH)₂, 10.06 g ZrO₂, and 922.51 g LiOH·H₂O was sintered at 700 °C for 15 h in an oxygen atmosphere to obtain cathode material A. Inductively coupled plasma (ICP) detection revealed that the chemical formula of cathode material A was Li₂. 1.015 Ni 0.9 Co 0.05 Mn 0.05 O2; 1000g of Ni with a D50 of 1.0μm 0.8 Co 0.1 Mn 0.1 A mixture of (OH)₂, 5.02 g ZrO₂, and 348.56 g LiOH·H₂O was sintered at 700 °C for 15 h in an oxygen atmosphere to obtain cathode material B. Inductively coupled plasma atomic emission spectrometry (ICP) analysis revealed that the chemical formula of cathode material B is Li₂.0.75 Ni 0.8 Co 0.1 Mn 0.1 O2;

[0084] 2) According to inductively coupled plasma detection (ICP), the residual lithium mass percentage of cathode material A is x1 = 1.17%, and the lithium mass percentage of cathode material B is x2 = 5.44%. Taking 800g of cathode material A, the mass of cathode material B is m = R*x1 / M*M. B / {1-(x2 / M)*[M 过渡 / (1-x2)]}*β, β=1.05, m=(800*1.17% / 6.94)*95.55 / {1-5.44% / 6.94*[58.345 / (1-5.44%)]}*1.05g=135.33g, that is, 135.33g of cathode material B and 800g of cathode material A are mixed in a high-speed mixer at a mixing speed of 250r / min and a mixing time of 10min to obtain mixed cathode material;

[0085] 3) The mixed cathode material from step 2) is annealed and sintered in an oxygen-containing atmosphere in a rotary kiln at 500°C for 10 hours. The heating rate during annealing and sintering is 5°C / min. Then, the annealed and sintered product is subjected to two stirring and sintering treatments. The stirring speed during the two stirring and sintering treatments is 150 r / min, and the stirring time is 10 min. The sintering temperature during the two stirring and sintering treatments is 700°C, and the sintering time is 10 hours, to obtain the low residual alkali and high nickel ternary cathode material.

[0086] Example 7

[0087] This embodiment provides a method for preparing a low-residue, high-nickel ternary cathode material, including the following steps:

[0088] 1) Take 2000g of Ni with a D50 of 20.0μm 0.90 Co 0.05 Mn 0.05 A mixture of (OH)₂, 10.06 g ZrO₂, and 922.51 g LiOH·H₂O was sintered at 900 °C for 8 h in an oxygen atmosphere to obtain cathode material A. Inductively coupled plasma (ICP) detection revealed that the chemical formula of cathode material A is Li₂. 1.015 Ni 0.9 Co 0.05 Mn 0.05 O2; 1000g of Ni with a D50 of 5.0μm 0.8 Co 0.1 Mn 0.1After mixing (OH)₂ with 5.02g ZrO₂ and 348.56g LiOH·H₂O, the mixture was sintered at 900℃ for 5h under an oxygen atmosphere to obtain cathode material B. Inductively coupled plasma atomic emission spectrometry (ICP) analysis revealed that the chemical formula of cathode material B is Li₂. 0.75 Ni 0.8 Co 0.1 Mn 0.1 O2;

[0089] 2) According to inductively coupled plasma detection (ICP), the residual lithium mass percentage of cathode material A is x1 = 1.17%, and the lithium mass percentage of cathode material B is x2 = 5.44%. Taking 800g of cathode material A, the mass of cathode material B is m = R*x1 / M*M. B / {1-(x2 / M)*[M 过渡 / (1-x2)]}*β, β=1.05, m=(800*1.17% / 6.94)*95.55 / {1-5.44% / 6.94*[58.345 / (1-5.44%)]}*1.05g=135.33g, that is, 135.33g of positive electrode material B and 800g of positive electrode material A are mixed in a high-speed mixer at a mixing speed of 150r / min and a mixing time of 20min to obtain mixed positive electrode material;

[0090] 3) The mixed cathode material from step 2) is annealed and sintered at 700°C for 10 hours in an oxygen-containing atmosphere in a rotary kiln. The heating rate during annealing and sintering is 2°C / min. Then, the annealed and sintered product is stirred and sintered three times. The stirring speed during the three stirring and sintering steps is 150 r / min, the stirring time is 20 min, and the sintering temperature during the three stirring and sintering steps is 700°C, and the sintering time is 10 hours to obtain the low residual alkali and high nickel ternary cathode material.

[0091] Comparative Example 1

[0092] This comparative example provides a method for preparing a ternary cathode material. The only difference between this method and Example 3 is that in step 3), the mixed cathode material from step 2) is annealed and sintered at 650°C for 8 hours in an oxygen-containing atmosphere in a rotary kiln. The heating rate during annealing and sintering is 3°C / min, thereby obtaining the ternary cathode material.

[0093] Comparative Example 2

[0094] This comparative example provides a method for preparing a ternary cathode material, including the following steps:

[0095] 1) 2000g of Ni with a D50 of 15.0μm 0.90 Co 0.05Mn 0.05 After mixing (OH)₂ with 10.06 g ZrO₂ and 922.51 g LiOH·H₂O, the mixture was sintered at 780 °C for 10 h in an oxygen atmosphere to obtain cathode material A. Inductively coupled plasma (ICP) detection revealed that the chemical formula of cathode material A is Li₂. 1.015 Ni 0.9 Co 0.05 Mn 0.05 O2;

[0096] 2) Take 935.33g of cathode material A and mix it with 935.33g of pure water. The mixing speed is 400r / min and the mixing time is 10min. The material and water are separated by vacuum filtration. The material is dried at 120℃ for 10h to obtain the ternary cathode material.

[0097] Comparative Example 3

[0098] This comparative example provides a method for preparing a ternary cathode material, including the following steps:

[0099] 1) 2000g of Ni with a D50 of 15.0μm 0.90 Co 0.05 Mn 0.05 A mixture of (OH)₂, 10.06 g ZrO₂, and 922.51 g LiOH·H₂O was sintered at 780 °C for 10 h in an oxygen atmosphere to obtain cathode material A. Inductively coupled plasma atomic emission spectrometry (ICP) analysis revealed that the chemical formula of cathode material A is Li₂. 1.015 Ni 0.9 Co 0.05 Mn 0.05 O2; 1000g of Ni with a D50 of 3.0μm 0.8 Co 0.1 Mn 0.1 A mixture of (OH)₂, 5.02 g ZrO₂, and 462.85 g LiOH·H₂O was sintered at 780 °C for 10 h under an oxygen atmosphere to obtain cathode material B'. Inductively coupled plasma atomic emission spectrometry (ICP) analysis revealed the chemical formula of cathode material B' to be Li₂. 1.015 Ni 0.8 Co 0.1 Mn 0.1 O2, after titration, the total residual alkali content of the positive electrode material B' is 0.76wt% (LiOH 0.47wt%, Li2CO3 0.29wt%);

[0100] 2) Take 800g of positive electrode material A and mix it with 800g of pure water. The mixing speed is 400r / min and the mixing time is 10min. Use vacuum filtration to separate the material and water. Dry the material at 120℃ for 10h. Mix the obtained positive electrode material A with 135.33g of positive electrode material B' to obtain the ternary positive electrode material.

[0101] Test Example 1

[0102] The low-residue, high-nickel ternary cathode materials obtained in Examples 1-7 and the ternary cathode materials obtained in Comparative Examples 1-3 were dispersed in deionized water and stirred at 20 rpm for 30 min. The supernatant was then filtered, and the total residual alkali content was tested by titration: acid-base titration was performed with calibrated dilute hydrochloric acid, and phenolphthalein and methyl orange were used as indicators for the titration endpoint. Two titration endpoints were obtained, and the mass content of LiOH and Li2CO3 in the cathode material was calculated. The total residual alkali content = mass content of LiOH + mass content of Li2CO3.

[0103] The low-alkali, high-nickel ternary cathode materials obtained in Examples 1-7 and the ternary cathode materials obtained in Comparative Examples 1-3 were used as cathode active materials, respectively. The composition of the cathode sheet was m(cathode active material):m(acetylene black):m(polyvinylidene fluoride (PVDF)) = 90:5:5. A coin cell was assembled using lithium foil as the negative electrode and lithium hexafluorophosphate as the electrolyte. The Blue Electric testing system was used for testing. Under the conditions of a charge / discharge current of 0.2C and a voltage range of 2.5-4.25V, the initial charge / discharge specific capacity was tested, and the initial efficiency was calculated as (initial discharge specific capacity / initial charge specific capacity) * 100%. The capacity retention rate was tested after 50 cycles at a charge / discharge current of 1C and a voltage range of 2.5-4.25V. The test results are shown in Table 1.

[0104] Table 1

[0105]

[0106] As shown in Table 1, the lithium content of the high-nickel cathode material decreases with increasing correction coefficient β, especially in Examples 3-5, where the residual alkali level is basically the same as or even lower than that of the water washing process (Comparative Example 2). However, with increasing correction coefficient β, the initial discharge specific capacity first increases and then decreases. The highest initial discharge capacity in Example 3 is 212.36 mAh / g. After 50 cycles, the high-nickel cathode materials in Examples 1-7 have similar capacity retention rates, all higher than those obtained in the comparative examples, and their overall electrochemical performance is higher than that of the comparative examples.

[0107] Test Example 2

[0108] Take 500g each of the low residual alkali and high nickel ternary cathode materials obtained in Examples 1-7 and the ternary cathode materials obtained in Comparative Examples 1-3, mix them with 2.86g of boric acid, and coat them at 250°C for 6 hours to obtain boric acid-coated ternary cathode materials.

[0109] The materials coated with boric acid corresponding to Examples 3 and Comparative Example 3 were subjected to electron microscopy scanning tests. The scanning results for Example 3 are as follows: Figure 1 As shown, Comparative Example 3 is as follows Figure 2 As shown.

[0110] The boric acid-coated ternary cathode materials corresponding to Examples 1-7 and Comparative Examples 1-3 were dispersed in deionized water and stirred at 200 rpm for 30 min. The supernatant was then filtered and titrated with standardized dilute hydrochloric acid. Phenolphthalein and methyl orange were used as indicators for the titration endpoints, respectively, to obtain two titration endpoints. The mass contents of LiOH and Li2CO3 in the cathode material were calculated. The total residual alkali content = mass content of LiOH + mass content of Li2CO3.

[0111] The ternary cathode materials coated with boric acid corresponding to Examples 1-7 and Comparative Examples 1-3 were used as the active materials for the cathode materials. The composition of the cathode sheet was m(active material):m(acetylene black):m(polyvinylidene fluoride (PVDF)) = 90:5:5. A coin cell battery was assembled using lithium sheet as the negative electrode and lithium hexafluorophosphate as the electrolyte. The Blue Electric testing system was used for testing. Under the conditions of a charge / discharge current of 0.2C and a voltage range of 2.5-4.25V, the initial charge / discharge specific capacity was tested, and the initial efficiency was calculated as (initial discharge specific capacity / initial charge specific capacity) * 100%. The capacity retention rate was tested after 50 cycles at a charge / discharge current of 1C and a voltage range of 2.5-4.25V. The test results are shown in Table 2. The cycle capacity retention rate test results for Example 3 and Comparative Example 3 are as follows: Figure 3 As shown.

[0112] Table 2

[0113]

[0114] After boric acid coating, Example 3 exhibited excellent cycle retention, maintaining 98.6% of its capacity after 50 cycles. In contrast, the positive electrode material obtained by water washing in Comparative Example 2, after boric acid coating, maintained 91.4% of its capacity after 50 cycles, and the positive electrode material obtained by water washing in Comparative Example 3, after boric acid coating, maintained 92.1% of its capacity after 50 cycles. Figure 3This also demonstrates that the residual alkali reduction scheme in Example 3 reduces residual alkali while avoiding damage to the material caused by the water washing process, resulting in a cathode material with excellent cycle performance. It is evident that the cathode material prepared by the method of this invention, even after boric acid coating, maintains excellent cycle capacity retention and exhibits good cycle performance.

[0115] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

Claims

1. A method for preparing a low-residue, high-nickel ternary cathode material, characterized in that, Includes the following steps: 1) The first precursor, the first additive, and the first lithium salt are mixed and then subjected to a first sintering to obtain cathode material A; the second precursor, the second additive, and the second lithium salt are mixed and then subjected to a second sintering to obtain cathode material B; wherein the particle size D50 of the first precursor is 15-20 μm; and the particle size D50 of the second precursor is 1-5 μm. In the cathode material A, the molar ratio n of lithium to transition metal elements is... Li / n 过渡 >1.00; In the cathode material B, the molar ratio n of lithium to transition metal elements is... Li / n 过渡 <1.00; 2) Mix cathode material A and cathode material B to obtain a mixed cathode material; 3) The mixed cathode material in step 2) is annealed and sintered in an oxygen-containing atmosphere, and then the annealed and sintered product is stirred and sintered at least twice to obtain the low residual alkali and high nickel ternary cathode material.

2. The method for preparing the low-residual-alkali, high-nickel ternary cathode material according to claim 1, characterized in that, In step 3), the annealed and sintered product is stirred and sintered 2-3 times.

3. The method for preparing the low-residue, high-nickel ternary cathode material according to claim 1, characterized in that, In step 1), the first additive and the second additive are each independently selected from at least one of ZrO2, WO3, MoO3, TiO2, Y2O3, Mg(OH)2, Al2O3, TiO2, and H3BO3; The first precursor and the second precursor are each independently selected from at least one of nickel-cobalt-manganese composite oxide, nickel-cobalt-aluminum composite oxide, nickel-cobalt-manganese composite hydroxide, and nickel-cobalt-aluminum hydroxide.

4. The method for preparing the low residual alkali and high nickel ternary cathode material according to claim 1, characterized in that, In step 1), the mass ratio of the first precursor, the first additive, and the first lithium salt is 1:(0.005-0.006):(0.450-0.470). The mass ratio of the second precursor, the second additive, and the second lithium salt is 1:(0.005-0.006):(0.270-0.360).

5. The method for preparing the low residual alkali, high nickel ternary cathode material according to any one of claims 1-4, characterized in that, The general formula of the positive electrode material A is Li a Ni x Co y Q 1-x-y O2, where Q is Mn or Al, 1.00 < a < 1.03, 0.8 ≤ x ≤ 1, 0 ≤ y ≤ 0.2; The cathode material B is selected from Li b Ni x Co y Q 1-x-y O2, where Q is Mn or Al, 0.6 < b < 1, 0.8 ≤ x ≤ 1, 0 ≤ y ≤ 0.

2.

6. The method for preparing the low residual alkali and high nickel ternary cathode material according to claim 1, characterized in that, In step 1), the first lithium salt and the second lithium salt are each independently selected from lithium hydroxide; In step 1), the first sintering temperature is 700-900℃, and the first sintering time is 8-15h; The second sintering temperature is 700-900℃, and the second sintering time is 8-15h; The first sintering is carried out in an oxygen-containing atmosphere; The second sintering is carried out in an oxygen-containing atmosphere.

7. The method for preparing the low-residue, high-nickel ternary cathode material according to claim 6, characterized in that, The lithium hydroxide is selected from LiOH·H2O.

8. The method for preparing the low residual alkali and high nickel ternary cathode material according to claim 1, characterized in that, The mixing speed in step 2) is 150-250 r / min, and the mixing time is 10 min-20 min; The added mass m of cathode material B and the added mass R of cathode material A in step 2) satisfy the following relationship: ,1.01≤ β ≤1.2; In the formula, x1 is the percentage of residual lithium in cathode material A as detected; x2 represents the lithium mass percentage of cathode material B; M is the molar mass of lithium, expressed in mol / g; M 过渡 The molar mass of the transition metal in cathode material B is expressed in mol / g. M B The molar mass of cathode material B is expressed in mol / g. m is the mass of cathode material B added, in grams; R represents the mass of cathode material A added, in grams.

9. The method for preparing the low-residual-alkali, high-nickel ternary cathode material according to claim 8, characterized in that, 1.05≤ β ≤1.2。 10. The method for preparing the low-residue, high-nickel ternary cathode material according to claim 1, characterized in that, The annealing and sintering temperature in step 3) is 500-700℃, the annealing and sintering time is 6-10h, and the heating rate of the annealing and sintering is 2-5℃ / min.

11. The method for preparing the low-residue, high-nickel ternary cathode material according to claim 1, characterized in that, In step 3), the product after annealing and sintering is subjected to stirring and sintering at least twice. The stirring speed is 150-250 r / min and the stirring time is 10 min-20 min. In step 3), the product after annealing and sintering is stirred and sintered at least twice, and the sintering temperature is 500-700℃ and the sintering time is 6-10h.

12. The application of the low-alkali high-nickel ternary cathode material prepared by the preparation method of any one of claims 1-11 in lithium-ion batteries.

Citation Information

Patent Citations

  • Preparation method of high-capacity high-pressure real-density and high-nickel cathode material

    CN107785550A

  • Lithium metal composite oxide powder

    CN109643795A