Layered oxides, their preparation methods, positive electrode sheets, secondary batteries, battery modules, battery packs, and electrical devices.
By using NaxMnyAaQbCcO2 oxide as the positive electrode material, the oxygen holes are stabilized by the charge compensation of Fe and Ni, the hybrid orbitals of 3d or 4d orbital electron transition metals and oxygen, and the formation of covalent bonds between Al or B with high ionic potential. This solves the problem of structural instability of layered oxides under high voltage and achieves improved specific capacity and coulombic efficiency.
Patent Information
- Application Number
- CN202280012902.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-05-31
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-05-31
AI Technical Summary
Layered transition metal oxide cathode materials are prone to generating unstable oxygen holes under high voltage, resulting in poor specific capacity and coulombic efficiency.
The oxide of NaxMnyAaQbCcO2 is used as the cathode material, where A is Fe and Ni, Q is a 3d or 4d orbital electronic transition metal element other than Fe and Ni, and C is Al or B. The hybrid orbitals stabilize oxygen holes and suppress oxygen loss, and the high ionic potential C element forms covalent bonds with oxygen to ensure structural stability.
It improves the specific capacity and coulombic efficiency of layered oxides, enhancing the battery's cycle performance and power cycle stability.
Smart Images

Figure CN117501495B_ABST
Abstract
Description
Technical Field
[0001] This application relates to the field of battery technology, and in particular to a layered oxide, its preparation method, a positive electrode, a secondary battery, a battery module, a battery pack, and an electrical device. Background Technology
[0002] Rechargeable battery technology, as a crucial means of energy storage and conversion, has a wide range of applications in daily life, industrial production, military defense, and aerospace. Currently, lithium-ion batteries, the fastest-growing and most technologically mature rechargeable battery system, have received widespread attention. Rechargeable battery systems, represented by lithium-ion batteries, have become the power source for various portable electronic devices and pure electric vehicles, greatly promoting the development of the electronics and electric vehicle industries. However, lithium resources in the Earth's crust are extremely limited. Statistics show that global lithium carbonate reserves are currently approximately 13 million tons, while the annual consumption of lithium carbonate is increasing at a rate of 16.5% per year. It is estimated that global lithium resources will only last for 28 years. This will severely restrict the further development of lithium-ion batteries and energy storage technologies.
[0003] Sodium and lithium have similar physicochemical properties, but sodium ions have a larger radius than lithium ions, which results in sodium-ion batteries performing worse than lithium-ion batteries. However, the reserves of sodium in the Earth's crust are far greater than those of lithium, giving sodium-ion batteries a natural advantage in terms of cost and supply.
[0004] The cathode material is a crucial component of sodium-ion batteries, responsible for providing active sodium ions. It requires a high redox potential, and its activity directly impacts the battery's capacity and operating voltage. For layered transition metal oxides, based on the sodium content and its position within the crystal structure, the most studied layered materials are primarily classified into O3-type and P2-type. Compared to P2-type layered materials, the main advantage of O3-type layered materials lies in their higher sodium content, resulting in a higher initial discharge specific capacity and the ability to provide more active sodium for the formation of the hard carbon film at the negative electrode throughout the entire battery.
[0005] O3-NaNi 0.4 Mn 0.4 Fe 0.2 O2 material is a transition metal layered oxide cathode material with a high sodium content. This cathode material typically exhibits good cycle stability only at charging voltages between 2.0V and 4.0V. Therefore, it can only provide a relatively limited capacity. Under deep charge-discharge conditions, especially when the charging voltage is increased to above 4.0V, the layered oxide becomes highly unstable due to the loss of electrons from oxygen at high voltages, creating holes that are prone to side reactions. This leads to structural damage and oxygen loss, resulting in reduced specific capacity and coulombic efficiency, and poor cycle stability. Summary of the Invention
[0006] This application provides a layered oxide, its preparation method, a positive electrode sheet, a secondary battery, a battery module, a battery pack, and an electrical device to solve the problem that layered transition metal oxide positive electrode materials are prone to generating unstable local holes on oxygen under high voltage, resulting in poor specific capacity and coulombic efficiency.
[0007] A first aspect of this application provides a layered oxide comprising the general formula Na. x Mn y A a Q b C c O2 oxide, where A is one or both of Fe and Ni; Q is one or more transition metal elements other than Fe and Ni that contain 3d or 4d orbital electrons; C is one or both of Al and B, 0.66 <x≤1,0.2≤y≤0.6,0.3≤a≤0.6,0<b≤0.2,0<c≤0.1,1≤b / c≤100。
[0008] As is well known in the art, the values of x, y, a, b, and c within the aforementioned range make the general formula Na x Mn y A a Q b C c The oxidation state of oxides of O2 is zero.
[0009] The aforementioned layered oxides can be used as positive electrode materials. The Na in this application... x Mn y A a Q b C c In O2 oxides, element A undergoes valence changes during charging and discharging, providing charge compensation and thus improving the specific capacity of layered oxides. Q is one or more transition metal elements (excluding Fe and Ni) containing 3d or 4d orbital electrons. The d orbital of Q hybridizes with the 2p orbital of oxygen in the oxide, forming a hybrid orbital. Local holes on oxygen can be stabilized through this hybrid orbital, thereby suppressing irreversible oxygen loss and structural collapse under high voltage. Simultaneously, element C in its ionic state has a high ionic potential and strong interaction with oxygen, exhibiting a high covalent bond composition, effectively suppressing oxygen loss. Furthermore, with 1 ≤ b / c ≤ 100, the synergy between Q and C effectively suppresses the loss of oxygen and metal during sodium deintercalation under high voltage, further improving the specific capacity of Na. x Mn y A a Q b C cThe structural stability of O2 oxides improves the specific capacity and coulombic efficiency of layered oxides.
[0010] In any embodiment of the first aspect, Q is selected from one or more of the group consisting of Cu, Zn, Y, and Ti. When Q is selected from the aforementioned transition metals, the hybrid orbital formed by its d orbital and the 2p orbital of oxygen is more stable for local holes on oxygen, thus providing a better suppression effect against irreversible oxygen loss.
[0011] In any embodiment of the first aspect, the A contains Fe and Ni to simultaneously utilize iron and nickel to provide stable charge compensation.
[0012] In any embodiment of the first aspect, the layered oxide is in the O3 phase, and the space group is R3m. The O3 phase layered oxide has a high Na content, and therefore has a higher initial charge specific capacity.
[0013] In any embodiment of the first aspect, the interlayer spacing d of the (003) crystal plane of the above-mentioned layered oxide 003 The wavelength is set to 0.53 nm to 0.55 nm to make the structure of the layered oxide more stable.
[0014] In any embodiment of the first aspect, the intensity of the characteristic peak (003) in the X-ray diffraction spectrum of the layered oxide before immersion is I0, and the intensity of the characteristic peak (003) in the X-ray diffraction spectrum of the layered oxide after immersion in water at room temperature for 24 hours is I1, and I1 / I0≥0.2. I1 / I0≥0.2 indicates that the layered oxide has good water stability, and the sodium-ion battery containing it has high energy density and good cycle performance.
[0015] In any embodiment of the first aspect, the pH value of the 10% (w / w) aqueous layered oxide solution is between 11 and 13. A lower pH value makes it easier to prepare and coat the cathode slurry, while a pH value that is too high can cause gelation during the preparation process and make coating difficult.
[0016] In any embodiment of the first aspect, the volume average particle size D of the above-mentioned layered oxide is... v50 The thickness ranges from 3μm to 30μm, and optionally from 5μm to 15μm.
[0017] In any embodiment of the first aspect, the specific surface area (BET) of the layered oxide is 0.1 m². 2 / g~5m 2 / g, optionally 0.3m 2 / g~3m 2 / g.
[0018] In any embodiment of the first aspect, the tap density of the above-mentioned layered oxide is 1 g / cm³.3 ~3g / cm 3 , optionally 1.5g / cm 3 ~2.5g / cm 3 .
[0019] In any embodiment of the first aspect, the powder compaction density of the layered oxide under a pressure of 300MPa is 3.0g / cm 3 ~4.0g / cm 3 .
[0020] When any one of the volume-average particle size D v50 , specific surface area BET, tap density, or powder compaction density under 300MPa pressure of the layered oxide is within the above range, the conduction distance of sodium ions inside the particles is short, and the surface side reactions are few, which is beneficial for the material to exhibit better specific capacity, and the battery using this material has excellent cycle performance.
[0021] A second aspect of the present application provides a preparation method of a layered oxide, wherein the preparation method comprises: Step S1, mixing a Na source, a Mn source, an A source, a Q source, and a C source to obtain a precursor powder, wherein the molar ratio of Na:Mn:A:Q:C of the Na source, Mn source, A source, Q source, and C source is (0.85~1.2):(0.2~0.6):(0.3~0.6):(0~0.2):(0~0.1), the molar amounts of Q and C are not 0, the element A in the A source is one or two of Fe and Ni; the element Q in the Q source is one or more transition metal elements with 3d or 4d orbital electrons other than Fe and Ni; the element C in the C source is one or two of Al and B; Step S2, calcining and pulverizing the precursor powder in an oxidizing atmosphere to obtain the layered oxide. The above preparation method is implemented by a solid-phase method, which is simple to operate and easy to realize. During calcination, part of the Na source is burned and lost, so the sodium source is appropriately excessive during batching, to ensure that the obtained layered oxide contains as much sodium element as possible on the basis of containing the transition metal elements and the C element in the above ratio.
[0022] Using the above preparation method, a layered oxide with the general formula Na x Mn y A a Q b C c O2 can be obtained, wherein 0.66<x≤1, 0.2≤y≤0.6, 0.3≤a≤0.6, 0<b≤0.2, 0<c≤0.1, 1≤b / c≤100. The layered oxide with the general formula Na x Mn y A a Q b C cIn the layered oxide of O2, element A provides charge compensation during charge and discharge by changing its valence, thereby improving the specific capacity of the layered oxide. Q is one or more transition metal elements containing 3d or 4d orbital electrons, excluding Fe and Ni. The d orbital of element Q hybridizes with the 2p orbital of oxygen in the oxide, forming a hybrid orbital. Local holes on oxygen can be stabilized through this hybrid orbital, thus suppressing irreversible oxygen loss and structural collapse under high voltage. Simultaneously, element C in its ionic state has a high ionic potential and strong interaction with oxygen, exhibiting a high covalent bond composition, effectively suppressing oxygen loss. Furthermore, with 1 ≤ b / c ≤ 100, the synergy between element Q and element C effectively suppresses the loss of oxygen and metal during sodium deintercalation under high voltage, further improving the specific capacity of Na. x Mn y A a Q b C c The structural stability of O2 oxides improves the specific capacity and coulombic efficiency of layered oxides.
[0023] In any embodiment of the second aspect, step S1 is performed by ball milling or mechanical stirring. Both ball milling and mechanical stirring can achieve thorough mixing of the substances, especially ball milling under certain conditions, which can achieve more thorough and uniform mixing.
[0024] In any embodiment of the second aspect, the Na source is selected from one or more of the group consisting of Na₂CO₃, NaHCO₃, NaOH, and Na₂O₂; optionally, the Mn source is selected from one or more of the group consisting of Mn₂O₃, Mn₃O₄, MnO, and MnO₂; optionally, the A source is selected from one or more of the group consisting of oxides of A and salts containing the element A, optionally, the element A contains Fe and Ni; optionally, the Q source is one or more of the group consisting of oxides of Q and salts containing the element Q, optionally, the element Q is selected from one or more of the group consisting of Cu, Zn, Y, and Ti; optionally, the C source is one or more of the group consisting of oxides of C and salts containing the element C. The above-mentioned raw materials are widely available and have low costs.
[0025] In any embodiment of the second aspect, the oxidizing atmosphere is selected from air, oxygen, a mixture of oxygen and air, or a mixture of oxygen and an inert gas. Using this oxidizing atmosphere, Mn, A, Q, and C are fully oxidized during the calcination process, achieving a better coordination between the various ion orbitals.
[0026] In any embodiment of the second aspect, the calcination temperature is 700℃~1000℃, and the holding time is 10 hours~30 hours. Optionally, step S2 includes a first calcination stage and a second calcination stage performed sequentially. The calcination temperature of the first calcination stage is 400℃~900℃, and the holding time is 2 hours~20 hours. The calcination temperature of the second calcination stage is 700℃~1000℃, and the holding time is 10 hours~30 hours. The first calcination stage allows the raw materials to undergo a preliminary reaction at a lower temperature, generating layered oxides and allowing the elements to diffuse evenly beforehand. The second calcination stage, with its higher temperature, further enhances the crystallinity of the layered oxides and further promotes the diffusion of different elements. Compared to single calcination conditions, the product obtained by two-stage calcination has a more uniform element distribution and better crystallinity.
[0027] A third aspect of this application provides a positive electrode sheet, comprising a positive current collector and a positive electrode film layer disposed on at least one surface of the positive current collector. The positive electrode film layer comprises a positive electrode active material, which includes a layered oxide of any of the methods described in the first aspect or a layered oxide obtained by any of the preparation methods described in the second aspect. Optionally, the content of the layered oxide in the positive electrode film layer is more than 60% by weight, and more preferably 80% to 98% by weight, based on the total weight of the positive electrode film layer. As a positive electrode active material in the positive electrode film layer, the layered oxide has a stable structure and is not prone to irreversible oxygen loss and metal loss even during sodium deintercalation and deintercalation under high voltage. Therefore, it can provide a high specific capacity and coulombic efficiency for the positive electrode sheet.
[0028] The fourth aspect of this application provides a secondary battery comprising any of the layered oxides of the first aspect, or layered oxides obtained by any of the preparation methods of the second aspect, or a positive electrode sheet of the third aspect.
[0029] The fifth aspect of this application provides a battery module including a secondary battery, wherein the secondary battery is the secondary battery of the fourth aspect.
[0030] The sixth aspect of this application provides a battery pack including a battery module, wherein the battery module is the same as the battery module of the fifth aspect.
[0031] The seventh aspect of this application provides an electrical device including a secondary battery, a battery module, or a battery pack, wherein the secondary battery is selected from the secondary battery of the fourth aspect, the battery module is the battery module of the fifth aspect, or the battery pack is the battery pack of the sixth aspect.
[0032] The layered oxides of this application enable secondary batteries, battery modules, and battery packs incorporating them to exhibit high cycle performance, first-cycle coulombic efficiency, and specific capacity, thereby providing high power cycle stability for electrical devices incorporating secondary batteries, battery modules, or battery packs of this application. Attached Figure Description
[0033] To more clearly illustrate the technical solutions of the embodiments of this application, the drawings used in the embodiments of this application will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on the drawings without creative effort.
[0034] Figure 1 The discharge capacity C1 and charge capacity C0 of the coin cell obtained by testing in Example 1 are shown.
[0035] Figure 2 The discharge capacity C1 and charge capacity C0 of the coin cell obtained from the test of Comparative Example 1 are shown.
[0036] Figure 3 The capacity retention of the coin cells obtained from Example 1 and Comparative Example 1 after 50 cycles is shown.
[0037] Figure 4 The SEM image of the layered oxide of Example 1 after 50 cycles is shown.
[0038] Figure 5 The SEM image of the layered oxide of Comparative Example 1 after 50 cycles is shown.
[0039] Figure 6 This is a schematic diagram of a secondary battery according to one embodiment of this application.
[0040] Figure 7 yes Figure 6 An exploded view of a secondary battery according to one embodiment of this application is shown.
[0041] Figure 8 This is a schematic diagram of a battery module according to one embodiment of this application.
[0042] Figure 9 This is a schematic diagram of a battery pack according to one embodiment of this application.
[0043] Figure 10 yes Figure 9 An exploded view of a battery pack according to one embodiment of this application is shown.
[0044] Figure 11 This is a schematic diagram of an electrical device that uses a secondary battery as a power source according to one embodiment of this application.
[0045] The accompanying drawings are not drawn to scale.
[0046] Explanation of reference numerals in the attached figures:
[0047] 1 Battery pack; 2 Upper housing; 3 Lower housing; 4 Battery module; 5 Secondary battery; 51 Housing; 52 Electrode assembly; 53 Top cover assembly. Detailed Implementation
[0048] The embodiments of this application will be described in further detail below with reference to the accompanying drawings and examples. The detailed description of the following embodiments and the accompanying drawings are used to illustrate the principles of this application by way of example, but should not be used to limit the scope of this application, that is, this application is not limited to the described embodiments.
[0049] The following detailed description, with appropriate reference to the accompanying drawings, discloses embodiments of the layered oxide, its preparation method, positive electrode sheet, secondary battery, battery module, battery pack, and power-consuming device of this application. However, unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repetitive descriptions of practically identical structures may be omitted. This is to avoid unnecessarily lengthy descriptions and to facilitate understanding by those skilled in the art. Furthermore, the accompanying drawings and the following description are provided for a full understanding of this application by those skilled in the art and are not intended to limit the subject matter of the claims.
[0050] The "range" disclosed in this application is defined by a lower limit and an upper limit. A given range is defined by selecting a lower limit and an upper limit, which define the boundaries of a particular range. Ranges defined in this way can include or exclude endpoints and can be arbitrarily combined; that is, any lower limit can be combined with any upper limit to form a range. For example, if ranges of 60–120 and 80–110 are listed for a specific parameter, it is understood that ranges of 60–110 and 80–120 are also expected. Furthermore, if minimum range values of 1 and 2 are listed, and if maximum range values of 3, 4, and 5 are listed, then the following ranges are all expected: 1–3, 1–4, 1–5, 2–3, 2–4, and 2–5. In this application, unless otherwise stated, the numerical range "a–b" represents a shortened representation of any combination of real numbers between a and b, where a and b are real numbers. For example, the numerical range "0~5" indicates that all real numbers between "0~5" have been listed in this article; "0~5" is simply a shortened representation of these numerical combinations. Furthermore, when a parameter is stated as an integer ≥2, it is equivalent to disclosing that the parameter is, for example, an integer such as 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0051] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions.
[0052] Unless otherwise specified, all technical features and optional technical features of this application may be combined to form new technical solutions.
[0053] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, optionally sequentially. For example, the method includes steps (a) and (b), indicating that the method may include steps (a) and (b) performed sequentially, or it may include steps (b) and (a) performed sequentially. For example, the method may also include step (c), indicating that step (c) may be added to the method in any order. For example, the method may include steps (a), (b), and (c), or it may include steps (a), (c), and (b), or it may include steps (c), (a), and (b), etc.
[0054] Unless otherwise specified, the terms "comprising" and "including" as used in this application can be open-ended or closed-ended. For example, "comprising" and "including" can mean that other components not listed may also be included, or that only the listed components may be included.
[0055] Unless otherwise specified, the term "or" is inclusive in this application. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, the condition "A or B" is satisfied by any of the following conditions: A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0056] [Rechargeable Battery]
[0057] Secondary batteries, also known as rechargeable batteries or storage batteries, are batteries that can be recharged after being discharged to activate the active materials and continue to be used.
[0058] Typically, a secondary battery consists of a positive electrode, a negative electrode, a separator, and an electrolyte. During charging and discharging, active ions (such as lithium ions or sodium ions) repeatedly insert and extract between the positive and negative electrodes. The separator, positioned between the positive and negative electrodes, primarily prevents short circuits while allowing active ions to pass through. The electrolyte, also positioned between the positive and negative electrodes, mainly serves to conduct active ions.
[0059] [Layered oxides]
[0060] One embodiment of this application provides a layered oxide, which includes a general formula Na.x Mn y A a Q b C c O2 oxide, where A is one or both of Fe and Ni; Q is one or more transition metal elements with 3d or 4d orbital electrons other than Fe and Ni; C is one or both of Al and B, 0.66<x≤1, for example, x is 0.67, 0.70, 0.75, 0.80, 0.85, 0.90, 0.95 or 1; 0.2≤y≤0.6, for example, a is 0.2, 0.3, 0.4, 0.5 or 0.6; 0.3≤a≤0.6, for example, a is 0.3, 0.4, 0.5 or 0.6; 0<b≤0.2, for example, b is 0.01, 0.05, 0.1, 0.15 or 0.2; 0<c≤0.1, for example, c is 0.01, 00.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09 or 0.1; 1≤b / c≤100, for example, b / c is 1, 5, 10, 20, 30, 40, 50, 60, 70, 80, 90 or 100.
[0061] The above layered oxide can be used as a positive electrode material.
[0062] Na of the present application x Mn y A a Q b C c In the O2 oxide, element A undergoes valence change during charge and discharge to provide charge compensation, thereby increasing the specific capacity of the layered oxide; Q is one or more transition metal elements with 3d or 4d orbital electrons other than Fe and Ni, whose d orbitals hybridize with the 2p orbitals of oxygen in the layered oxide structure. When oxygen is oxidized to lose electrons and form holes at high voltage, the holes can be stabilized through the hybrid orbitals formed by the hybridization of the d orbitals and the 2p orbitals of oxygen in the structure, thereby inhibiting irreversible oxygen loss and structural collapse of oxygen at high voltage; while elements without d orbitals, such as Li and Mg, cannot effectively hybridize with the 2p orbitals of oxygen in the structure, resulting in the presence of non-bonding 2p orbitals of oxygen. Therefore, even if Li or Mg is doped, neither of them can prevent the loss of oxygen atoms at high voltage, and thus cannot alleviate local structural collapse and metal loss, causing problems such as low charge-discharge energy conversion efficiency and poor cycle stability.
[0063] The mere presence of element Q is not sufficient to effectively inhibit the irreversible oxygen loss and structural collapse of oxygen at high voltage. The present application finds that Al with high ionic potential 3+ or B 3+ and the transition metal element containing d orbital electrons can synergistically greatly inhibit the loss of oxygen, because Al with high ionic potential 3+Or B 3+ It has a strong interaction with oxygen, and its bond with oxygen has a high covalent component, which can effectively inhibit oxygen loss.
[0064] However, Al with high ionic potential 3+ Or B 3+ The ionic potential between the transition metal and the element containing d-orbital electrons must be maintained within the range of 1 ≤ b / c ≤ 100. If b / c < 1, the local ionic potential of the layered oxide is too high, the d-orbitals of the transition metal hybridize less with the 2p-orbitals of oxygen in the structure, the metal-oxygen octahedron undergoes significant distortion, the layered structure becomes locally unstable, and the mixing of metal ions and sodium ions easily occurs, forming a local spinel / rock salt phase, which hinders the diffusion and deintercalation of sodium ions. If b / c < 100, the ionic potential is too high. 3+ Or B 3+ If the content is too low, it is insufficient to synergistically suppress oxygen loss with transition metal elements containing d-orbital electrons. Only when 1≤b / c≤100 is the resulting layered oxide possessing a relatively stable layered structure, and oxygen and metal loss is not easily observed during sodium insertion / extraction under high pressure.
[0065] Therefore, when 1 ≤ b / c ≤ 100, the Q and C elements work together to effectively suppress the loss of oxygen and metal during sodium deintercalation under high voltage, further improving the performance of Na. x Mn y A a Q b C c The structural stability of O2 oxides improves the specific capacity and coulombic efficiency of layered oxides.
[0066] In some embodiments, the aforementioned 0.7≤x≤1 can optionally be 0.8≤x≤1 or 0.9≤x≤1; optionally, 0.01≤b≤0.2 or 0.05≤b≤0.15; optionally, 0.01≤c≤0.1 or 0.01≤c≤0.05 or 0.01≤c≤0.02; optionally, 1≤b / c≤100 or 1≤b / c≤50 or 1≤b / c≤10 or 4≤b / c≤50. Through the further control of x, b, c, and b / c, the synergistic effect between the elements is optimized, further improving the inhibitory effect on irreversible oxygen loss.
[0067] There are many types of transition metal elements with 3d or 4d orbital electrons. To fully enhance the stabilizing effect of the hybrid orbitals formed by the 3d and 4d orbitals and the 2p orbital of oxygen on localized holes in oxygen, in some embodiments of the first aspect, the aforementioned Q is selected from one or more of the group consisting of Cu, Zn, Y, and Ti. When Q is selected from the aforementioned transition metals, the hybrid orbitals formed by its d orbitals and the 2p orbital of oxygen have a stronger stabilizing effect on localized holes in oxygen, thus resulting in a better suppression effect on irreversible oxygen loss.
[0068] In some embodiments, the A above contains Fe and Ni to simultaneously utilize iron and nickel to provide stable charge compensation, and the presence of iron and nickel also helps to maintain a more stable layered structure.
[0069] In some embodiments, the phase state of the above-mentioned layered oxide is O3 phase, and the space group is The O3 phase layered oxide has a high Na content, thus exhibiting a higher initial charge specific capacity.
[0070] In some embodiments, the interlayer spacing d of the (003) crystal plane of the above-mentioned layered oxide is... 003 The wavelength is set to 0.53 nm to 0.55 nm to make the structure of the layered oxide more stable.
[0071] In some embodiments, the intensity of the (003) characteristic peak in the X-ray diffraction spectrum of the layered oxide before immersion is I0, and the intensity of the (003) characteristic peak in the X-ray diffraction spectrum of the layered oxide after immersion in water at room temperature for 24 hours is I1, and I1 / I0 ≥ 0.2. I1 / I0 can represent the water stability of the layered oxide cathode active material. The smaller the I1 / I0, the worse the water stability of the layered oxide cathode active material, and the more sensitive it is to water. Studies have found that I1 / I0 ≥ 0.2 indicates that the layered oxide has good water stability, and sodium-ion batteries containing it have higher energy density and better cycle performance. The change in the intensity of the (003) characteristic peak in the X-ray diffraction spectrum of the layered oxide cathode active material before and after immersion in water for 24 hours can be observed using an X-ray powder diffractometer.
[0072] The layered oxide has residual alkali on its surface, thus making it alkaline. After doping with the A, Q, and C elements described in this application, the residual alkali on the surface is reduced. In any of the embodiments of the first aspect, the pH value of the 10% (w / w) aqueous solution of the layered oxide is between 11 and 13. A lower pH value makes it easier to prepare and coat the cathode slurry, while a pH value that is too high can cause gelation during the preparation process and make coating difficult.
[0073] It should be noted that in this paper, the volume average particle size D v50This refers to the particle size corresponding to a cumulative volumetric distribution percentage of 50% for layered oxides. In this application, the volume average particle size D of the layered oxides... v50 The particle size distribution can be determined using laser diffraction particle size analysis. For example, it can be determined using a laser particle size analyzer (e.g., MalvernMaster Size 3000) according to standard GB / T 19077-2016. In some embodiments of the first aspect, the D of the above-mentioned layered oxide... v50 The thickness ranges from 3μm to 30μm, and optionally from 5μm to 15μm. This is achieved through the analysis of D... v50 The control of particle size ensures that the specific capacity of the secondary battery using this layered oxide is fully utilized, while also avoiding the agglomeration of ions caused by excessively small particle size, which would affect the dispersion effect of the material.
[0074] In some embodiments, the specific surface area (BET) of the layered oxide is 0.1 m². 2 / g~5m 2 / g, optionally 0.3m 2 / g~3m 2 / g, and optionally 0.3m 2 / g~0.7m 2 / g. When the specific surface area is less than the above range, the conductivity of the layered oxide is relatively reduced, affecting the rate performance improvement of the secondary battery; when the specific surface area is greater than the above range, the contact area between the layered oxide and the non-aqueous electrolyte increases, making it easier to initiate interfacial side reactions, thus affecting the cycle performance and storage performance of the secondary battery. The specific surface area of the layered oxide has a well-known meaning in the art and can be determined using instruments and methods well-known in the art. For example, it can be tested using the nitrogen adsorption specific surface area analysis method according to GB / T 19587-2017 and calculated using the BET (Brunauer Emmett Teller) method.
[0075] In some embodiments, the tap density of the above-mentioned layered oxide is 1 g / cm³. 3 ~3g / cm 3 Optionally, it can be 1.5 g / cm³. 3 ~2.5g / cm 3 Tap density can be determined using instruments and methods known in the art, such as according to GB / T5162-2006. When the tap density is within the above range, the material stacking is more dense, which is beneficial for improving the electrode compaction density and the volumetric energy density of the battery cell.
[0076] In some embodiments, the compacted density of the layered oxide powder at 300 MPa pressure is 3.0 g / cm³. 3 ~4.0g / cm 3. The higher the compaction density, the greater the weight of the layered oxide per unit volume, so increasing the compaction density is beneficial to improving the volumetric energy density of the cell. The compaction density can be measured according to GB / T 24533-2009.
[0077] When the volume average particle size D of the layered oxide v50 , any one of the specific surface area BET, tap density, or powder compaction density at 300MPa is within the above range, the conduction distance of sodium ions in the particles is short, and the surface side reactions are few, which is conducive to the material exhibiting better specific capacity, and the battery using this material has excellent cycle performance.
[0078] The above-mentioned layered oxide of the present application can be prepared by a conventional solid-phase method or a co-precipitation method in the art.
[0079] Another embodiment of the present application provides a method for preparing a layered oxide, wherein the preparation method comprises: Step S1, mixing a Na source, a Mn source, an A source, a Q source, and a C source to obtain a precursor powder, where the molar ratio of Na:Mn:A:Q:C of the Na source, Mn source, A source, Q source, and C source is (0.85-1.2):(0.2-0.6):(0.3-0.6):(0-0.2):(0-0.1), the molar amounts of Q and C are not 0, the element A in the A source is one or two of Fe and Ni; the element Q in the Q source is one or more transition metal elements with 3d or 4d orbital electrons other than Fe and Ni; the element C in the C source is one or two of Al and B; Step S2, calcining and pulverizing the precursor powder in an oxidizing atmosphere to obtain the layered oxide. Implementing the above preparation method by the solid-phase method has simple operation and is easy to realize. During calcination, part of the Na source is burned and lost, so the sodium source is appropriately excessive during batching to ensure that the obtained layered oxide contains as much sodium element as possible on the basis of containing the transition metal elements and the C element in the above ratio.
[0080] Using the above preparation method, a layered oxide with the general formula Na x Mn y A a Q b C c O2 can be obtained, where 0.66<x≤1, 0.2≤y≤0.6, 0.3≤a≤0.6, 0<b≤0.2, 0<c≤0.1, 1≤b / c≤100. The above general formula is Na x Mn y A a Q b C cIn the layered oxide of O2, element A provides charge compensation during charge and discharge by changing its valence, thereby improving the specific capacity of the layered oxide. Q is one or more transition metal elements containing 3d or 4d orbital electrons, excluding Fe and Ni. The d orbital of element Q hybridizes with the 2p orbital of oxygen in the oxide, forming a hybrid orbital. Local holes on oxygen can be stabilized through this hybrid orbital, thus suppressing irreversible oxygen loss and structural collapse under high voltage. Simultaneously, element C in its ionic state has a high ionic potential and strong interaction with oxygen, exhibiting a high covalent bond composition, effectively suppressing oxygen loss. Furthermore, with 1 ≤ b / c ≤ 100, the synergy between element Q and element C effectively suppresses the loss of oxygen and metal during sodium deintercalation under high voltage, further improving the specific capacity of Na. x Mn y A a Q b C c The structural stability of O2 oxides improves the specific capacity and coulombic efficiency of layered oxides.
[0081] In some embodiments, step S1 above is performed by ball milling or mechanical stirring. Both ball milling and mechanical stirring can achieve thorough mixing of the substances, especially ball milling, which can achieve more thorough mixing under certain conditions. A dry ball mill can be selected, using zirconium balls as grinding balls. The specific operating conditions for ball milling and mechanical stirring, such as grinding ball diameter and rotation speed, can be referenced using conventional methods and will not be elaborated here.
[0082] The Na source, Mn source, A source, Q source, and C source used in the preparation method described above in this application can be any salt, oxide, hydroxide, etc., commonly used in the art. In some embodiments of the second aspect, the Na source is selected from one or more of the group consisting of Na₂CO₃, NaHCO₃, NaOH, and Na₂O₂; optionally, the Mn source is selected from one or more of the group consisting of Mn₂O₃, Mn₃O₄, MnO, and MnO₂; optionally, the A source is selected from one or more of the group consisting of oxides of A and salts containing A, optionally, the A element contains Fe and Ni; optionally, the Q source is one or more of the group consisting of oxides of Q and salts containing Q, optionally, the Q element is selected from one or more of the group consisting of Cu, Zn, Y, and Ti; optionally, the C source is one or more of the group consisting of oxides of C and salts containing C. The above-mentioned raw materials are widely available and have low cost.
[0083] In some embodiments, the oxidizing atmosphere is selected from air, oxygen, a mixture of oxygen and air, or a mixture of oxygen and an inert gas. Utilizing this oxidizing atmosphere provides sufficient active oxygen during calcination, resulting in layered oxides with better crystallinity. The volume ratio of oxygen to air in the oxygen-air mixture can be 1:99 to 99:1, and the volume ratio of oxygen to inert gas in the oxygen-inert gas mixture can be 10:90 to 90:10, wherein the inert gas is argon, helium, or nitrogen, which are well known to those skilled in the art.
[0084] In some embodiments, the calcination temperature is 700℃~1000℃, and the holding time is 10 hours~30 hours. Optionally, step S2 includes a first calcination stage and a second calcination stage performed sequentially. The calcination temperature of the first calcination stage is 400℃~900℃, and the holding time is 2 hours~20 hours. The calcination temperature of the second calcination stage is 700℃~1000℃, and the holding time is 10 hours~30 hours. The first calcination stage allows the raw materials to undergo a preliminary reaction at a lower temperature, generating layered oxides and allowing the elements to diffuse evenly beforehand. The second calcination stage, with its higher temperature, further enhances the crystallinity of the layered oxides and further promotes the diffusion of different elements. Compared to single calcination conditions, the product obtained by two-stage calcination has a more uniform element distribution and better crystallinity.
[0085] [Positive electrode plate]
[0086] The positive electrode typically includes a positive current collector and a positive electrode film layer disposed on at least one surface of the positive current collector. The positive electrode film layer includes a positive electrode active material, which includes any layered oxide of this application or a layered oxide obtained by any of the preparation methods described in the second aspect above.
[0087] As an example, the positive current collector has two surfaces opposite each other in its own thickness direction, and the positive electrode film layer is disposed on either or both of the two opposite surfaces of the positive current collector.
[0088] In some embodiments, the positive current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer substrate and a metal layer formed on at least one surface of the polymer substrate. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0089] In some embodiments, the content of layered oxide in the positive electrode film layer, based on the total weight of the positive electrode film layer, is 60% by weight or more, optionally from 80% by weight to 98% by weight. Furthermore, the positive electrode active material may also be a known positive electrode active material for batteries. As an example, the positive electrode active material may include at least one of the following materials: sodium phosphate, sodium Prussian cyanide. However, this application is not limited to these materials, and other conventional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Examples of sodium phosphate include, but are not limited to, at least one of sodium vanadium phosphate (such as Na3V2(PO4)3), a composite material of sodium vanadium phosphate and carbon, Na4Fe3(PO4)2(P2O7), a composite material of Na4Fe3(PO4)2(P2O7) and carbon, Na3V2(PO4)2O2F, and a composite material of Na3V2(PO4)2O2F and carbon. Examples of sodium-containing Prussian cyanide may include, but are not limited to, Na2Mn[Fe(CN)6], composites of Na2Mn[Fe(CN)6] and carbon, Na2Fe[Fe(CN)6], and composites of Na2Fe[Fe(CN)6] and carbon.
[0090] In some embodiments, the positive electrode film layer may optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF-tetrafluoroethylene-propylene terpolymer, PVDF-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorinated acrylate resin.
[0091] In some embodiments, the positive electrode film may optionally include a conductive agent. As an example, the conductive agent may include at least one selected from superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0092] In some embodiments, the positive electrode sheet can be prepared by dispersing the above-mentioned components for preparing the positive electrode sheet, such as positive active material, conductive agent, binder and any other components, in a solvent (e.g., N-methylpyrrolidone) to form a positive electrode slurry; coating the positive electrode slurry onto the positive electrode current collector, and then obtaining the positive electrode sheet after drying, cold pressing and other processes.
[0093] [Negative electrode plate]
[0094] The negative electrode sheet includes a negative current collector and a negative electrode film layer disposed on at least one surface of the negative current collector, the negative electrode film layer including a negative electrode active material.
[0095] As an example, the negative electrode current collector has two surfaces opposite each other in its own thickness direction, and the negative electrode film layer is disposed on either or both of the two opposite surfaces of the negative electrode current collector.
[0096] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymeric material substrate and a metal layer formed on at least one surface of the polymeric material substrate. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymeric material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0097] In some embodiments, the negative electrode active material may be a negative electrode active material known in the art for use in batteries. As an example, the negative electrode active material may include at least one of the following materials: soft carbon, hard carbon, silicon-based materials, tin-based materials, and sodium titanate, etc. Silicon-based materials may be selected from at least one of elemental silicon, silicon oxides, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. Tin-based materials may be selected from at least one of elemental tin, tin oxides, and tin alloys. However, this application is not limited to these materials, and other conventional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0098] In some embodiments, the negative electrode film layer may optionally include a binder. As an example, the binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).
[0099] In some embodiments, the negative electrode film may optionally include a conductive agent. As an example, the conductive agent may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0100] In some embodiments, the negative electrode film may optionally include other additives, such as thickeners (e.g., sodium carboxymethyl cellulose (CMC-Na)).
[0101] In some embodiments, the negative electrode sheet can be prepared by dispersing the components used to prepare the negative electrode sheet, such as the negative electrode active material, conductive agent, binder and any other components, in a solvent (e.g., deionized water) to form a negative electrode slurry; coating the negative electrode slurry onto the negative electrode current collector, and then obtaining the negative electrode sheet after drying, cold pressing and other processes.
[0102] [Electrolytes]
[0103] The electrolyte acts as a conductor of ions between the positive and negative electrodes. This application does not impose specific restrictions on the type of electrolyte; it can be selected according to requirements. For example, the electrolyte can be liquid, gel, or entirely solid.
[0104] In some embodiments, the electrolyte is liquid and includes an electrolyte salt and a solvent.
[0105] In some embodiments, the electrolyte salt may be selected from at least one of NaPF6, NaClO4, NaBF4, NaNO3, NaPOFA, NaSCN, NaCN, NaAsF6, NaCF3CO2, NaSbF6, NaC6HsCO2, Na(CH3)C6H4SO3, NaHSO4, and NaB(C6Hs)4.
[0106] In some embodiments, the solvent may be selected from at least one of ethylene carbonate, propylene carbonate, methyl ethyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butyl carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, sulfolane, dimethyl sulfone, methyl ethyl sulfone, and diethyl sulfone.
[0107] In some embodiments, the electrolyte may optionally include additives. As examples, additives may include negative electrode film-forming additives, positive electrode film-forming additives, and may also include additives that can improve certain battery performance, such as additives that improve battery overcharge performance, additives that improve battery high-temperature or low-temperature performance, etc.
[0108] [Isolation membrane]
[0109] In some embodiments, the secondary battery also includes a separator. This application does not impose any particular limitation on the type of separator; any known porous separator with good chemical and mechanical stability can be selected.
[0110] In some embodiments, the material of the separator can be selected from at least one of glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0111] In some implementations, the positive electrode, negative electrode, and separator can be fabricated into an electrode assembly using a winding or stacking process.
[0112] In some embodiments, the secondary battery may include an outer packaging. This outer packaging may be used to encapsulate the aforementioned electrode assembly and electrolyte.
[0113] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, or a steel shell. The outer packaging of the secondary battery can also be a soft pack, such as a pouch. The material of the soft pack can be plastic; examples of plastics include polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0114] This application does not impose any particular limitation on the shape of the secondary battery; it can be cylindrical, square, or any other arbitrary shape. For example, Figure 6 This is an example of a square-structured secondary battery 5.
[0115] In some implementations, refer to Figure 7 The outer packaging may include a housing 51 and a cover 53. The housing 51 may include a base plate and side plates connected to the base plate, the base plate and side plates forming a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the cover 53 can be placed over the opening to close the receiving cavity. A positive electrode, a negative electrode, and a separator can be formed into an electrode assembly 52 using a winding or stacking process. The electrode assembly 52 is encapsulated within the receiving cavity. Electrolyte is immersed in the electrode assembly 52. The secondary battery 5 may contain one or more electrode assemblies 52, which can be selected by those skilled in the art according to specific practical needs.
[0116] In some implementations, the secondary batteries can be assembled into a battery module, and the number of secondary batteries contained in the battery module can be one or more, the specific number of which can be selected by those skilled in the art according to the application and capacity of the battery module.
[0117] Figure 8 This is battery module 4, used as an example. (See reference...) Figure 8 In battery module 4, multiple secondary batteries 5 can be arranged sequentially along the length of battery module 4. Of course, they can also be arranged in any other manner. Furthermore, these multiple secondary batteries 5 can be fixed in place using fasteners.
[0118] Optionally, the battery module 4 may also include a housing with a receiving space in which a plurality of secondary batteries 5 are received.
[0119] In some embodiments, the battery modules described above can also be assembled into a battery pack, and the number of battery modules contained in the battery pack can be one or more, the specific number of which can be selected by those skilled in the art according to the application and capacity of the battery pack.
[0120] Figure 9 and Figure 10 This is battery pack 1 as an example. (See reference...) Figure 9 and Figure 10 The battery pack 1 may include a battery box and multiple battery modules 4 disposed within the battery box. The battery box includes an upper body 2 and a lower body 3, with the upper body 2 covering the lower body 3 to form a closed space for accommodating the battery modules 4. The multiple battery modules 4 can be arranged in any manner within the battery box.
[0121] In addition, this application also provides an electrical device, which includes at least one of the secondary battery, battery module, or battery pack provided in this application. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device, or as an energy storage unit for the electrical device. The electrical device may include, but is not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.
[0122] As the electrical device, a secondary battery, battery module, or battery pack can be selected according to its usage requirements.
[0123] Figure 11 This is an example of an electrical device. The device could be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. To meet the high power and high energy density requirements of the secondary battery for this device, a battery pack or battery module can be used.
[0124] [Example]
[0125] The following describes embodiments of this application. The embodiments described below are exemplary and are only used to explain this application, and should not be construed as limiting this application. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Reagents or instruments used, unless otherwise specified, are all conventional products that can be obtained commercially.
[0126] Example 1
[0127] Preparation of aluminum-doped layered oxides
[0128] A total of 30 g of sample was weighed, consisting of Na₂CO₃, Mn₂O₃, Fe₂O₃, NiO, Al₂O₃, and CuO, in a molar ratio of Na:Mn:Fe:Ni:Al:Cu of 1:0.49:0.2:0.2:0.01:0.1. The sample was pre-ground in an agate mortar and then ball-milled for 1 hour in a planetary ball mill at a ball-to-material ratio of 8:1 (zirconia balls) at 500 rpm to obtain a precursor mixture. This precursor mixture was then uniformly placed in an open crucible and heated in a muffle furnace from room temperature to 950°C at a rate of 5°C / min, and held at 950°C for 15 hours. After natural cooling, layered oxide Na₂CO₃ was obtained. 0.81 Mn 0.49 Fe 0.2 Ni 0.2 Al 0.01 Cu 0.1 O2.
[0129] Example 2
[0130] The difference from Example 1 is that 30g of sample was weighed, consisting of Na2CO3, Mn2O3, Fe2O3, NiO, B2O3, and CuO, in a molar ratio of Na:Mn:Fe:Ni:B:Cu of 1:0.49:0.2:0.2:0.01:0.1. The remaining procedures were the same as in Example 1.
[0131] Example 3
[0132] The difference from Example 1 is that 30g of sample was weighed, consisting of Na2CO3, Mn2O3, Fe2O3, NiO, Al2O3, and Y2O3 in a molar ratio of Na:Mn:Fe:Ni:Al:Y of 1:0.49:0.2:0.2:0.01:0.1. The remaining procedures were the same as in Example 1.
[0133] Example 4
[0134] The difference from Example 1 is that 30g of sample was weighed, consisting of Na2CO3, Mn2O3, Fe2O3, NiO, B2O3, and ZnO in a molar ratio of Na:Mn:Fe:Ni:B:Zn of 1:0.48:0.2:0.2:0.02:0.1. The remaining procedures were the same as in Example 1.
[0135] Example 5
[0136] The difference from Example 1 is that 30g of sample was weighed, consisting of Na2CO3, Mn2O3, Fe2O3, NiO, B2O3, and TiO2, in a molar ratio of Na:Mn:Fe:Ni:B:Ti of 1:0.48:0.2:0.2:0.02:0.1. The remaining procedures were the same as in Example 1.
[0137] Example 6
[0138] The difference from Example 1 is that 30g of sample was weighed, consisting of Na2CO3, Mn2O3, Fe2O3, NiO, B2O3, and Y2O3 in a molar ratio of Na:Mn:Fe:Ni:B:Y of 1:0.49:0.2:0.2:0.01:0.1. The remaining procedures were the same as in Example 1.
[0139] Example 7
[0140] The difference from Example 1 is that 30g of sample was weighed, consisting of Na2CO3, Mn2O3, Fe2O3, NiO, Al2O3, and TiO2, in a molar ratio of Na:Mn:Fe:Ni:Al:Ti of 1:0.398:0.2:0.2:0.002:0.2. The remaining procedures were the same as in Example 1.
[0141] Example 8
[0142] The difference from Example 1 is that: 30g of sample was weighed, consisting of Na₂CO₃, Mn₂O₃, Fe₂O₃, NiO, B₂O₃, and CuO, in a molar ratio of Na:Mn:Fe:Ni:B:Cu of 1:0.49:0.2:0.1:0.01:0.2. The remaining procedures were the same as in Example 1.
[0143] Example 9
[0144] The difference from Example 1 is that 30g of sample was weighed, consisting of Na2CO3, Mn2O3, Fe2O3, NiO, B2O3, and CuO, in a molar ratio of Na:Mn:Fe:Ni:B:Cu of 1:0.29:0.3:0.3:0.01:0.1. The remaining procedures were the same as in Example 1.
[0145] Example 10
[0146] The difference from Example 1 is that 30g of sample was weighed, consisting of Na2CO3, Mn2O3, Fe2O3, NiO, B2O3, and CuO, in a molar ratio of Na:Mn:Fe:Ni:B:Cu of 1:0.4:0.2:0.2:0.1:0.1. The remaining procedures were the same as in Example 1.
[0147] Example 11
[0148] The difference from Example 1 is that 30g of sample was weighed, consisting of Na2CO3, Mn2O3, Fe2O3, NiO, A2O3, and CuO, in a molar ratio of Na:Mn:Fe:Ni:Al:Cu of 1:0.49:0.2:0.2:0.055:0.055. The remaining procedures were the same as in Example 1.
[0149] Example 12
[0150] The difference from Example 1 is that 30g of sample was weighed, consisting of Na2CO3, Mn2O3, Fe2O3, NiO, Al2O3, and CuO, in a molar ratio of Na:Mn:Fe:Ni:Al:Cu of 1:0.49:0.2:0.2:0.02:0.09. The remaining procedures were the same as in Example 1.
[0151] Example 13
[0152] The difference from Example 1 is that 30g of sample was weighed, consisting of Na2CO3, Mn2O3, Fe2O3, NiO, Al2O3, and CuO, in a molar ratio of Na:Mn:Fe:Ni:Al:Cu of 1:0.49:0.2:0.2:0.005:0.105. The remaining procedures were the same as in Example 1.
[0153] Example 14
[0154] The difference from Example 1 is that 30g of sample was weighed, consisting of Na2CO3, Mn2O3, Fe2O3, NiO, Al2O3, and CuO, in a molar ratio of Na:Mn:Fe:Ni:Al:Cu of 1:0.49:0.2:0.2:0.002:0.108. The remaining procedures were the same as in Example 1.
[0155] Example 15
[0156] The difference from Example 1 is that 30g of sample was weighed, consisting of Na2CO3, Mn2O3, Fe2O3, NiO, Al2O3, and CuO, in a molar ratio of Na:Mn:Fe:Ni:Al:Cu of 1:0.49:0.2:0.2:0.0012:0.1088. The remaining procedures were the same as in Example 1.
[0157] Example 16
[0158] The difference from Example 1 is that 30g of sample was weighed, consisting of Na2CO3, Mn2O3, Fe2O3, NiO, Al2O3, and CuO, in a molar ratio of Na:Mn:Fe:Ni:Al:Cu of 0.85:0.49:0.2:0.2:0.01:0.1. The remaining procedures were the same as in Example 1.
[0159] Example 17
[0160] The difference from Example 1 is that 30g of sample was weighed, consisting of Na2CO3, Mn2O3, Fe2O3, NiO, Al2O3, and CuO, in a molar ratio of Na:Mn:Fe:Ni:Al:Cu of 1.2:0.49:0.2:0.2:0.01:0.1. The remaining procedures were the same as in Example 1.
[0161] Example 18
[0162] The difference from Example 1 is that 30g of sample was weighed, consisting of Na₂CO₃, Mn₂O₃, Fe₂O₃, NiO, Al₂O₃, and CuO, in a molar ratio of Na:Mn:Fe:Ni:Al:Cu of 1:0.2:0.25:0.25:0.1:0.2. The remaining procedures were the same as in Example 1. Layered oxides
[0163] Example 19
[0164] The only difference from Example 1 is the calcination conditions of the sodium source and precursor mixture, as detailed below:
[0165] The sodium source used was NaOH. The mixture of the obtained precursor and NaOH was uniformly placed in an open crucible, and then heated from room temperature to 700℃ in a muffle furnace at a heating rate of 5℃ / min. This temperature was then held at 700℃ for 30 hours. After natural cooling, layered oxide Na₂ was obtained. 0.81 Mn 0.49 Fe 0.2 Ni 0.2 Al 0.01 Cu 0.1 O2.
[0166] Example 20
[0167] The only difference from Example 1 is the calcination conditions of the precursor mixture, as follows:
[0168] The obtained precursor mixture was uniformly placed in an open crucible, and then heated from room temperature to 1000℃ in a muffle furnace at a heating rate of 5℃ / min, and held at 1000℃ for 10 hours. After natural cooling, layered oxide Na was obtained. 0.81 Mn 0.49 Fe 0.2 Ni 0.2 Al 0.01 Cu 0.1 O2.
[0169] Example 21
[0170] The only difference from Example 1 is the calcination conditions of the precursor mixture, as follows:
[0171] The obtained precursor mixture was uniformly placed in an open crucible, and then heated from room temperature to 1100℃ in a muffle furnace at a heating rate of 5℃ / min, and held at 1100℃ for 8 hours. After natural cooling, layered oxide Na was obtained. 0.72 Mn 0.49 Fe 0.2 Ni 0.2 Al 0.01 Cu 0.1 O2.
[0172] Example 22
[0173] The only difference from Example 1 is the calcination conditions of the sodium source and precursor mixture, as detailed below:
[0174] NaOH was used as the sodium source. The mixture of the obtained precursor and NaOH was uniformly placed in an open crucible, and then heated from room temperature to 400℃ in a muffle furnace at a heating rate of 5℃ / min, and held at 400℃ for 20h. Then, the temperature was further increased from 400℃ to 700℃ at a heating rate of 5℃ / min, and held at 700℃ for 30h. After natural cooling, layered oxide Na was obtained. 0.86 Mn 0.49 Fe 0.2 Ni 0.2 Al 0.01 Cu 0.1 O2.
[0175] Example 23
[0176] The only difference from Example 1 is the calcination conditions of the precursor mixture, as follows:
[0177] The obtained precursor mixture was uniformly placed in an open crucible, and then heated from room temperature to 400℃ in a muffle furnace at a heating rate of 5℃ / min, and held at 400℃ for 20 h; then the temperature was further increased from 400℃ to 1000℃ at a heating rate of 5℃ / min, and held at 1000℃ for 10 h. After natural cooling, layered oxide Na was obtained. 0.78 Mn 0.49 Fe 0.2 Ni 0.2 Al 0.01 Cu 0.1 O2.
[0178] Example 24
[0179] The only difference from Example 1 is the calcination conditions of the precursor mixture, as follows:
[0180] The obtained precursor mixture was uniformly placed in an open crucible, and then heated from room temperature to 900℃ in a muffle furnace at a heating rate of 5℃ / min, and held at 900℃ for 2 hours. Then, the temperature was further increased from 900℃ to 1000℃ at a heating rate of 5℃ / min, and held at 1000℃ for 10 hours. After natural cooling, layered oxide Na was obtained. 0.79 Mn 0.49 Fe 0.2 Ni 0.2 Al 0.01 Cu 0.1 O2.
[0181] Comparative Example 1
[0182] The difference from Example 1 is that 30g of sample was weighed, consisting of Na2CO3, Mn2O3, Fe2O3, NiO, and CuO in a molar ratio of Na:Mn:Fe:Ni:Cu of 1:0.5:0.2:0.2:0.1. The remaining procedures were the same as in Example 1.
[0183] Comparative Example 2
[0184] The difference from Example 1 is that: 30g of sample was weighed, consisting of Na₂CO₃, Mn₂O₃, Fe₂O₃, NiO, Al₂O₃, and CuO, in a molar ratio of Na:Mn:Fe:Ni:Al:Cu of 1:0.4991:0.2:0.2:0.0009:0.1. The remaining procedures were the same as in Example 1.
[0185] Comparative Example 3
[0186] The difference from Example 1 is that 30g of sample was weighed, consisting of Na2CO3, Mn2O3, Fe2O3, NiO, B2O3, and CuO, in a molar ratio of Na:Mn:Fe:Ni:B:Cu of 1:0.4981:0.3:0.2:0.01:0.009. The remaining procedures were the same as in Example 1.
[0187] Comparative Example 4
[0188] The difference from Example 1 is that 30g of sample was weighed, consisting of Na2CO3, Mn2O3, Fe2O3, NiO, Al2O3, and CuO, in a molar ratio of Na:Mn:Fe:Ni:Al:Cu of 1:0.69:0.1:0.1:0.01:0.1. The remaining procedures were the same as in Example 1.
[0189] Comparative Example 5
[0190] The difference from Example 1 is that 30g of sample was weighed, consisting of Na2CO3, Mn2O3, Fe2O3, NiO, Al2O3, and CuO, in a molar ratio of Na:Mn:Fe:Ni:Al:Cu of 1:0.34:0.2:0.2:0.01:0.25. The remaining procedures were the same as in Example 1.
[0191] Comparative Example 6
[0192] The difference from Example 1 is that 30g of sample was weighed, consisting of Na2CO3, Mn2O3, Fe2O3, NiO, Al2O3, and CuO, in a molar ratio of Na:Mn:Fe:Ni:Al:Cu of 1:0.36:0.2:0.2:0.12:0.12. The remaining procedures were the same as in Example 1.
[0193] Comparative Example 7
[0194] The difference from Example 1 is that 30g of sample was weighed, consisting of Na2CO3, Mn2O3, Fe2O3, NiO, B2O3, and Li2CO3 in a molar ratio of Na:Mn:Fe:Ni:B:Li of 1:0.49:0.2:0.2:0.01:0.1. The remaining procedures were the same as in Example 1.
[0195] Comparative Example 8
[0196] The difference from Example 1 is that 30g of sample was weighed, consisting of Na2CO3, Mn2O3, Fe2O3, NiO, B2O3, and MgO, in a molar ratio of Na:Mn:Fe:Ni:B:Mg of 1:0.49:0.2:0.2:0.01:0.1. The remaining procedures were the same as in Example 1.
[0197] Test section
[0198] (1) The interlayer spacing d of the (003) crystal plane of layered oxides 003 and space group testing
[0199] Grind the sample to be tested into a fine powder in an agate mortar and pestle in a drying room or glove box, then pass it through a 350-mesh sieve. Take an appropriate amount of the sieved sample and place it in the center of the sample holder groove, ensuring the loose sample powder is slightly higher than the sample holder plane. Gently press a glass slide onto the sample surface to level it with the frame plane, and scrape off any excess powder. After sample preparation, use a Brucker D8A_A25 X-ray powder diffractometer from BruckerAXS, Germany, with CuKα rays as the radiation source, and the wavelength of the rays is [not specified]. The scanning angle range of 2θ is 5° to 60°, and the scanning rate is 4° / min. After the test, the interlayer spacing d of the (003) crystal plane can be obtained by using the angle corresponding to the 003 crystal plane, according to the Bragg equation 2d·sinθ=λ, and the fact that each unit cell of the 003 crystal plane contains three transition metal layers. 003 By comparing the XRD diffraction peaks of the sample with the standard card of the XRD analysis software, it can be confirmed that the space group of the sample belongs to O3 type layered oxide.
[0200] (2) Elemental composition determined by inductively coupled plasma atomic emission spectrometry
[0201] The instrument standard references EPA 6010D-2014, "Inductively Coupled Plasma Atomic Emission Spectrometry". The sample is chemically treated and digested into a solution, then atomized and injected into the plasma to elicit characteristic spectral lines of the elements. The elemental content is qualitatively and quantitatively analyzed based on the wavelength and intensity of the spectral lines (which are proportional to the concentration).
[0202] (3)D v50 test
[0203] Equipment Model: MasterSizer 2000 laser particle size analyzer; Reference Standard Procedure: GB / T19077-2016 / ISO 13320:2009; Specific Test Procedure: Take an appropriate amount of the sample to be tested (the sample concentration should be 8-12% opacity), add 20ml of deionized water, and sonicate for 5 minutes (53KHz / 120W) to ensure complete dispersion of the sample. Then, measure the sample according to the GB / T19077-2016 / ISO 13320:2009 standard.
[0204] (4) Powder compaction density test at 300MPa
[0205] The instrument used is the Yuaneng Technology PRCD1100 compaction density meter. A measured amount of powder is placed in a special compaction mold, which is then placed on the compaction density meter. The pressure is set to 300 MPa. The thickness of the powder at this pressure can be read on the device. The compacted density is calculated using the formula density = mass / volume. The test can be performed with reference to the GB / T 24533-2009 standard.
[0206] (5) First-cycle coulombic efficiency and 50-cycle capacity retention test of layered oxide coin cells
[0207] At 25℃, layered oxide cells were fabricated into coin cells and charged at a constant current density of 10 mA / g to 4.3V, yielding the discharge capacity C0. The cells were then discharged at a constant current density of 10 mA / g to 1.5V, yielding the discharge capacity C1. The first-cycle coulombic efficiency of the layered oxide cells is calculated as the discharge capacity C1 / the charge capacity C0. After the first charge-discharge cycle, the current density was increased to 1C based on the discharge capacity C1, yielding the discharge capacity C2. After 50 cycles, the discharge capacity C3 was obtained, and its capacity retention after 50 cycles is calculated as C3 / C2.
[0208] The button cell is prepared according to the steps shown below.
[0209] Preparation of positive electrode sheet: Layered oxide, conductive agent carbon black (Super P), and binder polyvinylidene fluoride (PVDF) are thoroughly mixed in an appropriate amount of solvent NMP at a mass ratio of 80:15:5 to form a uniform positive electrode slurry; the positive electrode slurry is uniformly coated on the surface of the positive electrode current collector aluminum foil, and after drying and cold pressing, it is punched into a disc with a diameter of 14mm to obtain the positive electrode sheet.
[0210] Negative electrode: Made of metallic sodium.
[0211] Preparation of electrolyte: Equal volumes of ethylene carbonate (EC) and diethyl carbonate (DEC) are mixed to obtain an organic solvent. Then, NaClO4 is dissolved in the organic solvent to prepare an electrolyte with a concentration of 1 mol / L.
[0212] Separator membrane: Porous polyethylene membrane is used as the separator membrane.
[0213] Preparation of button cell: Stack the above-mentioned positive electrode, separator, and negative electrode in sequence, so that the separator is placed between the positive electrode and the negative electrode to play a role in isolation. Add the prepared electrolyte to complete the preparation of button cell.
[0214] The discharge capacity C1 and charge capacity C0 of the coin cell obtained from tests in Example 1 and Comparative Example 1 are recorded sequentially in [the relevant data]. Figure 1 and Figure 2 The 50-cycle capacity retention of the coin cells obtained from Example 1 and Comparative Example 1 is recorded in Figure 3 In addition, the SEM images of the layered oxides of Example 1 and Comparative Example 1 obtained by disassembling the batteries after 50 cycles and performing SEM tests on the cathode materials are shown in the following figures. Figure 4 and Figure 5 .
[0215] (6) Immersion test of layered oxides
[0216] Take 5g of layered oxide and place it in a beaker. Add 15mL of deionized water and stir at 500rpm for 1min. After standing for 24h, filter and vacuum dry at 60℃ for 6h to obtain the soaked layered oxide positive electrode active material.
[0217] The X-ray powder diffractometer described in test (1) above was used to detect the change in the intensity of the (003) characteristic peak in the X-ray diffraction spectrum of the layered oxide cathode active material before and after immersion in water for 24 hours. I1 represents the intensity of the (003) characteristic peak in the X-ray diffraction spectrum of the layered oxide cathode active material after immersion in water for 24 hours, and I0 represents the intensity of the (003) characteristic peak in the X-ray diffraction spectrum of the layered oxide cathode active material before immersion. I1 / I0 can represent the water stability of the layered oxide cathode active material. The smaller the I1 / I0, the worse the water stability of the layered oxide cathode active material and the more sensitive it is to water.
[0218] (7) pH test of layered oxides
[0219] Take 2g of layered oxide and place it in a beaker. Add 18mL of deionized water and stir at 500rpm for 1min. After standing for 30min, use a general pH meter to test the pH of the supernatant according to GB / T 9724-2007 standard.
[0220] (8) Specific surface area
[0221] According to GB / T 19587-2017, the specific surface area and pore size were tested using the nitrogen adsorption specific surface area analysis method on a Quadrasorb EVO type specific surface area and pore size analyzer, and the results were calculated using the BET (Brunauer Emmett Teller) method.
[0222] (9) Tap density
[0223] Measurements were performed according to GB / T5162-2006.
[0224] The test results are recorded in Tables 1 and 2.
[0225] Table 1
[0226] Table 2
[0227] Based on the data in Table 2 and the appendix Figure 1 and 2The comparison shows that Example 1 exhibits higher first-cycle coulombic efficiency. The co-doping of Q element (containing d-orbital electrons) and C element (with high ionic potential) stabilizes the holes generated by oxygen losing electrons under high voltage, thus suppressing oxygen loss. In Comparative Example 1, where high ionic potential C element is used, the holes generated by oxygen losing electrons under high voltage cannot be effectively stabilized, leading to irreversible oxygen evolution and lower first-cycle coulombic efficiency. Furthermore, a comparison of the data from Example 1, Comparative Example 2, and Comparative Example 3 shows that the improvement in discharge specific capacity, coulombic efficiency, and cycle stability is more effective when the ratio of Q element to C element meets the range specified in this application.
[0228] In addition, according to Figure 4 and 5 The comparison shows that Figure 4 After 50 cycles of medium circulation, no obvious cracks were found on the surface of the layered oxide particles in Example 1. Figure 5 After 50 cycles of medium circulation, the surface of the layered oxide particles in Comparative Example 1 showed no obvious cracks, indicating that the elements were severely lost.
[0229] Although this application has been described with reference to preferred embodiments, various modifications can be made thereto and components can be replaced with equivalents without departing from the scope of this application. In particular, the technical features mentioned in the various embodiments can be combined in any manner, provided there is no structural conflict. This application is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
Claims
1. A layered oxide, said layered oxide comprising Na x Mn y A a Q b C c O2 oxide, where A contains Fe and Ni; Q is one or more transition metal elements other than Fe and Ni that contain 3d or 4d orbital electrons; C is one or both of Al and B, 0.66 <x≤1,0.2≤y≤0.6,0.3≤a≤0.6,0< b≤0.2,0< c≤0.1,1≤b / c≤100。 2. The layered oxide according to claim 1, wherein, Q is selected from one or more of the group consisting of Cu, Zn, Y and Ti.
3. The layered oxide according to claim 1 or 2, wherein, 0.01≤b≤0.2。 4. The layered oxide according to claim 3, wherein, 0.05≤b≤0.15。 5. The layered oxide according to claim 4, wherein, 0.1≤b≤0.2。 6. The layered oxide according to claim 1 or 2, wherein, 0.0012< c≤0.1。 7. The layered oxide according to claim 6, wherein, 0.0012≤c≤0.02。 8. The layered oxide according to claim 6, wherein, 0.01≤c≤0.02。 9. The layered oxide according to claim 6, wherein, 0.0012≤c≤0.01。 10. The layered oxide according to claim 1 or 2, wherein, 1≤b / c≤272 / 3.
11. The layered oxide according to claim 10, wherein, 1≤b / c≤50.
12. The layered oxide according to claim 10, wherein, 1≤b / c≤10.
13. The layered oxide according to claim 10, wherein, 4.5≤b / c≤54.
14. The layered oxide according to claim 10, wherein, 2≤b / c≤50.
15. The layered oxide according to claim 10, wherein, 4≤b / c≤50.
16. The layered oxide according to claim 10, wherein, 5≤b / c≤20.
17. The layered oxide according to claim 10, wherein, 5≤b / c≤10.
18. The layered oxide according to claim 10, wherein, 10≤b / c≤20.
19. The layered oxide according to claim 1 or 2, wherein, 0.4≤a≤0.6。 20. The layered oxide according to claim 19, wherein, 0.4≤a≤0.5。 21. The layered oxide according to claim 1 or 2, wherein, 0.7≤x≤1。 22. The layered oxide according to claim 21, wherein, 0.8≤x≤1。 23. The layered oxide according to claim 21, wherein, 0.9≤x≤1。 24. The layered oxide according to claim 1 or 2, wherein, 0.7 <x≤1,0.3≤y≤0.5,0.4≤a≤0.6,0.01≤b≤0.2,0.0012≤c≤0.02,4≤b / c≤50。 25. The layered oxide according to claim 24, wherein, 10≤b / c≤20.
26. The layered oxide according to claim 1 or 2, wherein, C stands for Al.
27. The layered oxide according to claim 26, wherein, 0.002< c≤0.02。 28. The layered oxide according to claim 26, wherein, 0.01< c≤0.02。 29. The layered oxide according to claim 1 or 2, wherein, C is B.
30. The layered oxide according to claim 29, wherein, 0.01< c≤0.1。 31. The layered oxide according to claim 1 or 2, wherein, C represents Al and B.
32. The layered oxide according to claim 31, wherein, 0.01< c≤0.02。 33. The layered oxide according to claim 1 or 2, wherein, Q contains Cu, and 0.055 ≤ b ≤ 0.
2.
34. The layered oxide according to claim 33, wherein, 0.09≤b≤0.108。 35. The layered oxide according to claim 33, wherein, 0.1≤b≤0.2。 36. The layered oxide according to claim 33, wherein, 0.09≤b≤0.1。 37. The layered oxide according to claim 1 or 2, wherein, Q contains Ti, and 0.1 ≤ b ≤ 0.
2.
38. The layered oxide according to claim 1 or 2, wherein, 0.75≤x≤1, Q contains Cu, C contains Al, 0.055≤b≤0.2, 0.0012≤c≤0.1, 1≤b / c≤272 / 3.
39. The layered oxide according to claim 38, wherein, 0.09≤b≤0.108、0.002≤c≤0.02、4.5≤b / c≤54.
40. The layered oxide according to claim 38, wherein, 0.09≤b≤0.1、0.01≤c≤0.02、4.5≤b / c≤10.
41. The layered oxide according to claim 1 or 2, wherein, 0.75≤x≤1, Q includes Cu, C includes B, 0.1≤b≤0.2, 0.01≤c≤0.1, 1≤b / c≤20.
42. The layered oxide according to claim 41, wherein, 10≤b / c≤20.
43. The layered oxide according to claim 41, wherein, 0.4≤a≤0.6。 44. The layered oxide according to claim 1 or 2, wherein, 0.75≤x≤1, Q contains Y, C contains Al or B, b=0.1, c=0.01, b / c=10.
45. The layered oxide according to claim 1 or 2, wherein, 0.75≤x≤1, Q contains Ti, C contains Al or B, 0.1≤b≤0.2, 0.002≤c≤0.02, 5≤b / c≤100.
46. The layered oxide according to claim 1 or 2, wherein, A contains Fe and Ni; Q contains Cu, Zn, Y and Ti; C is Al and B.
47. The layered oxide according to claim 1 or 2, wherein, The layered oxide is in the O3 phase, space group [space group number missing]. .
48. The layered oxide according to claim 1 or 2, wherein, The interlayer spacing d of the (003) crystal plane of the layered oxide 003 The wavelength range is 0.53nm to 0.55nm.
49. The layered oxide according to claim 1 or 2, wherein, The intensity of the characteristic peak (003) in the X-ray diffraction spectrum of the layered oxide before soaking is I0, and the intensity of the characteristic peak (003) in the X-ray diffraction spectrum of the layered oxide after soaking in water at room temperature for 24 hours is I1, and I1 / I0≥0.
2.
50. The layered oxide according to claim 1 or 2, wherein, The pH value of the aqueous solution of the layered oxide with a mass concentration of 10% is between 11 and 13.
51. The layered oxide according to claim 1 or 2, wherein, The volume average particle size D of the layered oxide v50 The range is 3μm to 30μm.
52. The layered oxide according to claim 51, wherein, The volume average particle size D of the layered oxide v50 The size ranges from 5μm to 15μm.
53. The layered oxide according to claim 1 or 2, wherein, The specific surface area (BET) of the layered oxide is 0.1 m². 2 / g~5m 2 / g.
54. The layered oxide according to claim 53, wherein, The specific surface area (BET) of the layered oxide is 0.3 m². 2 / g~3m 2 / g.
55. The layered oxide according to claim 1 or 2, wherein, The tap density of the layered oxide is 1 g / cm³. 3 ~3g / cm 3 .
56. The layered oxide according to claim 55, wherein, The tap density of the layered oxide is 1.5 g / cm³. 3 ~2.5g / cm 3 .
57. The layered oxide according to claim 1 or 2, wherein, The compacted density of the layered oxide powder at a pressure of 300 MPa is 3.0 g / cm³. 3 ~4.0g / cm 3 .
58. The layered oxide according to claim 1 or 2, wherein, The specific discharge capacity of the layered oxide is 156 mAh / g - 177 mAh / g.
59. The layered oxide according to claim 58, wherein, The specific discharge capacity of the layered oxide is 160 mAh / g - 168 mAh / g.
60. A method for preparing a layered oxide, wherein, The preparation method includes: Step S1: Mix layered oxides of Na source, Mn source, A source, Q source, and C source to obtain precursor powder. The molar ratio of Na:Mn:A:Q:C is (0.85~1.2):(0.2~0.6):(0.3~0.6):(0~0.2):(0~0.1), and the molar number of Q and C is not 0. The A element in the A source contains Fe and Ni; the A element in the Q source is one or more transition metal elements containing 3d or 4d orbital electrons other than Fe and Ni; the C element in the C source is one or both of Al and B. Step S2: The precursor powder is calcined and pulverized in an oxidizing atmosphere to obtain the layered oxide, wherein the layered oxide includes compounds with the general formula Na. x Mn y A a Q b C c Oxides of O2, 0.66 <x≤1,0.2≤y≤0.6,0.3≤a≤0.6,0< b≤0.2,0< c≤0.1,1≤b / c≤100。 61. The preparation method according to claim 60, wherein, The mixing in step S1 is carried out by ball milling or mechanical stirring.
62. The preparation method according to claim 60, wherein, The Na source is selected from one or more of the group consisting of Na2CO3, NaHCO3, NaOH, and Na2O2.
63. The preparation method according to claim 60, wherein, The Mn source is selected from one or more of the group consisting of Mn2O3, Mn3O4, MnO and MnO2.
64. The preparation method according to claim 60, wherein, The A source is selected from one or more of the group consisting of oxides of A and salts containing the element A.
65. The preparation method according to claim 60, wherein, The Q source is one or more of the group consisting of oxides of Q and salts containing the element Q.
66. The preparation method according to claim 60, wherein, The Q element is selected from one or more of the group consisting of Cu, Zn, Y, and Ti.
67. The preparation method according to claim 60, wherein, The C source is one or more of the group consisting of C oxides and salts containing C.
68. The preparation method according to claim 60, wherein, The oxidizing atmosphere is selected from air, oxygen, a mixture of oxygen and air, or a mixture of oxygen and an inert gas.
69. The preparation method according to claim 68, wherein, The calcination temperature is 700℃~1000℃, and the calcination holding time is 10 hours~30 hours.
70. The preparation method according to claim 68, wherein, Step S2 includes a first calcination stage and a second calcination stage performed sequentially. The calcination temperature of the first calcination stage is 400℃~900℃, and the holding time of the first calcination stage is 2 hours~20 hours. The calcination temperature of the second calcination stage is 700℃~1000℃, and the holding time of the second calcination stage is 10 hours~30 hours.
71. A positive electrode sheet, comprising a positive current collector and a positive electrode film layer disposed on at least one surface of the positive current collector, wherein the positive electrode film layer comprises a positive electrode active material, wherein, The positive electrode active material includes the layered oxide according to any one of claims 1 to 59, or the layered oxide obtained by the preparation method according to any one of claims 60 to 70.
72. The positive electrode sheet according to claim 71, wherein the content of the layered oxide in the positive electrode film layer is 60% by weight or more based on the total weight of the positive electrode film layer.
73. The positive electrode sheet according to claim 72, wherein the content of the layered oxide in the positive electrode film layer is 80% to 98% by weight based on the total weight of the positive electrode film layer.
74. A secondary battery, wherein, The layered oxide includes any one of claims 1 to 59, or the layered oxide obtained by the preparation method of any one of claims 60 to 70, or the positive electrode sheet of any one of claims 71 to 73.
75. A battery module comprising a secondary battery, wherein, The secondary battery is the secondary battery as described in claim 74.
76. A battery pack comprising a battery module, wherein the battery module is the battery module of claim 75.
77. An electrical device comprising a secondary battery, a battery module, or a battery pack, wherein, The secondary battery is selected from the secondary battery of claim 74, the battery module is the battery module of claim 75, or the battery pack is the battery pack of claim 76.
Citation Information
Patent Citations
O3 / p2 mixed phase sodium-containing doped layered oxide materials
CN112262109A