A method for extracting vanadium from vanadium-containing molten iron and vanadium-containing slag
By controlling the alkalinity of vanadium-containing slag and performing multiple cycles of blowing to form vanadium ferro-spinel, combined with magnetic separation, the problem of low vanadium extraction efficiency in the existing technology from vanadium-containing iron water is solved, and the extraction rate of vanadium and vanadium slag are improved. quality, shortening the steelmaking cycle and reducing costs.
Patent Information
- Application Number
- CN202311605769.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-11-29
AI Technical Summary
The existing vanadium extraction process from vanadium-containing molten iron is inefficient, resulting in prolonged steelmaking cycles and poor quality vanadium slag.
By controlling the alkalinity of vanadium-containing slag within the range of 1.3-2.0, adding iron oxide and performing multiple cycles of blowing to form vanadium-iron spinel, combined with magnetic separation to extract vanadium-containing magnetic substances, the vanadium enrichment efficiency is improved.
It significantly improves the vanadium extraction rate and the quality of vanadium slag, shortens the steelmaking cycle, and reduces the cost of molten iron treatment.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of molten iron treatment, and in particular to a method for extracting vanadium from vanadium-containing molten iron and vanadium-containing slag. Background Art
[0002] Before vanadium-containing hot metal enters steelmaking, the process of oxidizing vanadium in the hot metal into vanadium slag and separating it from the hot metal is called hot metal pretreatment process. Therefore, the steelmaking process includes: blast furnace hot metal desulfurization - vanadium extraction (to obtain semi-steel) - steelmaking - to obtain finished steel. Specifically, blast furnace ironmaking obtains vanadium-containing hot metal, and the hot metal is stored in the iron furnace to uniform the composition and temperature, and then the vanadium-containing hot metal is added to the converter to blow oxygen to oxidize the vanadium into the vanadium slag, and then the hot metal after vanadium extraction is loaded into the converter to obtain finished steel.
[0003] At present, the processes for extracting vanadium from vanadium-containing hot metal include the double process and the converter single slag method. The double process is to first blow vanadium slag in a vanadium blowing furnace, and then dephosphorize and steel-make semi-steel in another converter. Although this vanadium extraction process can first extract the useful vanadium element for use and has a high vanadium extraction rate, operating in two furnaces increases the semi-steel turnover time, prolongs the smelting cycle, and reduces the production efficiency of steelmaking in the converter workshop. The converter single slag method does not affect the steelmaking efficiency, but the vanadium slag quality of this method is low, the average mass fraction of V205 is less than 10%, and the vanadium extraction efficiency is low. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] In view of the shortcomings of the prior art, the present invention provides a method for extracting vanadium from vanadium-containing molten iron and vanadium-containing slag, which solves the technical problem of low vanadium extraction efficiency in the prior molten iron treatment method.
[0006] (II) Technical solution
[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0008] A method for extracting vanadium from vanadium-containing molten iron comprises the following steps:
[0009] S1, adding vanadium-containing molten iron and coolant into a steelmaking container, and then blowing with a gun, adding iron oxides in batches during the blowing process, and obtaining vanadium-containing slag at the end of the blowing;
[0010] S2, pouring out the vanadium-containing slag, cooling it, crushing it into 250-400 meshes, and performing magnetic separation to obtain a vanadium-containing magnetic material;
[0011] The basicity of the vanadium-containing slag is 1.3-2.0, and the vanadium-containing slag includes FeO, and the mass of the FeO accounts for 9-15% of the mass of the vanadium-containing slag.
[0012] Preferably, the vanadium-containing slag further comprises metallic iron, and the mass of the metallic iron accounts for 4-12% of the mass of the vanadium-containing slag.
[0013] Preferably, in the vanadium-containing molten iron, the mass of vanadium accounts for 0.15-0.4% or 0.06-0.09% of the total mass of the molten iron.
[0014] Preferably, the coolant is selected from one or two of pig iron, iron oxide balls, ore, sintered ore, vanadium-containing sludge balls, and the vanadium-containing slag.
[0015] Preferably, the iron oxide is selected from any one of pig iron, iron oxide balls, ferrous oxide, ferrous oxide, ferroferric oxide, and the vanadium-containing magnetic material.
[0016] Preferably, when the blowing lance is stopped, the basicity of the vanadium-containing slag is controlled to be 1.3-2.0 by adding SiO2 to the molten iron.
[0017] Preferably, the basicity of the vanadium-containing slag is 1.3-1.5.
[0018] Preferably, the lower lance blowing adopts a low lance position and high oxygen supply intensity blowing process, wherein the low lance position is 100-200 mm lower than the lance position in the early stage of blowing in a conventional process, and the high oxygen supply intensity is ≥3.0 m / (min·t).
[0019] Preferably, the vanadium-containing slag basicity is within the range of 1.3-1.5 and the blowing end temperature is 1330-1400°C; the vanadium-containing slag basicity is within the range of 1.5-2.0 and the blowing end temperature is controlled at 1350-1450°C.
[0020] On the other hand, a vanadium-containing slag obtained by the method of extracting vanadium from vanadium-containing molten iron is provided, wherein the vanadium-containing slag includes a magnetic phase and a non-magnetic phase, wherein the magnetic phase includes vanadium-iron spinel, iron oxide, and metallic iron, and the mass of the vanadium element accounts for 2.1-10% of the total mass of the vanadium-iron spinel, iron oxide, and metallic iron, and the non-magnetic phase includes silicon dioxide, calcium phosphate phase, and calcium silicate phase.
[0021] (III) Beneficial effects
[0022] The present invention provides a method for extracting vanadium from vanadium-containing molten iron and vanadium-containing slag. Compared with the prior art, the present invention has the following beneficial effects:
[0023] The method for extracting vanadium from vanadium-containing molten iron of the present invention controls the basicity of vanadium-containing slag to be 1.3-2.0, and controls the mass of Fe0 in the vanadium-containing slag to account for 9-15% of the mass of the vanadium-containing slag, so that the vanadium element in the molten iron forms vanadium-iron spinel with the iron-containing phase in the vanadium-containing slag in the form of V2O5, V2O3, and V3O4, forming a vanadium-containing magnetic phase, and then combines magnetic separation to collect the vanadium-containing magnetic material, thereby achieving the purpose of extracting vanadium. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention are clearly and completely described. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] The embodiments of the present application provide a method for extracting vanadium from vanadium-containing molten iron and vanadium-containing slag, thereby solving the problem of low vanadium extraction efficiency in existing molten iron treatment methods.
[0026] The technical solution in the embodiment of the present application is to solve the above technical problems, and the overall idea is as follows:
[0027] The method for extracting vanadium from vanadium-containing molten iron of the present invention comprises the following steps:
[0028] S1. Provide a steelmaking container, add vanadium-containing molten iron and a coolant into the steelmaking container, then blow the steel under a gun, add iron oxides in batches during the blowing process, and obtain a first vanadium-containing slag at the end of the blowing process;
[0029] S2, leaving the first vanadium-containing slag in the steelmaking container, repeating step S1, obtaining a second vanadium-containing slag, leaving the second vanadium-containing slag in the steelmaking container, repeating step S1, obtaining a third vanadium-containing slag, and so on, leaving the N-1 vanadium-containing slag in the steelmaking container, repeating step S1, obtaining an Nth vanadium-containing slag, N≥2; the N-1 vanadium-containing slag is left in the steelmaking container, on the one hand, because vanadium is enriched in the vanadium-containing slag, and the vanadium-containing slag left in the steelmaking container can act as a carrier, which is of great significance to improving the vanadium enrichment effect. On the other hand, repeated enrichment can make the vanadium in the vanadium-containing slag more saturated, thereby increasing the vanadium content in the vanadium-containing slag and improving the quality of the vanadium-containing slag.
[0030] In the method for extracting vanadium from vanadium-containing molten iron of the present invention, the coolant is selected from one or two of pig iron, iron oxide balls, ore, sintered ore, vanadium-containing sludge balls, and the vanadium-containing slag. The vanadium-containing slag of the present invention can also be repeatedly used as a coolant, thereby reducing the cost of molten iron treatment.
[0031] In the method for extracting vanadium from vanadium-containing molten iron of the present invention, the iron oxide is selected from any one of pig iron, iron oxide balls, ferrous oxide, ferric oxide, ferroferric oxide, and the vanadium-containing magnetic material. The vanadium-containing magnetic material of the present invention can also be repeatedly used as iron oxide, thereby reducing the cost of molten iron treatment.
[0032] In the method for extracting vanadium from vanadium-containing molten iron of the present invention, the mass of MgO in the vanadium-containing slag accounts for 0-5% of the total mass of the vanadium-containing slag, and the basicity of the vanadium-containing slag is controlled at 1.3-2.0.
[0033] The vanadium-containing slag obtained by the method for extracting vanadium from vanadium-containing molten iron of the present invention comprises a magnetic phase and a non-magnetic phase, wherein the magnetic phase comprises vanadium-iron spinel, iron oxide and metallic iron, the mass of the vanadium element accounts for 2.1-10% of the total mass of the vanadium-iron spinel, iron oxide and metallic iron, and the non-magnetic phase comprises silicon dioxide, calcium phosphate phase and calcium silicate phase.
[0034] In order to better understand the above technical solution, the above technical solution will be described in detail below in conjunction with specific implementation methods.
[0035] Embodiment 1:
[0036] This embodiment provides a method for extracting vanadium from vanadium-containing molten iron. The properties of the molten iron are shown in Table 1.
[0037] Table 1 Properties of molten iron
[0038] Hot metal composition C V P S Si Temperature, °C content,% 4.4 0.18 0.10 0.015 0.3 1290
[0039] The method for extracting vanadium from molten iron comprises the following steps:
[0040] S1. Add 120 tons of molten iron and 10 tons of pig iron into the converter. Speed up the dust removal fan and add molten iron and pig iron. After the operation of adding molten iron and pig iron is completed, turn the converter upward to zero position in the main control room, click "Start main blowing", ignite the lower gun, and after the oxygen gun is ignited successfully, quickly lower the gun to the low gun position of 1.1 meters from the nozzle to the gold liquid surface for blowing (the conventional process is 0.8 meters), the oxygen supply intensity is 3.06m / min / t, and the bottom blowing nitrogen intensity is 0.2Nm 3 / t.min control, without adding any slag, the slag basicity is controlled at 1.42 during the blowing process, the MgO content is <5%, and iron oxide balls are added in batches during the blowing process, and the addition amount is controlled at 25kg / t, and the FeO content of the vanadium-containing slag is controlled at 9%. The FeO content is 9%, and the vanadium element in the molten iron forms vanadium-iron spinel with the FeO in the vanadium-containing slag in the form of V2O5, V2O3, and V3O4, forming a vanadium-containing magnetic phase. Blow oxygen for 5 minutes and 30 seconds to obtain vanadium-containing slag and semi-steel;
[0041] S2, pour out the vanadium-containing slag, and the remaining semi-steel is smelted in the converter, the semi-steel temperature is 1390℃. About 6.2t of vanadium-containing slag is poured out.
[0042] Sampling and testing revealed that the semi-steel composition was: C 3.8%, V 0.021%, P 0.034%. Therefore, the vanadium extraction rate was 88% and the dephosphorization rate was 66%.
[0043] Vanadium extraction rate = (vanadium content in molten iron before blowing - vanadium content in molten iron after blowing) / vanadium content in molten iron before blowing × 100%.
[0044] Dephosphorization rate = (phosphorus content in molten iron before blowing - phosphorus content in molten iron after blowing) / phosphorus content in molten iron before blowing × 100%.
[0045] After sampling and testing, the main components of the vanadium-containing slag obtained were: basicity of the vanadium-containing slag was 1.42, P2O5 content was 3.5%, V2O5 content was 4.5%, total iron content was 8%, and metallic iron content was 6.2%.
[0046] The poured vanadium-containing slag is transported to the slag treatment site, and after cooling, it is transported to the vanadium-containing slag crushing, grinding and separation site. The vanadium-containing slag is ground to 300 mesh and subjected to magnetic separation. It is estimated that 20 kg of vanadium-containing magnetic material and 40 kg of phosphorus-containing non-magnetic material are obtained per ton of steel. In the vanadium-containing magnetic material, the mass of vanadium element accounts for 7.2% of the mass of the vanadium-containing magnetic material, and in the phosphorus-containing non-magnetic material, the mass of vanadium element accounts for less than 1% of the mass of the phosphorus-containing non-magnetic material.
[0047] The steel consumption per ton of steel is 1068kg / t of steel.
[0048] Example 2
[0049] This embodiment provides a method for extracting vanadium from vanadium-containing molten iron. The properties of the first furnace of molten iron are shown in Table 2.
[0050] Table 2 Properties of the first molten iron
[0051] Hot metal composition C V P S Si Temperature, °C content,% 4.4 0.18 0.10 0.015 0.3 1290
[0052] The method for extracting vanadium from the first molten iron comprises the following steps:
[0053] S1. Add 120 tons of molten iron and 10 tons of pig iron into the converter. Speed up the dust removal fan and start the operation of adding molten iron and pig iron. After the operation of adding molten iron and pig iron is completed, turn the converter upward to zero position in the main control room, click "Start main blowing", ignite the lower gun, and after the oxygen gun is successfully ignited, quickly lower the gun to the low gun position 1.1 meters from the nozzle to the gold liquid surface for blowing. The oxygen supply intensity is 3.06m / min / t, and the bottom blowing nitrogen intensity is 0.2Nm 3 / t.min, without adding any slag, the slag basicity is controlled at 1.42 and the MgO content is <5% during the blowing process, iron oxide balls are added in batches during the blowing process, the addition amount is controlled at 25kg / t, the FeO content is controlled at 9%, oxygen is blown for 5 minutes and 30 seconds, and the first vanadium-containing slag and the first half steel are obtained. The first vanadium-containing slag is about 6.2t, and the temperature of the first half steel is 1390℃.
[0054] Sampling and testing revealed that the first half steel composition was: C 3.8%, V 0.021%, P 0.034%. Therefore, the vanadium extraction rate was 88% and the dephosphorization rate was 66%.
[0055] Sampling and testing revealed that the main components of the first vanadium-containing slag were as follows: basicity of the vanadium-containing slag was 1.42, P2O5 content was 3.5%, V2O5 content was 4.5%, total iron content was 8%, and metallic iron content was 6.2%.
[0056] S2. Pour out the first half of the steel, and leave all the first vanadium-containing slag in the furnace. Add 125 tons of molten iron from the second furnace into the converter, add 12 tons of pig iron, speed up the dust removal fan, and perform the operation of adding molten iron and pig iron: After the operation of adding molten iron and pig iron is completed, turn the converter upward to the zero position in the main control room, click "Start main blowing", ignite the lower gun, and after the oxygen gun is successfully ignited, quickly lower the gun to the low gun position 1.2 meters from the nozzle to the gold liquid surface for blowing, the oxygen supply intensity is 3.06m / min / t, and the bottom blowing nitrogen intensity is 0.2Nm 3 / t.min, without adding any slag, the basicity of the slag in the early stage was controlled at 1.5, the MgO content was <5%, and the vanadium-containing magnetic material and pig iron of Example 1 were added in batches during the blowing process, the addition amount was controlled at 30kg / t, the FeO content was controlled at 10%, and oxygen was blown for 5 minutes and 50 seconds to obtain the second vanadium-containing slag and the second semi-steel;
[0057] S3, pour out the second vanadium-containing slag, the remaining second half steel is in the converter, the second half steel temperature is 1400℃. The second vanadium-containing slag is about 6t.
[0058] The properties of the second furnace of molten iron are shown in Table 3.
[0059] Table 3 Properties of the second hot metal
[0060] Hot metal composition C V p S Si Temperature, °C content,% 4.1 0.38 0.08 0.012 0.035 1302
[0061] Sampling and testing revealed that the second half steel composition was: C 3.5%, V 0.0304%, P 0.025%. Therefore, the vanadium extraction rate was 92% and the dephosphorization rate was 68%.
[0062] After sampling and testing, the main components of the second vanadium-containing slag obtained were: basicity 1.5, P2O53.4%, V2O58.5%, total iron 11%, and metallic iron 9.1%.
[0063] The poured second vanadium-containing slag is transported to the slag treatment site, cooled, and then transported to the vanadium-containing slag crushing, grinding and separation site. The vanadium-containing slag is ground to 300 mesh and subjected to magnetic separation. It is estimated that 30 kg of vanadium-containing magnetic material and 40 kg of phosphorus-containing non-magnetic material are obtained per ton of steel. Among the vanadium-containing magnetic material, the mass of vanadium element accounts for 9.2% of the mass of the vanadium-containing magnetic material, which is converted into V2O5, which is equivalent to the mass of V2O5 accounting for 16.4% of the mass of the vanadium-containing magnetic material. The mass percentage of vanadium element in the mass of the phosphorus-containing non-magnetic material is less than 1%.
[0064] The steel consumption per ton of steel is 1067kg / t of steel.
[0065] Example 3
[0066] This embodiment provides a method for extracting vanadium from vanadium-containing molten iron. The properties of the molten iron are shown in Table 4.
[0067] Table 4 Properties of molten iron
[0068] Hot metal composition C V P S Si Temperature, °C content,% 4.2 0.24 0.13 0.011 0.5 1308
[0069] The method for extracting vanadium from molten iron comprises the following steps:
[0070] S1. Add 15kg / t of lime while splashing slag in the previous furnace. After splashing slag, all the slag is left in the furnace. Use the full slag retention operation, add 123t of molten iron and 10t of pig iron, speed up the dust removal fan, and add molten iron and pig iron: After adding molten iron and pig iron, turn the converter upward to zero position in the main control room, click "Start main blowing", ignite the lower gun, and after the oxygen gun is successfully ignited, quickly lower the gun to the low gun position 1.1 meters from the nozzle to the gold liquid surface for blowing, the oxygen supply intensity is 3.06m / min / t, and the bottom blowing nitrogen intensity is 0.2Nm 3 / t.min control, without adding any slag, the early slag basicity is controlled at 1.35, MgO content <5%, the vanadium-containing magnetic material prepared by the present invention is added in batches during the blowing process, the addition amount is controlled at 45kg / t, the FeO content is controlled at 11%, the oxygen blowing is stopped for 6 minutes and 10 seconds, and while the oxygen lance is stopped, 500kg of quartz sand is added from the high-level silo, the furnace is poured and the slag is discharged, and the semi-steel temperature is 1420℃. The slag is about 6.5t.
[0071] Sampling and testing revealed that the semi-steel composition was: C 3.3%, V 0.024%, P 0.039%. Therefore, the vanadium extraction rate was 90% and the dephosphorization rate was 70%.
[0072] Sampling and testing showed that the main components of the vanadium-containing slag were: basicity 1.35, P2O53.8%, V2O56.5%, total iron 12%, metallic iron 7.2%
[0073] The poured vanadium-containing slag is transported to the slag treatment site, and after cooling, it is transported to the vanadium-containing slag crushing, grinding and separation site. The vanadium-containing slag is ground to 300 mesh and subjected to magnetic separation. It is estimated that 25 kg of vanadium-containing magnetic material and 45 kg of phosphorus-containing non-magnetic material are obtained per ton of steel. The mass of vanadium element accounts for 7.4% of the mass of vanadium-containing magnetic material, and the mass of vanadium element accounts for less than 1% of the mass of phosphorus-containing non-magnetic material.
[0074] The steel consumption per ton of steel is 1065kg / t of steel.
[0075] Example 4
[0076] This embodiment provides a method for extracting vanadium from vanadium-containing molten iron. The properties of the molten iron are shown in Table 5.
[0077] Table 5 Properties of molten iron
[0078] Hot metal composition C V P S Si Temperature, °C content,% 4.4 0.06 0.088 0.012 0.31 1323
[0079] The method for extracting vanadium from molten iron comprises the following steps:
[0080] S1. After the slag splashing of the previous furnace is completed, all the slag is left in the furnace. The full slag operation is adopted. 120 tons of molten iron and 11 tons of pig iron are added. The dust removal fan is accelerated to the right speed to add molten iron and pig iron: After the operation of adding molten iron and pig iron is completed, the converter furnace is tilted upward to the zero position in the main control room, and "Start main blowing" is clicked. The lower gun is ignited. After the oxygen gun is ignited successfully, the gun is quickly lowered to the low gun position of 1.1 meters from the nozzle to the gold liquid surface for blowing. The oxygen supply intensity is 3.06m / min / t, and the bottom blowing nitrogen intensity is 0.2Nm 3 / t.min, without adding any slag, the slag basicity is controlled at 1.45, the Mg0 content is <5%, the vanadium-containing magnetic material prepared by the present invention is added in batches during the blowing process, the addition amount is controlled at 25kg / t, the Fe0 content is controlled at 15%, oxygen is blown for 5 minutes and 20 seconds, vanadium-containing slag and semi-steel are obtained, the furnace is poured and the slag is discharged, and the semi-steel temperature is 1383℃. About 5.4t of slag is discharged.
[0081] Semi-steel composition: C 3.8%, V 0.009%, P 0.029%, vanadium extraction rate 85%, dephosphorization rate 66%.
[0082] The main components of vanadium-containing slag are: basicity 1.45, P2O5 3.1%, V2O5 1.8%, total iron 8%, and metallic iron 7.2%.
[0083] The poured vanadium-containing slag is transported to the slag treatment site, and after cooling, it is transported to the vanadium-containing slag crushing, grinding and separation site, where the vanadium-containing slag is ground to 300 mesh and subjected to magnetic separation. It is estimated that 20 kg of vanadium-containing magnetic material and 40 kg of phosphorus-containing non-magnetic material are obtained per ton of steel. The mass of vanadium element accounts for 2.1% of the mass of vanadium-containing magnetic material, and the mass of vanadium element accounts for less than 1% of the mass of phosphorus-containing non-magnetic material.
[0084] The consumption of one ton of steel is 1064kg / t of steel.
[0085] Example 5
[0086] This embodiment provides a method for extracting vanadium from vanadium-containing molten iron. The properties of the molten iron are shown in Table 6.
[0087] Table 6 Properties of molten iron
[0088] Hot metal composition C V P S Si Temperature, °C content,% 4.2 0.09 0.09 0.015 0.30 1310
[0089] The smelting steps of this embodiment are different from those of Embodiment 4 in that the vanadium-containing magnetic material and oxidized pellets prepared by the present invention are added in batches during the blowing process, the mass ratio of the vanadium-containing magnetic material to the oxidized pellets is 1:1, the slag basicity is controlled at 1.43, and the rest are the same as in Embodiment 4.
[0090] Semi-steel composition: C 3.8%, V 0.009%, P 0.033%, vanadium extraction rate 90%, dephosphorization rate 63%.
[0091] The main components of vanadium-containing slag are: basicity 1.43, P2O5 3.3%, V2O5 3.9%, total iron 6.5%, and metallic iron 7.2%.
[0092] The poured vanadium-containing slag is transported to the slag treatment site, and after cooling, it is transported to the vanadium-containing slag crushing, grinding and separation site. The vanadium-containing slag is ground to 300 mesh and subjected to magnetic separation. It is estimated that 25 kg of vanadium-containing magnetic material and 40 kg of phosphorus-containing non-magnetic material are obtained per ton of steel. The mass of vanadium element accounts for 2.2% of the mass of vanadium-containing magnetic material, and the mass of vanadium element accounts for less than 1% of the mass of phosphorus-containing non-magnetic material.
[0093] The steel consumption per ton of steel is 1066kg / t of steel.
[0094] Example 6
[0095] This embodiment provides a method for extracting vanadium from vanadium-containing molten iron. The properties of the molten iron are shown in Table 7.
[0096] Table 7 Properties of molten iron
[0097] Hot metal composition C V P S Si Temperature, °C content,% 4.3 0.06 0.081 0.014 0.34 1301
[0098] The smelting steps of this embodiment are different from those of Embodiment 5 in that the vanadium-containing magnetic material and oxidized pellets prepared by the present invention are added in batches during the blowing process, the mass ratio of the vanadium-containing magnetic material to the oxidized pellets is 1:3, the slag basicity is controlled at 1.3, and the rest are the same as in Embodiment 5.
[0099] Semi-steel composition: C 3.5%, V 0.009%, P 0.032%, vanadium extraction rate 85%, dephosphorization rate 60%.
[0100] The main components of vanadium-containing slag are: basicity 1.3, P2O5 3.2%, V2O5 5.5%, total iron (TFe) 6.5%, and metallic iron (MFe) 7.2%.
[0101] The poured vanadium-containing slag is transported to the slag treatment site, and after cooling, it is transported to the vanadium-containing slag crushing, grinding and separation site, where the vanadium-containing slag is ground to 300 mesh and subjected to magnetic separation. It is estimated that 25 kg of vanadium-containing magnetic material and 40 kg of phosphorus-containing non-magnetic material are obtained per ton of steel. The mass of vanadium element accounts for 5.2% of the mass of vanadium-containing magnetic material, and the mass of vanadium element accounts for less than 1% of the mass of phosphorus-containing non-magnetic material.
[0102] The consumption per ton of steel is 1063kg / t of steel.
[0103] Example 7
[0104] This embodiment provides a method for extracting vanadium from vanadium-containing molten iron. The properties of the molten iron are shown in Table 8.
[0105] Table 8 Properties of molten iron
[0106] Hot metal composition C V P S Si Temperature, °C content,% 4.3 0.06 0.088 0.011 0.34 1295
[0107] The difference between this embodiment and embodiment 5 is that the vanadium-containing slag in this embodiment is enriched through five cycles, and the slag basicity is controlled at 1.5. The rest is the same as embodiment 5.
[0108] Semi-steel composition: C 3.5%, V 0.0066%, P 0.035%, vanadium extraction rate 89%, dephosphorization rate 65%.
[0109] The main components of vanadium-containing slag are: basicity 1.5, P2O53.1%, V2O59.5%, TFe 6.5%, and MFe7.2%.
[0110] The poured vanadium-containing slag is transported to the slag treatment site, and after cooling, it is transported to the vanadium-containing slag crushing, grinding and separation site, where the vanadium-containing slag is ground to 300 mesh and subjected to magnetic separation. It is estimated that 25 kg of vanadium-containing magnetic material and 40 kg of phosphorus-containing non-magnetic material are obtained per ton of steel. The mass of vanadium element accounts for 8.5% of the mass of vanadium-containing magnetic material, and the mass of vanadium element accounts for less than 1% of the mass of phosphorus-containing non-magnetic material.
[0111] The steel consumption per ton of steel is 1065kg / t of steel.
[0112] Comparative Example 1
[0113] This comparative example provides a method for extracting vanadium from vanadium-containing molten iron. The properties of the molten iron are shown in Table 9.
[0114] Table 9 Properties of molten iron
[0115] Hot metal composition C V P S Si Temperature, °C content,% 4.3 0.07 0.089 0.013 0.32 1305
[0116] After the last furnace is finished, all the slag is left, and the slag splashing operation is carried out to protect the furnace. After splashing, the slag is left in the furnace. After adding 20.2t of scrap steel, 110t of molten iron, and 3t of iron sheet, the converter mouth is tilted upward to zero position, and the lower gun is ignited. After the oxygen gun is successfully ignited, constant pressure and gun position operation are adopted, the oxygen flow rate is 3.6Nm / t / min, the smelting gun position is controlled at 1.8m, and the oxygen supply is 36%. Lime is added in three batches for a total of 5.4t, and the blowing is 14min06s. At the end of smelting, the terminal temperature is 1648℃, the terminal phosphorus is 0.009%, the final slag basicity is 3.3, the final slag TFe is 15%, and V2O5 is 1.3%.
[0117] The steel consumption per ton of steel is 1065kg / t of steel.
[0118] It can be seen from Examples 1 and 2 that after enrichment by the technical solution of the present invention, the vanadium content in the vanadium-containing magnetic material reaches up to 9.2%, which is equivalent to 16.4% in terms of V2O5. The highest vanadium extraction rate is 88%, and the highest dephosphorization rate is 68%.
[0119] From Examples 3 to 7, it can be seen that after low-vanadium molten iron is enriched by the technical solution of the present invention, the vanadium content in the vanadium-containing magnetic material reaches up to 8.5%, which is equivalent to 15.17% V2O5. The highest vanadium extraction rate is 90%, and the highest dephosphorization rate is 70%.
[0120] By comparing Examples 1-7 with Comparative Example 1, it can be seen that the highest vanadium extraction rate of the molten iron in Examples 1-7 is 90%, and the steel material consumption is reduced by about 10kg / t steel. However, the vanadium in the molten iron of Comparative Example 1 is lost with the vanadium-containing slag. This is because the basicity of the vanadium-containing slag is controlled at 1.0-1.5, and the phosphorus element in the molten iron is enriched in the dicalcium silicate, dicalcium phosphate, and tricalcium phosphate in the vanadium-containing slag in the form of P2O5, forming a phosphorus-containing non-magnetic phase, and the vanadium element in the molten iron forms vanadium-iron spinel with the iron-containing phase in the vanadium-containing slag in the form of V2O5, V2O3, and V3O4, forming a vanadium-containing magnetic phase, thereby achieving vanadium extraction.
[0121] Example 8
[0122] This embodiment provides a method for extracting vanadium and dephosphorizing from vanadium-containing molten iron. The properties of the vanadium-containing molten iron are shown in Table 10.
[0123] Table 10 Properties of vanadium-containing molten iron
[0124] Hot metal composition C V P S Si Temperature, °C content,% 4.4 0.18 0.10 0.015 0.3 1290
[0125] The method for extracting vanadium and dephosphorizing molten iron comprises the following steps:
[0126] S1. Add 120 tons of molten iron and 10 tons of scrap steel into the converter. Speed up the dust removal fan and add scrap steel to the molten iron. After the addition of scrap steel and molten iron is completed, turn the converter upward to zero position in the main control room, click "Start main blowing", ignite the lower gun, and after the oxygen gun is successfully ignited, quickly lower the gun to the low gun position of 1.1 meters from the nozzle to the gold liquid surface for blowing (the conventional process is 0.8 meters), the oxygen supply intensity is 3.06m / min / t, and the bottom blowing nitrogen intensity is 0.2Nm 3 / t.min control, without adding any slag, the slag basicity is controlled at 1.0 during the blowing process, the MgO content is <5%, and iron oxide balls are added in batches during the blowing process, and the addition amount is controlled at 25kg / t, and the FeO content of the steel slag is controlled at 9%. The vanadium element in the molten iron forms vanadium-iron spinel with the FeO in the steel slag in the form of V2O5, V2O3, and V3O4, forming a vanadium-containing magnetic phase. Blow oxygen for 5 minutes and 30 seconds to obtain steel slag and semi-steel;
[0127] S2, pouring furnace slag, the remaining semi-steel in the converter for subsequent smelting, the semi-steel temperature is 1390 ℃. The pouring slag is about 6.2t.
[0128] Sampling and testing revealed that the semi-steel composition was: C 3.8%, V 0.021%, P 0.034%. Therefore, the vanadium extraction rate was 88% and the dephosphorization rate was 66%.
[0129] Vanadium extraction rate = (vanadium content in molten iron before blowing - vanadium content in molten iron after blowing) / vanadium content in molten iron before blowing × 100%.
[0130] Dephosphorization rate = (phosphorus content in molten iron before blowing - phosphorus content in molten iron after blowing) / phosphorus content in molten iron before blowing × 100%.
[0131] After sampling and testing, the main components of the steel slag obtained were: steel slag basicity 1.0, P2O5 content 3.5%, V2O5 content 4.5%, total iron content 8%, and metallic iron content 6.2%.
[0132] The poured steel slag is transported to the slag treatment site, and after cooling, it is transported to the steel slag crushing, grinding and separation site, the steel slag is ground to 300 mesh, and after magnetic separation, it is calculated that 20 kg of the first vanadium-containing magnetic material and 40 kg of the first phosphorus-containing non-magnetic material are obtained per ton of steel. In the first vanadium-containing magnetic material, the mass of vanadium element accounts for 7.2% of the mass of the first vanadium-containing magnetic material, and in the first phosphorus-containing non-magnetic material, the mass of vanadium element accounts for less than 1% of the mass of the first phosphorus-containing non-magnetic material.
[0133] The steel consumption per ton of steel is 1068kg / t of steel.
[0134] Example 9
[0135] This embodiment provides a method for extracting vanadium and dephosphorizing vanadium-containing molten iron. First, the first vanadium-containing molten iron is treated. The properties of the first vanadium-containing molten iron are shown in Table 11.
[0136] Table 11 Properties of the first vanadium-containing molten iron
[0137] Hot metal composition C V P S Si Temperature, °C content,% 4.4 0.18 0.10 0.015 0.3 1290
[0138] The method for extracting vanadium and dephosphorizing vanadium from molten iron containing vanadium comprises the following steps:
[0139] S1. Add 120 tons of the first vanadium-containing molten iron and 10 tons of scrap steel into the converter. Speed up the dust removal fan and add scrap steel to the molten iron. After the addition of scrap steel and molten iron is completed, turn the converter upward to zero position in the main control room, click "Start Main Blowing", ignite the lower gun, and after the oxygen gun is successfully ignited, quickly lower the gun to the low gun position of 1.1 meters from the nozzle to the gold liquid surface for blowing. The oxygen supply intensity is 3.06m / min / t, and the bottom blowing nitrogen intensity is 0.2Nm 3 / t.min, without adding any slag, the slag basicity is controlled at 1.3 and the MgO content is <5% during the blowing process, iron oxide balls are added in batches during the blowing process, the addition amount is controlled at 25kg / t, the FeO content is controlled at 9%, oxygen is blown for 5 minutes and 30 seconds, and the first steel slag and the first half steel are obtained. The first steel slag is about 6.2t, and the temperature of the first half steel is 1390℃.
[0140] Sampling and testing revealed that the first half steel composition was: C 3.8%, V 0.021%, P 0.034%. Therefore, the vanadium extraction rate was 88% and the dephosphorization rate was 66%.
[0141] After sampling and testing, the main components of the first steel slag obtained were: steel slag basicity 1.3, P2O5 content 3.5%, V2O5 content 4.5%, total iron content 8%, and metallic iron content 6.2%.
[0142] pouring out the first steel slag, cooling it, crushing it and sorting it to obtain a first vanadium-containing magnetic material and a first phosphorus-containing non-magnetic material;
[0143] S2. Add 125 tons of the second vanadium-containing molten iron into the converter, add 12 tons of scrap steel, speed up the dust removal fan, and add scrap steel to the molten iron: After the addition of scrap steel and molten iron is completed, turn the converter upward to the zero position in the main control room, click "Start Main Blowing", ignite the lower gun, and after the oxygen gun is successfully ignited, quickly lower the gun to the low gun position 1.2 meters from the nozzle to the gold liquid surface for blowing, the oxygen supply intensity is 3.06m / min / t, and the bottom blowing nitrogen intensity is 0.2Nm 3 / t.min, without adding any slag, the basicity of the slag in the early stage is controlled at 1.3-1.5, the MgO content is <5%, the first vanadium-containing magnetic material and pig iron prepared in this embodiment are added in batches during the blowing process, the addition amount is controlled at 30kg / t, the FeO content is controlled at 10%, and oxygen is blown for 5 minutes and 50 seconds to obtain the second steel slag and the second semi-steel;
[0144] S3, pour out the second steel slag, the remaining second half steel is in the converter, the second half steel temperature is 1400℃. The second steel slag is about 6t.
[0145] The properties of the second vanadium-containing molten iron are shown in Table 12.
[0146] Table 12 Properties of the second vanadium-containing molten iron
[0147] Hot metal composition C V p S Si Temperature, °C content,% 4.1 0.38 0.08 0.012 0.035 1302
[0148] Sampling and testing revealed that the second half steel composition was: C 3.5%, V 0.0304%, P 0.025%. Therefore, the vanadium extraction rate was 92% and the dephosphorization rate was 68%.
[0149] After sampling and testing, the main components of the second steel slag obtained were: basicity 1.5, P2O53.4%, V2O58.5%, total iron 11%, and metallic iron 9.1%.
[0150] The poured second steel slag is transported to the slag treatment site, and after cooling, it is transported to the steel slag crushing, grinding and separation site. The steel slag is ground to 300 mesh and subjected to magnetic separation. It is estimated that 30 kg of the second vanadium-containing magnetic material and 40 kg of the second phosphorus-containing non-magnetic material are obtained per ton of steel. In the second vanadium-containing magnetic material, the mass of vanadium element accounts for 9.2% of the mass of the second vanadium-containing magnetic material, which is converted into V2O5, which is equivalent to the mass of V2O5 accounting for 16.4% of the mass of the second vanadium-containing magnetic material. The mass percentage of vanadium element in the mass of the second phosphorus-containing non-magnetic material is less than 1%.
[0151] The steel consumption per ton of steel is 1067kg / t of steel.
[0152] Example 10
[0153] This embodiment provides a method for extracting vanadium and dephosphorizing from vanadium-containing molten iron. The properties of the vanadium-containing molten iron are shown in Table 13.
[0154] Table 13 Properties of molten iron
[0155] Hot metal composition C V P S Si Temperature, °C content,% 4.2 0.24 0.13 0.011 0.5 1308
[0156] The method for extracting vanadium and dephosphorizing molten iron comprises the following steps:
[0157] S1. Add 15kg / t of lime while splashing slag in the previous furnace. After splashing slag, all the slag is left in the furnace. The full slag retention operation is adopted. Add 123t of molten iron and 10t of scrap steel. The dust removal fan is accelerated to the right speed. Add scrap steel and molten iron: After adding scrap steel and molten iron, turn the converter upward to zero position in the main control room, click "Start main blowing", ignite the lower gun, and after the oxygen gun is successfully ignited, quickly lower the gun to the low gun position of 1.1 meters from the nozzle to the gold liquid surface for blowing. The oxygen supply intensity is 3.06m / min / t, and the bottom blowing nitrogen intensity is 0.2Nm 3 / t.min control, without adding any slag, the early slag basicity is controlled at 1.5, MgO content <5%, the second vanadium-containing magnetic material prepared in Example 2 is added in batches during the blowing process, the addition amount is controlled at 45kg / t, the FeO content is controlled at 11%, the oxygen blowing is stopped for 6 minutes and 10 seconds, while the oxygen lance is stopped, 500kg of quartz sand is added from the high-level silo, the furnace is poured and the slag is discharged, and the semi-steel temperature is 1420℃. About 6.5t of slag is discharged.
[0158] Sampling and testing revealed that the semi-steel composition was: C 3.3%, V 0.024%, P 0.039%. Therefore, the vanadium extraction rate was 90% and the dephosphorization rate was 70%.
[0159] Sampling and testing, the main components of the third steel slag obtained are: basicity 1.5, P2O53.8%, V2O56.5%, total iron 12%, metallic iron 7.2%
[0160] The poured slag is transported to the slag treatment plant, and after cooling, it is transported to the slag crushing, grinding and separation plant, where the slag is ground to 300 mesh and subjected to magnetic separation. It is estimated that 25 kg of the third vanadium-containing magnetic material and 45 kg of the third phosphorus-containing non-magnetic material are obtained per ton of steel. The mass of vanadium element accounts for 7.4% of the mass of the third vanadium-containing magnetic material, and the mass of vanadium element accounts for less than 1% of the mass of the third phosphorus-containing non-magnetic material.
[0161] The steel consumption per ton of steel is 1065kg / t of steel.
[0162] Embodiment 11
[0163] This embodiment provides a method for extracting vanadium and dephosphorizing from vanadium-containing molten iron. The properties of the vanadium-containing molten iron are shown in Table 14.
[0164] Table 14 Properties of vanadium-containing molten iron
[0165] Hot metal composition C V P S Si Temperature, °C content,% 4.4 0.06 0.088 0.012 0.31 1323
[0166] The method for extracting vanadium and dephosphorizing molten iron comprises the following steps:
[0167] S1. After the slag splashing of the previous furnace is completed, all the slag is left in the furnace. The full slag operation is adopted. 120 tons of molten iron and 11 tons of scrap steel are added. The dust removal fan is accelerated to the right speed. The operation of adding scrap steel and molten iron is carried out: After the operation of adding scrap steel and molten iron is completed, the converter furnace is tilted upward to the zero position in the main control room, and "Start main blowing" is clicked. The lower gun is ignited. After the oxygen gun is ignited successfully, the gun is quickly lowered to the low gun position of 1.1 meters from the nozzle to the gold liquid surface for blowing. The oxygen supply intensity is 3.06m / min / t, and the bottom blowing nitrogen intensity is 0.2Nm 3 / t.min, without adding any slag, the slag basicity is controlled at 1.5, the MgO content is <5%, the third vanadium-containing magnetic material of Example 3 is added in batches during the blowing process, the addition amount is controlled at 25kg / t, the FeO content is controlled at 15%, oxygen is blown for 5 minutes and 20 seconds, steel slag and semi-steel are obtained, the furnace is poured and the slag is discharged, and the semi-steel temperature is 1383°C. About 5.4t of slag is discharged.
[0168] Semi-steel composition: C 3.8%, V 0.009%, P 0.029%, vanadium extraction rate 85%, dephosphorization rate 66%.
[0169] The main components of vanadium-containing steel slag are: basicity 1.5, P2O5 3.1%, V2O5 1.8%, total iron 8%, and metallic iron 7.2%.
[0170] The poured slag is transported to the slag treatment plant, and after cooling, it is transported to the slag crushing, grinding and separation plant, where the slag is ground to 300 mesh and subjected to magnetic separation. It is estimated that 20 kg of the fourth vanadium-containing magnetic material and 40 kg of the fourth phosphorus-containing non-magnetic material are obtained per ton of steel. The mass of vanadium element accounts for 2.1% of the mass of the fourth vanadium-containing magnetic material, and the mass of vanadium element accounts for less than 1% of the mass of the fourth phosphorus-containing non-magnetic material.
[0171] The consumption of one ton of steel is 1064kg / t of steel.
[0172] Example 12
[0173] This embodiment provides a method for extracting vanadium and dephosphorizing from vanadium-containing molten iron. The smelting steps of this embodiment are different from those of Example 4 in that the third vanadium-containing magnetic material and oxidized pellets of Example 3 are added in batches during the blowing process, the mass ratio of the third vanadium-containing magnetic material to the oxidized pellets is 1:1, the slag basicity is controlled at 1.43, and the rest is the same as Example 4.
[0174] Semi-steel composition: C 3.8%, V 0.009%, P 0.033%, vanadium extraction rate 90%, dephosphorization rate 63%.
[0175] The main components of vanadium-containing steel slag are: basicity 1.43, P2O53.3%, V2O53.9%, total iron 6.5%, and metallic iron 7.2%.
[0176] The poured slag is transported to the slag treatment plant, and after cooling, it is transported to the slag crushing, grinding and separation plant, where the slag is ground to 300 mesh and subjected to magnetic separation. It is estimated that 25 kg of the fourth vanadium-containing magnetic material and 40 kg of the fourth phosphorus-containing non-magnetic material are obtained per ton of steel. The mass of vanadium element accounts for 2.2% of the mass of the fourth vanadium-containing magnetic material, and the mass of vanadium element accounts for less than 1% of the mass of the fourth phosphorus-containing non-magnetic material.
[0177] The steel consumption per ton of steel is 1066kg / t of steel.
[0178] Example 13
[0179] This embodiment provides a method for extracting vanadium and dephosphorizing from vanadium-containing molten iron. The properties of the molten iron are shown in Table 15.
[0180] Table 15 Properties of molten iron
[0181] Hot metal composition C V P S Si Temperature, °C content,% 4.3 0.06 0.081 0.014 0.34 1301
[0182] The smelting steps of this embodiment are different from those of embodiment 4 in that the third vanadium-containing magnetic material and oxidized pellets of embodiment 3 are added in batches during the blowing process, the mass ratio of the third vanadium-containing magnetic material to the oxidized pellets is 1:3, the slag basicity is controlled at 1.3, and the rest are the same as embodiment 4.
[0183] Semi-steel composition: C 3.5%, V 0.009%, P 0.032%, vanadium extraction rate 85%, dephosphorization rate 60%.
[0184] The main components of vanadium-containing steel slag are: basicity 1.3, P2O5 3.2%, V2O5 5.5%, total iron (TFe) 6.5%, and metallic iron (MFe) 7.2%.
[0185] The poured slag is transported to the slag treatment plant, and after cooling, it is transported to the slag crushing, grinding and separation plant, where the slag is ground to 300 mesh and subjected to magnetic separation. It is estimated that 25 kg of the fourth vanadium-containing magnetic material and 40 kg of the fourth phosphorus-containing non-magnetic material are obtained per ton of steel. The mass of vanadium element accounts for 5.2% of the mass of the fourth vanadium-containing magnetic material, and the mass of vanadium element accounts for less than 1% of the mass of the fourth phosphorus-containing non-magnetic material.
[0186] The consumption per ton of steel is 1063kg / t of steel.
[0187] Embodiment 14
[0188] This embodiment provides a method for extracting vanadium and dephosphorizing from vanadium-containing molten iron. The properties of the molten iron are shown in Table 16.
[0189] Table 16 Properties of molten iron
[0190] Hot metal composition C V P S Si Temperature, °C content,% 4.3 0.06 0.088 0.011 0.34 1295
[0191] The difference between this embodiment and embodiment 5 is that the steel slag in this embodiment is enriched after 5 iterations, and the slag basicity is controlled at 1.5. The rest is the same as embodiment 5.
[0192] Semi-steel composition: C 3.5%, V 0.0066%, P 0.035%, vanadium extraction rate 89%, dephosphorization rate 65%.
[0193] The main components of vanadium-containing steel slag are: basicity 1.5, P2O53.1%, V2O59.5%, TFe 6.5%, MFe7.2%.
[0194] The poured slag is transported to the slag treatment plant, and after cooling, it is transported to the slag crushing, grinding and separation plant, where the slag is ground to 300 mesh and subjected to magnetic separation. It is estimated that 25 kg of the sixth vanadium-containing magnetic material and 40 kg of the sixth phosphorus-containing non-magnetic material are obtained per ton of steel. The mass of vanadium element accounts for 8.5% of the mass of the sixth vanadium-containing magnetic material, and the mass of vanadium element accounts for less than 1% of the mass of the sixth phosphorus-containing non-magnetic material.
[0195] The steel consumption per ton of steel is 1065kg / t of steel.
[0196] Comparative Example 2
[0197] This comparative example provides a method for extracting vanadium and dephosphorizing from vanadium-containing molten iron. The properties of the molten iron are shown in Table 17.
[0198] Table 17 Properties of molten iron
[0199] Hot metal composition C V P S Si Temperature, °C content,% 4.3 0.07 0.089 0.013 0.32 1305
[0200] After the last furnace is finished, all the slag is left, and the slag splashing operation is carried out to protect the furnace. After splashing, the slag is left in the furnace. After adding 20.2t of scrap steel, 110t of molten iron, and 3t of iron sheet, the converter mouth is tilted upward to zero position, and the lower gun is ignited. After the oxygen gun is successfully ignited, constant pressure and gun position operation are adopted, the oxygen flow rate is 3.6Nm / t / min, the smelting gun position is controlled at 1.8m, and the oxygen supply is 36%. Lime is added in three batches for a total of 5.4t, and the blowing is 14min06s. At the end of smelting, the terminal temperature is 1648℃, the terminal phosphorus is 0.009%, the final slag basicity is 3.3, the final slag TFe is 15%, and V2O5 is 1.3%.
[0201] The steel consumption per ton of steel is 1065kg / t of steel.
[0202] It can be seen from Examples 8 and 9 that after enrichment of high-vanadium molten iron by the technical solution of this application, the vanadium content in the vanadium-containing magnetic material reaches up to 9.2%, which is equivalent to 16.4% in terms of V2O5. The highest vanadium extraction rate is 88%, and the highest dephosphorization rate is 68%.
[0203] From Examples 10 to 14, it can be seen that after low-vanadium molten iron is enriched by the technical solution of this application, the vanadium content in the vanadium-containing magnetic material reaches up to 8.5%, which is equivalent to 15.17% V2O5. The highest vanadium extraction rate is 90%, and the highest dephosphorization rate is 70%.
[0204] By comparing Examples 8-14 with Comparative Example 2, it can be seen that the maximum vanadium extraction rate of the molten iron in Examples 8-14 is 90%, and the steel material consumption is reduced by about 10kg / t steel. However, the vanadium in the molten iron in Comparative Example 2 is lost with the steel slag. This is because the basicity of the steel slag is controlled at 1.0-1.5, and the phosphorus element in the molten iron is enriched in the dicalcium silicate, dicalcium phosphate, and tricalcium phosphate in the steel slag in the form of P2O5, forming a phosphorus-containing non-magnetic phase, and the vanadium element in the molten iron forms vanadium-iron spinel with the iron-containing phase in the steel slag in the form of V2O5, V2O3, and V3O4, forming a vanadium-containing magnetic phase, thereby achieving vanadium extraction and dephosphorization.
[0205] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the presence of other identical elements in the process, method, article or device including the elements.
[0206] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them. Although the present invention is described in detail with reference to the above embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the above embodiments, or replace some of the technical features therein by equivalents. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention. Anything not described in detail in the present invention is a well-known technology to those skilled in the art.
Claims
1. A method for extracting vanadium from vanadium-containing molten iron, characterized in that: The steps include: S1. Provide a steelmaking container, add vanadium-containing molten iron and a coolant into the steelmaking container, then blow the steel under a gun, add iron oxides in batches during the blowing process, and obtain a first vanadium-containing slag at the end of the blowing process; S2, leaving the first vanadium-containing slag in the steelmaking container, repeating step S1 to obtain a second vanadium-containing slag, and so on, leaving the N-1th vanadium-containing slag in the steelmaking container, repeating step S1 to obtain an Nth vanadium-containing slag, N≥2; S3, pouring out the Nth vanadium-containing slag, cooling it, grinding it into 250-400 meshes, and sorting it to obtain a vanadium-containing magnetic material; The iron oxide in S1 is the vanadium-containing magnetic material in S3; The basicity of the Nth vanadium-containing slag is 1.3-2.0, and the Nth vanadium-containing slag includes FeO, and the mass of the FeO accounts for 9-15% of the mass of the Nth vanadium-containing slag; When the blowing gun is stopped, the basicity of the Nth vanadium-containing slag is controlled at 1.3-2.0 by adding SiO2 to the molten iron.
2. The method for extracting vanadium from vanadium-containing molten iron according to claim 1, characterized in that: The vanadium-containing slag also includes metallic iron, and the mass of the metallic iron accounts for 4-12% of the mass of the Nth vanadium-containing slag.
3. The method for extracting vanadium from vanadium-containing molten iron according to claim 1, characterized in that: In the vanadium-containing molten iron, the mass of vanadium accounts for 0.15-0.4% or 0.06-0.09% of the total mass of the molten iron.
4. The method for extracting vanadium from vanadium-containing molten iron according to claim 1, characterized in that: The coolant is selected from one or two of pig iron, iron oxide balls, ore, sintered ore, vanadium-containing sludge balls, and the Nth vanadium-containing slag.
5. The method for extracting vanadium from vanadium-containing molten iron according to claim 1, characterized in that: The basicity of the Nth vanadium-containing slag is 1.3-1.
5.
6. The method for extracting vanadium from vanadium-containing molten iron according to claim 1, characterized in that: The lower lance blowing adopts a low lance position and high oxygen supply intensity blowing process, and the high oxygen supply intensity is ≥3.0 m / (min·t).
7. The method for extracting vanadium from vanadium-containing molten iron according to claim 1, characterized in that: The Nth vanadium-containing slag basicity is blown in the range of 1.3-1.5, and the blowing end temperature is 1330-1400°C; the Nth vanadium-containing slag basicity is blown in the range of 2.0, and the blowing end temperature is controlled at 1350-1450°C.