Aluminum alloy hard anodizing method

Through the combination of secondary anodizing technology and specific electrolytes, a uniform and dense oxide film is formed, which solves the problem of insufficient surface hardness and corrosion resistance of aluminum alloys, significantly improves the hardness and corrosion resistance, and is suitable for transportation manufacturing.

CN117512735BActive Publication Date: 2024-10-18JIANGSU KAIWEITESI SEMICON TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311552478.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-20
Publication Date
2024-10-18
Estimated Expiration
2043-11-20

AI Technical Summary

Technical Problem

The surface of aluminum alloys is prone to scratches, wear, and insufficient hardness, and is susceptible to stress corrosion in environments such as moisture and salt spray. The pore structure of the existing anodized film is disordered, leading to cracking or falling off.

Method used

Secondary anodizing technology is adopted, by adjusting the electrolyte composition and process steps, including polishing, degreasing, alkali etching, dust removal, primary anodizing, corrosion demoulding, secondary anodizing and sealing, using sulfuric acid, organic acid, propylene A combination of electrolytes such as triols and additives, combined with ethylenediamine di-o-hydroxyphenyl sodium acetate chelating agent, forms a uniform and dense oxide film.

Benefits of technology

It significantly improves the hardness and corrosion resistance of the aluminum alloy surface, reduces the porosity of the oxide film, and enhances the stability and corrosion resistance of the oxide film. It is suitable for the transportation manufacturing industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117512735B_ABST
    Figure CN117512735B_ABST
Patent Text Reader

Abstract

The invention discloses a method for hard anodizing of aluminum alloy, and belongs to the technical field of anodizing of aluminum alloy. The method of the invention comprises the following processes: polishing, degreasing, washing, alkaline etching, washing, deashing, primary anodizing, washing, corrosion demoulding, washing, secondary anodizing, washing, sealing, washing, drying, etc., of the aluminum alloy in sequence. The method of the invention reduces the surface roughness of the aluminum alloy by using multiple anodizing processes, reduces the film defects caused by the presence of intermetallic compounds or elemental particles on the surface of the aluminum alloy, the holes of the generated oxide film are arranged regularly, the hardness and corrosion resistance of the oxide film are improved, and has great application prospects in the fields of transportation and equipment manufacturing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aluminum alloy anodizing, and in particular relates to an aluminum alloy hard anodizing method. Background Art

[0002] Aluminum alloys are widely used in the aerospace, shipbuilding, and vehicle manufacturing industries due to their low density, high strength, and good weldability. They have made great contributions to lightweight structures, energy conservation, and emission reduction. However, due to the easy scratching, wear, and insufficient hardness of aluminum alloy surfaces, there are many limitations in actual production and use. In addition, since aluminum alloys are widely used in the transportation industry, they need to be subjected to multiple tensile stresses as important load-bearing components, and they also need to be subjected to corrosion in environments such as humidity, salt spray, and the ocean. Under these two effects, aluminum alloy components are susceptible to severe stress corrosion, which poses a huge risk in actual use.

[0003] Aluminum alloy is an active metal. It will be passivated in acidic and alkaline environments. A layer of oxide film will naturally form on the surface, which improves the hardness, wear resistance and corrosion resistance of the aluminum alloy surface. However, due to the thin thickness and loose structure of the naturally formed oxide film, the performance cannot meet the production and life use. The anodizing technology of aluminum alloy can control the formation of a uniform and dense oxide film on the surface of aluminum alloy, thereby expanding the industrial use range of aluminum alloy, so it is widely used in industrial production.

[0004] Aluminum alloy anodizing technology can improve the performance of the oxide film by adjusting parameters such as current, voltage, and electrolyte composition to control the oxide film thickness and pore structure. However, due to defects such as the rough aluminum alloy matrix, stress concentration, and the presence of particles on the surface, the pore structure of the generated oxide film will be disordered and irregularly arranged, which will cause the oxide film to crack or even fall off. Summary of the invention

[0005]

Technical issues

[0006] In order to solve the above problems, the present invention uses secondary anodizing technology to adjust the electrolyte composition to obtain uniform, dense and orderly arranged oxide film pores, thereby improving the surface hardness and corrosion resistance of aluminum alloy. This is feasible and necessary. This technology has broad application prospects in the transportation manufacturing industry.

[0007] The purpose of the present invention is to overcome and supplement the deficiencies in the prior art and to provide an aluminum alloy hard anodizing technology.

[0008]

Technical solution

[0009] The object of the present invention is to provide a method for hard anodizing of aluminum alloy, comprising the following steps:

[0010] S1. Polishing: The surface of aluminum alloy is cut by CNC to be smooth and burr-free;

[0011] S2, degreasing: immerse the polished aluminum alloy in an acid solution for degreasing, and then take it out for water washing;

[0012] S3, alkaline etching: immerse the degreased aluminum alloy in a sodium hydroxide solution for alkaline etching, and then take it out and wash it with water;

[0013] S4, deashing: immerse the alkali-etched aluminum alloy in a mixed solution containing nitric acid and sulfuric acid, then take it out and rinse it with deionized water;

[0014] S5. Primary anodization: immersing the aluminum alloy after ash removal in an electrolyte as an anode, with graphite as the cathode, and the electrolyte being a mixed aqueous solution containing sulfuric acid, an organic acid, glycerol, and an additive. The current and voltage are increased over time, and compressed air is used for stirring. After oxidation is completed, the aluminum alloy is taken out and washed with water to obtain a primary anodized aluminum alloy;

[0015] S6, corrosion demoulding: immerse the primary anodized aluminum alloy in a mixture containing phosphoric acid and chromic acid to remove the primary oxide film, take it out, rinse it with deionized water, and dry it;

[0016] S7, secondary anodizing: immersing the aluminum alloy after corrosion demoulding in an electrolyte containing sulfuric acid and sodium ethylenediamine di-o-hydroxyphenyl acetate, the anode is the aluminum alloy, the cathode is graphite, the current and voltage increase over time, the electrolytic tank is stirred with compressed air, and the aluminum alloy is taken out and washed after oxidation is completed to obtain secondary anodized aluminum alloy;

[0017] S8. Sealing: Immerse the secondary anodized aluminum alloy in a chromate solution for sealing, then take it out, rinse it with water, and dry it.

[0018] In one embodiment of the present invention, CNC cutting and polishing is used in step S1.

[0019] In one embodiment of the present invention, in S2, the concentration of the sulfuric acid solution is 50-100 g / L.

[0020] In one embodiment of the present invention, in S2, the immersion temperature is 50-70° C. and the immersion time is 10-15 min.

[0021] In one embodiment of the present invention, in S2, the washing is performed with water for 5 to 10 seconds.

[0022] In one embodiment of the present invention, in S3, the concentration of the sodium hydroxide solution is 60-100 g / L.

[0023] In one embodiment of the present invention, in S3, the immersion temperature is 50-75° C. and the immersion time is 15-20 min.

[0024] In one embodiment of the present invention, in S3, the washing is performed with water for 5 to 10 seconds.

[0025] In one embodiment of the present invention, in S4, the concentration of nitric acid in the mixed solution is 90-130 g / L, and the concentration of sulfuric acid is 30-50 g / L.

[0026] In one embodiment of the present invention, in S4, the immersion time is 30 to 45 seconds.

[0027] In one embodiment of the present invention, in S4, the sample is taken out and rinsed with deionized water for 10 to 30 seconds.

[0028] In one embodiment of the present invention, in S5, the electrolyte is a mixed aqueous solution containing sulfuric acid, organic acid, propylene glycol, and additives; wherein, sulfuric acid is 40-100 g / L, organic acid is 20-60 g / L, propylene glycol is 5-15 g / L, additives are 10-15 g / L, and the rest is deionized water.

[0029] In one embodiment of the present invention, in S5, the organic acid includes any one or more of the following: oxalic acid, tartaric acid, salicylic acid.

[0030] In one embodiment of the present invention, in S5, the additive includes any one or more of the following: nickel sulfate, aluminum sulfate.

[0031] In one embodiment of the present invention, in S5, the mass ratio of sulfuric acid to organic acid is 2:1.

[0032] In one embodiment of the present invention, in S5, the pH value of the electrolyte is 2.2-2.6.

[0033] In one embodiment of the present invention, in S5, the temperature of the electrolyte is -5 to 2°C.

[0034] In one embodiment of the present invention, in S5, compressed air is used for stirring.

[0035] In one embodiment of the present invention, in S5, after the oxidation is completed, the mixture is taken out and washed with water for 5 to 10 seconds.

[0036] In one embodiment of the present invention, in S5, the primary anodic oxidation current and voltage increase with time, 0 to 5 min, the voltage is 10 to 15 V, and the current density is 2.5 to 3.5 A / dm 2 , 6 to 15 minutes, voltage 20 to 25 V, current density 6 to 8 A / dm 2 , 16~75min, voltage is 35~60V, current density is 10~15A / dm 2 .

[0037] In one embodiment of the present invention, in S5, the thickness of the oxide film layer of the primary anodized aluminum alloy obtained is 50 to 55 μm.

[0038] In one embodiment of the present invention, in S6, a mixed solution containing phosphoric acid and chromic acid is used for corrosion demolding, wherein the concentration of phosphoric acid in the mixed solution is 80-110 g / L, and the concentration of chromic acid is 50-80 g / L.

[0039] In one embodiment of the present invention, in S6, the immersion temperature is 70-80° C. and the immersion time is 30-45 min.

[0040] In one embodiment of the present invention, in S6, the sample is taken out and rinsed with deionized water for 10-30 seconds.

[0041] In one embodiment of the present invention, in S7, the aluminum alloy is subjected to secondary anodization using an electrolyte containing sulfuric acid and sodium ethylenediamine di-o-hydroxyphenyl acetate, wherein the concentration of sulfuric acid is 50-80 g / L, the concentration of sodium ethylenediamine di-o-hydroxyphenyl acetate is 10-20 g / L, and the rest is deionized water.

[0042] In one embodiment of the present invention, in S7, the pH value of the electrolyte is 2.5-3.2.

[0043] In one embodiment of the present invention, in S7, the temperature of the electrolyte is -5 to 2°C, and the electrolytic cell is stirred using compressed air.

[0044] In one embodiment of the present invention, in S7, after the oxidation is completed, the mixture is taken out and washed with water for 5 to 10 seconds.

[0045] In one embodiment of the present invention, in S7, the thickness of the film layer of the secondary anodized aluminum alloy obtained is 50-55 μm.

[0046] In one embodiment of the present invention, in S7, the secondary anodization is consistent with the primary anodization step in S5.

[0047] In one embodiment of the present invention, in S8, the concentration of the chromate solution is 50-100 g / L.

[0048] In one embodiment of the present invention, in S8, the immersion temperature is 90-95° C. and the immersion time is 30-60 min.

[0049] In one embodiment of the present invention, in S8, the product is taken out and rinsed with water for 5 to 10 seconds, and dried in a heat preservation furnace at 50 to 60°C.

[0050] Compared with the prior art, the present invention has the following beneficial effects:

[0051] 1. The primary anodizing electrolyte of the present invention uses a mixed aqueous solution of sulfuric acid, organic acid, glycerol, and additives. Organic acid is added to the electrolyte, and the acidity around the oxide film is reduced through the dissociation and complexation of the organic acid, which alleviates the dissolution effect of the electrolyte on the oxide film and makes the generated oxide film denser. Properly adding glycerol to the electrolyte adsorbs on the surface of the oxide film, increases the impedance of the oxide film, slows down the dissolution rate of the oxide film, and the electrolytic reaction tends to be gentle. Small and uniform holes are formed on the surface, which reduces the porosity and improves the corrosion resistance. Properly adding additives such as nickel sulfate and aluminum sulfate to the electrolyte can improve the conductivity of the solution, reduce the heat generated on the surface of the oxide film, allow oxidation to be carried out at a high current density, accelerate the film formation rate, and increase the thickness of the oxide film, thereby improving the hardness and corrosion resistance of the oxide film.

[0052] 2. The present invention uses a two-step anodizing process. The first step anodizing reduces the surface roughness of the aluminum alloy, so that the oxide film generated after the second step anodizing is arranged regularly; the first step anodizing removes the intermetallic compounds and elemental particles on the surface, reducing the internal defects of the second step anodizing; the first step anodizing reduces the surface stress of the aluminum alloy, and reduces the tendency of the second step anodizing to crack and fall off.

[0053] 3. The present invention adds ethylenediamine di-o-hydroxyphenyl sodium acetate chelating agent to the secondary anodizing electrolyte. The chelating agent has two amine groups, two carboxyl groups, and two hydroxyl groups, which can all serve as the teeth of the ligand. The two nitrogen atoms and four oxygen atoms can provide electron pairs to form coordination bonds, and bond with Al ions to form a stable six-membered ring network structure, such as Figure 1 As shown, due to the two symmetrical benzene ring structures, the chelation effect on aluminum ions is enhanced, and a larger chelate stability constant is obtained. Through the chelation effect of the chelating agent on aluminum ions, the concentration of the acidic solution on the surface of the oxide film is reduced, thereby reducing the dissolution rate of the oxide film by the electrolyte, increasing the deposition rate of the oxide film, and a larger current density can be used without damaging the oxide film. The interface state of the oxide film is effectively improved, the porosity is reduced, the oxide film is more dense and uniform, and the hardness and corrosion resistance are improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0054] Figure 1 This is a schematic diagram of chelated aluminum with sodium ethylenediamine di-o-hydroxyphenyl acetate.

[0055] Figure 2 This is a morphology diagram of the anodized film layer prepared on the aluminum alloy surface in Example 1 of the present invention.

[0056] Figure 3 This is a morphology diagram of the anodized film layer prepared on the aluminum alloy surface in Example 2 of the present invention.

[0057] Figure 4This is a morphology diagram of the anodized film layer prepared on the aluminum alloy surface in Example 3 of the present invention.

[0058] Figure 5 This is a morphology diagram of the anodized film layer prepared on the aluminum alloy surface in Comparative Example 1 of the present invention.

[0059] Figure 6 This is a morphology diagram of the anodized film layer prepared on the aluminum alloy surface in Comparative Example 2 of the present invention.

[0060] Figure 7 This is a morphology diagram of the anodized film layer prepared on the aluminum alloy surface in Comparative Example 3 of the present invention. DETAILED DESCRIPTION

[0061] The present invention will be further described below in conjunction with specific embodiments.

[0062] Example 1

[0063] S1. Polishing: The surface of aluminum alloy is cut by CNC to be smooth and burr-free;

[0064] S2, degreasing: immerse the polished aluminum alloy in a sulfuric acid solution with a concentration of 60g / L and a temperature of 65°C for 10min, then take it out and wash it with water for 10s;

[0065] S3, alkaline etching: immerse the degreased aluminum alloy in a sodium hydroxide solution with a concentration of 70g / L and a temperature of 70°C for 15min, then take it out and wash it with water for 10s;

[0066] S4. Deashing: immerse the alkali-etched aluminum alloy in a solution of 100 g / L nitric acid and 30 g / L sulfuric acid for 40 seconds, take it out and rinse it with deionized water for 20 seconds;

[0067] S5. Primary anodization: immerse the aluminum alloy after ash removal in the electrolyte as anode, and the cathode is graphite. The electrolyte contains 60g / L sulfuric acid, 20g / L oxalic acid, 10g / L tartaric acid, 10g / L propylene glycol, 10g / L nickel sulfate, and the rest is deionized water. The pH value of the electrolyte is 2.3; the current and voltage increase with time. From 0 to 5min, the voltage is 12V and the current density is 3A / dm 2 , 6~15min, voltage is 25V, current density is 8A / dm 2 , 16~75min, voltage is 50V, current density is 12A / dm 2 The electrolyte temperature was set to -2°C, the electrolytic cell was stirred with compressed air, and after oxidation was completed, the electrolytic cell was taken out and washed with water for 10 seconds to obtain a primary anodized aluminum alloy with an oxide film layer thickness of 50 to 55 μm;

[0068] S6, corrosion demoulding: immerse the primary anodized aluminum alloy in a mixed aqueous solution of 100g / L phosphoric acid and 60g / L chromic acid at 80°C for 30min to remove the primary oxide film, take it out and rinse it with deionized water for 20s, and dry it;

[0069] S7. Secondary anodization: The aluminum alloy after corrosion demoulding is immersed in a mixed aqueous solution of sulfuric acid and sodium ethylenediamine di-o-hydroxyphenyl acetate, with the aluminum alloy as the anode and graphite as the cathode. The concentration of sulfuric acid in the mixed aqueous solution is 60g / L, the concentration of sodium ethylenediamine di-o-hydroxyphenyl acetate is 15g / L, and the rest is deionized water. The pH value of the electrolyte is 2.8; the current and voltage increase with time, 0-5min, the voltage is 12V, and the current density is 3A / dm 2 , 6~15min, voltage is 25V, current density is 8A / dm 2 , 16~75min, voltage is 50V, current density is 12A / dm 2 The electrolyte temperature was set to -2°C, the electrolytic cell was stirred with compressed air, and after oxidation was completed, the electrolyte was taken out and washed with water for 10 seconds to obtain a secondary anodized aluminum alloy with a film thickness of 50 to 55 μm.

[0070] S8. Sealing: immerse the secondary anodized aluminum alloy in a chromate solution with a concentration of 90g / L and a temperature of 95°C for 30min. Take it out and rinse it with water for 10s, and dry it in a 60°C insulation furnace.

[0071] Example 2

[0072] S1. Polishing: The surface of aluminum alloy is cut by CNC to be smooth and burr-free;

[0073] S2, degreasing: immerse the polished aluminum alloy in a sulfuric acid solution with a concentration of 70g / L and a temperature of 70°C for 15min, then take it out and wash it with water for 10s;

[0074] S3, alkaline etching: immerse the degreased aluminum alloy in a sodium hydroxide solution with a concentration of 65g / L at a temperature of 70°C for 18min, then take it out and wash it with water for 10s;

[0075] S4. Deashing: immerse the alkali-etched aluminum alloy in a solution of 110 g / L nitric acid and 40 g / L sulfuric acid for 35 seconds, then take it out and rinse it with deionized water for 20 seconds;

[0076] S5, primary anodization: immerse the aluminum alloy after ash removal in the electrolyte as anode, the cathode is graphite, the electrolyte contains 70g / L sulfuric acid, 20g / L oxalic acid, 15g / L tartaric acid, 10g / L glycerol, 15g / L nickel sulfate, and the rest is deionized water, the pH value of the electrolyte is 2.2. The current and voltage increase with time, 0-5min, the voltage is 12V, the current density is 2.8A / dm 2 , 6~15min, voltage is 22V, current density is 8A / dm 2 , 16~75min, voltage is 45V, current density is 13A / dm 2 The electrolyte temperature was set to -3°C, the electrolytic cell was stirred with compressed air, and after oxidation was completed, the electrolytic cell was taken out and washed with water for 10 seconds to obtain a primary anodized aluminum alloy with an oxide film layer thickness of 50 to 55 μm.

[0077] S6, corrosion demoulding: immerse the primary anodized aluminum alloy in a mixed aqueous solution of 100g / L phosphoric acid and 50g / L chromic acid at 75°C for 35min to remove the primary oxide film, take it out and rinse it with deionized water for 20s, and dry it;

[0078] S7, secondary anodization: the aluminum alloy after corrosion demoulding is immersed in a mixed aqueous solution of sulfuric acid and sodium ethylenediamine di-o-hydroxyphenyl acetate as the anode, the cathode is graphite, the sulfuric acid concentration is 70g / L, the sodium ethylenediamine di-o-hydroxyphenyl acetate concentration is 15g / L, the rest is deionized water, and the pH value of the electrolyte is 2.7. The current and voltage increase with time, 0-5min, the voltage is 12V, and the current density is 2.8A / dm 2 , 6~15min, voltage is 22V, current density is 8A / dm 2 , 16~75min, voltage is 45V, current density is 13A / dm 2 The electrolyte temperature was set to -3°C, the electrolytic cell was stirred with compressed air, and after oxidation was completed, the electrolyte was taken out and washed with water for 10 seconds to obtain a secondary anodized aluminum alloy with a film thickness of 50 to 55 μm.

[0079] S8. Sealing: immerse the secondary anodized aluminum alloy in a chromate solution with a concentration of 80g / L and a temperature of 95°C for 35min. Take it out and rinse it with water for 10s, and dry it in a heat preservation furnace at 60°C.

[0080] Example 3

[0081] S1. Polishing: The surface of aluminum alloy is cut by CNC to be smooth and burr-free;

[0082] S2, degreasing: immerse the polished aluminum alloy in a sulfuric acid solution with a concentration of 90g / L and a temperature of 65°C for 10min, then take it out and wash it with water for 10s;

[0083] S3, alkaline etching: immerse the degreased aluminum alloy in a sodium hydroxide solution with a concentration of 80g / L, at a temperature of 70°C, for 20min, and then take it out and wash it with water for 10s;

[0084] S4. Deashing: immerse the alkali-etched aluminum alloy in a solution of 120 g / L nitric acid and 30 g / L sulfuric acid for 30 seconds, take it out and rinse it with deionized water for 20 seconds;

[0085] S5, primary anodization: immerse the aluminum alloy after ash removal in the electrolyte as anode, the cathode is graphite, the electrolyte contains 80g / L sulfuric acid, 20g / L oxalic acid, 20g / L tartaric acid, 10g / L glycerol, 10g / L aluminum sulfate, and the rest is deionized water, the pH value of the electrolyte is 2.1. The current and voltage increase with time, 0-5min, the voltage is 10V, the current density is 2.5A / dm 2 , 6~15min, voltage is 20V, current density is 6A / dm 2 , 16~75min, voltage is 40V, current density is 10A / dm 2 The electrolyte temperature was set to -2°C, the electrolytic cell was stirred with compressed air, and after oxidation was completed, the electrolytic cell was taken out and washed with water for 10 s to obtain a primary anodized aluminum alloy with an oxide film layer thickness of 50 to 55 μm.

[0086] S6, corrosion demoulding: immerse the primary anodized aluminum alloy in a mixed aqueous solution of 110g / L phosphoric acid and 60g / L chromic acid at 70°C for 30min to remove the primary oxide film, take it out and rinse it with deionized water for 20s, and dry it;

[0087] S7, secondary anodization: the aluminum alloy after corrosion demoulding is immersed in a mixed aqueous solution of sulfuric acid and sodium ethylenediamine di-o-hydroxyphenyl acetate as the anode, the cathode is graphite, the sulfuric acid concentration is 70g / L, the sodium ethylenediamine di-o-hydroxyphenyl acetate concentration is 15g / L, the rest is deionized water, and the pH value of the electrolyte is 2.7. The current and voltage increase with time, 0~5min, the voltage is 10V, and the current density is 2.5A / dm 2 , 6~15min, voltage is 20V, current density is 6A / dm 2 , 16~75min, voltage is 40V, current density is 10A / dm 2 The electrolyte temperature was set to -3°C, the electrolytic cell was stirred with compressed air, and after oxidation was completed, the electrolyte was taken out and washed with water for 10 seconds to obtain a secondary anodized aluminum alloy with a film thickness of 50 to 55 μm.

[0088] S8. Sealing: Immerse the aluminum alloy in a chromate solution with a concentration of 90g / L and a temperature of 95°C for 40min. Take it out and rinse it with water for 10s, and dry it in a heat preservation furnace at 60°C.

[0089] The aluminum alloy samples prepared in Examples 1 to 3 were subjected to hardness test, breakdown voltage test, corrosion resistance test and porosity test. The test results are shown in Table 1. Figures 2 to 4 shown.

[0090] The test standards are as follows:

[0091] 1. Hardness test: According to GB / T4340.1-2009 standard, the aluminum alloy is subjected to HV5 Vickers hardness test.

[0092] 2. Breakdown voltage test: According to GB / T 8754-2006 standard, the breakdown voltage test of aluminum alloy is carried out.

[0093] 3. Corrosion resistance test: According to GB / T8013.1-2018 standard, the aluminum alloy samples were subjected to neutral salt spray test.

[0094] 4. Porosity determination: Use SEM to determine the porosity of the aluminum alloy oxide film.

[0095] Table 1 Performance test results

[0096]

[0097] Comparative Example 1

[0098] Referring to Example 1, the steps S6 and S7 were removed, and the other steps were kept unchanged to obtain the corresponding aluminum alloy product. The test results are shown in Table 2. The microscopic SEM of the aluminum alloy oxide film is as follows Figure 5 shown.

[0099] Table 2 Performance test results

[0100] Test Project Example 1 Comparative Example 1 Hardness test (HV5) 498 401 Breakdown voltage test (V) 1352 1185 Corrosion resistance test (grade) 9.5 8.5 Porosity determination (%) 0.18 1.07

[0101] Comparative Example 2

[0102] Referring to Example 1, the sodium ethylenediamine di-o-hydroxyphenyl acetate in S4 was replaced with an equal amount of other chelating agents (as shown in Table 3), and the other steps remained unchanged to obtain the corresponding aluminum alloy product. The test results are shown in Table 3. Figure 6 shown.

[0103] Table 3 Performance test results

[0104]

[0105] Comparative Example 3

[0106] Referring to Example 1, the amount of sodium ethylenediamine di-o-hydroxyphenyl acetate in S4 was adjusted (as shown in Table 4), and the other steps remained unchanged to obtain the corresponding aluminum alloy product. The test results are shown in Table 4. Figure 7 shown.

[0107] Table 4 Performance test results

[0108]

[0109] The embodiments provided above are not intended to limit the scope of the present invention, and the steps described are not intended to limit the execution order thereof. Those skilled in the art may make obvious improvements to the present invention in combination with existing common knowledge, which also fall within the scope of protection defined by the claims of the present invention.

Claims

1. A method for hard anodizing of aluminum alloy, characterized in that: The steps include: S1. Polishing: The surface of aluminum alloy is cut by CNC to be smooth and burr-free; S2, degreasing: immerse the polished aluminum alloy in an acid solution for degreasing, and then take it out for water washing; S3, alkaline etching: immerse the degreased aluminum alloy in a sodium hydroxide solution for alkaline etching, and then take it out and wash it with water; S4, deashing: immerse the alkali-etched aluminum alloy in a mixed solution containing nitric acid and sulfuric acid, then take it out and rinse it with deionized water; S5, primary anodization: immersing the aluminum alloy after ash removal in an electrolyte as an anode, the cathode is graphite, the electrolyte is a mixed aqueous solution containing sulfuric acid, organic acid, glycerol, and additives, the current and voltage increase over time, and compressed air is used for stirring. After oxidation is completed, the aluminum alloy is taken out and washed with water to obtain a primary anodized aluminum alloy; wherein the organic acid is selected from any one or more of the following: oxalic acid, tartaric acid, salicylic acid; the additive is selected from any one or more of the following: nickel sulfate, aluminum sulfate; S6, corrosion demoulding: immerse the primary anodized aluminum alloy in a mixture containing phosphoric acid and chromic acid to remove the primary oxide film, take it out, rinse it with deionized water, and dry it; S7, secondary anodizing: immersing the aluminum alloy after corrosion demoulding in an electrolyte containing sulfuric acid and sodium ethylenediamine di-o-hydroxyphenyl acetate, the anode is the aluminum alloy, the cathode is graphite, the current and voltage increase over time, the electrolytic tank is stirred with compressed air, and the aluminum alloy is taken out and washed after oxidation is completed to obtain secondary anodized aluminum alloy; S8. Sealing: Immerse the secondary anodized aluminum alloy in a chromate solution for sealing, then take it out, rinse it with water, and dry it.

2. The method according to claim 1, characterized in that In S2, the acid solution is a sulfuric acid solution with a concentration of 50 to 100 g / L; in S2, the immersion temperature is 50 to 70°C and the time is 10 to 15 minutes; and the water washing is 5 to 10 seconds.

3. The method according to claim 1, characterized in that In S3, the concentration of the sodium hydroxide solution is 60-100 g / L; the immersion temperature is 50-75° C., the time is 15-20 min; and the water washing is 5-10 s.

4. The method according to claim 1, characterized in that: In S4, the concentration of nitric acid in the mixed solution is 90-130 g / L, and the concentration of sulfuric acid is 30-50 g / L; the immersion time is 30-45 seconds; and the mixture is taken out and rinsed with deionized water for 10-30 seconds.

5. The method according to claim 1, characterized in that In S5, the electrolyte is a mixed aqueous solution containing sulfuric acid, organic acid, propylene glycol, and additives; wherein, sulfuric acid is 40-100 g / L, organic acid is 20-60 g / L, propylene glycol is 5-15 g / L, additives are 10-15 g / L, and the rest is deionized water.

6. The method according to claim 1, characterized in that In S5, the mass ratio of sulfuric acid to organic acid in the electrolyte is 2:1; the pH value of the electrolyte is 2.2 to 2.6; and the temperature of the electrolyte is -5 to 2°C.

7. The method according to claim 1, characterized in that In S5, the primary anodic oxidation current and voltage increased with time. From 0 to 5 min, the voltage was 10 to 15 V, and the current density was 2.5 to 3.5 A / dm 2 , 6 to 15 minutes, voltage 20 to 25 V, current density 6 to 8 A / dm 2 , 16~75min, voltage is 35~60V, current density is 10~15A / dm 2 ; The thickness of the oxide film layer of the obtained single anodized aluminum alloy is 50 to 55 μm.

8. The method according to claim 1, characterized in that: In S6, a mixed solution containing phosphoric acid and chromic acid is used for corrosion demolding, wherein the concentration of phosphoric acid in the mixed solution is 80-110 g / L, and the concentration of chromic acid is 50-80 g / L; the immersion temperature is 70-80°C, and the time is 30-45 minutes; and the sample is taken out and rinsed with deionized water for 10-30 seconds.

9. The method according to claim 1, characterized in that: In S7, the aluminum alloy is subjected to secondary anodization using an electrolyte containing sulfuric acid and sodium ethylenediamine di-o-hydroxyphenyl acetate, wherein the concentration of sulfuric acid is 50-80 g / L, the concentration of sodium ethylenediamine di-o-hydroxyphenyl acetate is 10-20 g / L, and the remainder is deionized water; the pH value of the electrolyte is 2.5-3.2; the temperature of the electrolyte is -5-2°C, and the electrolytic cell is stirred using compressed air; the film layer thickness of the obtained secondary anodized aluminum alloy is 50-55 μm.

10. The method according to any one of claims 1 to 9, characterized in that: In S8, the concentration of the chromate solution is 50-100 g / L; the immersion temperature is 90-95°C, and the time is 30-60 min; the solution is taken out and rinsed with water for 5-10 s, and dried in a heat preservation furnace at 50-60°C.

Citation Information

Patent Citations

  • Aluminium alloy hard anodizing electrolyte and method

    CN102888641A

  • Surface treatment process of aluminum material

    CN114808077A