Laminated cells, prismatic lithium batteries, battery packs and applications
By controlling the electrode size and using lithium manganese iron phosphate material and carbon coating, the problem of balancing internal resistance and energy density in lithium batteries has been solved, thereby improving the performance and stability of lithium batteries.
Patent Information
- Application Number
- CN202311566713.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-21
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-11-21
AI Technical Summary
How to adjust the size of the electrode to achieve both low cell resistance and high energy density in lithium batteries.
By controlling the ratio of the length, width, and thickness of the positive and negative electrode plates, the stacked cell is ensured to have acceptable internal resistance. Furthermore, by using lithium manganese iron phosphate as the positive electrode active material, combined with a carbon coating layer, the energy density and cycle stability of the battery are improved.
This technology enables stacked cells to have lower internal resistance and higher energy density, improving the actual capacity, rate performance, and cycle stability of lithium batteries, while also enhancing safety.
Smart Images

Figure CN117543093B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of lithium battery technology, specifically to a stacked cell, a square lithium battery, a battery pack, and their applications. Background Technology
[0002] With the continuous development of portable electronic devices, new energy vehicles, and the large-scale energy storage market, the demand for lithium batteries continues to grow. The electrode size of lithium batteries affects their performance in practical applications. For example, the internal resistance of a lithium battery cell is related not only to the length of the electrode but also to its thickness. Assuming the length and width of the electrode are constant, a thicker electrode results in a longer lithium-ion diffusion distance and a higher internal resistance. Conversely, assuming the length and width of the electrode are constant, a thinner electrode results in a lower internal resistance. However, if the electrode is too thin, it will lead to a decrease in the energy density of the lithium battery.
[0003] Therefore, how to adjust the size of the electrode to make the lithium battery achieve both low cell internal resistance and high energy density is the technical problem to be solved by this invention. Summary of the Invention
[0004] This invention provides a stacked cell, a square lithium battery, a battery pack, and applications, enabling the lithium battery to achieve both low cell internal resistance and high energy density.
[0005] In a first aspect, the present invention provides a stacked battery cell, the stacked battery cell comprising a plurality of battery cell units stacked sequentially along a first direction, each battery cell unit comprising a positive electrode plate, a separator, and a negative electrode plate stacked sequentially, and a separator being disposed between two adjacent battery cell units, the first direction being perpendicular to a first surface of the positive electrode plate near the separator, each battery cell unit having a sub-tab on its positive electrode plate, and each battery cell unit having a sub-tab on its negative electrode plate; the sub-tabs of the positive electrode plates of the plurality of battery cell units are sequentially connected to form a positive electrode tab, and the sub-tabs of the negative electrode plates of the plurality of battery cell units are sequentially connected to form a negative electrode tab;
[0006] The ratio of the length to the thickness of the positive electrode and the ratio of the length to the thickness of the negative electrode are each independently selected from 6.3 × 10⁻⁶. 2 ~9.4×10 2 The width-to-thickness ratio of the positive electrode and the width-to-thickness ratio of the negative electrode are each independently selected from 6.3 × 10⁻⁶. 2 ~9.4×10 2 .
[0007] In a second aspect, the present invention provides a square lithium battery, the square lithium battery comprising one or more stacked cells as described in any of the first aspects.
[0008] Thirdly, this application provides a battery pack, the battery pack including a housing, and a plurality of stacked cells as described in any of the first aspects, or a plurality of square lithium batteries as described in any of the second aspects, the housing forming an accommodating space, and the plurality of square lithium batteries being arranged sequentially in the accommodating space.
[0009] Fourthly, this application provides an application of a stacked cell as described in any of the first aspects, a square lithium battery as described in any of the second aspects, or a battery pack as described in any of the third aspects in a vehicle, wherein the cell, the square lithium battery, or the battery pack serves as the power source for the vehicle.
[0010] This invention provides a stacked battery cell, a square lithium battery, a battery pack, and its applications, which have the following technical advantages:
[0011] In the stacked cell, the dimensions of the positive and negative electrodes are controlled to ensure that the stacked cell has an acceptable internal resistance, thereby improving the actual capacity, energy density, rate performance, and cycle stability of the square lithium battery containing the stacked cell, and also contributing to the improvement of the safety of the square lithium battery. Attached Figure Description
[0012] To more clearly illustrate the technical solutions in the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below.
[0013] Figure 1 This is a schematic diagram of a stacked battery cell provided in an embodiment of the present invention.
[0014] Figure 2 This is a schematic diagram of a positive electrode sheet provided in an embodiment of the present invention.
[0015] Figure 3 This is a schematic diagram of a square lithium battery provided in an embodiment of the present invention.
[0016] Figure 4 This is a schematic diagram of a battery pack provided in an embodiment of the present invention.
[0017] The attached figures are labeled as follows:
[0018] 1: Battery pack, 10: Square lithium battery, 20: Housing, 30: Cover, 40: Buffer, 101: Stacked cell, 102: Housing, 103: Positive terminal, 104: Negative terminal, 105: Connecting piece, 201: Accommodation space, 202: Housing wall, 1011: Cell unit, 1012: Positive tab, 1013: Negative tab, 10111: Positive electrode sheet, 10112: Separator, 10113: Negative electrode sheet, 101110: Sub-tab, 101111: First surface, 101112: Positive current collector, 101113: Positive active material layer. Detailed Implementation
[0019] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0020] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those familiar to those skilled in the art, and the materials or reagents used in the embodiments and comparative examples of this invention are commercially available. Furthermore, any methods and materials similar to or equivalent to those described herein may be applied to this invention. The preferred embodiments and materials described herein are for illustrative purposes only and do not limit the scope of this invention.
[0021] It should be noted that the order of description of the following embodiments is not intended to limit the preferred order of embodiments. Each embodiment of the present invention may exist in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a rigid limitation on the scope of the present invention; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single numbers within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. In addition, whenever a numerical range is referred to herein, it means including any referenced number (fraction or integer) within the referred range.
[0022] In the description of this invention, the term "comprising" means "including but not limited to".
[0023] The terms “multiple,” “repeatedly,” or similar expressions refer to two or more times, such as two, three, four, five, six, etc.
[0024] The term "and / or" encompasses any one of two or more of the listed items, as well as any and all combinations of the listed items. These combinations include any two listed items, any number of listed items, or a combination of all listed items. For example, "A and / or B" includes three parallel solutions: A, B, and A+B. Similarly, the technical solution "A, and / or, B, and / or, C, and / or, D" includes any one of A, B, C, and D (i.e., all connected by "logical OR"), any and all combinations of A, B, C, and D, including combinations of any two or three of A, B, C, and D, and combinations of all four of A, B, C, and D (i.e., all connected by "logical AND").
[0025] The term "solid content" refers to the proportion of the mass of solids in a slurry to the total mass of the slurry.
[0026] This invention provides a stacked battery cell, such as... Figure 1 and Figure 3 As shown, the stacked battery cell 101 includes a plurality of battery cell units 1011 stacked sequentially along a first direction X1. Each battery cell unit 1011 includes a positive electrode 10111, a separator 10112, and a negative electrode 10113 stacked sequentially. A separator 10112 is provided between two adjacent battery cell units 1011. The first direction X1 is perpendicular to the first surface 101111 of the positive electrode 10111 near the separator 10112. Each cell unit 1011 has a positive electrode 10111 with a sub-tab 101110 (positive electrode sub-tab). Each cell unit 1011 also has a negative electrode 10113 with a sub-tab 101110 (negative electrode sub-tab). The sub-tabs 101110 of the positive electrode 10111 of multiple cell units 1011 are connected sequentially to form a positive electrode 1012, and the sub-tabs 101110 of the negative electrode 10113 of multiple cell units 1011 are connected sequentially to form a negative electrode 1013. It should be noted that a separator 10112 is also provided on the surface of the outermost electrode sheet of the stacked cell 101.
[0027] The lengths of the positive electrode 10111 and the negative electrode 10113 are independently selected from 135mm to 165mm, for example, they can be 135mm to 140mm, 135mm to 145mm, 135mm to 150mm, 135mm to 155mm, 135mm to 160mm, 145mm to 150mm, 145mm to 155mm, 145mm to 160mm, 145mm to 165mm, 150mm to 155mm, 150mm to 160mm, 150mm to 165mm, 155mm to 160mm, 155mm to 165mm, or 160mm to 165mm. Examples include 135mm, 140mm, 145mm, 151mm, 155mm, 160mm, 165mm, or any value between the aforementioned two values.
[0028] The width of the positive electrode 10111 and the width of the negative electrode 10113 are each independently selected from 135mm to 165mm. For example, they can be 135mm to 140mm, 135mm to 145mm, 135mm to 150mm, 135mm to 155mm, 135mm to 160mm, 145mm to 150mm, 145mm to 155mm, 145mm to 160mm, 145mm to 165mm, 150mm to 155mm, 150mm to 160mm, 150mm to 165mm, 155mm to 160mm, 155mm to 165mm, or 160mm to 165mm. Examples include 135mm, 140mm, 145mm, 148mm, 155mm, 160mm, 165mm, or any value between the aforementioned two values.
[0029] The length-to-thickness ratio of the positive electrode 10111 and the length-to-thickness ratio of the negative electrode 10113 are each independently selected from 6.3 × 10⁻⁶. 2 ~9.4×10 2 For example, it could be 6.3 × 10 2 ~8.0×10 2 6.3×10 2 ~7.5×10 2 7.7×10 2 ~8.5×10 2 or 8.0×10 2 ~8.5×10 2 Example: 6.3 × 10 2 6.5×10 2 7.0×10 2 7.4×10 2 7.7×10 2 8.0×10 28.5×10 2 9.0×10 2 9.4×10 2 Or a value between any two of the aforementioned values. The width-to-thickness ratio of the positive electrode 10111 and the width-to-thickness ratio of the negative electrode 10113 are each independently selected from 6.3 × 10⁻⁶. 2 ~9.4×10 2 For example, it could be 6.3 × 10 2 6.5×10 2 7.0×10 2 7.4×10 2 7.7×10 2 8.0×10 2 8.5×10 2 9.0×10 2 9.4×10 2 Or the value between any two of the aforementioned values.
[0030] It should be noted that, as Figure 2 As shown, the positive electrode 10111 includes a positive current collector 101112 and a positive active material layer 101113, with the positive active material layer 101113 disposed on the surface of the positive current collector 101112. Under the premise that the thickness of the positive current collector 101112 is constant and all other structures and compositions in the lithium battery, except for the positive electrode 10111, remain unchanged, a thicker positive active material layer 101113 results in a higher internal resistance of the cell, corresponding to a longer ion diffusion distance and a higher impedance. Conversely, a thinner positive active material layer 101113 results in a lower internal resistance and a lower battery capacity. To increase the battery capacity to a preset value, the number of positive electrode sheets 10111 needs to be increased, leading to an increase in the amount of foil used in the positive current collector 101112, thereby increasing the weight and manufacturing cost of the lithium battery and reducing its energy density. Similarly, the negative electrode sheet includes a negative electrode current collector and a negative electrode active material layer, with the negative electrode active material layer disposed on the surface of the negative electrode current collector. Under the premise that the thickness of the negative electrode current collector is constant and all other structures and compositions in the lithium battery remain unchanged except for the negative electrode sheet, if the thickness of the negative electrode active material layer is thicker, the internal resistance of the cell will be greater, and the impedance of the lithium battery will be greater. If the thickness of the negative electrode active material layer is thinner, the internal resistance of the cell will be smaller, and the battery capacity of the lithium battery will be reduced. If the battery capacity is to be increased to the preset value, the number of negative electrode sheets needs to be increased, thereby increasing the weight and manufacturing cost of the lithium battery and reducing the energy density of the lithium battery.
[0031] Based on this, in the stacked cell 101 of the present invention, under the premise that the length of the positive electrode 10111 and the length of the negative electrode 10113 are controlled within the range of 135mm to 165mm, and the width of the positive electrode 10111 and the width of the negative electrode 10113 are controlled within the range of 135mm to 165mm, within the aforementioned range of the ratio of length to thickness and the ratio of width to thickness of the electrode, it can be ensured that the stacked cell 101 has an acceptable internal resistance, and that the lithium battery including the stacked cell 101 has a good energy density.
[0032] To further achieve both low cell resistance and high energy density in lithium batteries, in some embodiments of the present invention, the thickness of the positive electrode 10111 and the thickness of the negative electrode 10113 are independently selected from 180μm to 215μm, for example, they can be 180μm to 190μm, 180μm to 200μm, 180μm to 210μm, 190μm to 200μm, 190μm to 210μm, 190μm to 215μm, 200μm to 210μm or 210μm to 215μm, examples are 180μm, 185μm, 190μm, 193μm, 197μm, 200μm, 205μm, 210μm, 215μm or any value between the aforementioned two values.
[0033] To further improve the actual capacity and cycle life of the lithium battery comprising the stacked cell 101, further reference is made in some embodiments of the present invention. Figure 2 The positive electrode active material layer 101113 includes lithium manganese iron phosphate, whose general chemical formula is Li. a Mn x Fe y M z (PO4) b a, x, y, z, and b represent the molar amounts of the corresponding elements, and the sum of x, y, and z is c. M is selected from one or more of Mg, Ca, Sr, Co, Ti, Zr, Mo, V, Nb, Nd, Y, Ni, Sc, Cr, Cu, Zn, Be, La, and Al.
[0034] In the general chemical formula Li a Mn x Fe y M z (PO4) bIn this context, 0.10 ≤ x ≤ 0.70, where x is, for example, 0.10, 0.20, 0.30, 0.40, 0.50, 0.60, 0.70, or any value between any two of the aforementioned values. It should be noted that the higher the x, the higher the molar content of Mn in the lithium manganese iron phosphate material, and the higher the average voltage of the positive electrode 10111. If x is greater than 0.7, lithium-ion diffusion may be weakened in practical applications, leading to a decrease in the conductivity of the positive electrode 10111, thereby reducing the power of the lithium battery containing the stacked cell 101.
[0035] In order to further improve the average voltage of the positive electrode 10111 and ensure that the positive electrode 10111 has good conductivity, thereby improving the electrochemical performance of the stacked cell 101, in some embodiments of the present invention, 0.10≤x≤0.68, 0.26≤x≤0.68, or 0.4≤x≤0.68.
[0036] In the general chemical formula Li a Mn x Fe y M z (PO4) b In this context, the ratio of a to c, a / c, is 1.01 ≤ a / c ≤ 1.10. For example, a / c can be 1.01~1.03, 1.01~1.05, 1.01~1.08, 1.015~1.035, 1.035~1.05, 1.035~1.08, 1.035~1.10, 1.05~1.08, or 1.05~1.10. Examples include 1.01, 1.02, 1.03, 1.04, 1.05, 1.06, 1.07, 1.08, 1.09, 1.10, or any value between any two of the aforementioned values. If the a / c ratio is lower than 1.01 (i.e., the Li content is low), the actual specific capacity of the lithium manganese iron phosphate material will decrease. If the a / c ratio is greater than 1.10 (i.e., the Li content is high), the residual alkali content on the surface of the lithium manganese iron phosphate material will increase when it is wetted with water. If the residual alkali content is too high, the lithium battery will "swell" and the cycle performance of the square lithium battery will decrease.
[0037] The stoichiometry of phosphorus is one of the key factors affecting the performance of lithium manganese iron phosphate materials. To ensure that lithium batteries containing lithium manganese iron phosphate materials have good rate performance and cycle stability, the stoichiometry of phosphorus is crucial. a Mn x Fe y M z (PO4) bIn this context, the ratio of a to b is a / b, where 0.95 < a / b < 1.10. For example, it could be 0.95 < a / b ≤ 1.00, 0.95 < a / b ≤ 1.03, 0.95 < a / b ≤ 1.05, 0.95 < a / b ≤ 1.08, 1.00 ≤ a / b ≤ 1.03, 1.00 ≤ a / b ≤ 1.08, 1.00 ≤ a / b < 1.10, or 1.03 < a / b < 1.10. Examples of a / b include 0.96, 0.98, 1.00, 1.01, 1.02, 1.03, 1.05, 1.08, 1.10, or any of the aforementioned values. The value of c; the ratio of c to b is c / b, 0.90 < c / b < 1.10, for example it can be 0.90 < c / b ≤ 1.00, 0.90 < c / b ≤ 1.01, 0.90 < c / b < 1.02, 0.90 < c / b ≤ 1.05, 0.90 < c / b ≤ 1.07, 0.90 < c / b ≤ 1.09, or 0.95 ≤ c / b ≤ 1.10, and c / b examples are 0.91, 0.93, 0.95, 0.97, 0.99, 1.00, 1.01, 1.02, 1.05, 1.07, 1.10 or any value between the aforementioned two values.
[0038] The element type M is one of the key factors affecting the performance of lithium manganese iron phosphate (LFP) materials. For example, selecting Mg as M can improve the sinterability of LFP materials, which is beneficial for improving the rate performance of lithium batteries containing LFP materials. Given a specific element type M, the molar amount of M also affects the performance of LFP materials. To ensure that M has a good modification effect on LFP materials and to avoid poor electrochemical performance due to excessively high molar amounts of M, the molar amount should be 0.01≤z≤0.12. Examples include 0.01≤z≤0.03, 0.01≤z≤0.05, 0.01≤z≤0.08, 0.01≤z≤0.10, 0.05≤z≤0.08, or 0.05≤z≤0.12. Examples of values between any two of the aforementioned values are 0.01, 0.02, 0.03, 0.05, 0.08, 0.10, 0.12, or any two of the aforementioned values.
[0039] To further improve the electron transport efficiency and ionic conductivity of lithium manganese iron phosphate (LMP) materials, in some embodiments of the present invention, a coating layer is provided on the surface of the LMP material. The coating layer is made of carbon material, and the mass of the carbon material accounts for 0.5% to 3% of the sum of the mass of the carbon material and the LMP material. It should be noted that the coating layer also has a protective effect on the LMP material, improving or preventing the dissolution of Fe and Mn due to moisture (e.g., electrolyte) wetting of the LMP material. The thickness of the coating layer is, for example, 3 nm to 5 nm.
[0040] This invention also provides a method for preparing lithium manganese iron phosphate material, which can be used to prepare any of the lithium manganese iron phosphate materials described above, comprising the following steps:
[0041] S1. Provide a first slurry including lithium source, manganese source, iron source, phosphorus source and M source;
[0042] S2. Grind the first slurry to obtain the second slurry;
[0043] S3. Spray dry the second slurry to obtain pre-calcined material;
[0044] S4. The pre-burned material is sintered to obtain lithium manganese iron phosphate material.
[0045] Specifically, in step S1, each raw material can be selected according to conventional methods in the art. The lithium source can be one or more of lithium oxide, lithium hydroxide, and lithium salt. The lithium oxide includes, but is not limited to, Li2O. The anions generated by the ionization of lithium salt include, but are not limited to, one or more of oxalate ions, carbonate ions, sulfate ions, nitrate ions, acetate ions, halide ions, phosphate ions, and dihydrogen phosphate ions. Examples of lithium salts include one or more of lithium carbonate, lithium sulfate, lithium nitrate, lithium acetate, lithium dihydrogen phosphate, lithium phosphate, and lithium oxalate.
[0046] The manganese source can be one or more of manganese oxides, manganese hydroxide, and manganese salts. Manganese oxides include, but are not limited to, one or more of manganese monoxide, manganese dioxide, and manganese tetroxide. The anions generated by the ionization of manganese salts include, but are not limited to, one or more of oxalate ions, carbonate ions, sulfate ions, nitrate ions, acetate ions, halide ions, and phosphate ions. Examples of manganese sources include one or more of manganese carbonate, manganese phosphate, manganese oxalate, manganese nitrate, manganese acetate, manganese sulfate, and manganese chloride.
[0047] The iron source may be one or more of iron oxides, ferric hydroxide, and iron salts. Iron oxides include, but are not limited to, one or more of iron(III) oxide, iron(II) oxide, and ferrous oxide. The anions generated by the ionization of iron salts include, but are not limited to, one or more of oxalate ions, carbonate ions, sulfate ions, nitrate ions, acetate ions, halide ions, and phosphate ions. Examples of iron salts include, but are not limited to, one or more of ferrous sulfate, ferric chloride, ferrous phosphate, ferric phosphate, ferrous pyrophosphate, ferric pyrophosphate, ferric nitrate, ferric acetate, ferric citrate, ferrous oxalate, and ferrous chloride.
[0048] The phosphorus source includes, but is not limited to, phosphoric acid and one or more phosphorus-containing metal salts, wherein the phosphorus-containing metal salts include, but are not limited to, ammonium phosphate, ammonium dihydrogen phosphate, potassium dihydrogen phosphate, sodium dihydrogen phosphate and iron phosphate.
[0049] For example, the M source can be a compound comprising one or more of Mg, Ca, Sr, Co, Ti, Zr, Mo, V, Nb, Nd, Y, Ni, Sc, Cr, Cu, Zn, Be, La, and Al, wherein the compound can be an oxide, hydroxide, or metal salt compound. Taking M as a titanium source as an example, the titanium source can be one or more of titanium oxides, metatitanic acid, tetrabutyl titanate, titanium hydroxide, and titanium salts. Titanium oxides include, but are not limited to, TiO2. The anions generated by the ionization of titanium salts include, but are not limited to, one or more of oxalate ions, carbonate ions, sulfate ions, nitrate ions, acetate ions, halide ions, and phosphate ions. Examples of titanium salts include, but are not limited to, one or more of titanium sulfate, titanium nitrate, and titanium chloride. Taking M as a cobalt source as an example, the cobalt source includes, but is not limited to, one or more of cobalt tetroxide, cobalt nitrate, cobalt suboxide, cobalt acetate, and cobalt phosphate. Taking M as a nickel source as an example, the nickel source includes, but is not limited to, […]. Limited to one or more of nickel oxide, nickel oxide, nickel nitrate, nickel acetate, and nickel phosphate; taking M source as a magnesium source as an example, the magnesium source includes, but is not limited to, one or more of magnesium oxide, magnesium chloride, magnesium sulfate, magnesium nitrate, and magnesium acetate; taking M source as a zinc source as an example, the zinc source includes, but is not limited to, one or more of zinc oxide, zinc nitrate, zinc sulfate, zinc chloride, and zinc acetate; taking M source as a vanadium source as an example, the vanadium source includes, but is not limited to, one or more of vanadium oxide, vanadium pentoxide, vanadium trioxide, vanadium nitrate, and vanadium acetate; taking M source as a niobium source as an example, the niobium source includes, but is not limited to, one or more of niobium pentoxide, niobium hydroxide, niobium oxalate, niobium acetate, and niobium nitrate.
[0050] It should be noted that if the surface of the obtained lithium manganese iron phosphate material has a coating layer, the first slurry also includes a carbon source. The carbon source can be one or more of inorganic and organic carbon sources. Inorganic carbon sources include, but are not limited to, one or more of graphene, carbon nanotubes, and graphite. Organic carbon sources include, but are not limited to, one or more of glucose, sucrose, lactose, starch, organic acids, vitamins, and phenolic resins. The carbon source can act as a reducing agent, effectively improving or avoiding the reduction of Mn in the sintering process. 2+ and Fe 2+ The problem of oxidation. Furthermore, those skilled in the art know how to determine the amount of raw materials used to ensure that the molar amounts of each element in the resulting lithium manganese iron phosphate material reach the desired values.
[0051] In step S1, the solvent for the first slurry can be, for example, water and / or an organic solvent. Water is preferably deionized water. Selectable organic solvents include, but are not limited to, alcohols with 1 to 10 carbon atoms, such as one or more of methanol, ethanol, n-propanol, 2-propanol, n-butanol, 2-methyl-2-propanol, n-pentanol, 2-methyl-1-butanol, and 2,2-dimethyl-1-1-propanol. Water is preferred as the solvent for the first slurry because it is less expensive than organic solvents and has advantages such as being environmentally friendly, requiring less sophisticated equipment, and being safer.
[0052] In some embodiments of the present invention, the solid content of the first slurry is 10% to 40%, for example, it can be 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40% or any two of the aforementioned values, so that the first slurry has a suitable viscosity to facilitate subsequent grinding.
[0053] In step S2, the purpose of the grinding process is to refine the raw material, thereby improving the uniformity of subsequent spray drying and sintering processes, and facilitating the control of crystal growth particle size during sintering. The grinding methods include, but are not limited to, one or more of sand milling, ball milling, mechanical stirring milling, and air jet milling. The grinding process conditions can refer to conventional conditions used in the art, for example, sand milling at a speed of 200 r / min to 1000 r / min for 1 h to 6 h.
[0054] In step S3, the process conditions for spray drying can refer to the conventional conditions used in the art.
[0055] In step S4, the purpose of the sintering process is to induce a solid-state reaction in all raw materials to generate lithium manganese iron phosphate. It should be noted that when the surface of the obtained lithium manganese iron phosphate material has a carbon coating layer, the sintering process must be carried out in an oxygen-free environment, such as an inert gas atmosphere. Inert gases include, but are not limited to, one or more of nitrogen, argon, helium, neon, krypton, and xenon. When the surface of the obtained lithium manganese iron phosphate material does not have a carbon coating layer, the sintering process can be carried out in an oxygen-containing atmosphere or an inert gas atmosphere. The equipment used for the sintering process includes, but is not limited to, muffle furnaces, tube furnaces, rotary kilns, roller kilns, or pusher kilns.
[0056] In order to obtain lithium manganese iron phosphate material with a specific particle size, in some embodiments of the present invention, after the sintering treatment step and before the step of obtaining lithium manganese iron phosphate material, the preparation method of lithium manganese iron phosphate material further includes the step of: crushing the sintered material obtained after the sintering treatment, and then passing the crushed material through a 150-200 mesh sieve for sieving treatment, wherein the material passing through the sieve is lithium manganese iron phosphate material.
[0057] It should also be noted that the material of the positive electrode active material layer 101113 further includes a positive electrode binder and a positive electrode conductive agent. The materials of the positive electrode current collector 101112, the positive electrode binder, and the positive electrode conductive agent can be conventional materials in the art. For example, the material of the positive electrode current collector 101112 includes, but is not limited to, aluminum foil or composite aluminum foil; the positive electrode binder includes, but is not limited to, one or more of vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, and polytetrafluoroethylene; and the positive electrode conductive agent includes, but is not limited to, one or more of carbon black, graphite, and graphene.
[0058] The preparation method of the positive electrode 10111 includes, for example, the steps of: mixing lithium manganese iron phosphate material, positive electrode conductive agent, positive electrode binder and a first solvent to obtain a first mixture; then, coating the first mixture onto the positive electrode current collector 101112, and then performing a drying process and a rolling process in sequence to obtain the positive electrode 10111. It is understood that the first mixture can also be cast on a separate carrier to form a film layer, then the film layer is separated from the carrier, and then the film layer is stacked on the surface of the positive electrode current collector 101112. The first solvent includes, but is not limited to, N-methylpyrrolidone, dimethylformamide or ethylene glycol dimethyl ether.
[0059] The materials of the negative electrode active material layer include a negative electrode active substance, a negative electrode binder and a negative electrode conductive agent. The materials of the negative electrode current collector, the negative electrode active substance, the negative electrode binder and the negative electrode conductive agent may be conventional materials in the art, for example: the material of the negative electrode current collector includes, but is not limited to, copper foil, composite copper foil or copper mesh; the negative electrode active substance includes, but is not limited to, one or more of lithium simple substance, metals capable of alloying with lithium, semimetals, transition metal oxides, non-transition metal oxides and carbon materials, the metals or semimetals capable of alloying with lithium include, but are not limited to, Si, Sn, Al, Ge, Pb, Bi, Sb, Si-Y1 alloy (Y1 is an alkali metal, alkaline earth metal, Group 13 to 16 element, transition metal, rare earth element, or a combination thereof, except Si), and Sn-Y2 alloy (Y2 is an alkali metal, alkaline earth metal, Group 13 to 16 element, transition metal, rare earth element, or a combination thereof, except Sn), the transition metal oxides include, but are not limited to, one or more of lithium titanium oxide, vanadium oxide, lithium vanadium oxide and titanium niobium oxide, and the non-transition metal oxides include, but are not limited to, SnO₂ and SiO x (0<x<2), the carbon material includes, but is not limited to, one or more of crystalline carbon (e.g., graphite) and amorphous carbon, the negative electrode binder is deionized water or may be the same as the positive electrode binder, and the negative electrode conductive agent may be the same as the positive electrode conductive agent. The preparation method of the negative electrode sheet 10113 may be performed with reference to the preparation method of the positive electrode sheet 10111.
[0060] The material of the separator 10112 includes, but is not limited to, one or more of glass fiber, polyester, Teflon, polyethylene, polypropylene and polytetrafluoroethylene.
[0061] The embodiment of the present invention further provides a prismatic lithium battery, as shown in Figure 3 , the prismatic lithium battery 10 includes one or more of the laminated cells 101 described in any one of the preceding contents, and the one or more laminated cells 101 constitute the cell of the prismatic lithium battery 10.
[0062] In some embodiments of the present invention, the length-to-width ratio of the square lithium battery 10 is 1.00 to 1.13, for example, it can be 1.00 to 1.03, 1.00 to 1.05, 1.00 to 1.08, 1.00 to 1.12, 1.06 to 1.07, or 1.06 to 1.13, with examples being 1.00, 1.03, 1.05, 1.08, 1.10, 1.13, or any value between any two of the aforementioned values. Furthermore, the length of the square lithium battery is selected from 165mm to 185mm, for example, it can be 165mm to 170mm, 170mm to 180mm, 174mm to 180mm, 175mm to 176mm, or 180mm to 185mm, with examples being 165mm, 170mm, 175mm, 180mm, 185mm, or any value between any two of the aforementioned values; and / or, the width of the square lithium battery is selected from 155mm to 170mm, for example, it can be 160mm to 170mm, 160mm to 165mm, 164mm to 165mm, or 165mm to 170mm, with examples being 155mm, 160mm, 165mm, 170mm, or any value between any two of the aforementioned values.
[0063] It should be noted that when the square lithium battery 10 is used as a battery element in a vehicle battery pack, especially in commercial vehicles (including but not limited to trucks, logistics vehicles or engineering vehicles), the aforementioned design of the length and width of the square lithium battery 10 is beneficial to improving the internal space utilization and range of the battery pack, while also taking into account the structural strength and heat dissipation effect of the square lithium battery 10.
[0064] In some embodiments of the present invention, the length-to-thickness ratio of the square lithium battery 10 is 3.4 to 4.5, for example, it can be 3.4 to 3.8, 3.4 to 4.0, 3.4 to 4.3, 3.8 to 4.0, 4.0 to 4.1, or 4.0 to 4.5, with examples being 3.4, 3.8, 4.0, 4.5, or any value between any two of the aforementioned values; the width-to-thickness ratio of the square lithium battery 10 is 3.3 to 4.3, for example, it can be 3.3 to 3.5, 3.3 to 4.0, 3.3 to 4.3, 3.7 to 3.8, 3.8 to 4.0, or 4.0 to 4.3, with examples being 3.3, 3.8, 4.0, 4.3, or any value between any two of the aforementioned values.
[0065] Furthermore, the thickness of the square lithium battery 10 is selected from 35mm to 55mm, for example, it can be 35mm to 40mm, 35mm to 45mm, 35mm to 50mm, 40mm to 45mm, 40mm to 50mm, 43mm to 44mm or 45mm to 50mm, examples are 35mm, 40mm, 43mm, 44mm, 45mm, 50mm, 55mm or any value between the aforementioned two values.
[0066] It should be noted that when the square lithium battery 10 is used as a battery element in a vehicle battery pack, especially in commercial vehicles (including but not limited to trucks, logistics vehicles, or engineering vehicles), the aforementioned design of the length-to-thickness ratio and the width-to-thickness ratio of the square lithium battery 10 can optimize the spatial distribution of energy in the battery pack. In addition, the aforementioned thickness design of the square lithium battery 10 can ensure that there is sufficient heat dissipation area between any two adjacent square lithium batteries 10 in the battery pack, thereby ensuring heat dissipation effect and reducing the volume ratio of a single square lithium battery 10, which is conducive to the compact arrangement of multiple square lithium batteries 10 in the battery pack.
[0067] It should be noted that the square lithium battery 10 also includes other conventional structural components, for example, see [link to relevant documentation] Figure 1 and Figure 3 The square lithium battery 10 also includes a casing 102, a positive electrode post 103, and a negative electrode post 104. The positive electrode post 103 and the negative electrode post 104 are respectively disposed on the surface of the casing 102. The stacked cell 101 is disposed inside the casing 102. The material of the casing 102 is, for example, aluminum. The positive electrode tab 1012 and the positive electrode post 103 are welded together by a spot welding process using a connecting piece 105 to form the positive electrode of the square lithium battery 10. Similarly, the negative electrode tab 1013 and the negative electrode post 104 are welded together by a spot welding process using a connecting piece 105 to form the negative electrode of the square lithium battery 10.
[0068] In addition, the square lithium battery 10 also includes an electrolyte, which impregnates the stacked cell 101. The electrolyte can be composed of conventional components in the art, for example, the electrolyte includes lithium salt and organic solvent, wherein the organic solvent is selected from two or more combinations of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, methyl ethyl carbonate, propylene sulfite, ethyl acetate, diethyl sulfite, and 1,3-propanesulfonate lactone; the lithium salt is selected from LiPF6, LiClO4, LiBF4, LiSbF6, LiAsF6, LiCF3SO3, Li(CF3SO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiODFB, LiTFSI, LiFSI, LiCl, LiI, and LiN(C x F 2x+1 SO2)(C y F 2y+1 One or more of SO2, wherein x and y are integers from 1 to 20, and the mass of lithium salt accounts for 10% to 15% of the total mass of the electrolyte.
[0069] In some embodiments of the present invention, the internal resistance of the prismatic lithium battery 10 cell (composed of one or more stacked cells 101) at 25°C is 0.2mΩ to 0.5mΩ, and / or the energy density of the prismatic lithium battery is 190Wh / kg to 220Wh / kg, and / or the capacity of the prismatic lithium battery is 175Ah to 250Ah, and / or the voltage of the prismatic lithium battery is 2.5V to 4.2V.
[0070] This invention also provides a battery pack, such as... Figure 4 As shown, the battery pack 100 includes a housing 20 and a plurality of square lithium batteries 10 as described above. The housing 20 forms a receiving space 201, in which the plurality of square lithium batteries 10 are arranged sequentially.
[0071] It should be noted that the battery pack 100 also includes other conventional structural components, such as those described in [see below]. Figure 4 The battery pack 100 also includes a cover 30 and a buffer 40. The cover 30 is used to cover the internal space of the housing 20, and the buffer 40 is disposed inside the housing 20 and located on the housing wall 202 of the housing 20. It is understood that the battery pack 100 may also include components such as a battery management system and a cooling device.
[0072] This invention also provides an application of any of the stacked battery cells, square lithium batteries, or battery packs described above in a vehicle, wherein the battery cells, square lithium batteries, or battery packs serve as the power source for the vehicle.
[0073] In some embodiments of the invention, the vehicle is selected from trucks, logistics vehicles, or engineering vehicles.
[0074] The technical solutions and effects of the present invention will be described in detail below through specific embodiments, comparative examples and experimental examples. The following embodiments are only some embodiments of the present invention and are not intended to specifically limit the present invention.
[0075] Example 1
[0076] This embodiment provides a square lithium battery, such as Figure 3 As shown, the square lithium battery 10 includes a stacked cell 101, a casing 102, a positive electrode post 103, and a negative electrode post 104. The stacked cell 101 is disposed within the casing 102, which is made of, for example, aluminum. The positive electrode post 103 and the negative electrode post 104 are respectively disposed on the surface of the casing 102. Figure 1As shown, the stacked battery cell 101 includes 55 battery cell units 1011 stacked sequentially along a first direction X1. Each battery cell unit 1011 includes a positive electrode 10111, a separator 10112, and a negative electrode 10113 stacked sequentially. The first direction X1 is perpendicular to the first surface 101111 of the positive electrode 10111 near the separator 10112. The sub-tabs 101110 of the positive electrode 10111 of all battery cell units 1011 are connected sequentially to form a positive electrode 1012, and the sub-tabs 101110 of the negative electrode 10113 of all battery cell units 1011 are connected sequentially to form a negative electrode 1013. (Continue reading) Figure 3 The positive electrode tab 1012 and the negative electrode tab 1013 are located at the openings of the casing 102. The positive electrode tab 1012 is welded to the positive electrode post 103 to form the positive electrode of the square lithium battery 10, and the negative electrode tab 1013 is welded to the negative electrode post 104 to form the negative electrode of the square lithium battery 10. The square lithium battery 10 also includes an electrolyte, which impregnates the stacked cell 101.
[0077] like Figure 2 As shown, the positive electrode 10111 includes a positive current collector 101112 and a positive active material layer 101113. The positive active material layer 101113 is disposed on the surface of the positive current collector 101112. The material of the positive current collector 101112 is carbon-coated aluminum foil (12 μm thick), and the material of the positive active material layer 101113 includes Li-coated carbon material. 0.96 Fe 0.3 Mn 0.6 Mg 0.04 PO4, with an average coating thickness of 3 nm, and the mass of carbon material accounts for a certain percentage of the total mass of carbon material and Li. 0.96 Fe 0.3 Mn 0.6 Mg 0.04 1.5% of the total mass of PO4.
[0078] The preparation method of the positive electrode 10111 includes the following steps: Li coated with carbon material... 0.96 Fe 0.3 Mn 0.6 Mg 0.04 The following four raw materials are weighed in a mass ratio of PO4: super conductive carbon black (Super PLL): carbon nanotubes: polyvinylidene fluoride of 97:0.4:0.5:2.1. The four raw materials are mixed evenly with N-methylpyrrolidone to obtain a positive electrode slurry with a solid content of 65%. Then, the positive electrode slurry is coated onto an aluminum foil with a thickness of 12μm (coated on both sides) using a coating machine. It is then baked and cured at 120℃ to form a positive electrode active material layer. Finally, it is cold-pressed to the corresponding thickness using a roller press to obtain a positive electrode sheet.
[0079] Among them, carbon-coated Li 0.96 Fe 0.3 Mn 0.6 V 0.04 The preparation method of PO4 includes the following steps:
[0080] S1.1 Take 45.76 kg of manganese tetroxide, 45.25 kg of ferric phosphate, 35.46 kg of lithium carbonate, 1.6 kg of magnesium oxide, 80.68 kg of 85% phosphoric acid aqueous solution, and 2.72 kg of glucose and add them to a mixer to mix the raw materials. The mixing time is 2 hours to obtain a mixture. Then, transfer the mixture to a sand mill and add deionized water to the mixture at a mass ratio of 1:1.5 to obtain the first slurry.
[0081] S1.2. The first slurry is subjected to sand milling. The process parameters for sand milling are: sand milling speed of 500 r / min and sand milling time of 1.5 h to obtain the second slurry.
[0082] S1.3. The second slurry is spray-dried once. During the entire spray-drying process, the slurry is kept in a stirring state to obtain pre-calcined material. The particle size distribution range of the pre-calcined material is 2μm to 5μm.
[0083] S1.4 Place the pre-fired material in a kiln, introduce protective gas N2 at a flow rate of 80 mL / min, then raise the temperature from room temperature to 750°C at a rate of 5°C / min, sinter at 750°C for 6 hours, and cool to room temperature to obtain the calcined material.
[0084] S1.5. The calcined material is sequentially subjected to air jet milling and sieve treatment using a 150-mesh sieve. The material passing through the 150-mesh sieve undergoes a process to remove elemental iron, thereby obtaining Li coated with carbon material. 0.96 Fe 0.3 Mn 0.6 V 0.04 PO4.
[0085] The negative electrode 10113 comprises a negative electrode current collector and a negative electrode active material layer. The negative electrode active material layer is disposed on the surface of the negative electrode current collector, which is made of aluminum foil (12 μm thick). The negative electrode active material layer is made of graphite. The preparation method of the negative electrode 10113 includes the following steps: weighing the aforementioned four raw materials according to a mass ratio of graphite:conductive carbon black (Super PLL):carboxymethyl cellulose:styrene-butadiene rubber of 97:0.7:1.25:1.05; mixing the aforementioned four raw materials uniformly with N-methylpyrrolidone to obtain a negative electrode slurry with a solid content of 55%; then coating the negative electrode slurry onto an 8 μm thick aluminum foil (coated on both sides) using a coating machine; then baking and curing at 80°C to form the negative electrode active material layer; and finally cold pressing to the appropriate thickness using a roller press to obtain the negative electrode.
[0086] The preparation method of the electrolyte includes the following steps: mixing ethylene carbonate (EC): diethyl carbonate (DEC): methyl ethyl carbonate (EMC) in a volume ratio of 4:3:3 to obtain a solvent; then adding LiPF6 and an additive to the solvent and mixing them evenly to obtain the electrolyte. The concentration of LiPF6 in the electrolyte is 1.0 mol / L, and the mass of the additive accounts for 10% of the total mass of the electrolyte. The additive is composed of vinylene carbonate, 1,3-propanesulfonate lactone, fluoroethylene carbonate, and cyclohexylbenzene, with a mass ratio of vinylene carbonate: 1,3-propanesulfonate lactone: fluoroethylene carbonate: cyclohexylbenzene of 3:2:1:1.
[0087] The preparation method of the square lithium battery 10 includes the following steps: a positive electrode 10111, a PP separator 10112 with a thickness of 12μm and a negative electrode 10113 are stacked to form a cell unit 1011; 55 cell units 1011 are stacked to form a stacked cell 101; two stacked cells 101 are assembled with an aluminum shell; electrolyte is injected; and the square lithium battery 10 is obtained by aging, formation, shaping and packaging processes.
[0088] In this embodiment, the positive electrode 10111 and the negative electrode 10113 are exactly the same size (the positive electrode active material layer and the negative electrode active material layer are exactly the same size). The dimensions of the positive electrode 10111, the negative electrode 10113, and the square lithium battery 10 in this embodiment are shown in Table 1 below:
[0089] Table 1
[0090] project numerical values Length (mm) of the positive electrode (negative electrode) 151 Width (mm) of the positive electrode (negative electrode) 148 Thickness (μm) of the positive electrode (negative electrode) 197 Length (mm) of a square lithium battery 175 Width (mm) of a square lithium battery 164 Thickness (mm) of a square lithium battery 43
[0091] Example 2
[0092] This embodiment provides a square lithium battery. Compared with the square lithium battery provided in Embodiment 1, the only difference of the square lithium battery in this embodiment is that the thickness of the positive electrode and the negative electrode are replaced with "190μm".
[0093] Example 3
[0094] This embodiment provides a square lithium battery. Compared with the square lithium battery provided in Embodiment 1, the only difference of the square lithium battery in this embodiment is that the thickness of the positive electrode and the negative electrode are replaced with "180μm".
[0095] Example 4
[0096] This embodiment provides a square lithium battery. Compared with the square lithium battery provided in Embodiment 1, the only difference of the square lithium battery in this embodiment is that the thickness of the positive electrode and the negative electrode are replaced with "210μm".
[0097] Example 5
[0098] This embodiment provides a square lithium battery. Compared with the square lithium battery provided in Embodiment 1, the only difference of the square lithium battery in this embodiment is that the thickness of the positive electrode and the negative electrode are replaced with "215μm".
[0099] Example 6
[0100] This embodiment provides a square lithium battery. Compared with the square lithium battery provided in Embodiment 1, the only difference of the square lithium battery in this embodiment is that the width of the positive electrode and the negative electrode are replaced with "145mm".
[0101] Example 7
[0102] This embodiment provides a square lithium battery. Compared with the square lithium battery provided in Embodiment 1, the only difference of the square lithium battery in this embodiment is that the width of the positive electrode and the negative electrode are replaced with "155mm".
[0103] Example 8
[0104] This embodiment provides a square lithium battery. Compared with the square lithium battery provided in Embodiment 1, the only difference of the square lithium battery in this embodiment is that the width of the positive electrode and the negative electrode are replaced with "135mm".
[0105] Example 9
[0106] This embodiment provides a square lithium battery. Compared with the square lithium battery provided in Embodiment 1, the only difference of the square lithium battery in this embodiment is that the width of the positive electrode and the negative electrode are replaced with "165mm".
[0107] Example 10
[0108] This embodiment provides a square lithium battery. Compared with the square lithium battery provided in Embodiment 1, the only difference of the square lithium battery in this embodiment is that the lengths of the positive electrode and the negative electrode are replaced with "145mm".
[0109] Example 11
[0110] This embodiment provides a square lithium battery. Compared with the square lithium battery provided in Embodiment 1, the only difference of the square lithium battery in this embodiment is that the lengths of the positive electrode and the negative electrode are replaced with "155mm".
[0111] Example 12
[0112] This embodiment provides a square lithium battery. Compared with the square lithium battery provided in Embodiment 1, the only difference of the square lithium battery in this embodiment is that the lengths of the positive electrode and the negative electrode are replaced with "135mm".
[0113] Example 13
[0114] This embodiment provides a square lithium battery. Compared with the square lithium battery provided in Embodiment 1, the only difference of the square lithium battery in this embodiment is that the lengths of the positive electrode and the negative electrode are replaced with "165mm".
[0115] Example 14
[0116] This embodiment provides a square lithium battery. Compared with the square lithium battery provided in Embodiment 1, the only difference of the square lithium battery in this embodiment is that the length of the positive electrode and the negative electrode are replaced with "145mm" and the width of the positive electrode and the negative electrode are replaced with "140mm".
[0117] Example 15
[0118] This embodiment provides a square lithium battery. Compared with the square lithium battery provided in Embodiment 1, the only difference of the square lithium battery in this embodiment is that the length of the positive electrode and the negative electrode are replaced with "150mm" and the width of the positive electrode and the negative electrode are replaced with "140mm".
[0119] Example 16
[0120] This embodiment provides a square lithium battery. Compared with the square lithium battery provided in Embodiment 1, the only difference of the square lithium battery in this embodiment is that the length of the positive electrode and the negative electrode are replaced with "155mm" and the width of the positive electrode and the negative electrode are replaced with "155mm".
[0121] Example 17
[0122] This embodiment provides a square lithium battery. Compared with the square lithium battery provided in Embodiment 1, the only difference of the square lithium battery in this embodiment is that the length of the positive electrode and the negative electrode are replaced with "165mm" and the width of the positive electrode and the negative electrode are replaced with "135mm".
[0123] Example 18
[0124] This embodiment provides a square lithium battery. Compared with the square lithium battery provided in Embodiment 1, the only difference of the square lithium battery in this embodiment is that the thickness of the square lithium battery is replaced with "35mm".
[0125] Example 19
[0126] This embodiment provides a square lithium battery. Compared with the square lithium battery provided in Embodiment 1, the only difference of the square lithium battery in this embodiment is that the thickness of the square lithium battery is replaced with "55mm".
[0127] Example 20
[0128] This embodiment provides a square lithium battery. Compared with the square lithium battery provided in Embodiment 1, the only difference of the square lithium battery in this embodiment is that the thickness of the square lithium battery is replaced with "40mm".
[0129] Example 21
[0130] This embodiment provides a square lithium battery. Compared with the square lithium battery provided in Embodiment 1, the only difference of the square lithium battery in this embodiment is that the thickness of the square lithium battery is replaced with "50mm".
[0131] Example 22
[0132] This embodiment provides a square lithium battery. Compared with the square lithium battery provided in Embodiment 1, the only difference of the square lithium battery in this embodiment is that the width of the square lithium battery is replaced with "170mm".
[0133] Example 23
[0134] This embodiment provides a square lithium battery. Compared with the square lithium battery provided in Embodiment 1, the only difference of the square lithium battery in this embodiment is that the width of the square lithium battery is replaced with "155mm".
[0135] Example 24
[0136] This embodiment provides a square lithium battery. Compared with the square lithium battery provided in Embodiment 1, the only difference of the square lithium battery in this embodiment is that the length of the square lithium battery is replaced with "165mm".
[0137] Example 25
[0138] This embodiment provides a square lithium battery. Compared with the square lithium battery provided in Embodiment 1, the only difference of the square lithium battery in this embodiment is that the length of the square lithium battery is replaced with "185mm".
[0139] Example 26
[0140] This embodiment provides a square lithium battery. Compared to the square lithium battery provided in Embodiment 1, the only difference in this embodiment is that the "Li" in the positive electrode active material layer 101113 is... 0.96 Fe 0.3 Mn 0.6 Mg 0.04 Replace "PO4" with "Li" 0.96 Fe 0.3 Mn 0.6 V 0.04 PO4.
[0141] Among them, Li 0.96 Fe 0.3 Mn 0.6 V 0.04 The preparation method of PO4 includes the following steps: replacing "1.6 kg of magnesium oxide" in step S1.1 with "3 kg of vanadium trioxide".
[0142] Example 27
[0143] This embodiment provides a square lithium battery. Compared to the square lithium battery provided in Embodiment 1, the only difference in this embodiment is that the "Li" in the positive electrode active material layer 101113 is... 0.96 Fe 0.3 Mn 0.6 Mg 0.04 Replace "PO4" with "Li" 0.96 Fe 0.3 Mn 0.6 Mg 0.02 V 0.02 PO4.
[0144] Among them, Li 0.96 Fe 0.3 Mn 0.6 Mg 0.02 V 0.02The preparation method of PO4 includes the following steps: replacing "1.6 kg of magnesium oxide" in step S1.1 with "0.8 kg of magnesium oxide and 1.5 kg of vanadium trioxide".
[0145] Comparative Example 1
[0146] This comparative example provides a square lithium battery. Compared with the square lithium battery provided in Example 1, the only difference in this comparative example is that the thickness of the positive electrode and the negative electrode are replaced with "250μm".
[0147] Comparative Example 2
[0148] This comparative example provides a square lithium battery. Compared with the square lithium battery provided in Example 1, the only difference in this comparative example is that the width of the positive electrode and the negative electrode are replaced with "110mm".
[0149] Comparative Example 3
[0150] This comparative example provides a square lithium battery. Compared with the square lithium battery provided in Example 1, the only difference in this comparative example is that the lengths of the positive and negative electrode plates are replaced with "110mm".
[0151] Comparative Example 4
[0152] This comparative example provides a square lithium battery. Compared with the square lithium battery provided in Example 1, the only difference in this comparative example is that the width of the square lithium battery is replaced with "140mm".
[0153] Comparative Example 5
[0154] This comparative example provides a square lithium battery. Compared with the square lithium battery provided in Example 1, the only difference in this comparative example is that the length of the square lithium battery is replaced with "150mm".
[0155] Experimental Example 1
[0156] The AC internal resistance of the square lithium-ion batteries in Examples 1 to 17, Example 26, and Comparative Examples 1 to 3 was tested (25°C), and the results are shown in Table 2 below:
[0157] Table 2
[0158]
[0159] As shown in Table 2, compared with the AC internal resistance (25°C) of the square lithium battery cells in Comparative Examples 1 to 3, the AC internal resistance (25°C) of the square lithium battery cells in Examples 1 to 26 is smaller.
[0160] Experiment Example 2
[0161] Electrical performance and thermal runaway tests were performed on the square lithium batteries in Examples 1 to 26 and Comparative Examples 1 to 5, respectively. The electrical performance test method included the following steps: charging each square lithium battery at 25°C with a constant current and constant voltage at a rate of 0.2C to 4.2V, wherein the constant voltage charging cutoff current was 0.02C; subsequently discharging at a constant current of 0.2C until the voltage reached 2.5V; obtaining the initial discharge capacity and initial charge capacity under the conditions of 25°C and 0.2C rate; and calculating the initial charge-discharge efficiency of each square lithium battery under the conditions of 25°C and 0.2C rate (the ratio of initial discharge capacity to initial charge capacity × 100%). The thermal runaway test method was performed according to Appendix A of GB38032-2020.
[0162] The test results are shown in Table 3 below:
[0163] Table 3
[0164]
[0165]
[0166] As shown in Tables 2 and 3, the square lithium batteries in Examples 1 to 26 exhibit better overall performance compared to the square lithium batteries in Comparative Examples 1 to 5. This indicates that in square lithium batteries, controlling the lengths of the positive and negative electrodes within the ranges of 135mm to 165mm, the widths of the positive and negative electrodes within the ranges of 135mm to 165mm, the thicknesses of the positive and negative electrodes within the ranges of 190μm to 210mm, the length of the square lithium battery within the range of 165mm to 185mm, the width within the range of 155mm to 170mm, and the thickness within the range of 35mm to 55mm ensures that the square lithium battery cell has acceptable internal resistance. Furthermore, it improves the actual capacity, energy density, rate performance, and cycle stability of the square lithium battery, and also provides good safety.
[0167] The foregoing has provided a detailed description of a stacked battery cell, a square lithium battery, a battery pack, and their applications provided by embodiments of the present invention. Specific examples have been used to illustrate the principles and implementation methods of the present invention. The descriptions of the embodiments above are merely for the purpose of helping to understand the technical solutions and core ideas of the present invention. Those skilled in the art should understand that modifications can still be made to the technical solutions described in each of the foregoing embodiments, or equivalent substitutions can be made to some of the technical features; and these modifications or substitutions do not cause the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A laminated battery cell, characterized in that, The device includes multiple battery cell units stacked sequentially along a first direction. Each battery cell unit includes a positive electrode, a separator, and a negative electrode, all stacked sequentially. A separator is provided between two adjacent battery cell units. The first direction is perpendicular to the first surface of the positive electrode near the separator. Each positive electrode of each battery cell unit has a sub-tab, and each negative electrode of each battery cell unit has a sub-tab. The sub-tabs of the positive electrode units of the multiple battery cell units are connected sequentially to form a positive electrode, and the sub-tabs of the negative electrode units of the multiple battery cell units are connected sequentially to form a negative electrode. The ratio of the length to the thickness of the positive electrode and the ratio of the length to the thickness of the negative electrode are each independently selected from 6.3 × 10⁻⁶. 2 ~9.4×10 2 The width-to-thickness ratio of the positive electrode and the width-to-thickness ratio of the negative electrode are each independently selected from 6.3 × 10⁻⁶. 2 ~9.4×10 2 ; The length of the positive electrode and the length of the negative electrode are each independently selected from 135 mm to 165 mm, the width of the positive electrode and the width of the negative electrode are each independently selected from 135 mm to 165 mm, and the thickness of the positive electrode and the thickness of the negative electrode are each independently selected from 180 μm to 215 μm. The positive electrode includes a positive current collector and a positive active material layer disposed on the surface of the positive current collector; the material of the positive active material layer includes lithium manganese iron phosphate, and the surface of the lithium manganese iron phosphate is provided with a coating layer, the material of the coating layer including carbon material.
2. The laminated battery cell according to claim 1, characterized in that, The positive electrode has the same dimensions as the negative electrode.
3. The laminated battery cell according to claim 1 or 2, characterized in that, The lengths of the positive electrode and the negative electrode are 145 mm to 155 mm, respectively; and / or The width of the positive electrode and the width of the negative electrode are 145 mm to 155 mm, respectively; and / or The ratio of the length to the thickness of the positive electrode and the ratio of the length to the thickness of the negative electrode are both 7.7 × 10⁻⁶. 2 ~8.5×10 2 ; and / or The width-to-thickness ratio of the positive electrode and the width-to-thickness ratio of the negative electrode are both 7.7 × 10⁻⁶. 2 ~8.5×10 2 ; and / or The thickness of the positive electrode and the thickness of the negative electrode are each independently selected from 190 μm to 210 μm.
4. The laminated battery cell according to claim 1 or 2, characterized in that, The general chemical formula of the lithium manganese iron phosphate material is Li. a Mn x Fe y M z (PO4) b a, x, y, z, and b represent the molar amounts of the corresponding elements, and the sum of x, y, and z is c. M is selected from one or more of Mg, Ca, Sr, Co, Ti, Zr, Mo, V, Nb, Nd, Y, Ni, Sc, Cr, Cu, Zn, Be, La, and Al. 0.10≤x≤0.70, 0.01≤z≤0.12; the ratio of a to c is a / c, 1.01≤a / c≤1.10; the ratio of a to b is a / b, 0.95<a / b<1.10; the ratio of c to b is c / b, 0.90<c / b<1.
10.
5. The stacked cell according to claim 4, characterized in that, In the aforementioned lithium manganese iron phosphate material, 0.26 ≤ x ≤ 0.68, and / or 0.01 ≤ z ≤ 0.05, and / or 1.015 ≤ a / c ≤ 1.035, and / or 0.95 < a / b < 1.03, and / or 0.90 < c / b < 1.02; and / or The mass of the carbon material accounts for 0.5% to 3% of the sum of the mass of the carbon material and the lithium manganese iron phosphate material.
6. A square lithium battery, characterized in that, The square lithium battery includes one or more stacked cells as described in any one of claims 1 to 5.
7. The square lithium battery according to claim 6, characterized in that, The length-to-width ratio of the square lithium battery is 1.00–1.13, the length-to-thickness ratio is 3.4–4.5, and the width-to-thickness ratio is 3.3–4.3; and / or The square lithium battery further includes a casing, and the stacked cells are disposed within the casing; and / or The internal resistance of the prismatic lithium battery cell at 25 °C is 0.2 mΩ to 0.5 mΩ, and / or the energy density of the prismatic lithium battery is 190 Wh / kg to 220 Wh / kg, and / or the capacity of the prismatic lithium battery is 175 Ah to 250 Ah, and / or the voltage of the prismatic lithium battery is 2.5 V to 4.2 V.
8. The square lithium battery according to claim 6 or 7, characterized in that, The length-to-width ratio of the square lithium battery is 1.06 to 1.07; and / or The length-to-thickness ratio of the square lithium battery is 4.0 to 4.1; and / or The width-to-thickness ratio of the square lithium battery is 3.7 to 3.8; and / or The length of the square lithium battery is selected from 165 mm to 185 mm; and / or The width of the square lithium battery is selected from 155 mm to 170 mm; and / or The thickness of the square lithium battery is selected from 35 mm to 55 mm.
9. The square lithium battery according to claim 6 or 7, characterized in that, The length of the square lithium battery is selected from 170 mm to 180 mm; and / or The width of the square lithium battery is selected from 160 mm to 170 mm; and / or The thickness of the square lithium battery is selected from 40 mm to 50 mm.
10. The square lithium battery according to claim 6 or 7, characterized in that, The length of the square lithium battery is selected from 174 mm to 180 mm; and / or The width of the square lithium battery is selected from 160 mm to 165 mm; and / or The thickness of the square lithium battery is selected from 40 mm to 45 mm.
11. A battery pack, characterized in that, The battery pack includes a housing and a plurality of stacked cells as described in any one of claims 1 to 5, or a plurality of square lithium batteries as described in any one of claims 6 to 10, wherein the housing forms an accommodating space and the plurality of square lithium batteries are arranged sequentially within the accommodating space.
12. The application of the stacked cell according to any one of claims 1 to 5, or the prismatic lithium battery according to any one of claims 6 to 10, or the battery pack according to claim 11 in a vehicle, characterized in that, The battery cell, or the square lithium battery, or the battery pack, serves as the power source for the vehicle.
13. The application according to claim 12, characterized in that, The vehicles are selected from trucks, logistics vehicles, or engineering vehicles.
Citation Information
Patent Citations
Nonaqueous electrolyte power storage element
JP2023056402A
Lithium-ion battery with medium and small capacity and high output
KR1020090003328A