A high heat-resistant separator for lithium-ion batteries and its preparation method
By controlling the speed difference of the transmission rollers during the lithium-ion battery separator preparation process, and combining heat-resistant polymer and inorganic material coatings, the stretching problem caused by excessive tension during the coating process of the separator was solved, thereby improving the thermal stability of the separator and the safety of the battery.
Patent Information
- Application Number
- CN202210936399.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-05
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-08-05
AI Technical Summary
Existing lithium-ion battery separators are prone to stretching due to excessive tension during the coating process, which leads to a decrease in thermal stability and affects battery safety performance. Furthermore, slippage of the drive rollers causes instability in porosity and thermal shrinkage rate.
By controlling the speed difference of the drive rollers in each process, the diaphragm is kept stable during unwinding, coating, solidification, washing, drying and setting processes to avoid diaphragm stretching. Multiple roller groups are staggered to reduce slippage. Heat-resistant polymer and inorganic material coatings are used.
This achieves low deformation and low thermal shrinkage of the separator, improving the safety and electrochemical performance of lithium-ion batteries.
Smart Images

Figure CN117559075B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium battery separator technology, specifically relating to a high heat-resistant separator for lithium-ion batteries and its preparation method. Background Technology
[0002] The separator is one of the four key materials in lithium-ion batteries. It directly affects the performance and safety of the battery. A separator with excellent appearance and performance has an important impact on improving the overall performance of lithium-ion batteries.
[0003] Conventional polyolefin separators suffer from poor thermal stability. To mitigate this, a single or double layer of inorganic filler is typically coated onto the surface, which can improve the high thermal shrinkage and deformation issues. However, ceramic-coated separators have high surface density, and once the temperature exceeds the melting point of polyolefins, the discontinuous inorganic coating cannot guarantee the separator's integrity. Therefore, an increasing number of separator products are using heat-resistant polymer materials as coatings to address the thermal shrinkage problem.
[0004] However, there are still some problems in the manufacturing process of the heat-resistant polymer-coated diaphragms currently being produced. For example, since most polymer materials have high solubility in organic solvents, the organic solvents need to be removed through processes such as coagulation and washing in the later stages of production to complete the pore formation of the coating.
[0005] The base film has already been heat-set during the molding process. During the coating stage, it is necessary to avoid stretching to prevent the already formed circular holes from turning into elliptical holes. The long axis direction is consistent with the stretching direction. In fact, when the tension increases, the distance between the filaments in the short axis direction continuously decreases, the holes are closed, the fibers break, and microscopic damage is caused, affecting the porosity and thermal shrinkage performance of the separator, and even the electrochemical performance and safety performance after the battery is assembled.
[0006] In the current production process of oil-coated diaphragms, the coagulation and washing tanks are driven by multi-roller sets. The liquid in the coagulation tank is generally a mixture of organic solvent and water, while the washing tank is generally composed of water and a small amount of organic solvent replaced in the coating. The solution in the washing tank overflows into the coagulation tank. The ratio of organic solvent to water in the coagulation tank is maintained by a concentration meter, and a certain amount of excessively high concentration mixed liquid is discharged.
[0007] The coagulation and washing tanks contain organic solvents, which cause good lubrication between the film and the drive rollers, making slippage likely. This necessitates adjusting and increasing tension to transfer the coated film to the next process. Excessive tension stretches the separator and affects coating thickness. Coatings with different solid contents exhibit different properties and have varying maximum acceptable tension values. The phased coating process, with its uniform speed, inevitably leads to separator stretching, affecting thermal stability and reducing the safety performance of lithium-ion batteries. Summary of the Invention
[0008] The purpose of this invention is to provide a high heat-resistant separator for lithium-ion batteries and its preparation method. The lithium-ion battery separator of this invention exhibits low deformation and low thermal shrinkage.
[0009] In a first aspect, the present invention provides a method for preparing a high heat-resistant separator for lithium-ion batteries. The base film sequentially undergoes unwinding, coating, coagulation, washing, drying, shaping, and rewinding processes. The coagulation and washing processes are both driven by a multi-roller assembly, which includes a lower drive roller, an upper drive roller, and a transition drive roller. During the preparation process, the following conditions are met: 1.05V0≥V 21 >V 23 >V 22 ≥V1≥V0, V 23 ≥V 31 >V 33 >V 32 ≥V4≥V5≥V0, V 21 + V 22 ≥2V 23 ;
[0010] in:
[0011] V0 is the speed of the drive rollers in the unwinding and rewinding processes;
[0012] V1 is the speed of the drive roller in the coating process;
[0013] V 21 V is the speed of the drive rollers during the solidification process. 22 V represents the speed of the drive rollers in the solidification process. 23 The speed of the transmission rollers is adjusted for the solidification process.
[0014] V 31 V is the speed of the drive roller in the washing process. 32 V is the speed of the drive roller in the water washing process. 33 The speed of the transition drive rollers in the water washing process;
[0015] V4 is the speed of the drive roller in the drying process;
[0016] V5 is the speed of the drive rollers in the shaping process.
[0017] Secondly, the present invention provides a diaphragm prepared by the method, wherein the thermal shrinkage rate of the diaphragm in the MD / TD direction satisfies: 130℃ / h, MD≤1.5%, TD≤1%.
[0018] This invention reduces the impact of membrane stretching by limiting and controlling the speed difference of the drive rollers in each process, thus maintaining the membrane's porosity and obtaining a highly heat-resistant membrane. Specifically, it controls the speed and speed difference between the rollers in the unwinding, coating, coagulation, washing, drying, setting, and winding processes. This ensures stable membrane transport and prevents the membrane from undergoing microscopic damage caused by the continuous reduction of the short-axis fiber distance, pore closure, and fiber breakage due to excessive tension. It also reduces slippage of the drive rollers during membrane transport caused by different concentrations of mixed solutions in the coagulation and washing processes. Attached Figure Description
[0019] Figure 1 This is a process flow diagram of the preparation method of the high heat-resistant separator for lithium-ion batteries according to the present invention;
[0020] Figure 2 A schematic diagram of the solidification tank used in the solidification process;
[0021] Figure 3 A schematic diagram of the water washing tank used in the water washing process;
[0022] Figure 4 A schematic diagram of the drying box used in the drying process;
[0023] Figure 5 This is a schematic diagram of the structure of the shaping oven used in the shaping process.
[0024] In the attached figures, the following labels are used:
[0025] 1-Coagulation tank; 2-Coated film; 3-Lower drive roller of coagulation tank; 4-Upper drive roller of coagulation tank; 5-Transition roller of coagulation tank; 6-Washing tank; 7-Lower drive roller of washing tank; 8-Upper drive roller of washing tank; 9-Transition roller of washing tank. Detailed Implementation
[0026] The present invention will now be described in detail through embodiments. It should be noted that the following embodiments are only for further illustration of the present invention and should not be construed as limiting the scope of protection of the present invention. Those skilled in the art can make some non-essential improvements and adjustments to the present invention based on the above description.
[0027] The first aspect of this invention provides a method for preparing a high heat-resistant separator for lithium-ion batteries. The base film sequentially undergoes unwinding, coating, coagulation, washing, drying, shaping, and rewinding processes. The coagulation and washing processes are both driven by a multi-roller assembly, which includes a lower drive roller, an upper drive roller, and a transition drive roller. During the preparation process, the following conditions are met: 1.05V0≥V 21 >V 23 >V 22≥V1≥V0, V 23 ≥V 31 >V 33 >V 32 ≥V4≥V5≥V0, V 21 + V 22 ≥2V 23 ;
[0028] in:
[0029] V0 is the speed of the drive rollers in the unwinding and rewinding processes;
[0030] V1 is the speed of the drive roller in the coating process;
[0031] V 21 V is the speed of the drive rollers during the solidification process. 22 V represents the speed of the drive rollers in the solidification process. 23 The speed of the transmission rollers is adjusted for the solidification process.
[0032] V 31 V is the speed of the drive roller in the washing process. 32 V is the speed of the drive roller in the water washing process. 33 The speed of the transition drive rollers in the water washing process;
[0033] V4 is the speed of the drive roller in the drying process;
[0034] V5 is the speed of the drive rollers in the shaping process.
[0035] Figure 1 This is a process flow diagram of the preparation method of the high heat-resistant separator for lithium-ion batteries according to the present invention. Figure 2 A schematic diagram of the solidification tank used in the solidification process; Figure 3 A schematic diagram of the water washing tank used in the water washing process; Figure 4 A schematic diagram of the drying box used in the drying process; Figure 5 This is a structural diagram of the shaping oven used in the shaping process. Please refer to it. Figures 1 to 5 In the preparation of the diaphragm, the base film is first unwound using an unwinding device, and then coated with a coating material using a coating device to obtain a coated film 2. The coated film 2 then enters a coagulation tank 1 for pre-coagulation. Figure 2As shown, the coagulation tank 1 contains three transmission zones: a lower transmission roller 3, an upper transmission roller 4, and a transition roller 5. The coagulation tank 1 contains a solution for pre-coating the coating to displace the organic solvent in the coating. The lower transmission roller 3 is immersed in this solution. Multiple lower transmission rollers 3 and upper transmission rollers 4 are arranged alternately. The coated film 2 first passes through the lower transmission roller 3 and is then moved upwards to the upper transmission roller 4, then downwards back to the lower transmission roller 3, and then upwards again to the upper transmission roller 4. This sequential transmission continues until finally, the film is conveyed by the transition roller 5 to the washing tank 6. Figure 3 As shown, the washing tank 6 contains three transmission zones: a lower transmission roller 7, an upper transmission roller 8, and a transition roller 9. The washing tank 6 is filled with water to clean residual organic solvents. The lower transmission roller 7 is immersed in water. There are multiple lower transmission rollers 7 and upper transmission rollers 8, which are arranged in an alternating manner. The coated film 2 is first passed through the lower transmission roller 7 and then upward to the upper transmission roller 8. Then it is passed downward to the lower transmission roller 7 and then upward to the upper transmission roller 8 again. This transmission is repeated in sequence. Finally, it is conveyed by the transition roller 9 to the drying oven of the drying process. After the drying process, it is conveyed to the setting oven of the setting process. After the setting process, the finished diaphragm is obtained and then wound up.
[0036] The base film described in this invention is a polyolefin base film, such as a polyethylene base film, a polypropylene base film, a mixed base film of polyethylene and polypropylene, or a multilayer film, preferably a polyethylene base film.
[0037] The source of the base film is not limited. It can be prepared by existing methods or purchased commercially. For example, polyolefin base films can be prepared by wet or dry processes of unidirectional or bidirectional stretching.
[0038] The thickness of the base film is not particularly limited in this invention, as long as it is suitable for use as a separator in lithium batteries. Generally, the thickness is less than 20 μm, for example, it can be 4~20 μm, such as 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20 μm.
[0039] The coating applied in the coating process of this invention includes heat-resistant polymer materials and heat-resistant inorganic materials, and the coating thickness is 1~6μm.
[0040] There are no particular limitations on the heat-resistant polymer material. It can be any polymer material known in the art with a melting point higher than that of the base film. The base film raw material is generally polyolefin. The heat-resistant polymer material can be, for example, polyamide, polyimide, polyetherimide, polyamideimide, polysulfone, polyethersulfone, polyarylsulfone, etc. Aromatic polyamide is preferred, and para-aromatic polyamide is particularly preferred.
[0041] There are no particular limitations on the heat-resistant inorganic material, which can be at least one of alumina, boehmite, magnesium oxide, calcium oxide, barium oxide, zinc oxide, silicon dioxide, titanium dioxide, zirconium dioxide, magnesium hydroxide, and aluminum hydroxide, with alumina being preferred.
[0042] In this invention, the alumina has a particle size of D99≤1μm and D50≤500 nm.
[0043] The para-aromatic polyamide is provided by a para-aromatic polyamide stock solution. Preferably, the weight percentage of para-aromatic polyamide in the stock solution is 2±1%. More preferably, the specific logarithmic viscosity of the para-aromatic polyamide stock solution is 2±1 dL / g, and more preferably 2±0.5 dL / g. It can be prepared in-house or purchased commercially, for example from companies such as Zhonglan Chenguang Chemical Co., Ltd., Shandong Jufang New Material Co., Ltd., Shanghai Huibo New Material Technology Co., Ltd., and Yantai Taihe New Material Co., Ltd.
[0044] In the specific coating process, the heat-resistant polymer material is dissolved in an organic compound solvent, and at the same time, a heat-resistant inorganic material is added to the solvent. The organic compound solvent can be an organic compound solvent known in the art that can dissolve heat-resistant polymers, such as at least one of N-methylpyrrolidone (NMP), dimethylacetamide (DMAC), N,N-dimethylformamide (DMF), acetone, and dichloromethane, preferably N-methylpyrrolidone (NMP).
[0045] The thickness of the coating is not particularly limited in this invention, as long as it is suitable for use as a separator in lithium batteries. For example, it can be 1-6 μm, such as 1, 2, 3, 4, 5, or 6 μm.
[0046] A second aspect of the present invention provides a diaphragm prepared by the method, wherein the diaphragm has a thermal shrinkage rate in the MD / TD direction satisfying: 130℃ / h, MD≤1.5%, TD≤1%.
[0047] The present invention will be further described below with reference to the embodiments, but the scope of the present invention is not limited to these embodiments.
[0048] The aramid fiber solution was purchased from Zhonglan Chenguang Chemical Design Institute Co., Ltd., with the grade T3 (para-aromatic polyamide solution, polymer content of 3% by weight, specific concentration logarithmic viscosity of para-aromatic polyamide solution of 2dL / g, solvent of NMP); the ceramic powder (D50=400nm) was purchased from Suzhou Jinyi New Material Technology Co., Ltd.
[0049] The preparation method of aramid slurry is as follows: ceramic powder (5 parts by weight) is added to aramid stock solution (95 parts by weight) and dispersed at high speed. The dispersed mixture is filtered (400# filter screen) to obtain aramid slurry.
[0050] The liquid in the coagulation tank consists of NMP and water, with an NMP volume concentration of 40%.
[0051] The base film is a polyethylene base film with a thickness of 15μm.
[0052] The numerical values of the examples and comparative examples are shown in Table 1.
[0053] Example 1
[0054] The base film is unwound at a production speed of V0 and enters the diaphragm coating unit. The aramid slurry is coated onto one side of the base film using a T-shaped narrow slit coating mechanism. The coating process is set to a speed of V1.
[0055] Then, the coating enters the coagulation process. The resulting coating film undergoes pre-coagulation in a coagulation bath, where the aramid fibers in the coating gradually precipitate out, forming a three-dimensional network structure. The NMP in the coating dissolves in the coagulation bath and is slowly displaced. At this point, the speed of the lower drive roller in the coagulation tank is set to V. 21 The speed of the upper drive guide roller is V 22 The transition roller speed is V 23 .
[0056] The coating film, pre-coated in the coagulation tank, enters the washing process to remove residual NMP. At this point, the speed of the lower drive roller in the coagulation tank is set to V. 31 The speed of the upper drive guide roller is V 32 The transition roller speed is V 33 .
[0057] After being washed, the aramid-coated diaphragm enters the drying process, with the drive roller speed set to V4 and the oven temperature set to 85℃.
[0058] After drying, the aramid-coated diaphragm enters the heat treatment process, with the drive roller speed set to V5 and the oven temperature set to 120℃.
[0059] Finally, the coated film is wound up, and the machine speed is set to V0.
[0060] The specific values for the roller speeds of each process are shown in Table 1.
[0061] Example 2
[0062] The base film is unwound at a production speed of V0 and enters the diaphragm coating unit. The aramid slurry is coated onto one side of the base film using a T-shaped narrow slit coating mechanism. The coating process is set to a speed of V1.
[0063] Then, the coating enters the coagulation process. The resulting coating film undergoes pre-coagulation in a coagulation bath, where the aramid fibers in the coating gradually precipitate out, forming a three-dimensional network structure. The NMP in the coating dissolves in the coagulation bath and is slowly displaced. At this point, the speed of the lower drive roller in the coagulation tank is set to V. 21The speed of the upper drive guide roller is V 22 The transition roller speed is V 23 .
[0064] The coating film, pre-coated in the coagulation tank, enters the washing process to remove residual NMP. At this point, the speed of the lower drive roller in the coagulation tank is set to V. 31 The speed of the upper drive guide roller is V 32 The transition roller speed is V 33 .
[0065] After being washed, the aramid-coated diaphragm enters the drying process, with the drive roller speed set to V4 and the oven temperature set to 85℃.
[0066] After drying, the aramid-coated diaphragm enters the heat treatment process, with the drive roller speed set to V5 and the oven temperature set to 120℃.
[0067] Finally, the coated film is wound up, and the machine speed is set to V0.
[0068] The specific values for the roller speeds of each process are shown in Table 1.
[0069] Example 3
[0070] The base film is unwound at a production speed of V0 and enters the diaphragm coating unit. The aramid slurry is coated onto one side of the base film using a T-shaped narrow slit coating mechanism. The coating process is set to a speed of V1.
[0071] Then, the coating enters the coagulation process. The resulting coating film undergoes pre-coagulation in a coagulation bath, where the aramid fibers in the coating gradually precipitate out, forming a three-dimensional network structure. The NMP in the coating dissolves in the coagulation bath and is slowly displaced. At this point, the speed of the lower drive roller in the coagulation tank is set to V. 21 The speed of the upper drive guide roller is V 22 The transition roller speed is V 23 .
[0072] The coating film, pre-coated in the coagulation tank, enters the washing process to remove residual NMP. At this point, the speed of the lower drive roller in the coagulation tank is set to V. 31 The speed of the upper drive guide roller is V 32 The transition roller speed is V 33 .
[0073] After being washed, the aramid-coated diaphragm enters the drying process, with the drive roller speed set to V4 and the oven temperature set to 85℃.
[0074] After drying, the aramid-coated diaphragm enters the heat treatment process, with the drive roller speed set to V5 and the oven temperature set to 120℃.
[0075] Finally, the coated film is wound up, and the machine speed is set to V0.
[0076] The specific values for the roller speeds of each process are shown in Table 1.
[0077] Example 4
[0078] The base film is unwound at a production speed of V0 and enters the diaphragm coating unit. The aramid slurry is coated onto one side of the base film using a T-shaped narrow slit coating mechanism. The coating process is set to a speed of V1.
[0079] Then, the coating enters the coagulation process. The resulting coating film undergoes pre-coagulation in a coagulation bath, where the aramid fibers in the coating gradually precipitate out, forming a three-dimensional network structure. The NMP in the coating dissolves in the coagulation bath and is slowly displaced. At this point, the speed of the lower drive roller in the coagulation tank is set to V. 21 The speed of the upper drive guide roller is V 22 The transition roller speed is V 23 .
[0080] The coating film, pre-coated in the coagulation tank, enters the washing process to remove residual NMP. At this point, the speed of the lower drive roller in the coagulation tank is set to V. 31 The speed of the upper drive guide roller is V 32 The transition roller speed is V 33 .
[0081] After being washed, the aramid-coated diaphragm enters the drying process, with the drive roller speed set to V4 and the oven temperature set to 85℃.
[0082] After drying, the aramid-coated diaphragm enters the heat treatment process, with the drive roller speed set to V5 and the oven temperature set to 120℃.
[0083] Finally, the coated film is wound up, and the machine speed is set to V0.
[0084] The specific values for the roller speeds of each process are shown in Table 1.
[0085] Example 5
[0086] The base film is unwound at a production speed of V0 and enters the diaphragm coating unit. The aramid slurry is coated onto one side of the base film using a T-shaped narrow slit coating mechanism. The coating process is set to a speed of V1.
[0087] Then, the coating enters the coagulation process. The resulting coating film undergoes pre-coagulation in a coagulation bath, where the aramid fibers in the coating gradually precipitate out, forming a three-dimensional network structure. The NMP in the coating dissolves in the coagulation bath and is slowly displaced. At this point, the speed of the lower drive roller in the coagulation tank is set to V. 21 The speed of the upper drive guide roller is V 22 The transition roller speed is V 23 .
[0088] The coating film, pre-coated in the coagulation tank, enters the washing process to remove residual NMP. At this point, the speed of the lower drive roller in the coagulation tank is set to V.31 The speed of the upper drive guide roller is V 32 The transition roller speed is V 33 .
[0089] After being washed, the aramid-coated diaphragm enters the drying process, with the drive roller speed set to V4 and the oven temperature set to 85℃.
[0090] After drying, the aramid-coated diaphragm enters the heat treatment process, with the drive roller speed set to V5 and the oven temperature set to 120℃.
[0091] Finally, the coated film is wound up, and the machine speed is set to V0.
[0092] The specific values for the roller speeds of each process are shown in Table 1.
[0093] Example 6
[0094] The base film is unwound at a production speed of V0 and enters the diaphragm coating unit. The aramid slurry is coated onto one side of the base film using a T-shaped narrow slit coating mechanism. The coating process is set to a speed of V1.
[0095] Then, the coating enters the coagulation process. The resulting coating film undergoes pre-coagulation in a coagulation bath, where the aramid fibers in the coating gradually precipitate out, forming a three-dimensional network structure. The NMP in the coating dissolves in the coagulation bath and is slowly displaced. At this point, the speed of the lower drive roller in the coagulation tank is set to V. 21 The speed of the upper drive guide roller is V 22 The transition roller speed is V 23 .
[0096] The coating film, pre-coated in the coagulation tank, enters the washing process to remove residual NMP. At this point, the speed of the lower drive roller in the coagulation tank is set to V. 31 The speed of the upper drive guide roller is V 32 The transition roller speed is V 33 .
[0097] After being washed, the aramid-coated diaphragm enters the drying process, with the drive roller speed set to V4 and the oven temperature set to 85℃.
[0098] After drying, the aramid-coated diaphragm enters the heat treatment process, with the drive roller speed set to V5 and the oven temperature set to 120℃.
[0099] Finally, the coated film is wound up, and the machine speed is set to V0.
[0100] The specific values for the roller speeds of each process are shown in Table 1.
[0101] Comparative Example 1
[0102] The base film is unwound at a production speed of V0 and enters the diaphragm coating unit. The aramid slurry is coated onto one side of the base film using a T-shaped narrow slit coating mechanism. The coating process is set to a speed of V1.
[0103] Then, the coating enters the coagulation process. The resulting coating film undergoes pre-coagulation in a coagulation bath, where the aramid fibers in the coating gradually precipitate out, forming a three-dimensional network structure. The NMP in the coating dissolves in the coagulation bath and is slowly displaced. At this point, the speed of the lower drive roller in the coagulation tank is set to V. 21 The speed of the upper drive guide roller is V 22 The transition roller speed is V 23 .
[0104] The coating film, pre-coated in the coagulation tank, enters the washing process to remove residual NMP. At this point, the speed of the lower drive roller in the coagulation tank is set to V. 31 The speed of the upper drive guide roller is V 32 The transition roller speed is V 33 .
[0105] After being washed, the aramid-coated diaphragm enters the drying process, with the drive roller speed set to V4 and the oven temperature set to 85℃.
[0106] After drying, the aramid-coated diaphragm enters the heat treatment process, with the drive roller speed set to V5 and the oven temperature set to 120℃.
[0107] Finally, the coated film is wound up, and the machine speed is set to V0.
[0108] The specific values for the roller speeds of each process are shown in Table 1.
[0109] Comparative Example 2
[0110] The base film is unwound at a production speed of V0 and enters the diaphragm coating unit. The aramid slurry is coated onto one side of the base film using a T-shaped narrow slit coating mechanism. The coating process is set to a speed of V1.
[0111] Then, the coating enters the coagulation process. The resulting coating film undergoes pre-coagulation in a coagulation bath, where the aramid fibers in the coating gradually precipitate out, forming a three-dimensional network structure. The NMP in the coating dissolves in the coagulation bath and is slowly displaced. At this point, the speed of the lower drive roller in the coagulation tank is set to V. 21 The speed of the upper drive guide roller is V 22 The transition roller speed is V 23 .
[0112] The coating film, pre-coated in the coagulation tank, enters the washing process to remove residual NMP. At this point, the speed of the lower drive roller in the coagulation tank is set to V. 31 The speed of the upper drive guide roller is V 32 The transition roller speed is V 33 .
[0113] After being washed, the aramid-coated diaphragm enters the drying process, with the drive roller speed set to V4 and the oven temperature set to 85℃.
[0114] After drying, the aramid-coated diaphragm enters the heat treatment process, with the drive roller speed set to V5 and the oven temperature set to 120℃.
[0115] Finally, the coated film is wound up, and the machine speed is set to V0.
[0116] The specific values for the roller speeds of each process are shown in Table 1.
[0117] Comparative Example 3
[0118] The base film is unwound at a production speed of V0 and enters the diaphragm coating unit. The aramid slurry is coated onto one side of the base film using a T-shaped narrow slit coating mechanism. The coating process is set to a speed of V1.
[0119] Then, the coating enters the coagulation process. The resulting coating film undergoes pre-coagulation in a coagulation bath, where the aramid fibers in the coating gradually precipitate out, forming a three-dimensional network structure. The NMP in the coating dissolves in the coagulation bath and is slowly displaced. At this point, the speed of the lower drive roller in the coagulation tank is set to V. 21 The speed of the upper drive guide roller is V 22 The transition roller speed is V 23 .
[0120] The coating film, pre-coated in the coagulation tank, enters the washing process to remove residual NMP. At this point, the speed of the lower drive roller in the coagulation tank is set to V. 31 The speed of the upper drive guide roller is V 32 The transition roller speed is V 33 .
[0121] After being washed, the aramid-coated diaphragm enters the drying process, with the drive roller speed set to V4 and the oven temperature set to 85℃.
[0122] After drying, the aramid-coated diaphragm enters the heat treatment process, with the drive roller speed set to V5 and the oven temperature set to 120℃.
[0123] Finally, the coated film is wound up, and the machine speed is set to V0.
[0124] The specific values for the roller speeds of each process are shown in Table 1.
[0125] The performance of the coated films prepared in the examples and comparative examples was tested:
[0126] Porosity test
[0127] The percentage of the volume of pores inside the diaphragm relative to the total volume of the diaphragm. The test is conducted using the method specified in GB / T 36363-2018.
[0128] Heat shrinkage test
[0129] The test shall be conducted in accordance with the method specified in GB / T12027-2004.
[0130] The specific results are shown in Table 1.
[0131] Table 1
[0132] As can be seen from Table 1, the high heat-resistant diaphragm prepared in Examples 1-6 has a significantly higher porosity and a significantly lower thermal shrinkage rate compared to the diaphragm obtained in Comparative Examples 1-3, which did not strictly control the speed and speed difference of the rollers in each process.
[0133] Of course, the present invention may have other various embodiments. Without departing from the spirit and essence of the present invention, those skilled in the art can make various corresponding changes and modifications according to the present invention, but these corresponding changes and modifications should all fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing a high heat-resistant separator for lithium-ion batteries, wherein the base film sequentially undergoes unwinding, coating, coagulation, washing, drying, shaping, and rewinding processes, wherein the coagulation and washing processes are both driven by a multi-roller group, the multi-roller group comprising a lower drive roller, an upper drive roller, and a transition drive roller, characterized in that, The following conditions must be met during the preparation process: 1.05V0≥V 21 >V 23 >V 22 ≥V1≥V0, V 23 ≥V 31 >V 33 >V 32 ≥V4≥V5≥V0, V 21 + V 22 ≥2V 23 ; in: V0 is the speed of the drive rollers in the unwinding and rewinding processes; V1 is the speed of the drive roller in the coating process; V 21 V represents the speed of the drive rollers during the solidification process. 22 V represents the speed of the drive rollers in the solidification process. 23 The speed of the transmission rollers is adjusted for the solidification process. V 31 V is the speed of the drive roller in the washing process. 32 V is the speed of the drive roller in the water washing process. 33 The speed of the transition drive rollers in the water washing process; V4 is the speed of the drive roller in the drying process; V5 is the speed of the drive rollers in the shaping process; The coated film is first passed through the lower drive roller of the coagulation tank and then passed upward to the upper drive roller of the coagulation tank. Then it is passed downward to the lower drive roller of the coagulation tank and then passed upward to the upper drive roller of the coagulation tank. This process is repeated in sequence, and finally the film is conveyed to the washing tank by the transition roller of the coagulation tank. The washing tank contains three transmission zones: a lower transmission roller, an upper transmission roller, and a transition roller. The washing tank is filled with water to clean residual organic solvents. The lower transmission roller is immersed in water. There are multiple lower and upper transmission rollers arranged alternately. The coated film first passes through the lower transmission roller and is then transferred upwards to the upper transmission roller, then downwards to the lower transmission roller, and then upwards again to the upper transmission roller. This process continues sequentially until the film is finally conveyed by the transition roller to the drying oven in the drying process.
2. The method for preparing a high heat-resistant separator for lithium-ion batteries according to claim 1, characterized in that, The base film is one of polyethylene base film, polypropylene base film, mixed base film of polyethylene and polypropylene, or multilayer film.
3. The method for preparing a high heat-resistant separator for lithium-ion batteries according to claim 1, characterized in that, The base film is a polyethylene base film.
4. The method for preparing a high heat-resistant separator for lithium-ion batteries according to claim 1, characterized in that, The thickness of the base film is less than or equal to 20 μm.
5. The method for preparing a high heat-resistant separator for lithium-ion batteries according to claim 1, characterized in that, The coating applied in the coating process includes heat-resistant polymer materials and heat-resistant inorganic materials, and the coating thickness is 1~6μm.
6. The method for preparing a high heat-resistant separator for lithium-ion batteries according to claim 5, characterized in that, The heat-resistant polymer material is a polymer material with a melting point higher than that of the base film.
7. The method for preparing a high heat-resistant separator for lithium-ion batteries according to claim 6, characterized in that, The polymer material is one of polyamide, polyimide, polyetherimide, polyamideimide, polysulfone, polyethersulfone, and polyarylsulfone.
8. The method for preparing a high heat-resistant separator for lithium-ion batteries according to claim 7, characterized in that, The polymer material is an aromatic polyamide.
9. The method for preparing a high heat-resistant separator for lithium-ion batteries according to claim 7, characterized in that, The polymer material is a para-aromatic polyamide.
10. The method for preparing a high heat-resistant separator for lithium-ion batteries according to claim 9, characterized in that, The para-aromatic polyamide is provided by a para-aromatic polyamide stock solution, wherein the weight percentage of para-aromatic polyamide in the stock solution is 2±1%.
11. The method for preparing a high heat-resistant separator for lithium-ion batteries according to claim 10, characterized in that, The specific logarithmic viscosity of the para-aromatic polyamide stock solution is 2 ± 1 dL / g.
12. The method for preparing a high heat-resistant separator for lithium-ion batteries according to claim 11, characterized in that, The specific logarithmic viscosity of the para-aromatic polyamide stock solution is 2 ± 0.5 dL / g.
13. The method for preparing a high heat-resistant separator for lithium-ion batteries according to claim 5, characterized in that, The heat-resistant inorganic material is at least one of alumina, boehmite, magnesium oxide, calcium oxide, barium oxide, zinc oxide, silicon dioxide, titanium dioxide, zirconium dioxide, magnesium hydroxide, and aluminum hydroxide.
14. The method for preparing a high heat-resistant separator for lithium-ion batteries according to claim 13, characterized in that, The heat-resistant inorganic material is alumina.
15. The method for preparing a high heat-resistant separator for lithium-ion batteries according to claim 13 or 14, characterized in that, The alumina has a particle size of D99≤1μm and D50≤500 nm.
16. The diaphragm prepared by the method according to any one of claims 1 to 15, characterized in that, The thermal shrinkage rate of the diaphragm in the MD / TD direction satisfies the following conditions: 130℃ / h, MD≤1.5%, TD≤1%.
Citation Information
Patent Citations
Wet spinning machine, chlorinated polyvinyl chloride fiber and preparation method thereof
CN107366031A
KR20220076143A