A precise forming method for vacuum isothermal forging of titanium-aluminum alloy components with fine and uniform lamellar structure.

By using vacuum isothermal forging technology to perform pressure-holding heat treatment during the forging process, the oxidation and cracking problems in the forging process of titanium-aluminum alloys are solved, and the fine, uniform, full-layer structure and precise forming of titanium-aluminum alloy components are achieved, thereby reducing costs.

CN117583521BActive Publication Date: 2026-11-17HARBIN INST OF TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202311664356.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-06
Publication Date
2026-11-17
Estimated Expiration
2043-12-06

AI Technical Summary

Technical Problem

Titanium-aluminum alloys are prone to oxidation and cracking during forging, resulting in low yield. The heat treatment process needs to be carried out separately, which increases energy consumption and cost, and makes it difficult to achieve precise forming.

Method used

Vacuum isothermal forging technology is adopted, and pressure holding heat treatment is carried out during the forging process to continuously complete the forging and heat treatment, avoiding oxidation and cracks. Pressure holding heat treatment is carried out in the forging die using vacuum isothermal forging equipment to ensure uniform structure and dimensional accuracy.

Benefits of technology

This method achieves a fine, uniform, full-lamellar microstructure in titanium-aluminum alloy components, improving yield, reducing costs, and ensuring the dimensional accuracy and excellent performance of forgings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117583521B_ABST
    Figure CN117583521B_ABST
Patent Text Reader

Abstract

A precise forming method for vacuum isothermal forging of titanium-aluminum alloy components with a fine, uniform, fully lamellar microstructure is disclosed. This invention relates to the field of titanium-aluminum alloy component preparation technology. The method employs vacuum isothermal forging technology to prepare titanium-aluminum alloy forgings, significantly improving the uniformity of the temperature field and preventing defects such as cracks in the forgings. After forging, without unloading the pressure, the temperature is directly adjusted to the α-phase temperature of the titanium-aluminum alloy. The titanium-aluminum alloy forging is subjected to pressure-holding isothermal heat treatment directly in the forging die, followed by furnace cooling. After cooling to below the phase transformation temperature of the titanium-aluminum alloy, the pressure is unloaded, and finally, the titanium-aluminum alloy component is removed. This invention shortens the process, obtaining a component with an ideal fine, uniform, fully lamellar microstructure in a single step. Furthermore, because the heat treatment is performed under external force constraints, it ensures that the titanium-aluminum alloy forging does not deform during the heat treatment process, achieving precise control of the forging's dimensional accuracy. This significantly reduces component manufacturing costs and demonstrates significant commercial value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of titanium-aluminum alloy component preparation technology, specifically to a precise forming method for vacuum isothermal forging of titanium-aluminum alloy components with fine and uniform full-layer structure. Background Technology

[0002] Titanium-aluminum alloy is a novel lightweight high-temperature structural material with broad application prospects in the fields of aviation, aerospace, military, and automotive engines. It possesses excellent properties such as low density, high specific strength, high specific stiffness, good oxidation resistance, creep resistance, fatigue resistance, and good flame retardancy. Its service temperature range reaches 600-850℃, and its density is only half that of nickel-based superalloys. It is an important lightweight, high-temperature resistant metallic structural material to replace high-density nickel-based superalloys, achieving weight reduction of 40-50%, thereby significantly improving equipment performance. Currently, titanium-aluminum alloy components have been successfully applied in engineering projects abroad. Since GE's titanium-aluminum alloy blades were first used in the GEnx engine of the Boeing 787 aircraft in 2007, there has been 15 years of application experience. Europe has also applied titanium-aluminum alloy blades to the Airbus A320 aircraft engine and successfully test-flown them. The application of titanium-aluminum alloys in civil aviation engines has achieved a weight reduction of 200 pounds per engine, greatly improving various engine performance indicators. In addition, Europe, the United States, Japan and other countries have successfully applied titanium-aluminum alloys to automobile turbochargers and exhaust valves, which has greatly improved the engine's startability and dynamic response, reduced engine exhaust emissions and improved engine fuel thermal efficiency.

[0003] Hot forging technology for titanium-aluminum alloys has always been one of the main directions of their research and development. As a difficult-to-machine material, titanium-aluminum alloys require very high forging temperatures, generally needing to be heated to 1200-1350℃. During ordinary high-temperature forging, due to heat dissipation, large temperature field changes, and severe oxidation of the titanium-aluminum alloy surface, a large amount of oxide scale easily forms on the surface, and the forging cracks, resulting in a very low yield and making large-scale production difficult. Currently, to prevent the uneven temperature field caused by the large heat dissipation during titanium-aluminum alloy forging and the severe high-temperature oxidation of the alloy, the near-isothermal cladding forging method is mainly used to prepare titanium-aluminum alloy forging blanks. However, because the titanium-aluminum alloy is clad with a relatively thick stainless steel or other materials, this method is only suitable for simple forging blank preparation such as upsetting and is not suitable for the manufacture of precision forgings.

[0004] The microstructure of titanium-aluminum alloys significantly affects their mechanical properties. After high-temperature forging, the microstructure of titanium-aluminum alloys must be controlled through heat treatment. It is generally believed that titanium-aluminum alloys with a fine and uniform lamellar microstructure have the best overall mechanical properties. To obtain this fine and uniform lamellar microstructure, both domestic and international methods currently involve heating the titanium-aluminum alloy forging to the α single-phase region, holding it at that temperature for a certain time, and then furnace cooling. In this technique, the high-temperature forging and heat treatment are carried out separately and cannot be completed continuously. Since the heat treatment process requires reheating the forging to the α single-phase region (generally at temperatures above 1300℃), the process is lengthened, inevitably consuming more electrical energy and significantly increasing costs. In addition, phase transformation and static recrystallization occur during heat treatment. Without external force constraints, these phase transformations and recrystallization inevitably cause changes in the dimensions of the titanium-aluminum alloy forgings, making it impossible to control the dimensional accuracy of the titanium-aluminum alloy components. This dimensional deviation caused by heat treatment makes it difficult to achieve precise forming of titanium-aluminum alloy components, requiring subsequent machining to meet the dimensional accuracy requirements, which inevitably leads to an increase in the cost of the final component. Summary of the Invention

[0005] This invention proposes a precise forming method for vacuum isothermal forging of titanium-aluminum alloy components with fine and uniform full-layer microstructure, in order to solve the problems existing in the above-mentioned titanium-aluminum alloy forgings.

[0006] This invention employs vacuum isothermal forging technology to prepare titanium-aluminum alloy forgings. Forging under vacuum conditions prevents dimensional deviations caused by severe oxidation. Furthermore, because it is isothermal forging, the uniformity of the temperature field of the titanium-aluminum alloy is significantly improved, preventing defects such as cracks and significantly enhancing quality. After forging, without unloading the pressure, the temperature is directly adjusted to the heat treatment temperature. The titanium-aluminum alloy forging is subjected to pressure-holding isothermal heat treatment directly in the forging die. After holding at this temperature for a certain period, it is furnace-cooled until it is below the phase transformation temperature of the titanium-aluminum alloy. Then, the pressure is unloaded, and finally, the vacuum isothermal forging equipment is opened to remove the titanium-aluminum alloy forging. This achieves continuous vacuum isothermal forging and heat treatment of titanium-aluminum alloys. The method of this invention does not require additional heat treatment equipment, shortens the process, and can obtain a component with a fine, uniform, full-layer structure in a single step. Furthermore, since the heat treatment is carried out under external force constraints, it ensures that the titanium-aluminum alloy forging does not deform during the heat treatment process, and achieves precise control of the forging dimensional accuracy. This achieves the goal of producing titanium-aluminum alloy components with ideal microstructure and high forming accuracy in one step. Compared with traditional methods, the component manufacturing cost is significantly reduced, and the commercial value is significant.

[0007] The present invention discloses a method for precise forming of titanium-aluminum alloy components with fine and uniform lamellar microstructure by vacuum isothermal forging, which is carried out according to the following steps:

[0008] Step 1: Apply a layer of forging lubricant evenly to the surface of the titanium-aluminum alloy and the forging die of the vacuum isothermal forging equipment;

[0009] Step 2: After the lubricant has dried, place the titanium-aluminum alloy material onto the lower die of the forging mold in the vacuum isothermal forging equipment, and evacuate the equipment to a vacuum degree of 10. -4 ~30Pa. After the vacuum degree reaches the required level, heating begins. The heating temperature is set at 1100-1250℃. Once the titanium-aluminum alloy and the mold reach the set temperature, they are kept at that temperature for 1-200 minutes.

[0010] Step 3: After the heat preservation is completed, vacuum isothermal forging of the titanium-aluminum alloy material at 1100-1250℃ is carried out: First, the forging head is lowered. After the head contacts the upper die and the upper die contacts the titanium-aluminum alloy, forging begins. The forging pressing rate is 0.001~10mm / s. After the titanium-aluminum alloy is pressed down to the preset deformation amount, the forging head is stopped.

[0011] Step 4: After stopping the forging head from pressing down, hold the pressure and perform heat treatment under the pressure holding condition. The heat treatment temperature is the α single-phase temperature of the titanium-aluminum alloy. Adjust the heating temperature of the vacuum isothermal forging equipment to the heat treatment temperature and hold it for 5 to 240 minutes. After the heat treatment is completed, stop heating and furnace cool.

[0012] Step 5: Cool the furnace to below the phase transformation temperature of the titanium-aluminum alloy, raise the forging head, and continue to cool the furnace to room temperature -500℃;

[0013] Step 6: After cooling is complete, remove the titanium-aluminum alloy forging from the vacuum isothermal forging equipment, and then remove the lubricant from the surface of the forging by sandblasting or grinding to obtain the titanium-aluminum alloy component.

[0014] Furthermore, the forging lubricant mentioned in step 1 is one or more of graphite lubricant, glass lubricant, and boron nitride lubricant.

[0015] Furthermore, the coating thickness of the lubricant described in step 1 is 0.05 to 1.5 mm.

[0016] Furthermore, in step 2, the equipment is evacuated to a vacuum level of 10. -3 ~20Pa.

[0017] Furthermore, the heating temperature set in step 2 is 1150–1200°C.

[0018] Furthermore, the heat preservation time mentioned in step 2 is 50 to 150 minutes.

[0019] Furthermore, after the heat preservation process described in step 3 is completed, the titanium-aluminum alloy material is subjected to vacuum isothermal forging at 1150–1200°C.

[0020] Furthermore, the forging reduction rate in step 3 is 0.01–5 mm / s.

[0021] Furthermore, the heat preservation time mentioned in step 4 is 50 to 150 minutes.

[0022] Furthermore, the furnace described in step 5 is cooled to room temperature -200°C.

[0023] The vacuum isothermal forging equipment mentioned is the one disclosed in CN115815505A, entitled "An Ultra-High Temperature Vacuum Isothermal Forging Device and a Bladeless Isothermal Forging Method for Intermetallic Compounds". Using this equipment, the goal of stably and uniformly raising the temperature to 1100-1450℃ and holding it at that temperature can be achieved.

[0024] The most important feature of this invention is:

[0025] 1. Continuous heat treatment after forging, with no cooling process between the two processes;

[0026] 2. Pressure heat treatment is applied to ensure that the forged components do not deform during the heat treatment process, thereby ensuring dimensional accuracy and precise forming.

[0027] The present invention has the following beneficial effects:

[0028] Vacuum isothermal forging is an ideal method for producing precision forgings of titanium-aluminum alloys. It avoids the excessive formation of oxide scale caused by high-temperature oxidation, defects such as cracks due to uneven temperature fields, and the reduction in dimensional accuracy caused by component deformation during heat treatment. It enables uniform deformation and microstructure control of titanium-aluminum alloys, as well as precise forming of forgings. Specific advantages are as follows:

[0029] (1) This invention involves continuous vacuum isothermal forging and heat treatment, rather than taking the forging out and then heat treating it again. This eliminates the need for heat treatment of titanium-aluminum alloys after forging. Forging and heat treatment are completed in the same equipment. It is only necessary to raise the temperature from the forging temperature to the heat treatment temperature. This achieves the goals of low cost (removing the heat treatment requires reheating to the heat treatment temperature), short process, and precise forming of titanium-aluminum alloy forgings. It has significant commercial value and can be used for industrial production. The economic benefits of this method for producing titanium-aluminum alloy forgings are significant.

[0030] (2) Since vacuum isothermal forging can be achieved, there is no severe oxidation problem of titanium-aluminum alloy during the forging process. Isothermal forging can achieve uniform dynamic recrystallization, which will inevitably lead to a significant improvement in the uniformity of the structure and a significant refinement of the grains.

[0031] (3) After the vacuum isothermal forging of titanium-aluminum alloy is completed (forging temperature is 1100-1250℃), the temperature is directly increased to the temperature range of the full lamellar structure (α single-phase region temperature, which is 1260~1395℃ depending on the composition of the titanium-aluminum alloy). Subsequently, heat treatment is carried out under pressure. This heat treatment will inevitably result in sufficient static recrystallization and ensure a continuous phase transformation from γ, α2, β0 and other phases to a single α phase. Since this heat treatment temperature is within the temperature range for the formation of the full lamellar structure, the α phase can be completely precipitated into a full lamellar structure composed of α2 / γ phases during the subsequent slow furnace cooling process. The microstructure transformation occurs during the heat treatment under pressure and cooling process in the vacuum isothermal forging equipment. After the phase transformation is completed, a microstructure with uniform and fine lamellar cluster size can be obtained, resulting in excellent comprehensive mechanical properties.

[0032] (4) Heat treatment under pressure in vacuum isothermal forging equipment will cause structural transformation during heat preservation and cooling. Due to the external constraint force of the vacuum isothermal forging die on the component, the component will not deform due to internal structural phase transformation and recrystallization. After cooling, it can still maintain the design shape of the component and has extremely high dimensional accuracy, which can realize the precise forming of titanium-aluminum alloy components. Attached Figure Description

[0033] Figure 1 This is a flowchart of the vacuum isothermal forging precision forming method of the present invention;

[0034] Figure 2 Photograph of the Ti-44Al-4Nb-0.5Mo-0.1B alloy component prepared in Example 1;

[0035] Figure 3 The image shows the full lamellar microstructure inside the Ti-44Al-4Nb-0.5Mo-0.1B alloy component prepared in Example 1.

[0036] Figure 4 Photograph of the Ti-45Al-8Nb alloy component prepared in Example 2;

[0037] Figure 5 This is a full-layer microstructure diagram of the Ti-45Al-8Nb alloy component prepared in Example 2. Detailed Implementation

[0038] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the spirit of the contents disclosed in the present invention will be described in detail below. After understanding the embodiments of the present invention, any person skilled in the art can make changes and modifications based on the technology taught in the present invention without departing from the spirit and scope of the present invention.

[0039] The illustrative embodiments and descriptions of the present invention are used to explain the present invention, but are not intended to limit the present invention.

[0040] Example 1:

[0041] A titanium-aluminum alloy with a nominal composition of Ti-44Al-4Nb-0.5Mo-0.1B (at.%) was selected as the raw material. After being processed into a pre-formed billet shape, the component was precisely formed by vacuum isothermal forging. The specific process is as follows:

[0042] (1) Apply a layer of boron nitride lubricant evenly to the surface of the Ti-44Al-4Nb-0.5Mo-0.1B alloy preform and the forging die of the vacuum isothermal forging equipment. The coating thickness of the lubricant is 0.3mm.

[0043] (2) After the lubricant has dried, place the Ti-44Al-4Nb-0.5Mo-0.1B alloy preform onto the lower die of the forging mold in the vacuum isothermal forging equipment, and evacuate the equipment until the vacuum degree reaches 5×10⁻⁶. -2 After Pa, heating begins, with the heating temperature set at 1180℃. Once the Ti-44Al-4Nb-0.5Mo-0.1B alloy and the mold reach the set temperature, they are held at that temperature for 20 minutes.

[0044] (3) After the heat preservation is completed, the Ti-44Al-4Nb-0.5Mo-0.1B alloy preform is vacuum isothermal forging at 1180℃: First, the forging head is lowered. After the head contacts the upper die and the upper die contacts the Ti-44Al-4Nb-0.5Mo-0.1B alloy, forging begins. The forging pressing rate is 0.2mm / s. After the Ti-44Al-4Nb-0.5Mo-0.1B alloy preform is pressed down to 75%, the forging head is stopped.

[0045] (4) After the forging head stops pressing down, pressure is maintained. Heat treatment is carried out under pressure maintenance. The heat treatment temperature is 1320℃. The vacuum isothermal forging equipment is heated to 1320℃ and maintained for 40 minutes. After the heat treatment is completed, heating is stopped and furnace cooling is carried out.

[0046] (5) When the furnace cools to 1050°C, raise the forging head and continue to cool the furnace to room temperature.

[0047] (6) After cooling is complete, remove the Ti-44Al-4Nb-0.5Mo-0.1B alloy forging from the vacuum isothermal forging equipment. Then, remove the surface lubricant of the forging by sandblasting to obtain the Ti-44Al-4Nb-0.5Mo-0.1B alloy component, such as... Figure 2 As shown.

[0048] The Ti-44Al-4Nb-0.5Mo-0.1B alloy component has a smooth and flawless appearance, achieving precise forming. This is evident from its internal microstructure (e.g., Figure 3 As shown, the Ti-44Al-4Nb-0.5Mo-0.1B alloy has a fully lamellar structure with uniform and fine lamellar clusters, with an average size of only 60μm, thus achieving the objective of this invention.

[0049] Example 2:

[0050] A titanium-aluminum alloy with a nominal composition of Ti-45Al-8Nb (at.%) was selected as the raw material. After being processed into a pre-formed billet shape, the component was precisely formed by vacuum isothermal forging. The specific process is as follows:

[0051] (1) Apply a layer of glass lubricant evenly to the surface of the Ti-45Al-8Nb alloy preform and the forging die of the vacuum isothermal forging equipment. The coating thickness of the lubricant is 0.5mm.

[0052] (2) After the lubricant has dried, place the Ti-45Al-8Nb alloy preform onto the lower die of the forging mold in the vacuum isothermal forging equipment, and evacuate the equipment until the vacuum degree reaches 10. -1 After Pa, heating begins, with the heating temperature set at 1230℃. Once the Ti-45Al-8Nb alloy and the mold reach the set temperature, they are held at that temperature for 20 minutes.

[0053] (3) After the heat preservation is completed, the Ti-45Al-8Nb alloy preform is vacuum isothermal forging at 1230℃: First, the forging head is lowered. After the head contacts the upper die and the upper die contacts the Ti-45Al-8Nb alloy, forging begins. The forging pressing rate is 0.05mm / s. After the Ti-45Al-8Nb alloy preform is pressed down to 70%, the forging head is stopped.

[0054] (4) After the forging head is stopped, pressure is maintained and heat treatment is carried out under pressure. The heat treatment temperature is 1360℃. The vacuum isothermal forging equipment is heated to 1360℃ and held for 60 minutes. After the heat treatment is completed, heating is stopped and furnace cooling is carried out.

[0055] (5) When the furnace cools to 1100°C, raise the forging head and continue to cool the furnace to 200°C.

[0056] (6) After cooling is complete, remove the Ti-45Al-8Nb alloy forging from the vacuum isothermal forging equipment. Then, remove the surface lubricant of the forging by sandblasting to obtain the Ti-45Al-8Nb alloy component, such as... Figure 4 As shown.

[0057] The Ti-45Al-8Nb alloy components have a smooth and flawless appearance, demonstrating precise forming. This is evident from the internal microstructure (e.g., ...). Figure 5 As shown, the Ti-45Al-8Nb alloy has a fully lamellar structure with uniform and fine lamellar clusters, with an average size of only 70μm, thus achieving the objective of this invention.

Claims

1. A method for precise forming of titanium-aluminum alloy components with fine, uniform, fully lamellar microstructure by vacuum isothermal forging, characterized in that... It is done in the following steps: Step 1: Apply a layer of forging lubricant evenly to the surface of the titanium-aluminum alloy and the forging die of the vacuum isothermal forging equipment; Step 2: After the lubricant has dried, place the titanium-aluminum alloy material onto the lower die of the forging mold in the vacuum isothermal forging equipment, and evacuate the equipment to a vacuum degree of 10. -4 ~30Pa, after the vacuum degree reaches the required level, start heating. The heating temperature is set at 1100-1250℃. After the titanium-aluminum alloy and forging mold reach the set temperature, keep them at that temperature for 1~200min. Step 3: After the heat preservation is completed, vacuum isothermal forging of the titanium-aluminum alloy material at 1100-1250℃ is carried out: First, the forging head is lowered. After the forging head contacts the upper die and the upper die contacts the titanium-aluminum alloy, forging begins. The forging pressing rate is 0.001~10mm / s. After the titanium-aluminum alloy is pressed down to the preset deformation amount, the forging head is stopped. Step 4: After stopping the forging head from pressing down, hold the pressure and perform heat treatment under the pressure holding condition. The heat treatment temperature is the α single-phase temperature of the titanium-aluminum alloy. Raise the heating temperature of the vacuum isothermal forging equipment to the heat treatment temperature and hold it for 5~240 minutes. After the heat treatment is completed, stop heating and furnace cool. Step 5: Cool the furnace to below the phase transformation temperature of the titanium-aluminum alloy, raise the forging head, and continue to cool the furnace to room temperature -500℃; Step 6: After cooling is complete, remove the titanium-aluminum alloy forging from the vacuum isothermal forging equipment, and then remove the lubricant from the surface of the forging by sandblasting or grinding to obtain the titanium-aluminum alloy component.

2. The method for precise forming of titanium-aluminum alloy components with fine and uniform lamellar microstructure by vacuum isothermal forging according to claim 1, characterized in that... The forging lubricant mentioned in step 1 is one or more of graphite lubricant, glass lubricant, and boron nitride lubricant.

3. A method for precise forming of titanium-aluminum alloy components with fine, uniform, fully lamellar microstructure by vacuum isothermal forging according to claim 1 or 2, characterized in that... The coating thickness of the forging lubricant mentioned in step 1 is 0.05~1.5mm.

4. The method for precise forming of titanium-aluminum alloy components with fine and uniform lamellar structure by vacuum isothermal forging according to claim 1, characterized in that... In step 2, the equipment is evacuated to a vacuum level of 10. -3 ~20Pa.

5. The method for precise forming of titanium-aluminum alloy components with fine and uniform lamellar structure by vacuum isothermal forging according to claim 1, characterized in that... The heating temperature set in step 2 is 1150~1200℃.

6. The method for precise forming of titanium-aluminum alloy components with fine and uniform lamellar microstructure by vacuum isothermal forging according to claim 1, characterized in that... The heat preservation time mentioned in step 2 is 50~150 minutes.

7. The method for precise forming of titanium-aluminum alloy components with fine and uniform lamellar structure by vacuum isothermal forging according to claim 1, characterized in that... After the heat preservation process described in step 3 is completed, the titanium-aluminum alloy material is subjected to vacuum isothermal forging at 1150~1200℃.

8. A method for precise forming of titanium-aluminum alloy components with fine, uniform, fully lamellar microstructure by vacuum isothermal forging according to claim 1, characterized in that... The forging reduction rate mentioned in step 3 is 0.01~5 mm / s.

9. A method for precise forming of titanium-aluminum alloy components with fine, uniform, fully lamellar microstructure by vacuum isothermal forging according to claim 1, characterized in that... The heat preservation time mentioned in step 4 is 50~150 minutes.

10. A method for precise forming of titanium-aluminum alloy components with fine, uniform, fully lamellar microstructure by vacuum isothermal forging according to claim 1, characterized in that... The furnace described in step 5 is cooled to room temperature -200°C.

Citation Information

Patent Citations

  • Ultrahigh-temperature vacuum isothermal forging device and intermetallic compound packaging-free isothermal forging method

    CN115815505A

  • Aluminum alloy forging die with fluid channels and aluminum alloy forging technique

    CN106391965A

  • Full-lamellar deformation TiAl alloy and preparation method thereof

    CN114657413A

  • Glass lubricant for vacuum isothermal forging process and application thereof

    CN116622430A

  • Forging forming method for aluminum alloy wheel of commercial vehicle

    CN116713420A