A method for judging the flexibility of lithium-ion battery electrodes
The method of cutting off the electrode sheet after winding and hot pressing for tensile testing solves the problem of judging the flexibility of lithium-ion battery electrode sheets, and realizes a fast, simple and low-cost flexibility assessment.
Patent Information
- Application Number
- CN202311380474.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-24
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-10-24
AI Technical Summary
The lack of a unified method for quickly assessing the flexibility of lithium-ion battery electrodes in current technology affects processing anomalies and safety during production.
By hot-pressing the diaphragm, standard electrode, and electrode to be tested into a core, the electrode containing the innermost R-angle is cut off for tensile testing, and the tensile strength is compared to determine the flexibility of the electrode.
It enables a quick and easy assessment of electrode flexibility, saves material costs, and is simple and efficient to operate.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium-ion battery technology, specifically relating to a method for judging the flexibility of lithium-ion battery electrodes. Background Technology
[0002] Lithium-ion batteries are widely used in mobile phones, tablets, electric vehicles, and other fields due to their advantages such as high single-cell voltage, high energy and power density, long lifespan, light weight, no memory effect, and no pollution. Especially in recent years, with their application in electric vehicles, higher performance requirements have been placed on lithium-ion batteries. The flexibility of the electrode coating in lithium-ion batteries has a significant impact on coating, baking, and rolling processes; therefore, assessing the flexibility of the electrode is of great importance in the research and development and production of batteries.
[0003] Many factors affect the flexibility of lithium-ion battery electrodes, such as the type and proportion of materials, the areal density of the electrode, and the compaction density of the electrode. Poor electrode flexibility can lead to processing abnormalities such as roll breakage, affecting yield, and can also increase burrs and material loss inside the core, resulting in short circuits and safety issues.
[0004] The flexibility of electrode sheets can be improved by optimizing materials and their proportions, selecting more suitable areal density and compaction density, and optimizing hot pressing processes. However, there is currently no unified method for judging and comparing the flexibility of electrode sheets in the early stages. Summary of the Invention
[0005] The purpose of this invention is to provide a method for judging the flexibility of lithium-ion battery electrodes, which can quickly assess the flexibility of electrodes and is convenient and simple to operate.
[0006] The technical solution adopted by this invention to solve the above problems is: a method for judging the flexibility of lithium-ion battery electrode sheets, comprising the following steps: (1) The diaphragm is wound with the standard electrode J to obtain the standard core JX, and the diaphragm is wound with the electrode J-1 to be tested to obtain the core J-1-X to be tested; (2) Hot pressing is performed on the standard core JX and the core to be tested J-1-X respectively; (3) After the hot-pressed standard core JX is unpacked, a standard tensile test electrode of a certain length and width is cut out and recorded as JXJ; in the same way, a tensile test electrode of the same length and width is cut out and recorded as J-1-XJ; (4) Under the same test conditions, tensile tests were performed on electrode JXJ and J-1-XJ respectively to obtain tensile strength; (5) Compare and judge the tensile strength results in step (4): If the tensile strength (JXJ) ≤ tensile strength (J-1-XJ), it is considered that the flexibility of the electrode J-1 to be tested is better than or equal to that of the standard electrode J; if the tensile strength (JXJ) > tensile strength (J-1-XJ), it is considered that the flexibility of the electrode J-1 to be tested is worse than that of the standard electrode J.
[0007] Preferably, the winding in step (1) is a single roll, and the number of turns is ≥1.
[0008] Preferably, in step (2), both the standard tensile test electrode and the tensile test electrode to be tested are electrodes from the innermost circle of the core, and include the innermost circle's radius (R-angle). This is because when the electrode is subjected to tensile testing after hot pressing, the first point where the electrode breaks is at the innermost circle's radius (R-angle).
[0009] Preferably, the standard tensile test electrode in step (3) has a length ≥ 50 mm and a width ≤ 50 mm.
[0010] Compared with the prior art, the advantages of the present invention are as follows: The present invention provides a method for judging the flexibility of lithium-ion battery electrodes by reflecting the difference in electrode flexibility through the magnitude of electrode tension. The test requires very few electrodes, including only the innermost circle R angle, which greatly saves material costs. Moreover, the operation process is simple, convenient and efficient. Implementation
[0011] The present invention will be further described in detail below with reference to the embodiments. Example 1
[0012] A method for determining the flexibility of lithium-ion battery electrodes includes the following steps: (1) Electrode preparation: According to the process of batching, coating (the substrate is aluminum foil, with the following specifications: thickness 13μm, tensile strength 200MPa, elongation 3.5%), and rolling, standard electrode J and electrode to be tested J-1 are obtained; the formula of standard electrode J is 97% lithium iron phosphate (B7-3): 1% carbon black (SP): 2% binder (Sowe 5130), and the coating surface density is 330 g / m 2 Compacted density 2.35 g / cm³ 3 The formulation of standard electrode J-1 is 97% lithium iron phosphate (B7-3): 1% carbon black (SP): 2% binder (Juhua JHS1020), and the coating surface density is 330 g / m². 2 Compacted density 2.35 g / cm³ 3 .
[0013] (2) Core preparation: The standard electrode J and the 9+3 wet-coated ceramic diaphragm are wound into single rolls on a winding machine. The electrode is wound into one turn to obtain the standard core JX. The same method is used to obtain the core J-1-X to be tested.
[0014] (3) Hot pressing: Set the temperature to 90℃, pressure to 3000Kgf and time to 60s for the hot press, and then hot press the standard core JX and the core to be tested J-1-X.
[0015] (4) Tensile test: Take the standard core JX after hot pressing, and cut a standard tensile test electrode with a length of 50mm and a width of 15mm after disassembly. The electrode includes the innermost circle R angle and is recorded as JXJ. In the same way, the core J-1-X to be tested is cut into a tensile test electrode with the same length and width and is recorded as J-1-XJ. Then, at the same speed of 25mm / min, tensile tests are performed on the electrode JXJ and J-1-XJ respectively to obtain the tensile strength.
[0016] (5) Compare and judge the above tensile strength test results: tensile strength (JXJ) = 85MPa < tensile strength (J-1-XJ) = 95MPa, so the flexibility of the electrode J-1 to be tested is better than that of the standard electrode J. Example 2
[0017] A method for determining the flexibility of lithium-ion battery electrodes includes the following steps: (1) Electrode preparation: According to the process of batching, coating (the substrate is aluminum foil, the specifications are: thickness 13μm, tensile strength 200MPa, elongation 3.5%), and rolling, standard electrode J and electrode to be tested J-2 are obtained; the formula of standard electrode J is: 97% lithium iron phosphate (B7-3): 1% carbon black (SP): 2% binder (Sowe 5130), and the coating surface density is 330g / m 2 Compacted density 2.35 g / cm³ 3 The formulation of the electrode J-2 to be tested is 97% lithium iron phosphate B7-3: 1% carbon black SP: 2% binder Solvay 5130, and the coating surface density is 360 g / m². 2 The compacted density is 2.47 g / cm³. 3 .
[0018] (2) Core preparation: The standard electrode J and the 9+3 wet-coated ceramic diaphragm are single-wound on the winding machine, with the electrode single-wound 1 turn to obtain the standard core JX; the core to be tested J-2-X is obtained by the same method.
[0019] (3) Hot pressing: Set the temperature to 90℃, pressure to 3000Kgf and time to 60s for the hot press, and then hot press the standard core JX and the core to be tested J-2-X.
[0020] (4) Tensile test: Take the standard core JX after hot pressing, unpack it and cut a standard tensile test electrode with a length of 50mm and a width of 15mm. The electrode includes the innermost circle's R angle and is denoted as JXJ. In the same way, cut a tensile test electrode of the same length and width and denoted as J-2-XJ. Then, at the same speed of 25mm / min, perform a tensile test on electrode JXJ and J-2-XJ to obtain the tensile strength.
[0021] (5) Compare and judge the above tensile strength test results: Since tensile strength (JXJ) = 85MPa > tensile strength (J-2-XJ) = 60MPa, it is considered that the flexibility of the electrode J-2 to be tested is worse than that of the standard electrode J.
[0022] In addition to the above embodiments, the present invention also includes other embodiments. All technical solutions formed by equivalent transformation or equivalent substitution should fall within the protection scope of the claims of the present invention.
Claims
1. A method for determining the flexibility of a lithium-ion battery electrode sheet, characterized by: Includes the following steps:
1. Wind the diaphragm and the standard electrode J to obtain the standard core JX. Wind the diaphragm and the electrode to be tested J-1 to obtain the core to be tested J-1-X.
2. Hot pressing is performed on the standard core JX and the core J-1-X to be tested respectively; 3. After the standard core JX is hot-pressed, cut a standard tensile test electrode of a certain length and width, and record it as JXJ; in the same way, cut a tensile test electrode of the same length and width, and record it as J-1-XJ; IV. Under the same test conditions, tensile tests were performed on the standard tensile test electrode JXJ and the tensile test electrode J-1-XJ to be tested to obtain the tensile strength.
5. Compare and judge the tensile strength results in step four: If the tensile strength of the standard tensile test electrode JXJ is less than or equal to the tensile strength of the electrode to be tested J-1-XJ, then the flexibility of the electrode to be tested J-1 is better than or equal to that of the standard electrode J; if the tensile strength of the standard tensile test electrode JXJ is greater than the tensile strength of the electrode to be tested J-1-XJ, then the flexibility of the electrode to be tested J-1 is worse than that of the standard electrode J. The winding described in step one is a single roll, with the number of turns being ≥ 1. In step three, both the standard tensile test electrode and the tensile test electrode to be tested are electrodes from the innermost circle of the core, and include the innermost circle's radius (R-angle).
2. The method of claim 1, wherein the method is characterized by: The standard tensile test electrode mentioned in step three has a length ≥ 50 mm and a width ≤ 50 mm.
Citation Information
Patent Citations
Battery pole piece flexibility detection method, detection device, equipment and medium
CN116183380A