FeCoNiAl alloy coating and its application in antibacterial and wear-resistant artificial bone

Through the combined technology of FeCoNiAl alloy coating and Cu-TiO2 antibacterial micro-arc oxidation film, the deficiencies in biocompatibility and wear resistance of titanium alloy artificial bone are solved, and good integration with human bone and antibacterial properties are achieved. The service life of artificial bone is extended.

CN117604520BActive Publication Date: 2024-10-25DALIAN POLYTECHNIC UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311620538.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-30
Publication Date
2024-10-25
Estimated Expiration
2043-11-30

AI Technical Summary

Technical Problem

Traditional titanium alloy artificial bone has problems with bioinertness on the implant surface, poor wear resistance, slow integration, and poor biocompatibility, leading to implant loosening and increased risk of infection.

Method used

FeCoNiAl alloy coating is used to prepare a porous artificial bone structure through powder sintering to form a Cu-TiO2 antibacterial micro-arc oxidation film, and the FeCoNiAl alloy coating is coated through laser cladding technology to improve surface strength and antibacterial performance.

Benefits of technology

It achieves elastic modulus matching between artificial bone and human bone, accelerates bone regeneration, improves antibacterial ability, reduces wear rate, extends service life, and enhances biocompatibility and osteogenic differentiation ability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117604520B_ABST
    Figure CN117604520B_ABST
Patent Text Reader

Abstract

The invention discloses an FeCoNiAl alloy coating comprising Fe powder, Co powder, Ni powder, Al powder, Ti powder and B powder, and an application of the FeCoNiAl alloy coating in antibacterial and wear-resistant artificial bone. A porous artificial bone structure is prepared by a molding powder sintering method; the porous artificial bone structure is immersed in an electrolyte for micro-arc oxidation treatment, and Cu-TiO 2 The present invention adopts the above steps to coat the FeCoNiAl alloy coating on the surface of the porous antibacterial artificial bone by laser cladding, so that the surface has high strength and high toughness, and the wear rate is reduced by 80.7%, which effectively improves the mechanical properties and promotes bone healing, and prolongs its service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of medical artificial bones, in particular to a FeCoNiAl alloy coating and its application in antibacterial and wear-resistant artificial bones. Background Art

[0002] At present, there are many people in the world who suffer bone tissue injuries every year due to various reasons. However, there are very few patients who can actually obtain natural bone transplants. In the absence of a large amount of natural bone, artificial bone has become a new option for patients. As a substitute for natural bone, the manufacturing materials of artificial bone must have excellent physical and mechanical properties and excellent biocompatibility, so that it can better match the natural bone system of the human body. Due to the excellent corrosion resistance, low elastic modulus, easy processing and other excellent properties of titanium and its alloys, they are widely used in the medical field. Although medical titanium alloys have become the main materials for implants or instruments in orthopedics, dentistry and cardiovascular, some problems have also been exposed in their applications.

[0003] Titanium is an active metalloid element, which makes it very easy to form an inert passivation film on the surface of titanium and its alloys, making it impossible for artificial bone implants to form a stable biological bond with natural bones, and only mechanical inlay bonding can be achieved. In addition, the friction coefficient of the surface of titanium and its alloys is large and the wear resistance is poor. Therefore, many patients experience slow integration of artificial bone implants after surgery. The elastic modulus of titanium alloy and human bone does not match, and stress shielding occurs after implantation, resulting in loose implants. After artificial bone is implanted into the human body, its surface not only needs to connect and run-in with the natural bone inside the human body, but also needs to meet a series of biological activities such as differentiation, proliferation, adhesion, and growth of human cells on its surface, which requires artificial bone to have antibacterial and antimicrobial properties and biocompatibility.

[0004] In summary, developing an artificial bone with excellent antibacterial and antimicrobial properties and high strength is a new research and application idea. Summary of the invention

[0005] The purpose of the present invention is to provide a FeCoNiAl alloy coating and its application in antibacterial and wear-resistant artificial bone, which solves the problems of traditional hard tissue replacement materials such as titanium alloy surface having biological inertness, poor wear resistance, severe wear of artificial bone implants, and poor biocompatibility of titanium alloy.

[0006] To achieve the above object, the present invention provides a FeCoNiAl alloy coating, which comprises Fe powder, Co powder, Ni powder, Al powder, Ti powder and B powder.

[0007] Preferably, the mixed molar ratio of the FeCoNiAl alloy coating is 20 at% Fe powder, 20 at% Co powder, 20 at% Ni powder, 4 at% Al powder, 26-31 at% Ti powder and 5-10 at% B powder.

[0008] Application of the above FeCoNiAl alloy coating in antibacterial and wear-resistant artificial bone:

[0009] S1, preparing a porous artificial bone structure by pressing titanium metal powder and a pore-forming agent and sintering at high temperature;

[0010] S2, the porous artificial bone structure in S1 is subjected to deoxidation film and degreasing operations in sequence, and then immersed in a Cu-containing electrolyte for micro-arc oxidation treatment to form Cu-TiO on the porous artificial bone structure. 2 The antibacterial micro-arc oxidation film layer is washed with deionized water and then dried to obtain a porous antibacterial artificial bone structure;

[0011] S3. The FeCoNiAl alloy coating composed of FeCoNiAl alloy powder is coated on the surface of the porous antibacterial artificial bone structure in S2 through laser cladding technology, and it is cut into the required size and then polished. It is then ultrasonically washed with acetone, anhydrous ethanol and distilled water in sequence to obtain a porous antibacterial and high-strength artificial bone structure.

[0012] Preferably, in S1, the pore-forming agent is urea.

[0013] Preferably, in S2, the treated porous artificial bone structure is connected to the positive electrode of the power supply as an anode and immersed in a cathode tank filled with an electrolyte, and the cathode tank is connected to the negative electrode of the power supply to perform a micro-arc oxidation operation on the porous artificial bone structure.

[0014] Preferably, in S2, the electrolyte contains 1-20 g / L of trisodium phosphate, 1-4 g / L of sodium hydroxide, 0.5-2 g / L of copper acetate, and 1-10 g / L of sodium ethylenediaminetetraacetate, and the solvent is deionized water.

[0015] Preferably, in S3, the laser cladding technology uses a semiconductor laser for single-pass cladding, and the parameters are set to a laser power of 800 W, a spot diameter of 3 mm, a scanning speed of 6 mm / s, and continuous introduction of argon gas.

[0016] Therefore, the FeCoNiAl alloy coating of the above composition and its application in antibacterial and wear-resistant artificial bone of the present invention have the following beneficial effects:

[0017] 1. The present invention uses powder sintering technology to form an internal porous artificial bone structure, so that its elastic modulus matches the elastic modulus of human bone, and the implant with an open porous structure allows bone growth and accelerates bone regeneration;

[0018] 2. Electrochemical processing of trisodium phosphate can change the surface morphology and increase the thickness of the natural oxide layer, which is suitable for bone integration. Micro-arc oxidation forms interconnected pores to increase protein adsorption and stimulate osteoblast migration, thereby accelerating bone integration;

[0019] 3. Cu, as an essential trace element for the human body, usually has limited cytotoxicity in vivo and also has enhanced antibacterial efficacy in vivo. Using Cu in the electrolyte to form an antibacterial coating improves the antibacterial ability of trisodium phosphate electrochemical processing on implant artificial bone;

[0020] 4. Coating Fe on the surface of porous antibacterial artificial bone by laser cladding technology 20 Co 20 Ni 20 Al 4 Ti 26 B 10 The alloy coating makes its surface have high strength and high toughness, and the wear rate is reduced by 80.7%. It has better friction and wear resistance, overcomes the shortcomings of ordinary artificial bone materials, can bear greater loads, and greatly extends the service life of artificial bones;

[0021] 5. The preparation method provided by the present invention can improve the strength of the surface of artificial bone on the one hand, and on the other hand, it can play an effective antibacterial and sterilization role to prevent infection at the bone defect site, and has good osteogenic differentiation ability, improves biocompatibility, effectively improves the mechanical properties of artificial bone, promotes bone healing and prolongs its service life.

[0022] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a schematic diagram of the application process of the FeCoNiAl alloy coating of the present invention in antibacterial and wear-resistant artificial bone;

[0024] Figure 2 is a hardness distribution curve diagram of Example 1, Example 2 and Comparative Example 1 of the present invention;

[0025] Figure 3 is a scanning electron microscope image of the surface morphology of the coating of Example 1 of the present invention;

[0026] Figure 4 This is a scanning electron microscope image of the cross-sectional morphology of the hole depression in Example 1 of the present invention. DETAILED DESCRIPTION

[0027] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.

[0028] The present invention can be explained in more detail by the following examples. The purpose of disclosing the present invention is to protect all changes and improvements within the scope of the present invention. The present invention is not limited to the following examples.

[0029] Example 1

[0030] like Figure 1 As shown, S1, titanium metal powder and pore-forming agent are sintered by a molded powder method to prepare a porous artificial bone structure;

[0031] In S1, the pore-forming agent is urea.

[0032] In S1, titanium metal powder is used as a raw material, mixed with urea, and then pressed and sintered at high temperature to prepare a porous artificial bone structure. During the entire molding powder sintering process, the titanium metal powder always remains in a solid state. The urea decomposes at high temperature, and the generated gas precipitates, causing the titanium metal to expand, thereby obtaining a porous artificial bone structure.

[0033] S2, the porous artificial bone structure in S1 is subjected to deoxidation film and degreasing operations in sequence, and then immersed in a Cu-containing electrolyte for micro-arc oxidation treatment, so that Cu-TiO containing the antibacterial agent Cu is formed on the surface and in the pores of the porous artificial bone structure. 2 The antibacterial micro-arc oxidation film layer was ultrasonically washed with deionized water for 5 min and then dried to obtain a porous antibacterial artificial bone structure, which was stored at room temperature.

[0034] In S2, the treated porous artificial bone structure is connected to the positive electrode of the power supply as an anode and immersed in a cathode tank filled with electrolyte. A stainless steel plate is used as a cathode plate. The cathode tank is connected to the negative electrode of the power supply. The electrolyte is maintained at 30°C through a circulating water treatment system. The porous artificial bone structure is subjected to micro-arc oxidation treatment at a constant voltage of 400V for 5 minutes.

[0035] In S2, the electrolyte contains 20 g / L of trisodium phosphate, 4 g / L of sodium hydroxide, 1.0 g / L of copper acetate, and 10 g / L of sodium ethylenediaminetetraacetate, and the solvent is deionized water.

[0036] S3, FeCoNiAl alloy coating composed of FeCoNiAl alloy powder is coated on the surface of the porous antibacterial artificial bone structure in S2 by laser cladding technology, cut it into the required size and then polish it, and then ultrasonically wash it with acetone, anhydrous ethanol and distilled water in turn to obtain a porous antibacterial high-strength artificial bone structure. The scanning electron microscope image of the coating surface morphology of the porous antibacterial high-strength artificial bone structure and the scanning electron microscope image of the cross-sectional morphology of the pore depression are shown in the figure. Figure 3 and Figure 4 shown.

[0037] In S3, the FeCoNiAl alloy powder contains Fe powder, Co powder, Ni powder, Al powder, Ti powder and B powder with purity higher than 99.5%, and the mixing molar ratio of the above powders is 20at% Fe powder, 20at% Co powder, 20at% Ni powder, 4at% Al powder, 31at% Ti powder and 5at% B powder.

[0038] In S3, since the use of adhesives is prone to introduce new impurities, the FeCoNiAl alloy powder was sputtered on the surface of the porous antibacterial artificial bone structure by the prefabricated powder method without adding adhesives, and the coating thickness was 1.4 mm. The laser cladding technology uses a semiconductor laser for single-pass cladding, and the parameters are set as laser power 800 W, spot diameter 3 mm, scanning speed 6 mm / s, and continuous argon gas. The porous antibacterial artificial bone structure after cladding was wire-cut perpendicular to the laser scanning direction, and the size was 15 mm × 15 mm × 8 mm.

[0039] Example 2

[0040] like Figure 1 As shown, S1, titanium metal powder and pore-forming agent are sintered by a molded powder method to prepare a porous artificial bone structure;

[0041] In S1, the pore-forming agent is urea.

[0042] In S1, titanium metal powder is used as a raw material, mixed with urea, and then pressed and sintered at high temperature to prepare a porous artificial bone structure. During the entire molding powder sintering process, the titanium metal powder always remains in a solid state. The urea decomposes at high temperature, and the generated gas precipitates, causing the titanium metal to expand, thereby obtaining a porous artificial bone structure.

[0043] S2, the porous artificial bone structure in S1 is subjected to deoxidation film and degreasing operations in sequence, and then immersed in a Cu-containing electrolyte for micro-arc oxidation treatment, so that Cu-TiO containing the antibacterial agent Cu is formed on the surface and in the pores of the porous artificial bone structure. 2 The antibacterial micro-arc oxidation film layer was ultrasonically washed with deionized water for 5 min and then dried to obtain a porous antibacterial artificial bone structure, which was stored at room temperature.

[0044] In S2, the treated porous artificial bone structure is connected to the positive electrode of the power supply as an anode and immersed in a cathode tank filled with electrolyte. A stainless steel plate is used as a cathode plate. The cathode tank is connected to the negative electrode of the power supply. The electrolyte is maintained at 30°C through a circulating water treatment system. The porous artificial bone structure is subjected to micro-arc oxidation treatment at a constant voltage of 400V for 5 minutes.

[0045] In S2, the electrolyte contains 20 g / L of trisodium phosphate, 4 g / L of sodium hydroxide, 1.0 g / L of copper acetate, and 10 g / L of sodium ethylenediaminetetraacetate, and the solvent is deionized water.

[0046] S3. The FeCoNiAl alloy coating composed of FeCoNiAl alloy powder is coated on the surface of the porous antibacterial artificial bone structure in S2 by laser cladding technology, and then polished and ultrasonically washed with acetone, anhydrous ethanol and distilled water in turn to obtain a porous antibacterial high-strength artificial bone structure.

[0047] In S3, the FeCoNiAl alloy powder contains Fe powder, Co powder, Ni powder, Al powder, Ti powder and B powder with a purity higher than 99.5%, and the mixing molar ratio of the above powders is 20at% Fe powder, 20at% Co powder, 20at% Ni powder, 4at% Al powder, 26at% Ti powder and 10at% B powder.

[0048] In S3, since the use of adhesives is prone to introduce new impurities, the FeCoNiAl alloy powder was sputtered on the surface of the porous antibacterial artificial bone structure by the prefabricated powder method without adding adhesives, and the coating thickness was 1.4 mm. The laser cladding technology uses a semiconductor laser for single-pass cladding, and the parameters are set as laser power 800 W, spot diameter 3 mm, scanning speed 6 mm / s, and continuous argon gas. The porous antibacterial artificial bone structure after cladding was wire-cut perpendicular to the laser scanning direction, and the size was 15 mm × 15 mm × 8 mm.

[0049] Example 3

[0050] a. Isolation and culture of bone marrow stromal cells (BMSCs) from the bone marrow of 4-week-old Sprague-Dawley (SD) rats. Bone marrow was first isolated from the tibia of mice and then suspended in α-minimal essential medium containing 10% fetal bovine serum and 1% penicillin-streptomycin. Primary cells were cultured at 37°C and 5% CO 2 The cells were cultured in a humidified atmosphere for 48 hours, and then the bone marrow stromal cells adhered to the bottom of the culture dish were collected. The culture medium was replaced every 3 days.

[0051] b. The sterilized porous antibacterial artificial bone structure (diameter = 14 mm) in Example 1 was placed in a 24-well plate as the experimental group, and the porous artificial bone structure was used as the control group. The experimental group and the control group were rinsed twice with PBS and the bone marrow stromal cells were cultured at 7×10 4 The density of cells / ml was inoculated into the experimental and control groups. Cytotoxicity was measured after 1, 3 and 5 days of culture. During the proliferation assay, the culture medium was changed every other day.

[0052] After the specified incubation time, CCK-8 dye was added to each well, and the plate was then incubated for another 2 hours at 37°C. Finally, the optical density (OD) was measured at 450nm by a plate reader. Five samples of the porous antibacterial artificial bone structure in Example 1 were set for testing. After incubation for 3 days, the cells were washed with PBS, fixed with 4% formaldehyde for 10 minutes at room temperature, and then dehydrated in ethanol for 10 minutes per gradient, followed by vacuum drying. After gold sputtering, the cell growth morphology of the sample was observed by SEM.

[0053] The cell vibration was tested with CCK-8, and the results showed that the OD values ​​of the porous antibacterial artificial bone structure increased significantly at 1, 3, and 5 days. Compared with the porous artificial bone structure, the porous antibacterial artificial bone structure showed higher viability at 3 and 5 days, and all compounds showed good cell biocompatibility with the porous antibacterial artificial bone structure. The cell morphology on different coatings after 3 days of incubation was observed by SEM. Compared with the control group, the cells were better distributed on the surface of the porous antibacterial artificial bone structure, and more cells adhered to the porous antibacterial artificial bone structure. The cell viability of BMSC on the porous antibacterial artificial bone structure was much higher than that of the porous artificial bone structure, which proved that the surface morphology of the porous antibacterial artificial bone structure was relatively suitable for BMSC proliferation.

[0054] c. Total protein was isolated after culturing with osteogenic medium for 0 and 7 days using RIPA lysis buffer containing protease inhibitors and phosphatase inhibitors. Protein concentration was measured using a BCA assay kit. GAPDH, ALP, and RUNX2 were diluted 1:5000, 1:500, and 1:500 in skim milk powder TBST solution, respectively, and incubated with the membrane in a 4°C room overnight. After washing with 0.5% TBST, the membrane was incubated with rabbit anti-mouse IgG conjugated to HRP at a dilution of 1:2000.

[0055] Using enhanced chemiluminescence detection of bound antibodies, three samples were tested for each porous artificial bone structure and porous antibacterial artificial bone structure, and each test was repeated three times. Alkaline phosphatase staining was performed using an alkaline phosphatase staining kit. After 7 days of induction, the cells were washed 3 times with PBS. They were then fixed with 4% formaldehyde for 10 minutes and stained with ALP reagent for 10 minutes. After washing with PBS, the stained cells were then observed.

[0056] The cells were cultured with osteogenic differentiation medium for 14 days, and the mineralization level in the cells was determined by an Alizarin Red staining kit. After fixation, the cells were stained with 1% Alizarin Red solution for 10 minutes and washed three times with distilled water. The osteogenic differentiation ability of BMSCs on the porous antibacterial artificial bone structure coating was evaluated by Western blotting, and the osteogenic-related mRNA (Alp, Opn, Ocn and Runx2) in the porous antibacterial artificial bone structure was significantly higher than that in the porous artificial bone structure. The results of ALP and Alizarin Red staining showed that the porous antibacterial artificial bone structure coating can enhance the ALP activity and the formation of mineralized nodules of BMSCs, and promote the bone integration of the porous antibacterial artificial bone structure.

[0057] Comparative Example 1

[0058] S1, preparing a porous artificial bone structure by using a molded powder sintering method with titanium metal powder and a pore-forming agent;

[0059] In S1, the pore-forming agent is urea.

[0060] In S1, titanium metal powder is used as a raw material, mixed with urea, and then pressed and sintered at high temperature to prepare a porous artificial bone structure. During the entire molding powder sintering process, the titanium metal powder always remains in a solid state. The urea decomposes at high temperature, and the generated gas precipitates, causing the titanium metal to expand, thereby obtaining a porous artificial bone structure.

[0061] S2, the porous artificial bone structure in S1 is subjected to deoxidation film and degreasing operations in sequence, and then immersed in a Cu-containing electrolyte for micro-arc oxidation treatment, so that Cu-TiO containing the antibacterial agent Cu is formed on the surface and in the pores of the porous artificial bone structure. 2 The antibacterial micro-arc oxidation film layer was ultrasonically washed with deionized water for 5 min and then dried to obtain a porous antibacterial artificial bone structure, which was stored at room temperature.

[0062] In S2, the treated porous artificial bone structure is connected to the positive electrode of the power supply as an anode and immersed in a cathode tank filled with electrolyte. A stainless steel plate is used as a cathode plate. The cathode tank is connected to the negative electrode of the power supply. The electrolyte is maintained at 30°C through a circulating water treatment system. The porous artificial bone structure is subjected to micro-arc oxidation treatment at a constant voltage of 400V for 5 minutes.

[0063] In S2, the electrolyte contains 20 g / L of trisodium phosphate, 4 g / L of sodium hydroxide, 2.0 g / L of copper acetate, and 10 g / L of sodium ethylenediaminetetraacetate, and the solvent is deionized water.

[0064] S3. The FeCoNiAl alloy coating composed of FeCoNiAl alloy powder is coated on the surface of the porous antibacterial artificial bone structure in S2 by laser cladding technology, and then polished and ultrasonically washed with acetone, anhydrous ethanol and distilled water in turn to obtain a porous antibacterial high-strength artificial bone structure.

[0065] In S3, the FeCoNiAl alloy powder contains Fe powder, Co powder, Ni powder, Al powder, Ti powder and B powder with purity higher than 99.5%, and the mixed molar ratio of the above powders is 22at% of Fe powder, 22at% of Co powder, 22at% of Ni powder, 12at% of Al powder and 22at% of Ti powder.

[0066] In S3, since the use of adhesives is prone to introduce new impurities, the FeCoNiAl alloy powder was sputtered on the surface of the porous antibacterial artificial bone structure using a prefabricated powder method without adding adhesives, and the coating thickness was 1.4 mm. The laser cladding technology uses a semiconductor laser for single-pass cladding, and the parameters are set to laser power 800W, spot diameter 3mm, scanning speed 6mm / s, and continuous argon gas. The porous antibacterial artificial bone structure after cladding was wire-cut perpendicular to the laser scanning direction, with a size of 15mm×15mm×8mm.

[0067] Table 1, Example 1, Example 2, Comparative Example 1 and porous artificial bone structure performance table

[0068]

[0069] like Figure 2 As shown, the Fe in Example 1 of the FeCoNiAl alloy coating 20 Co 20 Ni 20 Al 4 Ti 31 B 5 Alloy coating, Fe in Example 2 20 Co 20 Ni 20 Al 4 Ti 26 B 10 The hardness of the alloy coating is higher than that of the Fe 22 Co 22 Ni 22 Al 12 Ti 22 alloy coating, and its hardness gradually increases with the increase of B element content.

[0070] As shown in Table 1, the wear resistance of Comparative Example 1 is higher than that of the porous artificial bone structure, and the wear rate of Comparative Example 1 is reduced by 48.7% relative to the porous artificial bone structure. The hardness of Examples 1-2 is better than that of Comparative Example 1, and the wear rate of Examples 1-2 is reduced by 33%-62.4% relative to Comparative Example 1. It can be seen that with the increase of the B element content, the wear scar width decreases, and the wear resistance of the FeCoNiAl alloy coating provided by the present invention is gradually enhanced.

[0071] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. Application of FeCoNiAl alloy coating in antibacterial and wear-resistant artificial bone, characterized in that: The following steps are involved: S1, preparing a porous artificial bone structure by pressing titanium metal powder and a pore-forming agent and sintering at high temperature; S2, sequentially performing deoxidation film and degreasing operations on the porous artificial bone structure in S1, immersing the porous artificial bone structure in a Cu-containing electrolyte for micro-arc oxidation treatment after the treatment, forming a Cu-TiO2 antibacterial micro-arc oxidation film layer on the porous artificial bone structure, washing with deionized water and drying to obtain a porous antibacterial artificial bone structure; S3, coating the FeCoNiAl alloy coating composed of FeCoNiAl alloy powder on the surface of the porous antibacterial artificial bone structure in S2 by laser cladding technology, cutting it into the required size and then grinding and polishing it, and then ultrasonically washing it with acetone, anhydrous ethanol and distilled water in sequence to obtain a porous antibacterial high-strength artificial bone structure; In S1, the pore-forming agent is urea; In S2, the treated porous artificial bone structure is connected to the positive electrode of the power supply as an anode, immersed in a cathode tank filled with an electrolyte, and the cathode tank is connected to the negative electrode of the power supply, and a micro-arc oxidation operation is performed on the porous artificial bone structure; In S2, the treated porous artificial bone structure is connected to the positive electrode of the power supply as an anode, immersed in a cathode tank filled with an electrolyte, a stainless steel plate is used as a cathode plate, the cathode tank is connected to the negative electrode of the power supply, the electrolyte is maintained at 30° C. by a circulating water treatment system, and the porous artificial bone structure is subjected to micro-arc oxidation treatment at a constant voltage of 400 V for 5 minutes; In S2, the electrolyte contains 1-20 g / L of trisodium phosphate, 1-4 g / L of sodium hydroxide, 0.5-2 g / L of copper acetate, and 1-10 g / L of sodium ethylenediaminetetraacetate, and the solvent is deionized water; In S3, the laser cladding technology uses a semiconductor laser for single-pass cladding. The parameters are set to laser power 800W, spot diameter 3mm, scanning speed 6mm / s, and continuous argon gas flow. The FeCoNiAl alloy coating comprises Fe powder, Co powder, Ni powder, Al powder, Ti powder and B powder; The mixed molar ratio of the FeCoNiAl alloy coating is 20 at% of Fe powder, 20 at% of Co powder, 20 at% of Ni powder, 4 at% of Al powder, 26-31 at% of Ti powder and 5-10 at% of B powder.