A scandium-cerium-iron-doped lithium niobate crystal and its preparation method and application

By doping lithium niobate crystal with scandium cerium iron, a scandium cerium iron doped lithium niobate crystal with excellent holographic storage performance is prepared, which solves the problem of insufficient holographic storage performance of existing doped lithium niobate crystals in optical volumes. , achieving faster writing times, greater dynamic range and higher photorefractive sensitivity.

CN117604640BInactive Publication Date: 2024-10-11HARBIN UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311569349.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-23
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing doped lithium niobate crystals have insufficient performance in optical volume holographic storage, especially long writing time, small dynamic range, low saturation diffraction efficiency and insufficient photorefractive sensitivity.

Method used

Scandium cerium iron doped lithium niobate crystal is used. By doping Sc, Ce and Fe into LiNbO3, a scandium cerium iron doped lithium niobate crystal with a perovskite structure is prepared, and through sintering and pulling methods Preparation by crystal growth method, optimizing doping ratio and process conditions to improve the optical properties of the crystal.

Benefits of technology

Significantly shortening the writing time, increasing the dynamic range and saturation diffraction efficiency, improving the photorefractive sensitivity and light damage resistance, making the scandium cerium iron doped lithium niobate crystal an ideal three-dimensional volume holographic storage material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004564929990000091
    Figure BDA0004564929990000091
  • Figure BDA0004564929990000101
    Figure BDA0004564929990000101
  • Figure BDA0004564929990000102
    Figure BDA0004564929990000102
Patent Text Reader

Abstract

The present invention belongs to the technical field of composite material preparation, and specifically relates to a scandium-cerium-iron-doped lithium niobate crystal, and a preparation method and application thereof. The scandium-cerium-iron-doped lithium niobate crystal provided by the present invention has high gloss, uniform composition, no defects, no growth stripes and no cracks, which solves the problem that lithium niobate crystal cannot be used as a laser crystal material and the problem that lithium niobate crystal has low resistance to light damage. The scandium-cerium-iron-doped lithium niobate crystal provided by the present invention has no macroscopic defects, uniform composition, satisfactory performance, and better holographic storage performance. The scandium-cerium-iron-doped lithium niobate crystal prepared by the present invention has the advantages of fast photorefractive response speed, high sensitivity, low doping threshold and good crystal optical quality, and is an ideal three-dimensional holographic storage material. The scandium-cerium-iron-doped lithium niobate crystal provided by the present invention has an important position in the application fields of holographic optical storage, optical waveguide amplifiers and integrated optics, and is particularly suitable for optical volume holographic storage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite material preparation, and specifically relates to a scandium-cerium-iron-doped lithium niobate crystal and a preparation method and application thereof. Background Art

[0002] Optical volume holographic storage is a new storage technology that is different from traditional storage. It uses the coherence of light to form interference patterns to store information. Based on the Bragg selectivity of volume gratings, it can realize multiple information storage in the same area by using multiple multiplexing methods such as angle multiplexing, wavelength multiplexing and spatial multiplexing. Compared with other types of storage technologies, optical volume holographic storage has advantages in storage capacity, transmission rate and system portability.

[0003] Lithium niobate crystal is an important inorganic nonlinear optical crystal material with a high nonlinear optical coefficient. It can be used to produce high nonlinear optical effects, such as frequency doubling and optical modulation. It can maintain high nonlinear optical performance even at high temperatures, has good thermal stability, and a wide optical transparency window, and can perform effective nonlinear optical conversion in the visible and infrared light bands.

[0004] Chinese patent CN115261989A discloses a fast-response lithium niobate crystal and its preparation method, and prepares indium-uranium dual-doped lithium niobate crystals with an In ion doping amount of 2-6 mol% and a uranium ion doping amount of 0.6-2 mol%. The dual-doped lithium niobate polycrystalline powder is synthesized by solid phase sintering method, and the crystal is grown by crucible descent method, so that a crystal with uniform composition and good performance can be obtained.

[0005] Chinese patent CN116692946A discloses a doped lithium niobate powder and its preparation method and application, using an autoclave to prepare metal-doped lithium niobate powder by hydrothermal synthesis. The microscopic morphology of the powder is a cubic crystal structure, accompanied by a small amount of nano-scale irregular particles, to achieve the doping of multiple metal oxides, and by adjusting the synthesis temperature, synthesis time and heat treatment conditions, doped lithium niobate powders with different properties can be obtained.

[0006] However, the above-mentioned doped lithium niobate crystal still has the problem of insufficient holographic storage performance. Summary of the invention

[0007] The purpose of the present invention is to provide a scandium cerium iron doped lithium niobate crystal and its preparation method and application. The scandium cerium iron doped lithium niobate crystal provided by the present invention has excellent holographic storage performance, and the writing time τ w shortened, the dynamic range M / # becomes larger, and the saturation diffraction efficiency η s As α increases, the photorefractive sensitivity S increases.

[0008] In order to achieve the above object, the present invention provides the following technical solutions:

[0009] The present invention provides a scandium-cerium-iron doped lithium niobate crystal, the molecular formula of which is Sc:Ce:Fe:LiNbO3;

[0010] The doping amount of Sc in the scandium-cerium-iron-doped lithium niobate crystal is 1% to 4%.

[0011] Preferably, the Ce doping amount in the scandium-cerium-iron-doped lithium niobate crystal is 0.48% to 0.52%;

[0012] The doping amount of Fe in the scandium-cerium-iron-doped lithium niobate crystal is 0.028% to 0.032%.

[0013] Preferably, the crystal structure of the scandium-cerium-iron-doped lithium niobate crystal is a perovskite structure, has a ferroelectric phase and a paraelectric phase structure, and belongs to the trigonal crystal system and the hexagonal unit cell.

[0014] The present invention also provides a method for preparing the scandium-cerium-iron-doped lithium niobate crystal described in the above scheme, comprising the following steps:

[0015] (1) mixing Nb2O5, Li2CO3, Sc2O3, Ce2O3 and Fe2O3 to obtain a mixture;

[0016] (2) After sintering the mixture, cooling, Czochralski crystal growth and polarization are performed in sequence to obtain scandium cerium iron doped lithium niobate crystals.

[0017] Preferably, the sintering is: sintering at 730-748° C. for 2-4 hours, and then heating to 1180-1195° C. for 1-2 hours.

[0018] Preferably, the cooling rate is 70-90°C / h, and the final temperature is room temperature.

[0019] Preferably, the Czochralski crystal growth method comprises: sequentially performing seeding, necking, shoulder release, shoulder collection, equal diameter growth, pulling and annealing on the cooled product;

[0020] The seeding comprises: heating the cooled product and then maintaining the temperature at a constant temperature to obtain a melt, and then placing a seed crystal into the melt for seeding;

[0021] The temperature of the constant temperature insulation is 1245-1249° C., and the insulation time is based on the fact that no floating crystals appear in the melt; the depth of the seed crystal is 0.7-1.2 mm;

[0022] The pulling speed of the seeding is 0.8-1.3 mm / h, the axial temperature gradient is 32-37° C. / cm, and the rotation speed is 15-18 rpm.

[0023] Preferably, the molar ratio of Li in Li2CO3 to Nb in Nb2O5 is 0.945-0.947:1;

[0024] The doping molar amount of Sc2O3 accounts for 2.8% to 3.2% of the total molar amount of the raw materials;

[0025] The doping molar amount of Ce2O3 accounts for 0.48% to 0.52% of the total molar amount of the raw materials;

[0026] The doping mass fraction of the Fe2O3 accounts for 0.028-0.032% of the total mass of the raw materials.

[0027] Preferably, the polarization temperature is 1185-1210°C, and the current density is 4.8-5.2 mA / cm 2 , polarization time is 25 to 28 minutes.

[0028] The present invention also provides the use of the scandium cerium iron doped lithium niobate crystal described in the above scheme or the scandium cerium iron doped lithium niobate crystal obtained by the preparation method described in the above scheme in holographic optical storage, optical waveguide amplifier or integrated optics.

[0029] The present invention provides a scandium-cerium-iron-doped lithium niobate crystal. The scandium-cerium-iron-doped lithium niobate crystal provided by the present invention is doped with a specific proportion of scandium element in lithium niobate. 3+ Anti-site niobium in the crystal when ions are doped It is basically completely replaced, and combined with cerium and iron elements, the resulting crystal has no macroscopic defects, uniform composition, increased photoconductivity, satisfactory performance, and better holographic storage performance. The writing time is τ w shortened, the dynamic range M / # becomes larger, and the saturation diffraction efficiency η s Increase, the photorefractive sensitivity S increases. The scandium cerium iron doped lithium niobate crystal provided by the present invention solves the problem that lithium niobate crystal cannot be used as laser crystal material and the lithium niobate crystal has low light damage resistance.

[0030] The present invention also provides a method for preparing the scandium-cerium-iron-doped lithium niobate crystals described in the above scheme. The scandium-cerium-iron-doped lithium niobate crystals prepared by the present invention have the advantages of fast photorefractive response speed, high sensitivity, low doping threshold and good crystal optical quality, and are an ideal three-dimensional holographic storage material. The scandium-cerium-iron-doped lithium niobate crystals prepared by the present invention have high gloss, uniform composition, no defects, no growth stripes and no cracks, high resistance to light damage, and can be used as laser crystal materials. The preparation method provided by the present invention has simple steps, is easy to operate, and has high crystal preparation efficiency.

[0031] The present invention also provides the use of the scandium cerium iron doped lithium niobate crystal described in the above scheme or the scandium cerium iron doped lithium niobate crystal obtained by the preparation method described in the above scheme in holographic optical storage, optical waveguide amplifier or integrated optics. The scandium cerium iron doped lithium niobate crystal provided by the present invention is an ideal three-dimensional volume holographic storage material, has very important application value, plays an important role in the application fields of holographic optical storage, optical waveguide amplifier and integrated optics, and is particularly suitable for optical volume holographic storage. DETAILED DESCRIPTION

[0032] The invention provides a scandium-cerium-iron doped lithium niobate crystal, the molecular formula of which is Sc:Ce:Fe:LiNbO3.

[0033] In the present invention, the doping amount of Sc in the scandium cerium iron doped lithium niobate crystal is 1% to 4%, preferably 2.8% to 3.2%, more preferably 2.9% to 3.1%, and further preferably 3.0%; the doping amount of Ce in the scandium cerium iron doped lithium niobate crystal is preferably 0.48% to 0.52%, more preferably 0.49% to 0.51%, and further preferably 0.50%; the doping amount of Fe in the scandium cerium iron doped lithium niobate crystal is preferably 0.028% to 0.032%, more preferably 0.029% to 0.031%, and further preferably 0.03%.

[0034] In the present invention, the crystal structure of the scandium-cerium-iron-doped lithium niobate crystal is preferably a perovskite structure, having a ferroelectric phase and a paraelectric phase structure, and belonging to the trigonal system and the hexagonal unit cell.

[0035] The present invention also provides a method for preparing the scandium-cerium-iron-doped lithium niobate crystal described in the above scheme, comprising the following steps:

[0036] (1) mixing Nb2O5, Li2CO3, Sc2O3, Ce2O3 and Fe2O3 to obtain a mixture;

[0037] (2) After sintering the mixture, cooling, Czochralski crystal growth and polarization are performed in sequence to obtain scandium cerium iron doped lithium niobate crystals.

[0038] In the present invention, Nb2O5, Li2CO3, Sc2O3, Ce2O3 and Fe2O3 are mixed to obtain a mixed material. In the present invention, the mixing is preferably stirring.

[0039] In the present invention, the particle size of the Nb2O5 is preferably 200-400 mesh, more preferably 240-350 mesh, and further preferably 260-320 mesh.

[0040] In the present invention, the particle size of the Li2CO3 is preferably 200-380 mesh, more preferably 250-350 mesh, and further preferably 280-330 mesh; the molar ratio of Li in the Li2CO3 to Nb in the Nb2O5 is preferably 0.945-0.947:1, and more preferably 0.946:1.

[0041] In the present invention, the particle size of the Sc2O3 is preferably 250-450 mesh, more preferably 280-400 mesh, and further preferably 300-350 mesh; the doping molar amount of the Sc2O3 is preferably 2.8%-3.2% of the total molar amount of the raw material, more preferably 2.9%-3.1%, and further preferably 3%.

[0042] In the present invention, the particle size of the Ce2O3 is preferably 250-400 mesh, more preferably 280-380 mesh, and further preferably 300-340 mesh; the doping molar amount of the Ce2O3 is preferably 0.48%-0.52% of the total molar amount of the raw material, more preferably 0.49%-0.51%, and further preferably 0.5%.

[0043] In the present invention, the particle size of the Fe2O3 is preferably 200-400 mesh, more preferably 240-360 mesh, and further preferably 280-320 mesh; the doping mass fraction of the Fe2O3 is preferably 0.028-0.032% of the total mass of the raw material, more preferably 0.029-0.031%, and further preferably 0.030%.

[0044] After obtaining the mixture, the present invention sequentially cools, grows crystals by pulling and polarizes the mixture after sintering to obtain scandium cerium iron doped lithium niobate crystals. In the present invention, the sintering is preferably: sintering at 730-748°C (recorded as the first sintering temperature) for 2-4h (recorded as the first sintering time), and then heating to 1180-1195°C (recorded as the second sintering temperature) for 1-2h (recorded as the second sintering time).

[0045] In the present invention, the first sintering temperature is preferably 735-745° C., more preferably 738-742° C., and further preferably 740° C.; the first sintering time is preferably 2.5-3.5 h, and more preferably 3 h.

[0046] In the present invention, the second sintering temperature is preferably 1180-1195°C, more preferably 1183-1192°C, and further preferably 1187-1190°C; the second sintering time is preferably 1.2-1.8h, more preferably 1.4-1.6h, and further preferably 1.5h.

[0047] In the present invention, the sintering equipment is preferably a Pt crucible. The present invention generates LiNbO3 crystals through sintering, avoiding the generation of impurities and by-products.

[0048] In the present invention, the cooling rate is preferably 70-90°C / h, more preferably 75-85°C / h, and further preferably 78-82°C / h, and the final temperature is preferably room temperature. The present invention can eliminate two aspects of internal stress generated during the crystal growth process by cooling. The first is the stress generated by the unevenness of the components and the structural defects of the crystal, and the second is the chemical stress generated by impurities entering the crystal. The present invention effectively weakens the generated internal stress by cooling.

[0049] In the present invention, the Czochralski crystal growth method is preferably: the cooled product is sequentially subjected to seeding, necking, shoulder release, shoulder collection, equal diameter growth, pulling and annealing.

[0050] In the present invention, the seeding is preferably performed by heating the cooled product and then maintaining the temperature at a constant level to obtain a melt, and then placing a seed crystal into the melt for seeding.

[0051] In the present invention, the temperature of the constant temperature insulation is preferably 1245-1249°C, more preferably 1246-1248°C, and further preferably 1248°C. The insulation time is preferably based on the absence of floating crystals in the melt. The depth of the seed crystal (the distance between the seed crystal and the upper surface of the melt obtained by constant temperature insulation) is preferably 0.7-1.2 mm, more preferably 0.8-1.1 mm, and further preferably 0.9-1.0 mm.

[0052] In the present invention, the pulling speed of the seeding is preferably 0.8 to 1.3 mm / h, more preferably 0.9 to 1.2 mm / h, and further preferably 1.0 to 1.1 mm / h, the axial temperature gradient is preferably 32 to 37°C / cm, more preferably 33 to 36°C / cm, and further preferably 34 to 35°C / cm, and the rotation speed is preferably 15 to 18 rpm, and more preferably 16 to 17 rpm. The present invention grows crystals by the Czochralski method, and adopts the temperature of the lower crystal, which can reduce the dislocation density of the crystal.

[0053] The present invention adopts the above-mentioned rate to grow crystals, obtains a flat solid-liquid growth interface, and grows crystals with good quality and few defects. The present invention has found that too fast crystal rotation speed will cause a concave interface. Due to the effects of surface tension and gravity, the stability of the solid-liquid interface is poor, and the grown crystals are prone to growth stripes, making crystal processing difficult; if the rotation speed is too slow, the solid-liquid interface will become a concave interface. This shape of solid-liquid interface will cause slow heat exchange, and the grown crystals are prone to defects such as inclusions. The present invention adopts the above-mentioned rotation speed to obtain a flat solid-liquid growth interface, and grows crystals with good quality and few defects.

[0054] In the present invention, the polarization temperature is preferably 1185-1210°C, more preferably 1190-1205°C, and further preferably 1195-1200°C, and the current density is preferably 4.8-5.2 mA / cm 2 , more preferably 5 mA / cm 2 The polarization time is preferably 25 to 28 minutes, more preferably 26 to 27 minutes. The present invention converts the multi-domain crystal grown by the Czochralski method into a single domain by polarization. When electromagnetic waves pass through the multi-domain crystal, they are scattered at the "domain wall", thereby affecting the application of the crystal in optical devices.

[0055] In the present invention, after the polarization, the polarization product is preferably cut and polished; the cutting size is preferably 17-21mm×8-13mm×13-15mm, more preferably 18-20mm×9-12mm×13-14mm, further preferably 18mm×11mm×14mm; the polishing is preferably optical quality grade polishing.

[0056] The present invention also provides the use of the scandium cerium iron doped lithium niobate crystal described in the above scheme or the scandium cerium iron doped lithium niobate crystal obtained by the preparation method described in the above scheme in holographic optical storage, optical waveguide amplifier or integrated optics.

[0057] The scandium-cerium-iron-doped lithium niobate crystal provided by the present invention is an ideal three-dimensional volume holographic storage material, has very important application value, plays an important role in the application fields of holographic optical storage, optical waveguide amplifiers and integrated optics, and is particularly suitable for optical volume holographic storage. The scandium-cerium-iron-doped lithium niobate crystal provided by the present invention can be cut into crystal materials of any size and shape according to actual application scenarios.

[0058] In order to further illustrate the present invention, the scheme of the present invention is described in detail below in conjunction with embodiments, but they should not be understood as limiting the scope of protection of the present invention.

[0059] Example 1

[0060] (1) Mixing: Weighing five raw materials, uniformly mixing Nb2O5, Li2CO3, Sc2O3, Ce2O3 and Fe2O3 to obtain a mixture; the molar ratio of Li in Li2CO3 to Nb in Nb2O5 is 0.946:1, the doping molar amount of Sc2O3 accounts for 0% of the total molar amount of the five raw materials, the doping molar amount of Ce2O3 accounts for 0.5% of the total molar amount of the five raw materials, and the doping mass fraction of Fe2O3 is 0.03wt% of the total mass of the five raw materials;

[0061] (2) Czochralski method for growing crystals: the mixed material of step (1) is placed in a Pt crucible, and then sintered at 730°C for 4 hours, and then heated to 1180°C for sintering for 2 hours and then cooled, the cooling rate is 70°C / h, and the final temperature is room temperature; then the Czochralski method is used for crystal growth, the cooled product is heated and kept at a constant temperature, and then a seed crystal is placed in the product for seeding, and then necking, shoulder release, shoulder collection, equal diameter growth, pulling and annealing are performed to obtain a multi-domain crystal;

[0062] The temperature of the seed crystal inserted is 1245° C., and the depth of the seed crystal inserted (the distance between the seed crystal and the upper surface of the melt obtained by constant temperature insulation) is 1.2 mm;

[0063] The seeding pulling speed is 0.8 mm / h, the axial temperature gradient is 32°C / cm, and the rotation speed is 15 rpm;

[0064] (3) Polarization: The multi-domain crystal in step (2) is placed at a temperature of 1185°C and a current density of 5 mA / cm 2 Polarize for 28 min under the conditions of , and obtain the polarized crystal;

[0065] (4) Cutting and polishing: The polarized crystal in step (3) is cut into pieces with a size of 17 mm×8 mm×13 mm, and then the surface is polished to optical quality to obtain scandium cerium iron doped lithium niobate crystal (Sc:Ce:Fe:LiNbO3 crystal).

[0066] Example 2

[0067] The preparation method of this embodiment is the same as that of embodiment 1, the only difference being that the doping molar amount of Sc2O3 accounts for 1% of the total molar amount of the five raw materials.

[0068] Example 3

[0069] The preparation method of this embodiment is the same as that of embodiment 1, the only difference being that the doping molar amount of Sc2O3 accounts for 2% of the total molar amount of the five raw materials.

[0070] Example 4

[0071] The preparation method of this embodiment is the same as that of embodiment 1, the only difference being that the doping molar amount of Sc2O3 accounts for 3% of the total molar amount of the five raw materials.

[0072] Example 5

[0073] (1) Mixing: Weighing five raw materials, uniformly mixing Nb2O5, Li2CO3, Sc2O3, Ce2O3 and Fe2O3 to obtain a mixed material; the molar ratio of Li in Li2CO3 to Nb in Nb2O5 is 0.946:1, the doping molar amount of Sc2O3 accounts for 3% of the total molar amount of the five raw materials, the doping molar amount of Ce2O3 accounts for 0.5% of the total molar amount of the five raw materials, and the doping mass fraction of Fe2O3 is 0.03wt% of the total mass of the five raw materials;

[0074] (2) Czochralski method for growing crystals: the mixed material of step (1) is placed in a Pt crucible, and then sintered at 748°C for 2h, and then heated to 1195°C for sintering for 1h and then cooled, the cooling rate is 90°C / h, and the final temperature is room temperature; then the Czochralski method is used for crystal growth, the cooled product is heated and kept at a constant temperature, and then a seed crystal is placed in the product for seeding, and then necking, shoulder release, shoulder collection, equal diameter growth, pulling and annealing are performed to obtain a multi-domain crystal;

[0075] The temperature of the seed crystal inserted is 1249° C., and the depth of the seed crystal inserted (the distance between the seed crystal and the upper surface of the melt obtained by constant temperature insulation) is 0.7 mm;

[0076] The seeding pulling speed is 1.3 mm / h, the axial temperature gradient is 37°C / cm, and the rotation speed is 18 rpm;

[0077] (3) Polarization: The multi-domain crystal in step (2) is placed at a temperature of 1210°C and a current density of 5 mA / cm 2 Polarize for 25 min under the conditions of , and obtain the polarized crystal;

[0078] (4) Cutting and polishing: The polarized crystal in step (3) is cut into pieces with a size of 21 mm×13 mm×15 mm, and then the surface is polished to optical quality level to obtain scandium cerium iron doped lithium niobate crystal (Sc:Ce:Fe:LiNbO3 crystal).

[0079] Example 6

[0080] (1) Mixing: Weighing five raw materials, uniformly mixing Nb2O5, Li2CO3, Sc2O3, Ce2O3 and Fe2O3 to obtain a mixed material; the molar ratio of Li in Li2CO3 to Nb in Nb2O5 is 0.946:1, the doping molar amount of Sc2O3 accounts for 3% of the total molar amount of the five raw materials, the doping molar amount of Ce2O3 accounts for 0.5% of the total molar amount of the five raw materials, and the doping mass fraction of Fe2O3 is 0.03wt% of the total mass of the five raw materials;

[0081] (2) Czochralski method for growing crystals: the mixed material of step (1) is placed in a Pt crucible, and then sintered at 740°C for 3 hours, and then heated to 1190°C for sintering for 1.5 hours and then cooled, the cooling rate is 80°C / h, and the final temperature is room temperature; then the Czochralski method is used for crystal growth, the cooled product is heated and kept at a constant temperature, and then a seed crystal is placed in the product for seeding, and then necking, shoulder release, shoulder collection, equal diameter growth, pulling and annealing are performed to obtain a multi-domain crystal;

[0082] The temperature of the seed crystal inserted is 1247° C., and the depth of the seed crystal inserted (the distance between the seed crystal and the upper surface of the melt obtained by constant temperature insulation) is 1.0 mm;

[0083] The seeding pulling speed is 1.0 mm / h, the axial temperature gradient is 35°C / cm, and the rotation speed is 16 rpm;

[0084] (3) Polarization: The multi-domain crystal in step (2) is placed at a temperature of 1200°C and a current density of 5 mA / cm 2 Polarize for 26 min under the conditions of , and obtain the polarized crystal;

[0085] (4) Cutting and polishing: The polarized crystal in step (3) is cut into pieces with a size of 19 mm×10 mm×14 mm, and then the surface is polished to optical quality level to obtain scandium cerium iron doped lithium niobate crystal (Sc:Ce:Fe:LiNbO3 crystal).

[0086] The optical uniformity of the scandium cerium iron doped lithium niobate crystals prepared in Examples 1 to 4 of the present invention was tested by the birefringence gradient method. Optical uniformity refers to the degree of unevenness of the refractive index change of each part of the crystal. The present invention uses a He-Ne diode laser as an excitation light source. The laser first irradiates the polarizer, then passes through the sample placed at an angle of π / 4 with the C axis, then passes through the wave plate, analyzer and detector, and finally is transmitted to the computer for data collection and analysis. The results are shown in Table 1.

[0087] Table 1 Birefringence gradient of scandium cerium iron doped lithium niobate crystals prepared in Examples 1 to 4

[0088] Crystal <![CDATA[Birefringence gradient ΔR / cm -1 > Example 1 <![CDATA[12.3×10 -5 ]]> Example 2 <![CDATA[8.2×10 -5 ]]> Example 3 <![CDATA[6.5×10 -5 ]]> Example 4 <![CDATA[3.3×10 -5 ]]>

[0089] According to Table 1, as Sc 3+ As the doping concentration increases, the birefringence gradient of the crystal gradually decreases. The birefringence gradient of the crystal prepared in Example 4 is the largest, and the birefringence gradient of the crystal prepared in Example 1 is the smallest. Based on this, it can be inferred that the Sc in Sc:Ce:Fe:LiNbO3 crystal is 3+ The higher the doping concentration, the better the optical uniformity of the crystal; among Examples 1 to 4, the optical uniformity of the crystal of Example 4 reaches the best value.

[0090] The present invention adopts a double-wave coupling experiment to test the photorefractive performance of the scandium-cerium-iron-doped lithium niobate crystals prepared in Examples 1 to 4. The physical principle of the experiment is double-beam interference. When two light beams of the same state are symmetrically irradiated on the crystal, due to the coherence of the light beam interference, a light intensity distribution grating will be caused inside the crystal, and then a refractive index distribution grating will be formed. In the photorefractive material, the two distribution gratings are inconsistent and have a phase difference of π / 2. In this way, the two gratings will produce an energy conversion phenomenon, which is called the double-wave coupling phenomenon. The results are shown in Table 2.

[0091] Table 2 Holographic storage performance of scandium cerium iron doped lithium niobate crystals prepared in Examples 1 to 4

[0092]

[0093]

[0094] According to Table 2, when the doping concentration reaches the threshold value (3 mol%), the anti-site niobium Almost all of them have been replaced. 3+ Ions begin to occupy normal Nb sites to form defects The intrinsic defect concentration is further reduced, the conductivity is increased, and the writing time is reduced. Fe and Ce ions are doped to occupy the normal Li position and enter the LiNbO3 crystal to form a photorefractive center. and The present invention believes that as Sc 3+ The increase of ion doping concentration will promote the entry of Fe and Ce ions into the crystal, so the concentration of photorefractive centers increases. 3+ With the increase of ion doping concentration, the saturation diffraction efficiency of scandium cerium iron doped lithium niobate crystal also increases.

[0095] Therefore, the dynamic range M / # increases with the doping of Sc 3+ The increase of ion concentration increases the saturation diffraction efficiency and reduces the writing time, which leads to the increase of photorefractive sensitivity. 3+ With the increase of concentration, the writing time τ w shortened, the dynamic range M / # becomes larger, and the saturation diffraction efficiency η s As α increases, the photorefractive sensitivity S increases.

[0096] The present invention uses the light scattering energy flow threshold method to quantitatively test the Sc 3+The influence of ions on the scattering of crystals against light damage. The scattering of incident light is the cumulative effect of time. Even if the intensity of the incident light is very small, as long as the crystal is irradiated for a long enough time, light damage will occur. That is, light damage will occur after the cumulative effect of irradiation light intensity and time reaches a certain level. The present invention uses exposure energy to describe the ability to resist light scattering. When the energy irradiated on the crystal reaches a certain value, the phenomenon of anti-light damage occurs. Er is used to represent this critical amount. The larger Er is, the stronger the crystal's ability to resist light scattering. The test results are shown in Table 3.

[0097] Table 3 Anti-light scattering performance of scandium cerium iron doped lithium niobate crystals of Examples 1 to 4

[0098]

[0099] According to Table 3, the light damage resistance of the scandium cerium iron doped lithium niobate crystal gradually increases with the increase of Sc doping concentration. When the Sc doping concentration reaches 3 mol%, the light damage resistance increases significantly. The exposure energy flow threshold of the crystal in Example 4 is 895.76 J / cm 2 The exposure energy flow threshold of the crystal of Example 1 with a doping concentration of 0 is 4.13 J / cm 2 , both of which are improved by two orders of magnitude compared to Example 4.

[0100] The performance test results of Examples 5 to 6 are similar to those of Examples 1 to 4, and are not described in detail here.

[0101] It can be seen from the above embodiments that the scandium-cerium-iron-doped lithium niobate crystal provided by the present invention has strong resistance to light damage, high gloss, uniform composition, no defects, no growth stripes and cracks, rich performance levels, better optical application performance, solves the problem that lithium niobate crystal cannot be used as laser crystal material, and has excellent holographic storage performance.

[0102] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A scandium-cerium-iron doped lithium niobate crystal, the molecular formula of which is Sc:Ce:Fe:LiNbO3; The doping amount of Sc in the scandium-cerium-iron-doped lithium niobate crystal is 1% to 4%; The Ce doping amount in the scandium-cerium-iron-doped lithium niobate crystal is 0.48% to 0.52%; The Fe doping amount in the scandium cerium iron doped lithium niobate crystal is 0.028% to 0.032%; the scandium cerium iron doped lithium niobate crystal is a perovskite structure, has a ferroelectric phase and a paraelectric phase structure, and belongs to the trigonal system and the hexagonal unit cell; The method for preparing the scandium-cerium-iron-doped lithium niobate crystal comprises the following steps: (1) mixing Nb2O5, Li2CO3, Sc2O3, Ce2O3 and Fe2O3 to obtain a mixture; (2) after sintering the mixture, sequentially cooling, Czochralski crystal growth and polarization are performed to obtain scandium cerium iron doped lithium niobate crystals; The Czochralski crystal growth method comprises: sequentially performing seeding, necking, shoulder release, shoulder collection, equal diameter growth, pulling and annealing on the cooled product; The seeding comprises: heating the cooled product and then maintaining the temperature at a constant temperature to obtain a melt, and then placing a seed crystal into the melt for seeding; The temperature of the constant temperature insulation is 1245-1249° C., and the insulation time is based on the fact that no floating crystals appear in the melt; the depth of the seed crystal is 0.7-1.2 mm; The seeding pulling speed is 0.8-1.3 mm / h, the axial temperature gradient is 32-37°C / cm, and the rotation speed is 15-18 rpm; The polarization temperature is 1185-1210°C, and the current density is 4.8-5.2 mA / cm 2 , polarization time is 25 to 28 minutes.

2. The method for preparing the scandium-cerium-iron-doped lithium niobate crystal according to claim 1, comprising the following steps: (1) mixing Nb2O5, Li2CO3, Sc2O3, Ce2O3 and Fe2O3 to obtain a mixture; (2) after sintering the mixture, sequentially cooling, Czochralski crystal growth and polarization are performed to obtain scandium cerium iron doped lithium niobate crystals; The Czochralski crystal growth method comprises: sequentially performing seeding, necking, shoulder release, shoulder collection, equal diameter growth, pulling and annealing on the cooled product; The seeding comprises: heating the cooled product and then maintaining the temperature at a constant temperature to obtain a melt, and then placing a seed crystal into the melt for seeding; The temperature of the constant temperature insulation is 1245-1249° C., and the insulation time is based on the fact that no floating crystals appear in the melt; the depth of the seed crystal is 0.7-1.2 mm; The seeding pulling speed is 0.8-1.3 mm / h, the axial temperature gradient is 32-37°C / cm, and the rotation speed is 15-18 rpm; The polarization temperature is 1185-1210°C, and the current density is 4.8-5.2 mA / cm 2 , polarization time is 25 to 28 minutes.

3. The preparation method according to claim 2, characterized in that: The sintering is as follows: sintering at 730-748° C. for 2-4 hours, and then heating to 1180-1195° C. for 1-2 hours.

4. The preparation method according to claim 2, characterized in that: The cooling rate is 70-90°C / h, and the final temperature is room temperature.

5. The preparation method according to claim 2, characterized in that: The molar ratio of Li in Li2CO3 to Nb in Nb2O5 is 0.945-0.947:1; The doping molar amount of Sc2O3 accounts for 2.8% to 3.2% of the total molar amount of the raw materials; The doping molar amount of Ce2O3 accounts for 0.48% to 0.52% of the total molar amount of the raw materials; The doping mass fraction of the Fe2O3 accounts for 0.028-0.032% of the total mass of the raw materials.

6. Application of the scandium-cerium-iron-doped lithium niobate crystal according to claim 1 or the scandium-cerium-iron-doped lithium niobate crystal obtained by the preparation method according to any one of claims 2 to 5 in holographic optical storage, optical waveguide amplifier or integrated optics.