Housing, wearable device and manufacturing method

By using a printed coil sintered into a ceramic base shell in the wearable device housing, and then covering the surface of the nanocrystalline film with a protective film for nano-injection molding, the problems of insufficient housing thickness and bonding strength are solved, thereby achieving a reduction in housing thickness and an improvement in waterproof performance.

CN117641785BActive Publication Date: 2026-11-10HUAWEI TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202210968025.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-12
Publication Date
2026-11-10
Estimated Expiration
2042-08-12

AI Technical Summary

Technical Problem

Existing wearable devices have thick casings, which affects user experience and waterproofing, and the bonding force between the wireless charging coil and the casing is insufficient.

Method used

The printed coil and ceramic base shell are sintered into one structure, and a protective film is covered on the surface of the nanocrystalline film. The plastic inner shell is formed by nano-injection molding, which reduces the shell thickness and improves the bonding force.

Benefits of technology

Significantly reduces the thickness of the casing, improves the user experience and waterproof performance, while also increasing charging efficiency and the bonding strength of the casing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117641785B_ABST
    Figure CN117641785B_ABST
Patent Text Reader

Abstract

This application provides a housing, a wearable device, and a manufacturing method. The housing can be applied to wearable devices such as smartwatches, smart bands, and smart bracelets. By reducing the thickness of at least one of the following: the ceramic base shell, the charging coil, and the plastic inner shell, the thickness of the housing and the wearable device can be reduced, thus improving the user experience. This application provides a housing, a wearable device, and a manufacturing method that solves the problem of excessively thick housings affecting user experience.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of terminal technology, and in particular to a housing, wearable device, and manufacturing method. Background Technology

[0002] Wearable devices generally refer to portable devices that can be worn on a user's body, shoes, clothing, or other accessories. In addition, wearable devices can be used independently or as portable accessories for mobile terminals, such as smartwatches, wristbands, and other wearable devices.

[0003] In related technologies, to enable wearable devices to have wireless charging capabilities, a wireless charging coil is installed inside the device's casing, and the wireless charging coil is electrically connected to the main circuitry within the wearable device. The casing includes a ceramic base shell, a plastic inner shell, and the wireless charging coil sandwiched between the ceramic base shell and the plastic inner shell.

[0004] However, the existing casings are quite thick, which reduces the user experience of wearing devices. Summary of the Invention

[0005] This application provides a housing, a wearable device, and a manufacturing method. By reducing the thickness of the charging coil and / or the ceramic base shell, as well as the thickness of the plastic inner shell, the thickness of the housing can be reduced, which helps to improve the user experience of using the wearable device.

[0006] A first aspect of this application provides a housing comprising at least: a ceramic base shell, a charging coil, a plastic inner shell, a nanocrystalline film, and a protective film. The charging coil is disposed on the inner side of the ceramic base shell and is a printed coil sintered integrally with the ceramic base shell. The nanocrystalline film covers the surface of the charging coil and is securely connected to it. The protective film covers the surface of the nanocrystalline film and is securely connected to it, serving to prevent damage to the nanocrystalline film during the injection molding process of the plastic inner shell. The plastic inner shell is formed on the inner side of the ceramic base shell by nano-injection molding and covers the protective film, thus making the plastic inner shell, the ceramic base shell, and the protective film an integral structure.

[0007] In the housing provided in this application embodiment, which can serve as the outer shell of a wearable device, the charging coil is a printed coil, which can reduce the thickness of the charging coil. The charging coil and the ceramic base shell are sintered into a single structure, which can further reduce the thickness of the assembled charging coil and ceramic base shell, thereby reducing the thickness of the housing. By covering the charging coil with a nanocrystalline film, the eddy currents caused by magnetic reluctance during electromagnetic induction of the charging coil can be improved, thereby increasing the charging efficiency of the wearable device. By covering the surface of the nanocrystalline film with a protective film, the base shell assembly defined by the assembled ceramic base shell, charging coil, nanocrystalline film, and protective film can be placed into a mold. Nano-injection molding is used to directly form a plastic inner shell integral with the base shell assembly on the inner surface of the protective film and the ceramic base shell, which can reduce the thickness of the plastic inner shell. In addition, combined with the printed coil sintered into a single structure with the ceramic base shell, the thickness of the housing can be further reduced, resulting in a significant reduction in the thickness of the housing. The protective film can prevent the nanocrystalline film from being damaged by the high-temperature and high-pressure plastic liquid during the injection molding process, and nano-injection molding can be performed directly on the base shell assembly to form the plastic inner shell. In addition, since the plastic inner shell forms an integral structure with the protective film and the ceramic bottom shell, it helps to improve the bonding force between the plastic inner shell and the ceramic bottom shell, which can improve the waterproof performance of wearable devices.

[0008] In one possible implementation, the ceramic base shell is a ceramic base shell formed by hot bending of a ceramic sheet. Since the ceramic base shell is a hot-bent ceramic sheet, its thickness can be reduced, thus decreasing the overall thickness of the casing. Furthermore, the production time for the ceramic base shell can be reduced. Therefore, using a ceramic base shell formed by hot bending of a ceramic sheet can reduce the thickness of the casing and help improve the user experience of wearing devices.

[0009] In one possible implementation, the charging coil is made of nano-silver paste or conductive ceramic. When the printed coil is made of conductive ceramic, it is insulated from the ceramic substrate.

[0010] In one possible implementation, the protective film is a metal film, or the protective film is a non-metallic film made of plastic or fiber.

[0011] In one possible implementation, the plastic inner shell has a mating portion, and the inner edge of the ceramic bottom shell has a snap-fit ​​portion that snaps into the mating portion. The charging coil is disposed on the inner surface of the ceramic bottom shell.

[0012] In one possible implementation, the snap-fit ​​portion and the inner side surface of the ceramic base shell together define a first stepped surface, and the mating portion is a slot for the snap-fit ​​portion to be inserted.

[0013] In one possible implementation, a protrusion extends from the center of the inner side surface of the ceramic base shell, and the protrusion, together with the inner side surface of the ceramic base shell, defines a second stepped surface. The charging coil is disposed on the inner side surface of the ceramic base shell and is positioned close to the second stepped surface.

[0014] In one possible implementation, the housing further includes a transparent cover plate. A through-hole is provided in the center of the ceramic base shell, the inner wall of which defines a third stepped surface, and the transparent cover plate is mounted on the third stepped surface.

[0015] In one possible implementation, the ceramic base shell includes a connecting portion and a transparent portion. The connecting portion is made of an opaque ceramic material, and the transparent portion is made of transparent ceramic and sintered with the connecting portion into a single structure.

[0016] In one possible implementation, the transparent portion includes a first transparent portion and an annular second transparent portion. The first transparent portion is located within the second transparent portion, and an annular gap is defined between the first transparent portion and the second transparent portion for accommodating a portion of the connecting portion.

[0017] A second aspect of this application provides a housing comprising at least: a ceramic base shell, a charging coil, and a plastic inner shell. The ceramic base shell is formed by hot bending a ceramic sheet. The charging coil is securely mounted on the inner side of the ceramic base shell. The plastic inner shell covers the surface of the charging coil and contacts the inner side of the ceramic base shell, and is securely connected to the ceramic base shell. The charging coil is a conductive coil wound with metal wire.

[0018] A third aspect of this application provides a wearable device, including a conductive element and a housing as described in any of the preceding claims, wherein the charging coil of the housing is electrically connected to the host circuit of the wearable device through the conductive element.

[0019] In one possible implementation, the conductive element is conductive silicone or a spring.

[0020] A fourth aspect of this application provides a method for preparing a shell, comprising:

[0021] A charging coil, integral with the ceramic base shell, is formed on the inner surface of the ceramic base shell.

[0022] A nanocrystalline film is coated on the surface of the charging coil having the ceramic base shell;

[0023] A protective film is applied to the surface of the nanocrystalline film having the charging coil to form a bottom shell assembly;

[0024] The bottom shell assembly with the protective film is placed into a mold for nano-injection molding to form a plastic inner shell that is integral with the protective film and the ceramic bottom shell.

[0025] In one possible implementation, the step of forming a charging coil integrally with the ceramic base shell on the inner surface of the ceramic base shell includes:

[0026] Provide conductive paste;

[0027] The conductive paste is coated onto the inner surface of the ceramic base shell using a printing process to form a charging coil on the ceramic base shell.

[0028] The ceramic base shell containing the charging coil is sintered to form an integral structure with the charging coil and the ceramic base shell.

[0029] In one possible implementation, the conductive paste is a nano-silver paste or a conductive ceramic.

[0030] In one possible implementation, the printing process includes any one of the following processes: screen printing, pad printing, 3D printing, sticker printing, and photolithography.

[0031] In one possible implementation, before forming the charging coil integrally with the ceramic base shell on the inner surface of the ceramic base shell, the method further includes:

[0032] Prepare a ceramic base shell that has been hot-bent.

[0033] In one possible implementation, the preparation of the hot-bent ceramic base shell includes:

[0034] Ceramic sheets of equal thickness are available;

[0035] A stepped structure is prepared on the ceramic sheet;

[0036] The ceramic sheet having the stepped structure is subjected to a hot bending process to form the ceramic base shell.

[0037] In one possible implementation, the step structure fabrication on the ceramic sheet includes:

[0038] A first annular groove is formed on the bottom surface of the ceramic sheet. The inner wall of the first annular groove is formed with a first step surface and a second step surface that are spaced apart in the radial direction. The second step surface is arranged close to the axis of the first annular groove.

[0039] A mounting through hole is formed through the ceramic sheet. The mounting through hole is located within the first annular groove and is set close to the second step surface. The inner wall of the mounting through hole forms a third step surface.

[0040] In one possible implementation, the step structure fabrication on the ceramic sheet includes:

[0041] A second annular groove is formed on the bottom surface of the ceramic sheet. The inner wall of the second annular groove forms a first step surface and a second step surface that are spaced apart in the radial direction. The second step surface is arranged close to the axis of the second annular groove.

[0042] In one possible implementation, providing ceramic sheets of uniform thickness includes:

[0043] It provides a non-transparent ceramic substrate, a circular first transparent ceramic sheet, and an annular second transparent ceramic sheet;

[0044] A first through-hole penetrating the ceramic substrate and an annular second through-hole are formed, wherein the first through-hole is located within the second through-hole;

[0045] The first transparent ceramic sheet is filled into the first through hole;

[0046] The second transparent ceramic sheet is filled into the second through hole;

[0047] The first transparent ceramic sheet, the second transparent ceramic sheet, and the ceramic substrate are sintered to form the ceramic sheet with an integral structure. Attached Figure Description

[0048] Figure 1 An exploded view of a portion of a wearable device;

[0049] Figure 2 A cross-sectional view of a housing provided in an embodiment of this application;

[0050] Figure 3 for Figure 2 A partial enlarged view of the embodiment shown;

[0051] Figure 4 for Figure 3 A magnified view of a portion of point A in the middle;

[0052] Figure 5 A cross-sectional view of a ceramic base shell provided in an embodiment of this application;

[0053] Figure 6 A cross-sectional view of another ceramic base shell provided in an embodiment of this application;

[0054] Figure 7 A cross-sectional view of yet another ceramic base shell provided in an embodiment of this application;

[0055] Figure 8 A cross-sectional view of another ceramic base shell provided in an embodiment of this application;

[0056] Figure 9 A cross-sectional view of yet another ceramic base shell provided in an embodiment of this application;

[0057] Figure 10 A flowchart illustrating a method for preparing a shell according to an embodiment of this application;

[0058] Figure 11 for Figure 10 A schematic diagram of the preparation process of the preparation method shown;

[0059] Figure 12 A flowchart of the method for preparing printed coils provided in this application embodiment;

[0060] Figure 13 A partial cross-sectional view of another housing provided in an embodiment of this application;

[0061] Figure 14 A partial perspective view of another type of housing provided in the embodiments of this application;

[0062] Figure 15 for Figure 14 The front view of the casing shown;

[0063] Figure 16 A flowchart illustrating another method for preparing a shell according to an embodiment of this application;

[0064] Figure 17 for Figure 16 A schematic diagram of the preparation process of the preparation method shown;

[0065] Figure 18 A flowchart illustrating a method for preparing a hot-bent ceramic bottom shell, as provided in an embodiment of this application;

[0066] Figure 19 A flowchart illustrating a method for preparing a ceramic sheet with transparent ceramic components, provided in an embodiment of this application;

[0067] Figure 20 for Figure 19 A schematic diagram of the preparation process of the preparation method shown;

[0068] Figure 21 A schematic diagram illustrating the fabrication process of a stepped structure provided in an embodiment of this application;

[0069] Figure 22 A schematic diagram illustrating the preparation process of another stepped structure provided in this application embodiment;

[0070] Figure 23 This is a schematic diagram illustrating the preparation of a ceramic sheet with a stepped structure by hot pressing, as provided in an embodiment of this application.

[0071] Explanation of reference numerals in the attached figures:

[0072] 1000. Wearable devices;

[0073] 100. Shell;

[0074] 110. Ceramic base shell;

[0075] 111. Protrusion;

[0076] 112. Connecting part;

[0077] 113. First step surface;

[0078] 114. Install through holes;

[0079] 115. The third step surface;

[0080] 116. Connecting part; 1161. First connecting part; 1162. Second connecting part;

[0081] 117. Transparent area; 1171. First transparent area; 1172. Second transparent area;

[0082] 118. The second step surface;

[0083] 120. Charging coil; 130. Nanocrystalline film; 140. Protective film;

[0084] 150. Plastic inner shell; 151. Mating part;

[0085] 300. Transparent cover plate;

[0086] 410. Top cover; 420. Ceramic bottom cover; 430. Wireless charging coil;

[0087] 50. Bottom shell assembly;

[0088] 510. Ceramic matrix;

[0089] 600, Ceramic sheet; 610, Ceramic substrate; 620, First through hole; 630, Second through hole; 640, First transparent ceramic sheet; 650, Second transparent ceramic sheet; 660, First annular groove; 670, Second annular groove. Detailed Implementation

[0090] Wearable device 1000 refers to a portable device that can be worn on a user's body, shoes, clothing, or other accessories. Wearable device 1000 can be used independently or in conjunction with a mobile terminal. For example, wearable device 1000 can be an electronic product such as a smartwatch, watch, smart bracelet, or wristband. In this embodiment of the application, a smartwatch is used as an example of wearable device 1000 for illustration.

[0091] Figure 1 This is a partial exploded view of a wearable device 1000. The wearable device 1000 includes a watch face and a watch band (not shown) connected to the watch face. (See reference...) Figure 1 The dial includes at least a top cover 410, a ceramic bottom cover 420, and a wireless charging coil 430. The top cover 410 is placed on the ceramic bottom cover 420 and is fastened to the ceramic bottom cover 420. The top cover 410 and the ceramic bottom cover 420 define a cavity. The wireless charging coil 430 is located in the cavity and is used to realize the wireless charging function of the wearable device 1000.

[0092] In related technologies, the wearable device 1000 also includes a plastic inner shell 150. The wireless charging coil 430 is located between the ceramic base cover 420 and the plastic inner shell 150 and is clamped by the plastic inner shell 150 and the ceramic base cover 420. However, since the wireless charging coil 430 is a conductive coil made of wound metal wire, the thickness of the wireless charging coil 430 is relatively large. This increases the thickness of the component formed after the wireless charging coil 430, the ceramic base cover 420, and the plastic inner shell 150 are assembled, thus increasing the overall thickness of the wearable device 1000 and reducing the user experience. In addition, the presence of the wireless charging coil 430 reduces the bonding force between the plastic inner shell 150 and the ceramic base cover 420, which affects the waterproof performance of the wearable device 1000. In addition, in order to improve the charging efficiency of the wireless charging coil 430, a nanocrystalline film 130 can be covered on the surface of the wireless charging coil 120. Since the nanocrystalline film 130 is located between the wireless charging coil 430 and the plastic inner shell 150, it cannot be directly injection molded on the inner side of the ceramic base shell 110 to form a plastic inner shell 150 with an integral structure of the ceramic base shell 110, which limits the processing technology of the plastic inner shell 150.

[0093] In view of this, embodiments of this application provide a wearable device 1000, which includes at least a housing 100. The housing 100 may include a ceramic base shell 110, a charging coil 120, and a plastic inner shell 150. The charging coil 120 is disposed on the inner side of the ceramic base shell 110, and the plastic inner shell 150 covers the surface of the charging coil 120 and is securely connected to the ceramic base shell 110. In embodiments of this application, the thickness of the housing 100 can be reduced by reducing the thickness of at least one of the following: reducing the thickness of the ceramic base shell 110, reducing the thickness of the charging coil 120, and reducing the thickness of the plastic inner shell 150. In addition, by providing a protective film 140 on the surface of the nanocrystalline film 130, nano-injection molding can be performed on the surface of the protective film 140. During the injection molding process, the protective film 140 can prevent the nanocrystalline film 130 from being damaged by the high-temperature and high-pressure plastic liquid, thereby forming a plastic inner shell 150 that is integral with the protective film 140 and the ceramic base shell 110. This arrangement helps to improve the bonding force between the ceramic shell 100 and the plastic inner shell 150, and also reduces the thickness of the plastic inner shell 150, which helps to further reduce the thickness of the shell 100.

[0094] The methods for reducing the thickness of the housing 100 may include, but are not limited to, the following: 1. Reducing the thickness of one of the following: the ceramic base shell 110, the charging coil 120, or the plastic inner shell 150. 2. Simultaneously reducing the thickness of both the ceramic base shell 110 and the charging coil 120. 3. Simultaneously reducing the thickness of both the charging coil 120 and the plastic inner shell 150. 4. Simultaneously reducing the thickness of both the ceramic base shell 110 and the plastic inner shell 150. 5. Simultaneously reducing the thickness of all three: the ceramic base shell 110, the charging coil 120, and the plastic inner shell 150.

[0095] The wearable device 1000 provided in this application embodiment may further include a conductive component. The charging coil 120 can be electrically connected to the host circuit of the wearable device 1000 through the conductive component, thereby enabling wireless charging of the wearable device 1000. The conductive component may be a structure such as conductive silicone or a spring, and is not specifically limited herein.

[0096] The following describes one type of housing 100 and its preparation method provided in the embodiments of this application.

[0097] Figure 2 This is a cross-sectional view of a housing 100 provided in an embodiment of this application. Figure 3 for Figure 2 A partial enlarged view of the embodiment shown. Figure 4 for Figure 3 A magnified view of a portion of point A in the middle.

[0098] See Figures 2-4 As shown, the housing 100 provided in this embodiment includes at least: a charging coil 120, a plastic inner shell 150, a nanocrystalline film 130, and a protective film 140. The charging coil 120 is disposed on the inner side of the ceramic base shell 110, and is a printed coil sintered integrally with the ceramic base shell 110. The printed coil refers to a coil circuit printed on a predetermined area of ​​the inner surface of the ceramic base shell 110 using a printing process. The printed coil enables the wireless charging function of the wearable device 1000. Since the printed coil is a thin printed circuit, its thickness is significantly reduced compared to a wire-wound charging coil 120, thereby reducing the thickness of the housing 100. Sintering the printed coil and the ceramic base shell 110 into an integral structure helps reduce the thickness of the assembled charging coil 120 and ceramic base shell 110, and also improves the bonding strength between the charging coil 120 and the ceramic base shell 110.

[0099] The shape of the charging coil 120 can be flexibly adjusted according to the shape of the inner surface of the ceramic base shell 110. This embodiment does not impose specific limitations; for example, the shape of the charging coil 120 can be circular, square, elliptical, etc. Furthermore, the printing process can be screen printing, pad printing, 3D printing, sticker printing and transfer printing, or photolithography, etc., without specific limitations. It should be noted that the appropriate printing process can be selected according to the usage requirements or the structure of the ceramic base shell 110. For example, when the surface on the ceramic base shell 110 where the coil is arranged is concave or arc-shaped, 3D printing can be used to increase the line density of the charging coil 120; where line density refers to the spacing between adjacent turns of the charging coil 120. Alternatively, to obtain a finer charging coil 120, photolithography can be used to print the charging coil 120.

[0100] See Figure 3 and Figure 4 A nanocrystalline film 130 covers the surface of the charging coil 120 and is securely connected to the charging coil 120. The nanocrystalline film 130 can improve the eddy currents caused by magnetoresistance during electromagnetic induction in the charging coil 120, thereby improving the charging efficiency of the wearable device 1000. In some examples, the nanocrystalline film 130 can be securely connected to the charging coil 120 by adhesive bonding. Furthermore, the shape of the nanocrystalline film 130 can be a circular or polygonal plate structure. The area of ​​the nanocrystalline film 130 can also be greater than or equal to the area of ​​the charging coil 120 to cover the surface of the charging coil 120. The surface of the charging coil 120 is the surface of the charging coil 120 that faces away from the ceramic base shell 110.

[0101] It should be noted that when the area of ​​the nanocrystalline film 130 is larger than the area of ​​the charging coil 120, a gap can be created between the plastic inner shell 150 and the side wall of the charging coil 120 during the process of forming the plastic inner shell 150 by nano-injection molding, so as to prevent the plastic liquid used for nano-injection molding from impacting the charging coil 120.

[0102] See Figure 3 and Figure 4 A protective film 140 covers the surface of the nanocrystalline film 130 and is securely connected to it. The surface of the nanocrystalline film 130 refers to the surface of the nanocrystalline film 130 facing away from the charging coil 120. In some examples, the protective film 140 can be bonded to the nanocrystalline film 130. Of course, the connection method between the protective film 140 and the nanocrystalline film 130 is not limited to bonding. The shape of the protective film 140 can be a circular or polygonal plate structure. For example, in the embodiments of this application, the protective film 140 is an annular plate structure. The area of ​​the protective film 140 can be greater than or equal to the area of ​​the nanocrystalline film 130 to cover the nanocrystalline film 130. Thus, during the nano-injection molding process of forming the plastic inner shell 150, the protective film 140 can prevent the nanocrystalline film 130 from being damaged by the high-temperature and high-pressure plastic liquid, which would prevent the nanocrystalline film 130 from being unable to improve the eddy currents caused by the magnetic reluctance of the charging coil 120 during electromagnetic induction.

[0103] See Figure 3 and Figure 4 A plastic inner shell 150 covers the surface of the protective film 140 and also contacts the inner side of the ceramic base shell 110. Furthermore, the plastic inner shell 150 is formed on the inner side of the ceramic base shell 110 and covers the surface of the protective film 140 through nano-injection molding, making the plastic inner shell 150, protective film 140, and ceramic base shell 110 a single integrated structure. The surface of the protective film 140 refers to the surface of the protective film 140 facing away from the nanocrystalline film 130. Due to the presence of the protective film 140, nano-injection molding can be performed directly on the ceramic base shell 110 to form the plastic inner shell 150, which is an integral structure with the ceramic base shell 110 and the protective film 140. This reduces the thickness of the plastic inner shell 150, thereby reducing the thickness of the outer shell 100, and also improves the bonding strength between the ceramic base shell 110 and the plastic inner shell 150, contributing to improved waterproof performance of the wearable device 1000.

[0104] Understandably, the presence of the protective film 140 also increases the fastening methods between the ceramic base shell 110 and the plastic inner shell 150, so that the ceramic base shell 110 is not limited to being assembled with the plastic inner shell 150 by adhesive bonding.

[0105] In summary, the housing 100 provided in this application embodiment, by using a printed coil as the charging coil 120 and sintering it with the ceramic base shell 110 into an integral structure, and by nano-injection molding a plastic inner shell 150 on the protective film 140 to form an integral structure with the ceramic base shell 110 and the protective film 140, can reduce the thickness of the housing 100 and improve the user experience of the wearable device 1000. On the other hand, it can improve the bonding force between the ceramic base shell 110 and the plastic inner shell 150, which helps to improve the waterproof performance of the wearable device 1000.

[0106] In some feasible implementations, the charging coil 120 can be made of nano-silver paste or conductive ceramic. It should be noted that pure silver has a resistivity of 1.65 x 10⁻⁶. -8 The nano-silver paste and ceramic base shell 110 are firmly bonded together after high-temperature co-firing. The resistivity of the charging coil 120 may be slightly increased, approaching the resistivity of copper (1.7 x 10⁻⁶). -8 Ω. M, adjusting the wire width, thickness, and total length of the charging coil 120 ensures that the designed number of coil turns is achieved within a certain space, while also meeting the resistance value required for wireless charging. For example, the resistance value required for wireless charging is typically no greater than 0.5 ohms. In some examples, the enameled copper wire diameter is 0.25mm, and its cross-sectional area is 0.049mm². 2 If the line width of the charging coil 120 printed with nano silver paste is 0.3 mm, then the thickness of the nano silver paste of 0.16 mm is equivalent to the cross-sectional area of ​​the copper wire and the resistance value of the coil wound with copper wire.

[0107] When the printed coil is made of conductive ceramic, the conductive ceramic serves as the printed coil and is molded in two colors with the ceramic base shell 110. Furthermore, the printed coil is insulated from the ceramic base shell 110 to ensure the normal operation of the charging coil 120. The coil gap of the charging coil 120 can partially fill the ceramic base shell 110, and this portion of the ceramic base shell 110 acts as an insulating layer to achieve insulation between the conductive ceramic and the ceramic base shell 110. It is understood that the conductive ceramic and the ceramic base shell 110 can be sintered to form a single structure.

[0108] Two-color molding, also known as two-shot molding, involves the injection molding of two types of plastic or ceramic materials on a single injection molding machine.

[0109] In some feasible ways, the protective film 140 can be a metal film, or the protective film 140 can be a non-metallic film made of plastic or fiber.

[0110] Figure 5 A cross-sectional view of another ceramic base shell 110 provided in an embodiment of this application.

[0111] In some feasible ways, refer to Figure 5 The inner edge of the ceramic base shell 110 is provided with a snap-fit ​​portion 112, which is used to engage with a mating portion 151 provided on the plastic inner shell 150 (e.g., as described below). Figure 13 (As shown) The snap-fit ​​connection can improve the bonding force between the ceramic base shell 110 and the plastic inner shell 150.

[0112] Continue to refer to Figure 5 The snap-fit ​​portion 112 and the inner side of the ceramic base shell 110 together define the first stepped surface 113, which is used to mate with the plastic inner shell 150, and helps to improve the bonding force between the plastic inner shell 150 and the ceramic base shell 110.

[0113] The specific structure of the snap-fit ​​part 112 is not specifically limited here. For example, if the snap-fit ​​part 112 is a ring structure, the corresponding mating part 151 can be a slot surrounding the plastic inner shell 150, and the snap-fit ​​part 112 is inserted into the slot (for example, as described below). Figure 13 (As shown). Alternatively, the bottom of the ceramic base shell 110 is provided with a plurality of snap-fit ​​portions 112 circumferentially distributed in the axial direction around the ceramic base shell 110. Correspondingly, the side wall of the plastic inner shell 150 is provided with a plurality of mating portions 151, each of which corresponds to one of the snap-fit ​​portions 112. In addition, each of the mating portions 151 can be used to insert the snap-fit ​​portion 112 into a slot.

[0114] The longitudinal section of the snap-fit ​​portion 112 can be semi-circular, semi-elliptical, or polygonal. For example, in this embodiment, the longitudinal section of the snap-fit ​​portion 112 is rectangular. The longitudinal section of the snap-fit ​​portion 112 is parallel to the axial direction of the ceramic base shell 110.

[0115] Figure 6 A cross-sectional view of another ceramic base shell 110 provided in an embodiment of this application.

[0116] In some examples, reference Figure 6 A protrusion 111 extends from the center of the inner side of the ceramic base shell 110. The protrusion 111 and the inner side of the ceramic base shell 110 together define a second stepped surface 118. The second stepped surface 118 is disposed close to the charging coil 120 disposed on the inner side of the ceramic base shell 110. By providing the second stepped surface 118, the position of the charging coil 120 on the inner side of the ceramic base shell 110 can be positioned. On the other hand, it can also increase the contact area between the ceramic base shell 110 and the plastic inner shell 150, which helps to improve the bonding force between the ceramic base shell 110 and the plastic inner shell 150. In addition, it can also prevent the charging coil 120 from being damaged by the plastic injection molding process.

[0117] The specific structure and shape of the protrusion 111 are not specifically limited here. For example, the protrusion 111 can be a ring structure, a circular structure, or even a multi-segment protrusion provided at intervals along the circumferential direction of the ceramic base shell 110.

[0118] It is understood that there may be a gap between the sidewall of the charging coil 120 and the sidewall of the protrusion 111, or the sidewall of the charging coil 120 may be in contact with the sidewall of the protrusion 111; no specific restrictions are imposed here.

[0119] Figure 7 This is a cross-sectional view of a ceramic base shell 110 provided in an embodiment of this application.

[0120] See also some of the possible implementation methods. Figure 7 The ceramic base shell 110 has a through-hole 114 in its center, and the inner wall of the through-hole 114 defines a third stepped surface 115 for mating with the transparent cover plate 300 to meet the usage requirements of the wearable device 1000. The third stepped surface 115 can be used to position the relative positions of the transparent cover plate 300 and the ceramic base shell 110, and can provide a position for mounting the transparent cover plate 300.

[0121] Continue to refer to Figure 7 Along the thickness direction of the ceramic base shell 110, the mounting through hole 114 may include a first hole section and a second hole section coaxially arranged. The diameter of the first hole section is larger than the diameter of the second hole section and together they define a third step surface 115. The first hole section is close to the outer side of the ceramic base shell 110, and the second hole section is close to the inner side of the ceramic base shell 110.

[0122] The transparent cover plate 300 can be made of transparent materials such as glass or sapphire. In addition, the transparent cover plate 300 can be fastened to the ceramic base shell 110 by adhesive bonding.

[0123] It should be noted that in this embodiment, the first step surface 113, the second step surface 118, and the third step surface 115 are all obtained by machining (CNC machining, i.e., machining by machine tools). Therefore, the ceramic bottom shell 110 in this embodiment may have at least one of the first step surface 113, the second step surface 118, and the third step surface 115. Figure 8 A cross-sectional view of another ceramic base shell provided in an embodiment of this application. Figure 9 A cross-sectional view of another ceramic base shell provided in an embodiment of this application. For example, as... Figure 8 As shown, the ceramic base shell 110 has a first stepped surface 113 and a third stepped surface 115. Alternatively, refer to... Figure 9 The ceramic base shell 110 is provided with a first stepped surface 113, a second stepped surface 118 and a third stepped surface 115.

[0124] Figure 10 This is a flowchart illustrating a method for preparing a shell 100 according to an embodiment of this application. Figure 11 for Figure 10 The diagram illustrates the preparation process of the method shown. (Reference) Figure 10 and Figure 11 In the preparation process of this method, the nanocrystalline film 130 is first installed on the charging coil 120, and then the protective film 140 is installed on the nanocrystalline film 130. Of course, the nanocrystalline film 130 and the protective film 140 can also be pre-assembled to form a film assembly, and then the film assembly is assembled with the charging coil 120. Therefore, steps S103 and S104 can be combined into one step.

[0125] The following is about Figure 10 The preparation method shown is described in detail for each step:

[0126] S101, provides a ceramic base shell 110.

[0127] The specific shape of the ceramic back shell 110 can be designed according to the required size of the wearable device 1000. In addition, the ceramic back shell 110 can be set as a flat surface or a curved surface depending on the type of wearable device 1000. The material of the ceramic back shell 110 can be a non-conductive and opaque ceramic material, which can be determined according to the usage requirements. For example, zirconia ceramic material can be used.

[0128] The ceramic base shell 110 can be formed by dry pressing of ceramic powder, sintering to form a plate-shaped ceramic substrate 510, and then machining the ceramic substrate 510 to form the ceramic base shell 110. Alternatively, the ceramic base shell 110 can also be formed by ceramic injection molding to form a plate-shaped ceramic substrate 510, and then machining the ceramic substrate 510 to form the ceramic base shell 110. Of course, the forming methods of the ceramic base shell 110 are not limited to these two.

[0129] The purpose of machining is to form the structural features of the ceramic base shell 110. These features include at least one of a first stepped surface 113, a second stepped surface 118, and a third stepped surface 115. However, the structural features of the ceramic base shell 110 are not limited to the first stepped surface 113, the second stepped surface 118, and the third stepped surface 115. For example, by machining (e.g., CNC machining) the plate-like ceramic substrate 510, the features described above can be formed. Figure 5 The ceramic base shell 110 is shown. Alternatively, the plate-like ceramic substrate 510 can be machined to form the structure described above. Figure 8The ceramic base shell 110 is shown. Alternatively, the plate-like ceramic substrate 510 can be machined to form the structure described above. Figure 9 The ceramic base shell 110 shown.

[0130] S102. A charging coil 120, which is integral with the ceramic base shell 110, is formed on the inner surface of the ceramic base shell 110.

[0131] The shape of the charging coil 120 can be determined according to the shape of the inner surface of the ceramic base shell 110, for example, as described above. Figure 5 The ceramic base shell 110 and the charging coil 120 shown can be circular in shape.

[0132] Since the charging coil 120 is a printed coil, it can be formed at a predetermined position on the ceramic base shell 110 using a printing process.

[0133] The charging coil 120 and the ceramic base shell 110 are sintered at a predetermined temperature and time to form an integral structure. The predetermined temperature and time can be determined according to the materials of the ceramic base shell 110 and the charging coil 120, and no specific restrictions are imposed here.

[0134] Figure 12 The flowchart of the method for preparing the printed coil provided in the embodiments of this application is as follows. Figure 12 The preparation method shown is described in detail below:

[0135] S1021, Provide conductive paste.

[0136] Specifically, conductive paste refers to a liquid paste that can conduct electricity. For example, conductive paste can be conductive materials such as nano silver paste and conductive ceramics.

[0137] S1022. Conductive paste is coated on the inner surface of ceramic base 110 by printing process to form charging coil 120 on ceramic base 110.

[0138] Specifically, a printed circuit coil of a predetermined shape is printed on the ceramic base 110 using printing equipment to form a charging coil 120 on the inner surface of the ceramic base 110.

[0139] S1023. The ceramic base shell 110 with the charging coil 120 is sintered to form an integral structure with the charging coil 120 and the ceramic base shell 110.

[0140] Specifically, the sintering temperature and time can be determined based on the materials of the ceramic base shell 110 and the charging coil 120, and are not specifically limited here. For example, sintering at 140°C for 4 hours can make the ceramic base shell 110 and the charging coil 120 form an integral structure.

[0141] S103. A nanocrystalline film 130 is coated on the surface of the charging coil 120 having a ceramic base shell 110.

[0142] The shape and thickness of the nanocrystalline film 130 can be determined according to the application and are not specifically limited here. For example, in some examples, the nanocrystalline film 130 is annular in shape, with the outer diameter of the nanocrystalline film 130 being larger than the outer diameter of the charging coil 120 and the inner diameter of the nanocrystalline film 130 being larger than the inner diameter of the charging coil 120, which helps to prevent the plastic inner shell 150 from impacting the charging coil 120.

[0143] The nanocrystalline film 130 can be firmly connected to the charging coil 120 by adhesive bonding. For example, glue can be applied to the nanocrystalline film 130 so that the nanocrystalline film 130 can be attached to the charging coil 120.

[0144] S104. A protective film 140 is applied to the surface of the nanocrystalline film 130 having the charging coil 120 to form the bottom shell assembly 50.

[0145] Continue to refer to Figure 11 The base assembly 50 may include a ceramic base 110, a charging coil 120, a nanocrystalline film 130, and a protective film 140. The protective film 140 may have the same shape as the nanocrystalline film 130; therefore, the protective film 140 may be annular, with its inner diameter and outer diameter equal to those of the nanocrystalline film 130. The protective film 140 may be a metallic or non-metallic film; for example, in some examples, it may be plastic or fiber. The protective film 140 may be bonded to the nanocrystalline film 130 by adhesive bonding; for example, adhesive may be applied to the nanocrystalline film 130 and / or the protective film 140, thereby bonding the nanocrystalline film 130 to the protective film 140.

[0146] S105. The bottom shell assembly 50 with the protective film 140 is placed into the mold for nano-injection molding to form a plastic inner shell 150 with the protective film 140 and the ceramic bottom shell 110 as an integral structure.

[0147] After the bottom shell assembly 50 is placed into the mold, the outer surface of the ceramic bottom shell 110 of the bottom shell assembly 50 contacts the mold. During the nano-injection molding process, the liquid plastic will impact the ceramic bottom shell 110 and the protective film 140 along the thickness direction of the bottom shell assembly 50. Due to the presence of the protective film 140, the nanocrystalline film 130 will not be damaged by the liquid plastic. After nano-injection molding, a plastic inner shell 150 with the ceramic bottom shell 110 and the protective film 140 will be formed.

[0148] The specific shape of the plastic inner shell 150 can be determined according to the type and internal layout of the wearable device 1000, and no specific restrictions are imposed here. In addition, the material of the plastic inner shell 150 can be determined according to the usage requirements, and no specific restrictions are imposed here.

[0149] Nano-injection molding refers to nano-molding technology (NMT), which involves first nano-treating the metal surface, then directly injecting plastic onto the metal surface to obtain an integrated plastic and metal structure. In this application, nano-injection molding is used to allow the plastic inner shell 150 to be directly molded onto the bottom shell assembly 50 and form an integrated structure with the bottom shell assembly 50.

[0150] In this embodiment, a printed coil is used as the charging coil 120 and co-fired with the ceramic base shell 110 to form an integral structure. In addition, by setting a protective film 140, nano-injection molding can be performed on the surface of the protective film 140 to form a plastic inner shell 150 that is integral with the ceramic base shell 110 and the protective film 140. This arrangement can reduce the thickness of the shell 100 on the one hand, and improve the bonding force between the ceramic base shell 110 and the plastic inner shell 150 on the other hand.

[0151] The following describes another housing 100 provided in the embodiments of this application and the method for preparing the housing 100.

[0152] Figure 13 A partial cross-sectional view of another housing 100 provided in an embodiment of this application.

[0153] refer to Figure 13 Another housing 100 provided in this application embodiment includes at least: a ceramic bottom shell 110, a charging coil 120, a nanocrystalline film 130, a protective film 140, and a plastic inner shell 150. Figure 13 The housing 100 shown is Figure 3 The same parts of the housing 100 shown will not be described again here. Figure 13 The housing 100 shown is Figure 3The differences between the shown shell 100 are: the structure of the ceramic bottom shell 110, the structure of the plastic inner shell 150, and the ceramic bottom shell 110 in this embodiment is formed by hot bending of a ceramic sheet 600. Hot bending refers to first heating the ceramic sheet 600, and then bending the ceramic sheet 600 to change its shape to a predetermined shape.

[0154] Since the ceramic base shell 110 is manufactured using a hot bending forming process, the thickness of the ceramic sheet 600 can be reduced, thereby reducing the thickness of the ceramic base shell 110, and consequently, the thickness of the shell 100. Therefore, the hot bending process reduces both the thickness of the ceramic sheet 600 and the thickness of the ceramic base shell 110. It should be noted that the thickness of the ceramic base shell 110 refers to the distance between the top and bottom surfaces of the ceramic base shell 110.

[0155] The material, structure and shape of the charging coil 120 have been described in detail above and will not be repeated here. In addition, it should be emphasized that in this embodiment, the charging coil 120 is fastened to the inner side of the ceramic base shell 110.

[0156] In this embodiment, the charging coil 120 can be a printed coil or a conductive coil made of metal wire. The conductive coil can also be called an enameled conductive coil, meaning the charging coil 120 is made of enameled wire. In other words, the metal wire can be called enameled wire; for example, in some examples, the metal wire is copper wire. Furthermore, the conductive coil can be fixed to the inner surface of the ceramic base 110 by adhesive bonding. Of course, the method of fixing the conductive coil to the ceramic base 110 is not limited to adhesive bonding.

[0157] It should be noted that when the charging coil 120 is a printed coil, the printed coil and the ceramic base shell 110 can be sintered into a single structure, or the printed coil and the ceramic base shell 110 can be tightly connected but not into a single structure.

[0158] The structure and fit of the nanocrystalline film 130, the protective film 140, and the plastic inner shell 150 have been described in detail above and will not be described in detail here.

[0159] It should be noted that, Figure 13The housing 100 in this embodiment has a nanocrystalline film 130 and a protective film 140. However, in this embodiment, the housing 100 can also have the nanocrystalline film 130 and the protective film 140 removed. In this case, the plastic inner shell 150 covers the surface of the charging coil 120 and contacts the inner side of the ceramic base shell 110, and the plastic inner shell 150 is firmly connected to the ceramic base shell 110. Alternatively, the plastic inner shell 150 can be firmly connected to the ceramic base shell 110 by adhesive bonding. Of course, the connection method between the plastic inner shell 150 and the ceramic base shell 110 is not limited to adhesive bonding. For example, the plastic inner shell 150 can also be an integral structure with the ceramic base shell 110. The firm connection between the plastic inner shell 150 and the ceramic base shell 110 can clamp the charging coil 120, which helps to further improve the connection strength between the charging coil 120 and the ceramic base shell 110.

[0160] In this embodiment, the structure of the hot-bent ceramic base shell 110 can be as described above. Figures 5-9 The ceramic base shell 110 shown, therefore, the hot-bent ceramic base shell 110 has at least one of the following stepped surfaces: a first stepped surface 113, a second stepped surface 118, and a third stepped surface 115. For example, Figure 13 As shown, the ceramic base shell 110 has a first stepped surface 113, a second stepped surface 118, and a third stepped surface 115. Of course, the structure of the hot-bent ceramic base shell 110 can also be the same as... Figure 3 The structure of the ceramic base shell 110 is the same, that is, the first step surface 113, the second step surface 118 and the third step surface 115 may not be provided on the hot-bent ceramic base shell 110.

[0161] To meet the light transmission requirements of the wearable device 1000, a mounting through hole 114 is provided in the middle of the ceramic base shell 110, and the inner wall of the mounting through hole 114 defines a third stepped surface 115, so that the transparent cover plate 300 can be installed on the ceramic base shell 110. However, in addition to the method of providing a mounting through hole 114 on the ceramic base shell 110 to install the transparent cover plate 300, that is, the ceramic base shell 110 and the transparent cover plate 300 are separate structures, the transparent cover plate 300 and the ceramic base shell 110 can also be integrated into one structure.

[0162] The following describes the structure of the ceramic base shell 110, which does not have the through hole 114 installed, but can still meet the light transmission requirements of the wearable device 1000.

[0163] Figure 14 A partial perspective view of another housing 100 provided in the embodiments of this application. Figure 15 for Figure 14 The front view of the casing is shown. (Reference) Figure 14 and Figure 15 The ceramic base shell 110 may include a connecting portion 116 and a transparent portion 117. (Referring to...) Figure 18 The charging coil 120 is mounted on the inner side of the connecting part 116. The connecting part 116 is made of opaque ceramic material, while the transparent part 117 is made of transparent ceramic and is sintered with the connecting part 116 into a single structure. This configuration allows for the formation of a complete two-color integrated ceramic base shell 110 and reduces the cost of the ceramic base shell 110. Here, "two-color integrated" refers to two-shot integrated molding, which is the same concept as the two-color molding described above.

[0164] Compared to using a transparent cover plate 300 to achieve light transmission, applying transparent ceramic to the areas of the ceramic base 110 that require light transmission, and co-firing it with opaque ceramic to form a single integrated structure, allows for a seamless structure and improves the aesthetics of the ceramic base 110. Since transparent ceramic is used in the areas of the ceramic base 110 that require light transmission, the transparent cover plate 300 can be eliminated, simplifying the assembly process of the housing 100 and reducing its cost. Furthermore, because the connecting part 116 and the transparent part 117 are an integrated structure, their bonding strength is high, making it less likely for the transparent part 117 to detach from the connecting part 116.

[0165] It should be noted that the materials of the transparent part 117 and the connecting part 116 can be determined according to the application requirements, and no specific restrictions are imposed here. In addition, the connecting part 116 can be a flat surface or an arc-shaped surface, and the transparent part 117 can also be a flat surface or an arc-shaped surface.

[0166] The specific shape of the transparent portion 117 can be determined according to the light transmission requirements, and no specific limitation is made here. For example, in some examples, refer to Figure 14 and Figure 15 The transparent portion 117 includes a first transparent portion 1171 and an annular second transparent portion 1172. The first transparent portion 1171 is located within the second transparent portion 1172, and an annular gap for accommodating a portion of the connecting portion 116 is defined between the first transparent portion 1171 and the second transparent portion 1172. The connecting portion 116 includes a first connecting portion 1161 having a through hole in the middle and a second connecting portion 1162 with an annular structure. The first transparent portion 1171 is located within the second connecting portion 1162. The second connecting portion 1162 is located within the first transparent portion 1171 and the second transparent portion 1172. The second transparent portion 1172 is located within the through hole of the first connecting portion 1161 and is securely connected to the first connecting portion 1161.

[0167] It should be noted that the ceramic base shell 110, defined by the connecting portion 116 and the transparent portion 117, can also be as follows: Figure 5 and Figure 6Like the ceramic base shell 110 shown, it has at least one of a first stepped surface 113 and a second stepped surface 118. For example, at least one of the first stepped surface 113 and the second stepped surface 118 may be provided on the inner side of the connecting portion 116, without specific limitation. Figure 15 The inner side of the first connecting part 1161 is provided with a first stepped surface 113 and a second stepped surface 118. Of course, the first stepped surface 113 and the second stepped surface 118 may not be provided on the ceramic base shell 110 formed by the connecting part 116 and the transparent part 117.

[0168] In summary, since the ceramic base shell 110 of this embodiment is manufactured by hot bending, a thinner ceramic sheet 600 can be used. Therefore, by using a thinner ceramic sheet 600 to manufacture the ceramic base shell 110, the thickness of the ceramic base shell 110 can be reduced, thereby reducing the thickness of the housing 100. Furthermore, since the housing 100 of this embodiment can also use a printed coil as the charging coil 120, and / or perform nano-injection molding on the protective film 140 to form a plastic inner shell 150 that is integrally formed with the protective film 140 and the ceramic base shell 110, the thickness of the housing 100 can be further reduced. Additionally, the ceramic base shell 110 of this embodiment can also be made of transparent ceramic and non-transparent ceramic, which can improve the aesthetics of the ceramic base shell 110.

[0169] Figure 16 A flowchart illustrating another method for preparing the shell 100 provided in this application embodiment. Figure 17 for Figure 16 The schematic diagram of the preparation process of the preparation method shown is for reference. Figure 16 and Figure 17 The hot-bent ceramic base shell 110 can be assembled with the charging coil 120 and the plastic inner shell 150.

[0170] The following is about Figure 16 The preparation method shown is described in detail for each step:

[0171] S201. Prepare a hot-bent ceramic base shell 110.

[0172] Because the stepped ceramic sheet 600 undergoes hot bending, the stepped surface structure on its upper plane becomes a three-dimensional stepped structure. Compared to machining a three-dimensional stepped structure from a blank without steps in related technologies, this saves a significant amount of machining time and helps improve the production efficiency of the ceramic base shell 110. Furthermore, the hot bending process reduces the thickness of the ceramic base shell 110, while still maintaining sufficient strength to meet usage requirements.

[0173] Since the ceramic base shell 110 has a stepped structure, the preparation method of the ceramic base shell 110 may include the following: Figure 18 This is a flowchart illustrating a method for preparing a hot-bent ceramic base shell 110 according to an embodiment of this application. (Refer to...) Figure 18 A first method for preparing a hot-bent ceramic base shell 110 includes the following steps: S2011, providing a ceramic sheet 600 of uniform thickness; S2012, preparing a stepped structure on the ceramic sheet 600; S2013, hot-bending the ceramic sheet 600 with the stepped structure to form the ceramic base shell 110. Alternatively, a second method for preparing the hot-bent ceramic base shell 110 involves first obtaining a ceramic sheet 600 of uniform thickness with a stepped structure through ceramic injection molding, and then hot-bending the ceramic sheet 600 to form the ceramic base shell 110. Of course, the forming process for preparing the hot-bent ceramic base shell 110 is not limited to the two methods described above.

[0174] The following is about Figure 18 The preparation method shown is described in detail below:

[0175] S2011, Provides ceramic sheets of equal thickness 600.

[0176] Specifically, the ceramic sheet 600 has a plate-like structure, and the thickness of the ceramic sheet 600 can be determined according to the thickness of the ceramic base shell 110. For example, the thickness of the ceramic sheet 600 can be within 0.4 cm. In addition, the appropriate type of ceramic sheet 600 can be selected according to whether there is a third stepped surface 115 on the ceramic base shell 110.

[0177] When the ceramic base shell 110 has a third step surface 115, the ceramic sheet 600 is an opaque ceramic material. The ceramic sheet 600 can be a thin sheet with the same wall thickness obtained by processes such as ceramic casting, injection molding, gelation or dry pressing.

[0178] When the ceramic base shell 110 does not have a third step surface 115, since the area on the ceramic base shell 110 that needs to transmit light is made of transparent ceramic, a ceramic sheet 600 with transparent ceramic and equal wall thickness is used.

[0179] The method for preparing a ceramic sheet 600 with transparent ceramic and equal wall thickness can be as follows: sintering transparent ceramic and opaque ceramic to form a ceramic sheet 600 with equal wall thickness in an integral structure. Figure 19 This is a flowchart illustrating a method for preparing a ceramic sheet 600 with transparent ceramic components, as provided in an embodiment of this application. Figure 20 for Figure 19 The schematic diagram of the preparation process of the preparation method shown is for reference. Figure 19 and Figure 20The preparation of a ceramic sheet 600 with transparent ceramic and uniform thickness includes the following steps:

[0180] S20111, providing a non-transparent ceramic substrate 610, a circular first transparent ceramic sheet 640, and an annular second transparent ceramic sheet 650.

[0181] Specifically, the ceramic substrate 610 can be a circular or polygonal plate-like structure, which can be determined according to the type of wearable device 1000, and is not specifically limited here. The transparent ceramic sheet 600 refers to a ceramic sheet 600 that is translucent to meet the light transmission requirements of the wearable device 1000. The first transparent ceramic sheet 640 can be circular, or it can be polygonal, elliptical, or other shapes. The second transparent ceramic sheet 650 can be an elliptical, circular, or polygonal ring structure; for example, in this embodiment, the second transparent ceramic sheet 650 is a ring.

[0182] S20112, A first through hole 620 penetrating through the ceramic substrate 610 and an annular second through hole 630 are formed, wherein the first through hole 620 is located within the second through hole 630.

[0183] The shape of the first through hole 620 is the same as the shape of the first transparent ceramic sheet 640, so that the ceramic substrate 610 and the first transparent ceramic sheet 640 form an integral structure after sintering. Similarly, the shape of the second through hole 630 is the same as the shape of the second transparent ceramic sheet 650, so that the ceramic substrate 610 and the second transparent ceramic sheet 650 form an integral structure after sintering.

[0184] It should be noted that the first through hole 620 can be formed first, and then the second through hole 630 can be formed; or the second through hole 630 can be formed first, and then the first through hole 620 can be formed; or the first through hole 620 and the second through hole 630 can be formed simultaneously.

[0185] S20113. Fill the first through hole 620 with the first transparent ceramic sheet 640.

[0186] S20114. Fill the second through hole 630 with the second transparent ceramic sheet 650.

[0187] In this embodiment, step S20113 is executed first, and step S20114 is executed later. It can be understood that step S20114 can also be executed first, and step S20113 can be executed later, or steps S20113 and S20114 can be executed simultaneously.

[0188] S20115, The first transparent ceramic sheet 640, the second transparent ceramic sheet 650 and the ceramic substrate 610 are sintered to form a ceramic sheet 600 with an integral structure.

[0189] The sintering temperature and time for the first transparent ceramic sheet 640, the second transparent ceramic sheet 650, and the ceramic substrate 610 can be determined based on the materials of the first transparent ceramic sheet 640, the second transparent ceramic sheet 650, and the ceramic substrate 610, and are not specifically limited here. Furthermore, after step S20115 is completed, step S2012 is performed.

[0190] S2012. A stepped structure is prepared on ceramic sheet 600.

[0191] Specifically, the step structure may include at least one of the following step surfaces: a first step surface 113, a second step surface 118, and a third step surface 115. The specific number of step surfaces included in the step structure can be determined according to usage requirements and is not specifically limited here. In some examples, Figure 21 This is a schematic diagram illustrating the fabrication process of a stepped structure according to an embodiment of this application. (Refer to...) Figure 20 The stepped structure includes a first step surface 113, a second step surface 118, and a third step surface 115. Additionally, Figure 21 The method for preparing the stepped structure shown may include the following steps:

[0192] Step A: A first annular groove 660 is formed on the bottom surface of the ceramic sheet 600. The inner wall of the first annular groove 660 forms a first step surface 113 and a second step surface 118 spaced apart in the radial direction. The second step surface 118 is set close to the axis of the first annular groove 660. Step B: A mounting through hole 114 is formed through the ceramic sheet 600. The mounting through hole 114 is located inside the first annular groove 660 and close to the second step surface 118. The inner wall of the mounting through hole 114 forms a third step surface 115.

[0193] In step A, the specific shape of the first annular groove 660 can be determined according to the shape of the ceramic base shell 110, the shape of the first step surface 113 and the shape of the second step surface 118. For example, in some examples, the first annular groove 660 is a circular groove.

[0194] It should be noted that the order of steps A and B can be interchanged, that is, step B can be performed first and then step A. Of course, steps A and B can also be performed simultaneously.

[0195] In some examples, when the ceramic sheet 600 has transparent ceramic, the stepped structure includes a first stepped surface 113 and a second stepped surface 118. Therefore, the method for preparing the stepped structure may include the following steps: Step C, forming a second annular groove 670 on the bottom surface of the ceramic sheet 600, the inner wall of the second annular groove 670 forming a first stepped surface 113 and a second stepped surface 118 spaced apart in the radial direction, the second stepped surface 118 being disposed close to the axis of the second annular groove 670. Figure 22A schematic diagram illustrating the fabrication process of another stepped structure provided in this application embodiment, referencing... Figure 22 This allows for the production of ceramic sheets 600 that do not have a third step surface 115 and are of uniform thickness. The specific shape of the second annular groove 670 can be determined based on the shape of the ceramic base shell 110 and the shapes of the first step surface 113 and the second step surface 118. For example, in some examples, the second annular groove 670 is a circular groove.

[0196] S2013. The ceramic sheet 600 with a stepped structure is hot-bent to form a ceramic base shell 110.

[0197] Figure 23 This is a schematic diagram illustrating the hot pressing process of a ceramic sheet 600 with a stepped structure, as provided in an embodiment of this application. (Refer to...) Figure 23 By hot bending, the planar step structure on the ceramic sheet 600 can be transformed into a three-dimensional step structure to meet the application requirements. Compared with the machining of three-dimensional step structures in related technologies, the machining time is greatly reduced. In addition, a thinner ceramic sheet 600 can be used to reduce the thickness of the ceramic base shell 110.

[0198] S202, Install the charging coil 120 on the inner surface of the ceramic base shell 110.

[0199] Different processing methods are selected for the charging coil 120 to mount it on the inner surface of the ceramic base shell 110. For example, when the charging coil 120 is a conductive coil, it can be directly bonded to the inner surface of the ceramic base shell 110 by adhesive bonding. Alternatively, when the charging coil 120 is a printed coil, it can be formed on the inner surface of the ceramic base shell 110 using a printing process. The printed coil can be integrally formed with the ceramic base shell 110 through a sintering process, or it can be left unsintered.

[0200] For example, the method for preparing a printed coil integrally formed with the ceramic base shell 110 on the inner surface of the hot-bent ceramic base shell 110 can be as described above. Figure 12 The fabrication method described above will not be elaborated further here. It should be noted that when the printed coil does not need to be integrally formed with the ceramic base shell 110, it can be removed... Figure 12 Step S1023 can be performed. Alternatively, after the charging coil 120 is formed on the ceramic base shell 110 by printing, the charging coil 120 can be quickly cured on the inner surface of the ceramic base shell 110 by drying.

[0201] S203. Cover the surface of the charging coil 120 with the plastic inner shell 150 and secure it to the ceramic bottom shell 110.

[0202] Since the plastic inner shell 150 covers the charging coil 120, the plastic inner shell 150 is manufactured before being assembled with the charging coil 120. In addition, the plastic inner shell 150 can be fastened to the inner side of the ceramic base shell 110 by adhesive bonding. Of course, the connection method between the plastic inner shell 150 and the ceramic base shell 110 is not limited to adhesive bonding.

[0203] In this embodiment, in order to improve the efficiency of the charging coil 120, a nanocrystalline film 130 can be covered on the surface of the charging coil 120. Therefore, before the plastic inner shell 150 is assembled with the charging coil 120 and the ceramic bottom shell 110, the nanocrystalline film 130 is installed on the surface of the charging coil 120 before step S203 is performed.

[0204] In this embodiment, in order to reduce the thickness of the plastic inner shell 150, after step S202 is completed, a protective film 140 can be covered on the surface of the charging coil 120. Then, the ceramic bottom shell 110 with the protective film 140 and the charging coil 120 is placed into the mold for nano-injection molding. During the injection molding process, the plastic inner shell 150 is formed, and the plastic inner shell 150, the protective film 140 and the ceramic bottom shell 110 form an integral structure.

[0205] Of course, the protective film 140 and the nanocrystalline film 130 can coexist. In this embodiment, the method for preparing the shell 100 with the protective film 140 and the nanocrystalline film 130 is as follows: firstly, Figure 16 In steps S201 and S202, after step S202 is completed, proceed with... Figure 10 Steps S103, S104, and S105 in the process.

[0206] In the description of the embodiments of this application, it should be noted that, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to a fixed connection, an indirect connection through an intermediate medium, or the internal communication of two components or the interaction between two components. Those skilled in the art can understand the specific meaning of the above terms in the embodiments of this application according to the specific circumstances.

[0207] The devices or elements referred to in the embodiments of this application or implied herein must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be construed as limiting the embodiments of this application. In the description of the embodiments of this application, "a plurality of" means two or more, unless otherwise precisely specified.

[0208] The terms "first," "second," "third," "fourth," etc. (if present) in the specification, claims, and accompanying drawings of this application are used to distinguish similar objects and are not necessarily used to describe a specific order or sequence. It should be understood that such data can be interchanged where appropriate so that embodiments of the present application described herein can be implemented, for example, in orders other than those illustrated or described herein. Furthermore, the terms "comprising" and "having," and any variations thereof, are intended to cover non-exclusive inclusion; for example, a process, method, system, product, or apparatus that comprises a series of steps or units is not necessarily limited to those explicitly listed, but may include other steps or units not explicitly listed or inherent to such processes, methods, products, or apparatus.

[0209] The term "multiple" in this article refers to two or more. The term "and / or" in this article is merely a description of the relationship between related objects, indicating that three relationships can exist. For example, A and / or B can represent: A alone, A and B simultaneously, or B alone. Furthermore, the character " / " in this article generally indicates an "or" relationship between the preceding and following related objects; in formulas, the character " / " indicates a "division" relationship between the preceding and following related objects.

[0210] It is understood that the various numerical designations used in the embodiments of this application are merely for descriptive convenience and are not intended to limit the scope of the embodiments of this application.

[0211] It is understood that, in the embodiments of this application, the order of the above-mentioned process numbers does not imply the order of execution. The execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of this application.

Claims

1. A housing, characterized in that, It includes at least: a ceramic base shell, a charging coil, a plastic inner shell, a nanocrystalline film, and a protective film; The charging coil is disposed on the inner side of the ceramic base shell, and the charging coil is a printed coil and is sintered with the ceramic base shell as an integral structure. The nanocrystalline film covers the surface of the charging coil and is securely connected to the charging coil. The area of ​​the nanocrystalline film is larger than the area of ​​the charging coil, so that there is a gap between the plastic inner shell and the side wall of the charging coil. The protective film covers the surface of the nanocrystalline film and is securely connected to the nanocrystalline film. The area of ​​the protective film is greater than or equal to the area of ​​the nanocrystalline film. The protective film is used to prevent damage to the nanocrystalline film during the injection molding process of forming the plastic inner shell. The plastic inner shell is formed on the inner side of the ceramic bottom shell by nano-injection molding and covers the protective film, so that the plastic inner shell, the ceramic bottom shell and the protective film are integrated into one structure.

2. The housing according to claim 1, characterized in that, The ceramic base shell is formed by hot bending of ceramic sheets.

3. The housing according to claim 1 or 2, characterized in that, The plastic inner shell is provided with a mating part, and the inner side edge of the ceramic bottom shell is provided with a snap-fit ​​part, which snaps into the mating part; wherein, the charging coil is provided on the inner side of the ceramic bottom shell.

4. The housing according to claim 3, characterized in that, The snap-fit ​​portion and the inner side of the ceramic base shell together define a first stepped surface, and the mating portion is a slot for the snap-fit ​​portion to be inserted.

5. The housing according to any one of claims 1-4, characterized in that, A protrusion is provided extending from the middle of the inner side surface of the ceramic base shell, and the protrusion and the inner side surface of the ceramic base shell together define a second stepped surface. The charging coil is disposed on the inner side of the ceramic base and close to the second stepped surface.

6. The housing according to any one of claims 1-5, characterized in that, The housing further includes: a transparent cover plate; the ceramic bottom shell has a through hole in the middle, the inner wall of the through hole defines a third step surface, and the transparent cover plate is installed on the third step surface.

7. The housing according to any one of claims 1-5, characterized in that, The ceramic base shell includes a connecting part and a transparent part; The connecting part is made of opaque ceramic material, and the transparent part is made of transparent ceramic and is sintered with the connecting part into a single structure.

8. The housing according to claim 7, characterized in that, The transparent portion includes a first transparent portion and an annular second transparent portion; The first transparent portion is located within the second transparent portion, and the first transparent portion and the second transparent portion together define an annular gap for accommodating a portion of the connecting portion.

9. The housing according to any one of claims 1-8, characterized in that, The printed coil is made of nano silver paste or conductive ceramic. When the material of the printed coil is the conductive ceramic, the printed coil is insulated from the ceramic base and sintered into a single structure with the ceramic base.

10. The housing according to claim 9, characterized in that, The protective film is a metal film, or it is a non-metallic film made of plastic or fiber.

11. A wearable device, characterized in that, The device includes a conductive element and a housing as described in any one of claims 1-10, wherein the charging coil of the housing is electrically connected to the host circuit of the wearable device via the conductive element.

12. The wearable device according to claim 11, characterized in that, The conductive component is conductive silicone or a spring.

13. A method for preparing a shell, characterized in that, include: Provide conductive paste; The conductive paste is coated onto the inner surface of the ceramic base shell using a printing process to form a charging coil on the ceramic base shell. The ceramic base shell having the charging coil is sintered to form an integral structure of the charging coil and the ceramic base shell; A nanocrystalline film is coated on the surface of the charging coil having the ceramic base shell; A protective film is applied to the surface of the nanocrystalline film having the charging coil to form a bottom shell assembly; The bottom shell assembly with the protective film is placed into a mold for nano-injection molding to form a plastic inner shell that is integral with the protective film and the ceramic bottom shell. The area of ​​the nanocrystalline film is larger than the area of ​​the charging coil, so that there is a gap between the plastic inner shell and the side wall of the charging coil; the area of ​​the protective film is greater than or equal to the area of ​​the nanocrystalline film.

14. The preparation method according to claim 13, characterized in that, The conductive paste is either nano-silver paste or conductive ceramic.

15. The preparation method according to claim 13 or 14, characterized in that, The printing process includes any one of the following processes: screen printing, pad printing, 3D printing, sticker printing, and photolithography.

16. The preparation method according to any one of claims 13-15, characterized in that, Before forming the charging coil, which is integral with the ceramic base shell, on the inner surface of the ceramic base shell, the method further includes: Prepare a ceramic base shell that has been hot-bent.

17. The preparation method according to claim 16, characterized in that, The preparation of the hot-bent ceramic bottom shell includes: Ceramic sheets of equal thickness are available; A stepped structure is prepared on the ceramic sheet; The ceramic sheet having the stepped structure is subjected to a hot bending process to form the ceramic base shell.

18. The preparation method according to claim 17, characterized in that, The step structure fabrication on the ceramic sheet includes: A first annular groove is formed on the bottom surface of the ceramic sheet. The inner wall of the first annular groove is formed with a first step surface and a second step surface that are spaced apart in the radial direction. The second step surface is arranged close to the axis of the first annular groove. A mounting through hole is formed through the ceramic sheet. The mounting through hole is located within the first annular groove and is set close to the second step surface. The inner wall of the mounting through hole forms a third step surface.

19. The preparation method according to claim 17, characterized in that, The step structure fabrication on the ceramic sheet includes: A second annular groove is formed on the bottom surface of the ceramic sheet. The inner wall of the second annular groove forms a first step surface and a second step surface that are spaced apart in the radial direction. The second step surface is arranged close to the axis of the second annular groove.

20. The preparation method according to claim 17, characterized in that, The provision of ceramic sheets of uniform thickness includes: It provides a non-transparent ceramic substrate, a circular first transparent ceramic sheet, and an annular second transparent ceramic sheet; A first through-hole penetrating the ceramic substrate and an annular second through-hole are formed, wherein the first through-hole is located within the second through-hole; The first transparent ceramic sheet is filled into the first through hole; The second transparent ceramic sheet is filled into the second through hole; The first transparent ceramic sheet, the second transparent ceramic sheet, and the ceramic substrate are sintered to form the ceramic sheet with an integral structure.

Citation Information

Patent Citations

  • Mobile phone back housing capable of realizing wireless charging and preparation method thereof

    CN105162908A

  • Shell assembly, preparation method thereof and electronic equipment

    CN114478001A

  • Electronic product having wireless charging function and shell of electronic product

    CN204408794U