High-toughness low-w no-co martensitic heat-resistant steel and manufacturing method thereof
Patent Information
- Application Number
- CN202311647312.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-04
- Publication Date
- 2026-11-03
- Estimated Expiration
- 2043-12-04
AI Technical Summary
When existing martensitic heat-resistant steels operate at high temperatures for extended periods, the Fe2W Laves phase precipitates in large quantities, causing coarsening and reducing material stability and service life. At the same time, the addition of Co increases costs.
By employing a low-W and Co-free alloy design, combined with forging and solution tempering, the precipitation and coarsening of M23C6 carbides and Laves phase are controlled. Through reasonable element content and heat treatment processes, the high-temperature strength and toughness of the material are improved.
At temperatures above 650℃, the material exhibits high structural stability and thermal strength, reducing the cost of using alloying elements and extending its service life.
Smart Images

Figure CN117660839B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of martensitic heat-resistant steel, and particularly relates to a high-strength, high-toughness, low-W, Co-free martensitic heat-resistant steel and its manufacturing method. Background Technology
[0002] Currently, the 600°C USC power generation technology is widely used in commercial thermal power plants worldwide. Vigorously promoting the construction of USC demonstration power plants with temperatures of 650°C and above is an urgent need for the development of global thermal power plant construction at this stage. USC units, especially large-diameter boiler pipes, operate under complex and harsh environments, placing more stringent requirements on the high-temperature strength and oxidation and corrosion resistance of materials.
[0003] Currently, martensitic heat-resistant steels such as MARBN, T / P9 series, SAVE12AD, and G115 are widely used in commercial applications. To improve their thermal strength, these martensitic heat-resistant steels generally replace Mo with W and add Co. However, due to the large amount of W added, after prolonged operation at 650℃, a large amount of Fe2W Laves phase precipitates and coarsens rapidly, affecting the stable service of the material and even causing premature failure. On the other hand, insufficient W content leads to a sharp decrease in the high-temperature strength of the material, making it impossible to balance strength and toughness after prolonged high-temperature operation. The addition of Co significantly increases raw material costs and reduces economic viability. Summary of the Invention
[0004] To address the aforementioned issues, this invention provides a high-strength, high-toughness, low-W, Co-free martensitic heat-resistant steel, which exhibits high structural stability and thermal strength at temperatures above 650°C.
[0005] The technical objective of this invention is achieved through the following means.
[0006] This high-strength, high-toughness, low-W, and Co-free martensitic heat-resistant steel has the following chemical composition by mass percentage: C: 0.04–0.08, Cr: 8.0–9.5, Mo: 0.3–0.8, W: 0.5–1.2, V: 0.2–0.35, Nb: 0.02–0.06, Mn: 0.75–1.0, Ni: 1.0–2.0, Si: 0.9–1.3, N: 0.005–0.02, with the remainder being Fe and unavoidable impurities.
[0007] The manufacturing method of the aforementioned high-strength, high-toughness, low-W, Co-free martensitic heat-resistant steel, through forging and solution tempering, specifically includes the following steps:
[0008] 1) Molten steel is obtained by double vacuum smelting and then cast into ingots;
[0009] 2) Forging the ingot;
[0010] 3) The forged billet is subjected to solution treatment and tempering.
[0011] Furthermore, in step 2), the ingot is preheated before forging, and the preheating temperature is 1080-1150℃. After the ingot is fully heated, the preheating time is ≥16h.
[0012] Furthermore, in step 2), the final forging temperature after forging is 860–920℃, the forging ratio is 2.0–4.0, and the material is water-cooled after forging.
[0013] Furthermore, the solution treatment temperature is 1000–1050℃, the solution holding time is 40–120 min, and the solution is water-cooled after solution treatment. The tempering temperature is 720–780℃, and the tempering holding time is ≥60 min.
[0014] Compared with the prior art, the advantages of the present invention are:
[0015] This invention, through alloy composition design and manufacturing process control, can improve the martensitic matrix and M... 23 The C6 carbide and Laves phase exhibit thermal stability during high-temperature creep, improving the high-temperature strength and service life of martensitic heat-resistant steel. Furthermore, the alloy content is low, and no expensive Co element is added, significantly reducing costs. Attached Figure Description
[0016] Appendix Figure 1 This is a transmission electron microscope image of the heat-resistant steel manufactured in Example 1 after being subjected to 10,000 hours at 650°C.
[0017] Appendix Figure 2 This is a transmission electron microscope image of the heat-resistant steel manufactured in Comparative Example 1 after being subjected to 10,000 hours at 650°C. Detailed Implementation
[0018] The composition and manufacturing process design principles of this invention will be introduced below.
[0019] The inventors' research revealed that the recovery of the martensitic matrix, the coarsening of carbides and the Laves phase in martensitic heat-resistant steel are the main reasons for the decrease in strength during long-term high-temperature service. Existing martensitic heat-resistant steels contain excessive amounts of C and alloying elements, leading to... 23 Excessive precipitation and severe coarsening of the C6 and Laves phases not only reduce the solid solution strengthening effect but also impair high-temperature strength and toughness.
[0020] The main innovation of this invention lies in the use of a Co-free and low C and W elemental content design, achieved through thermodynamic simulation calculations and experimental verification, thereby reducing M. 23The total amount of C6 carbide and Fe2W Laves phase precipitation is reduced, decreasing the size after coarsening. Through pre-forging holding, forging, and solution tempering, carbide precipitation strengthening is regulated, compensating for the strength decrease caused by the reduction of alloying elements, and hindering martensite recovery and Laves phase coarsening, thereby improving high-temperature strength. Based on the aforementioned principles, the role of each element in this invention is explained.
[0021] C promotes martensitic phase transformation and M 23 Elements that precipitate C6 carbides and M(C,N) carbonitrides. Too low a C content will reduce the strength of the martensitic matrix and decrease the precipitation of carbonitrides, while too high a C content will result in excessive precipitates and accelerate coarsening, both of which reduce high-temperature strength. Therefore, the C content is 0.04-0.08%.
[0022] Cr is a major alloying element in martensitic heat-resistant steel, which can improve high-temperature strength, corrosion resistance, and oxidation resistance. In addition, the Cr content can be controlled by combining it with deformation heat treatment processes. 23 C6 carbide precipitation promotes the nucleation of (Fe,W)6C and the Laves phase. If the Cr content is too low, high-temperature strength and high-temperature oxidation resistance cannot be guaranteed; if the Cr content is too high, coarse Cr particles are easily formed. 23 C6 carbides also reduce high-temperature strength; therefore, the Cr content is 8.0–9.5%.
[0023] Mo and W mainly play a role in solid solution strengthening and can also inhibit M. 23 While C6 carbides are coarsened, W tends to form Fe2W-type Laves phases at high temperatures, which impairs toughness and affects service stability. Therefore, the Mo content is controlled at 0.3–0.8%, and the W content is controlled at 0.5–1.2%.
[0024] V and Nb can form M(C,N) carbonitrides, which are important elements for precipitation strengthening and hindering the recovery of the martensitic matrix. If the content of V and Nb is too low, the strengthening effect will not be obvious; if the content is too high, it will lead to coarsening of the carbonitrides and cause elemental segregation. Therefore, the V content should be controlled at 0.2-0.35%, and the Nb content at 0.02-0.06%.
[0025] Mn and Ni are elements that strengthen the matrix and increase the Ni equivalent. Reasonable content can ensure that the microstructure is full martensite. The Mn content is controlled at 0.75-1.0%, and the Ni content is controlled at 1.0-2.0%.
[0026] Si can strongly inhibit the coarsening of carbonitrides and help improve high-temperature oxidation resistance, but excessive content will lead to excessive precipitation of δ-ferrite and Laves phase. Therefore, the Si content should be controlled between 0.9% and 1.3%.
[0027] Nitrogen (N) can strengthen the matrix and promote precipitation strengthening. Excessive N content will form coarse primary nitrides during steel solidification, which cannot be eliminated during subsequent deformation heat treatment, thus worsening toughness. Insufficient N content will result in insufficient matrix strength. Therefore, the N content should be controlled between 0.005% and 0.02%.
[0028] This invention discloses a method for manufacturing a high-strength, high-toughness, low-W, Co-free martensitic heat-resistant steel, which specifically includes the following steps:
[0029] 1) The ingredients are prepared according to the chemical element content specified in this invention, and the double vacuum melting is carried out by VIM vacuum induction melting + VAR consumable electrode melting, and then cast into ingots.
[0030] 2) Heat the ingot to 1080-1150℃ for pre-forging heat preservation, and ensure that the heat preservation time of the ingot after heat preservation is ≥16h. Then forge, control the final forging temperature to be 860-920℃, the forging ratio to be 2.0-4.0, and water cool after forging.
[0031] 3) The forged billet is solution-treated at 1000-1050℃ for 40-120 min and then water-cooled, followed by tempering at 720-780℃ for ≥60 min.
[0032] The effect of the deformation heat treatment in this invention will be explained next.
[0033] Holding the ingot at 1080–1150℃ before forging, and ensuring a holding time of ≥16 hours after heat penetration, allows most carbides to dissolve. Only a small amount of undissolved NbC, NbN, and VN are coarsened to 200–300 nm by Oswald ripening. These coarser carbides and nitrides can pinningly hinder the growth of recrystallized austenite, refining the grains after forging and solution treatment. Furthermore, the small number of these coarse carbides does not significantly negatively impact strength and toughness. A forging ratio of 2.0–4.0 further refines the grains. Post-forging water cooling inhibits supersaturated carbide precipitation.
[0034] After forging, solution treatment at 1000–1050℃ for 40–120 min can redissolve the carbides induced by deformation during forging and those supersaturated during post-forging cooling, thus reducing M. 23 C6 carbides precipitate in large quantities at grain boundaries, preventing excessive coarsening of austenite grains. Subsequently, tempering at 720–780℃ for ≥60 min causes M... 23 C6 and MC carbides precipitate in large quantities at the dislocation and martensite lath boundaries. MC carbides can hinder martensite lath recovery, while M... 23 C6 carbides promote the nucleation of (Fe,W)6C carbides and Fe2WLaves phases, increasing their quantity and reducing the supersaturation of W in the matrix. As a result, the coarsening rate of the Laves phase decreases during long-term service.
[0035] To enable those skilled in the art to fully understand the technical solution and beneficial effects of the present invention, the following detailed description is provided in conjunction with specific embodiments.
[0036] Example 1
[0037] The chemical composition of the smelted billet is C: 0.05, Cr: 9.2, Mo: 0.55, W: 0.6, V: 0.3, Nb: 0.036, Mn: 0.8, Ni: 1.4, Si: 1.1, N: 0.014.
[0038] Before forging, the billet was held at 1130℃ for 24 hours after heat penetration. Forging was then carried out at a final forging temperature of 900℃ with a forging ratio of 3.5. After forging, the billet was water-cooled. Following forging, it was solution-treated at 1050℃ for 80 minutes and tempered at 750℃ for 120 minutes. The room temperature yield strength was 646 MPa, the tensile strength was 766 MPa, the impact energy was 230 J, and the critical stress for creep at 650℃ was 95.4 MPa.
[0039] The microstructure of the heat-resistant steel of this embodiment after 10,000 hours of calorific treatment at 650°C was analyzed using transmission electron microscopy. The results are as follows: Figure 1 As shown, the martensite laths are clearly visible, and the carbides and Laves phases are mainly distributed at the boundaries of the martensite laths. Their small size indicates that the carbides and the martensite matrix have good thermal stability, ensuring thermal strength.
[0040] Example 2
[0041] The chemical composition of the smelted billet is C: 0.08, Cr: 9.0, Mo: 0.55, W: 1.2, V: 0.27, Nb: 0.049, Mn: 0.92, Ni: 1.2, Si: 1.2, N: 0.007.
[0042] Before forging, the billet was held at 1140℃ for 24 hours after heat penetration. Forging was then carried out at a final forging temperature of 920℃ with a forging ratio of 4.0. After forging, the billet was water-cooled. Following forging, it was solution-treated at 1050℃ for 80 minutes and tempered at 780℃ for 120 minutes. The room temperature yield strength was 661 MPa, the tensile strength was 774 MPa, the impact energy was 212 J, and the critical stress for creep at 650℃ was 96.8 MPa.
[0043] Example 3
[0044] The chemical composition of the smelted billet is C: 0.04, Cr: 9.4, Mo: 0.55, W: 0.51, V: 0.33, Nb: 0.05, Mn: 0.83, Ni: 1.8, Si: 1.1, N: 0.013.
[0045] Before forging, the billet was held at 1080℃ for 24 hours after heat penetration. Forging was then carried out at a final forging temperature of 860℃ with a forging ratio of 2.0. After forging, the billet was water-cooled. Following forging, it was solution-treated at 1050℃ for 80 minutes and tempered at 780℃ for 120 minutes. The room temperature yield strength was 625 MPa, the tensile strength was 740 MPa, the impact energy was 203 J, and the critical stress for creep at 650℃ was 94.2 MPa.
[0046] Comparative Example 1
[0047] The chemical composition of the smelted billet is C: 0.12, Cr: 9.0, Mo: 0.34, W: 2.5, V: 0.3, Nb: 0.06, Mn: 0.92, Ni: 0.8, Si: 0.9, N: 0.07.
[0048] Before forging, the billet is held at 1100℃ for 24 hours after heat penetration. Then, forging is carried out with a final forging temperature of 880℃ and a forging ratio of 3.0. After forging, it is water-cooled. After forging, it is solution-treated at 1050℃ for 120 minutes and tempered at 780℃ for 100 minutes.
[0049] The microstructure of the heat-resistant steel in this comparison after 10,000 hours of intensive treatment at 650°C is as follows: Figure 2 As shown, the C and W content is too high, the martensite is fully recovered, the lath structure is basically gone, the carbide and Laves phase are large in size, the room temperature yield strength is 682 MPa, the tensile strength is 783 MPa, the impact absorption energy is 252 J, and the critical stress for creep at 650℃ is 90 MPa.
[0050] Comparative Example 2
[0051] The chemical composition of the smelted billet is C: 0.03, Cr: 9.5, Mo: 0.76, W: 1.18, V: 0.32, Nb: 0.06, Mn: 0.76, Ni: 1.6, Si: 1.2, N: 0.015.
[0052] Before forging, the billet is held at 1090℃, and the holding time after heat penetration is controlled to be 24 hours. Then, forging is carried out, and the final forging temperature is controlled to be 880℃ with a forging ratio of 3.0. After forging, it is water-cooled. After forging, it is solution-treated at 1050℃ for 80 minutes and tempered at 770℃ for 120 minutes.
[0053] The C content is too low, resulting in insufficient martensitic matrix strength and carbide quantity. The room temperature yield strength is 586 MPa, the tensile strength is 647 MPa, the impact absorption energy is 194 J, and the critical stress for creep at 650℃ is 83 MPa.
[0054] Comparative Example 3
[0055] The chemical composition of the smelted billet is C: 0.08, Cr: 9.4, Mo: 0.5, W: 0.81, V: 0.25, Nb: 0.04, Mn: 0.68, Ni: 1.0, Si: 0.9, N: 0.02.
[0056] Before forging, the billet is held at 1150℃, and the holding time after heat penetration is controlled to be 2 hours. Then, forging is carried out, and the final forging temperature is controlled at 880℃ with a forging ratio of 3.0. After forging, it is water-cooled. After forging, it is solution-treated at 1000℃ for 120 minutes and tempered at 750℃ for 200 minutes.
[0057] If the pre-forging holding time is too short, the carbides and nitrides cannot be fully dissolved, which reduces the precipitation strengthening effect and the hindering effect on the recovery of martensite laths. The room temperature yield strength is 622 MPa, the tensile strength is 724 MPa, the impact absorption energy is 201 J, and the critical stress for creep at 650℃ is 80 MPa.
Claims
1. A high-strength, high-toughness, low-W, Co-free martensitic heat-resistant steel, characterized in that, Its chemical composition, by mass percentage, is C: 0.04~0.08, Cr: 8.0~9.5, Mo: 0.3~0.8, W: 0.5~1.2, V: 0.2~0.35, Nb: 0.02~0.06, Mn: 0.75~1.0, Ni: 1.0~2.0, Si: 0.9~1.3, N: 0.005~0.02, with the remainder being Fe and unavoidable impurities; The preparation steps of the high-strength, high-toughness, low-W, Co-free martensitic heat-resistant steel are as follows: 1) Molten steel is obtained by double vacuum smelting and then cast into ingots; 2) Forging the ingot; 3) The forged billet is subjected to solution treatment and tempering; In step 2), the ingot is preheated before forging, and the preheating temperature is 1080~1150℃. After the ingot is fully heated, the preheating time is ≥16h. In step 2), the final forging temperature after forging is 860~920℃, the forging ratio is 2.0~4.0, and water cooling is performed after forging; The solution treatment temperature is 1000~1050℃, the solution holding time is 40~120min, and the solution is cooled by water after solution treatment. The tempering temperature is 720~780℃, and the tempering holding time is ≥60min.
2. A method for manufacturing high-strength, high-toughness, low-W, Co-free martensitic heat-resistant steel as described in claim 1, characterized in that, The forging and solution tempering process includes the following steps: 1) Molten steel is obtained by double vacuum smelting and then cast into ingots; 2) Forging the ingot; 3) The forged billet is subjected to solution treatment and tempering; In step 2), the ingot is preheated before forging, and the preheating temperature is 1080~1150℃. After the ingot is fully heated, the holding time is ≥16h. In step 2), the final forging temperature after forging is 860~920℃, the forging ratio is 2.0~4.0, and water cooling is performed after forging; The solution treatment temperature is 1000~1050℃, the solution holding time is 40~120min, and the solution is cooled by water after solution treatment. The tempering temperature is 720~780℃, and the tempering holding time is ≥60min.
Citation Information
Patent Citations
12% cr heat resisting steel
JP1986006256A
Rotor shaft for steam turbine, steam turbine power generating plant, and steam turbine thereof
JP1997287402A